Etching composition for silicon nitride film and method for etching silicon nitride film using the same

The silicon nitride film etching composition with phosphoric acid and specific compounds addresses bubble generation and selectivity issues, enhancing the efficiency and control of silicon nitride film etching processes.

JP2024169359AInactive Publication Date: 2024-12-05SAMSUNG SDI CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024082405
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-25
Filing Date
2024-05-21
Publication Date
2024-12-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing silicon nitride film etching processes generate bubbles due to physical friction, leading to inefficiencies and challenges in achieving the required etching selectivity ratio for silicon nitride and silicon oxide films.

Method used

A silicon nitride film etching composition comprising phosphoric acid, a compound represented by chemical formula 1, a compound represented by chemical formula 2, and water, with specific ratios and contents, is used to reduce bubble generation and enhance etching selectivity.

Benefits of technology

The composition effectively suppresses bubble formation, improves etching selectivity, and reduces the time required to reach etching temperature, ensuring efficient and controlled etching of silicon nitride films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169359000011
    Figure 2024169359000011
  • Figure 2024169359000001
    Figure 2024169359000001
  • Figure 2024169359000002
    Figure 2024169359000002
Patent Text Reader

Abstract

To provide: an etching composition for a silicon nitride film, the etching composition enabling reduction of bubbles caused by physical friction; and a method for etching the silicon nitride film using the etching composition.SOLUTION: An etching composition for a silicon nitride film is provided, including: phosphoric acid; a compound represented by the following chemical formula 1; a compound represented by the following chemical formula 2; and water, and the content of the water is 11 mass% to 16 mass% based on the total mass of the etching composition for a silicon nitride film, and a ratio of an area of a peak derived from Si-ORa (Ra is a substituted or unsubstituted alkyl group) to an area of a peak derived from Si-CH3 measured by 1H-NMR spectrum is 2 to 16.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composition for etching a silicon nitride film and a method for etching a silicon nitride film using the same. [Background technology]

[0002] Various semiconductor manufacturing processes require a selective etching process for a silicon nitride film. Recently, in the manufacturing process of V-NAND, a process for selectively removing only a silicon nitride film in a structure in which a silicon nitride film and a silicon oxide film are alternately stacked, and an etching composition for realizing such a process, have been actively developed. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Korean Patent Publication No. 10-2020-0119668 Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide a composition for etching a silicon nitride film that can reduce bubbles generated by physical friction.

[0005] Another object of the present invention is to provide an etching method using the above-mentioned composition for etching a silicon nitride film. [Means for solving the problem]

[0006] A composition for etching a silicon nitride film according to one embodiment of the present invention includes phosphoric acid, a compound represented by the following chemical formula 1, a compound represented by the following chemical formula 2, and water, and the content of the water is 11% by mass to 16% by mass based on the total mass of the composition for etching a silicon nitride film, 1Si-CH as measured by H-NMR spectroscopy 3 The area of ​​the peak due to Si-OR a (where R a is a substituted or unsubstituted alkyl group) is a substituted or unsubstituted alkyl group) having a ratio of the area of ​​the peak derived from the substituted or unsubstituted alkyl group to the area of ​​the peak derived from the substituted or unsubstituted alkyl group of 2 to 16:

[0007] [ka]

[0008] In the above chemical formula 1, R 1 and R 2 each independently represents a hydrogen atom, a deuterium atom, or a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, R 3 each independently represents a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a and b are each independently an integer of 0 to 2, and 0≦a+b≦2;

[0009] [ka]

[0010] In the above chemical formula 2, R 5 and R 6 each independently represents a hydrogen atom, a deuterium atom, an unsubstituted alkyl group having 1 to 10 carbon atoms, or a group in which at least one hydrogen atom is -NR c R d or at least one -CH 2 - -NR e is an alkyl group having 2 to 10 carbon atoms substituted with -; R 7 teeth, (i) at least one hydrogen atom is -NR f R g an alkyl group having 1 to 10 carbon atoms substituted with (ii) at least one -CH 2 - -NR h is an alkyl group having 2 to 10 carbon atoms substituted with -; In this case, R c ~R h each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 5 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 10 carbon atoms, a substituted or unsubstituted aryl group having 6 to 10 carbon atoms, or a combination thereof; R 8 is a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, c and d each independently represents an integer of 0 to 2, provided that 0≦c+d≦2.

[0011] R in the above Chemical Formula 1 1 ~R 3 is preferably each independently a substituted or unsubstituted alkyl group having 1 to 5 carbon atoms.

[0012] R in the above Chemical Formula 1 3 is preferably a methyl group, an ethyl group, or a propyl group.

[0013] In the above chemical formula 1, a+b is preferably 0.

[0014] R in the above chemical formula 2 5 ~R 7 are each independently (i) at least one hydrogen atom is -NR f R g an alkyl group having 1 to 10 carbon atoms substituted with (ii) at least one -CH 2 - -NR h is an alkyl group having 2 to 10 carbon atoms substituted with -; It is preferred.

[0015] Above R c ~R hIt is preferable that each of the is independently a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 5 carbon atoms, or a combination thereof.

[0016] In the above chemical formula 2, c+d is preferably 0.

[0017] The content of the water is preferably 12% by mass to 15% by mass based on the total mass of the composition.

[0018] The above Si-CH 3 The area of ​​the peak due to Si-OR a (where R a The ratio of the areas of the peaks derived from the groups (wherein m is a substituted or unsubstituted alkyl group) is preferably 2 to 10.

[0019] The content of the compound represented by the above chemical formula 1 is preferably 0.3 mass % to 10 mass % based on the total mass of the composition for etching silicon nitride film.

[0020] The content of the compound represented by the above chemical formula 2 is preferably 0.5% by mass to 30% by mass based on the total mass of the composition for etching silicon nitride film.

[0021] According to another embodiment, there is provided a method for etching a silicon nitride film, comprising contacting a silicon nitride film surface with a silicon nitride film etching composition according to an embodiment of the present invention. Effect of the Invention

[0022] According to the present invention, there is provided a composition for etching a silicon nitride film that can reduce bubbles generated by physical friction. [Brief description of the drawings]

[0023] [Figure 1] 1 is a 1H-NMR spectrum of the silicon nitride film etching composition according to Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to exemplary embodiments thereof, so that those skilled in the art can easily practice the present invention. However, the present invention may be embodied in many different forms and is not limited to the embodiments set forth herein.

[0025] Hereinafter, unless otherwise defined in this specification, "substituted" means that a hydrogen atom in a compound is replaced with a deuterium atom, a halogen atom (F, Br, Cl, or I), a hydroxy group, a nitro group, a cyano group, an amino group, an azide group, an amidino group, a hydrazino group, a hydrazono group, a carbonyl group, a carbamoyl group, a thiol group, an ester group, a carboxy group or a salt thereof, a sulfonic acid group or a salt thereof, a phosphate group or a salt thereof, an alkyl group having 1 to 30 carbon atoms, an alkoxy group having 2 to 30 carbon atoms, or a cyclic group having 2 to 30 carbon atoms. It means that the alkyl group is substituted with a substituent selected from the group consisting of an aryl group, an alkynyl group having 2 to 30 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, an alkoxy group having 1 to 30 carbon atoms, a heteroalkyl group having 1 to 20 carbon atoms, a heteroarylalkyl group having 3 to 20 carbon atoms, a cycloalkyl group having 3 to 30 carbon atoms, a cycloalkenyl group having 3 to 15 carbon atoms, a cycloalkynyl group having 6 to 15 carbon atoms, a heterocyclic group having 2 to 30 carbon atoms, and combinations thereof.

[0026] In addition, two adjacent substituents among the substituted halogen atoms (F, Br, Cl, or I), hydroxy groups, nitro groups, cyano groups, amino groups, azide groups, amidino groups, hydrazino groups, hydrazono groups, carbonyl groups, carbamoyl groups, thiol groups, ester groups, carboxy groups or salts thereof, sulfonic acid groups or salts thereof, phosphate groups or salts thereof, alkyl groups having 1 to 30 carbon atoms, alkenyl groups having 2 to 30 carbon atoms, alkynyl groups having 2 to 30 carbon atoms, aryl groups having 6 to 30 carbon atoms, arylalkyl groups having 7 to 30 carbon atoms, alkoxy groups having 1 to 30 carbon atoms, heteroalkyl groups having 1 to 20 carbon atoms, heteroarylalkyl groups having 3 to 20 carbon atoms, cycloalkyl groups having 3 to 30 carbon atoms, cycloalkenyl groups having 3 to 15 carbon atoms, cycloalkynyl groups having 6 to 15 carbon atoms, or heterocyclic groups having 2 to 30 carbon atoms may be condensed to form a ring.

[0027] As used herein, the term "aryl group" refers to a group having one or more aromatic hydrocarbon moieties, and broadly includes aromatic hydrocarbon moieties linked by single bonds, as well as non-aromatic fused rings to which aromatic hydrocarbon moieties are directly or indirectly fused. Aryl groups include monocyclic, polycyclic, or fused polycyclic (i.e., rings which share adjacent pairs of carbon atoms) functional groups.

[0028] More specifically, the substituted or unsubstituted aryl group may be, but is not limited to, a substituted or unsubstituted phenyl group, a substituted or unsubstituted naphthyl group, a substituted or unsubstituted anthracenyl group, a substituted or unsubstituted phenanthryl group, a substituted or unsubstituted naphthacenyl group, a substituted or unsubstituted pyrenyl group, a substituted or unsubstituted biphenyl group, a substituted or unsubstituted terphenyl group, a substituted or unsubstituted quaterphenyl group, a substituted or unsubstituted chrysenyl group, a substituted or unsubstituted triphenylenyl group, a substituted or unsubstituted perylenyl group, a combination thereof, or a condensed form of a combination thereof.

[0029] Unless otherwise specified herein, "combination" means blending or copolymerization.

[0030] In the past, in semiconductor manufacturing processes, a phosphoric acid solution heated to a high temperature has been used as an etching solution to remove silicon nitride film patterns formed on substrates. However, if this etching solution is used as is, not only the silicon nitride film but also the silicon oxide film is etched, which causes a problem that the etching selectivity of silicon nitride film / silicon oxide film required in the process cannot be satisfied. In order to solve this problem, active research is being conducted on various additives to be used with phosphoric acid.

[0031] In order to increase the etching selectivity of the silicon nitride film relative to the silicon oxide film, a silane-based compound may be used together with the phosphoric acid solution. When a silane-based compound is contained in a composition for etching a silicon nitride film, the etching selectivity can be improved, but if the content of the silane-based compound is high, bubbles may be generated due to physical friction, which may be disadvantageous in terms of the efficiency of the etching process. Therefore, it is required that the composition for etching a silicon nitride film contains a silane-based compound to improve the etching selectivity, while suppressing the generation of bubbles or quickly removing the generated bubbles.

[0032] The composition for etching a silicon nitride film according to the present invention contains phosphoric acid, a compound represented by the following chemical formula 1, a compound represented by the following chemical formula 2, and water, and the content of water is 11 mass% to 16 mass% based on the total mass of the composition for etching a silicon nitride film, 1 Si-CH as measured by H-NMR spectroscopy 3 The area of ​​the peak due to Si-OR a (where R a is a substituted or unsubstituted alkyl group) is 2 to 16 in terms of the area ratio of the peak derived from the alkyl group.

[0033] [ka]

[0034] In the above chemical formula 1, R 1 and R 2 each independently represents a hydrogen atom, a deuterium atom, or a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, R 3 each independently represents a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a and b are each independently an integer of 0 to 2, and 0≦a+b≦2;

[0035] [ka]

[0036] In the above chemical formula 2, R 5 and R 6 each independently represents a hydrogen atom, a deuterium atom, an unsubstituted alkyl group having 1 to 10 carbon atoms, or a group in which at least one hydrogen atom is -NR c R d or at least one -CH 2 - -NR e is an alkyl group having 2 to 10 carbon atoms substituted with -; R 7 teeth, (i) at least one hydrogen atom is -NR f R g an alkyl group having 1 to 10 carbon atoms substituted with (ii) at least one -CH 2 - -NR h an alkyl group having 2 to 10 carbon atoms substituted with -; and In this case, R c ~R h each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 5 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 10 carbon atoms, a substituted or unsubstituted aryl group having 6 to 10 carbon atoms, or a combination thereof; R 8 is a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, c and d each independently represents an integer of 0 to 2, provided that 0≦c+d≦2.

[0037] The composition for etching a silicon nitride film according to an embodiment of the present invention contains the compound represented by Chemical Formula 1 and the compound represented by Chemical Formula 2, and thus can increase the ratio of the etching rate of a silicon nitride film to the etching rate of a silicon oxide film (etching selectivity) and suppress abnormal growth of a silicon oxide film.

[0038] In addition, the silicon nitride film etching composition according to the present invention simultaneously satisfies the specific ranges of the water content and the relative content of alkoxysilyl groups to alkylsilyl groups, thereby suppressing the generation of bubbles due to friction between compounds and shortening the time required to heat the composition to an etching temperature.

[0039] R in the above Chemical Formula 1 1 ~R 3 may each independently be a substituted or unsubstituted alkyl group having 1 to 5 carbon atoms. More specifically, they may be, for example, a substituted or unsubstituted methyl group, a substituted or unsubstituted ethyl group, or a substituted or unsubstituted propyl group, but are not limited thereto.

[0040] The sum of a and b in the above Chemical Formula 1 may be 0 or 1, for example, 0, but is not limited thereto.

[0041] R in the above chemical formula 2 5 ~R 7 are each independently (i) at least one hydrogen atom is -NR f R g an alkyl group having 1 to 10 carbon atoms substituted with (ii) at least one -CH 2 - -NR h It may be an alkyl group having 2 to 10 carbon atoms substituted with -.

[0042] For example, R in the above formula 2 5 ~R 7 are each independently (iii) at least one hydrogen atom is -NR f R g an alkyl group having 1 to 5 carbon atoms substituted with (iv) at least one -CH 2 - -NR h It can be an alkyl group having 2 to 5 carbon atoms substituted with -, but is not limited thereto.

[0043] R in the above Chemical Formula 1 and Chemical Formula 2 c ~R h may each independently be a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 5 carbon atoms, a substituted or unsubstituted aryl group having 6 to 10 carbon atoms, or a combination thereof, for example, a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 5 carbon atoms, or a combination thereof, but is not limited to these.

[0044] The sum of c and d in the above Chemical Formula 2 can be 0 or 1, for example, 0, but is not limited thereto.

[0045] 1 In the H-NMR spectrum, Si-CH 3 The area of ​​the peak due to Si-OR a (where R a is a substituted or unsubstituted alkyl group) may be 2 to 16, for example, 3 to 16, for example, 4 to 16, for example, 4 to 15, for example, 4 to 14, for example, 4 to 13, for example, 4 to 12, for example, 4 to 11, for example, 4 to 10, but is not limited thereto. 3 The area of ​​the peak due to Si-OR a When the area ratio of the peak derived from is within the above range, the generation of bubbles due to friction between the compounds can be suppressed, and the time required to heat the composition to the etching temperature can be shortened.1 The H-NMR measurement can be carried out according to the methods and conditions described in the Examples.

[0046] The content of water is 11% by mass to 16% by mass based on the total mass of the silicon nitride film etching composition, for example, 11.5% by mass to 15% by mass, for example, 12% by mass to 15% by mass, for example, 12% by mass to 14.5% by mass, for example, 12% by mass to 14% by mass, for example, 12% by mass to 13.8% by mass, for example, 12% by mass to 13.5% by mass, for example, 12% by mass to 13% by mass, but is not limited thereto. If the content of water is within the above range, it is possible to suppress the generation of bubbles due to friction between compounds, and shorten the time required to heat the silicon nitride film etching composition to the etching temperature.

[0047] The above 1 By simultaneously satisfying the above ranges for the peak area ratio of the H-NMR spectrum and the water content in the composition for etching silicon nitride film, the effect of the composition according to the present invention can be maximized.

[0048] The content of the compound represented by the above chemical formula 1 is 0.3 mass% to 10 mass% based on the total mass of the silicon nitride film etching composition, for example, 0.5 mass% to 10 mass%, for example, 1 mass% to 10 mass%, for example, 2 mass% to 10 mass%, for example, 3 mass% to 10 mass%, for example, 3 mass% to 9 mass%, for example, 3 mass% to 8 mass%, and is not limited thereto. When the content of the compound represented by the chemical formula 1 is within the above range, the etching selectivity can be optimized.

[0049] The content of the compound represented by the above chemical formula 2 in the silicon nitride film etching composition according to the present invention may be, for example, 0.5 mass% to 30 mass%, for example, 0.5 mass% to 25 mass%, for example, 0.5 mass% to 20 mass%, for example, 1 mass% to 30 mass%, for example, 1 mass% to 25 mass%, for example, 1 mass% to 20 mass%, for example, 1 mass% to 15 mass%, based on the total mass of the silicon nitride film etching composition, but is not limited thereto. If the content of the compound represented by the chemical formula 2 is within the above range, the etching selectivity can be optimized while suppressing the abnormal growth of the silicon oxide film.

[0050] According to another embodiment, there is provided an etching method using the silicon nitride film etching composition.

[0051] The etching method may include, for example, contacting a silicon nitride film etching composition according to an embodiment of the present invention with a substrate having a silicon nitride film formed thereon.

[0052] The etching method according to the present invention may further include, after the contacting step, removing the silicon nitride film etching composition.

[0053] The substrate on which the silicon nitride layer is formed may further include a silicon oxide layer.

[0054] For example, the substrate is not particularly limited as long as it is one that is commonly used in the technical field, and may be, for example, a semiconductor wafer.

[0055] The step of contacting the silicon nitride film etching composition with the substrate on which the silicon nitride film is formed may include, but is not limited to, immersing the substrate on which the silicon nitride film is formed in an etching bath containing the silicon nitride film etching composition, or spraying the silicon nitride film etching composition onto the substrate on which the silicon nitride film is formed.

[0056] In one embodiment of the present invention, the method may further include a step of heating the silicon nitride film etching composition before the step of contacting the silicon nitride film etching composition with a substrate on which a silicon nitride film is formed. The silicon nitride film etching composition may be heated at a temperature of 100° C. or higher, for example, 100° C. to 500° C. For example, the silicon nitride film etching composition may be heated at a temperature of 150° C. to 300° C., but is not limited thereto.

[0057] By using the silicon nitride film etching composition according to the present invention, the time required for heating the silicon nitride film etching composition to the above temperature in the step of heating the silicon nitride film etching composition can be shortened.

[0058] The etching method may further include a step of drying the substrate from which the silicon nitride film has been removed, after etching with the silicon nitride film etching composition.

[0059] When a substrate containing a silicon nitride film and a silicon oxide film is etched using the composition for etching a silicon nitride film according to the present invention, the etching selectivity of the silicon nitride film to the silicon oxide film can be improved and the occurrence of abnormal growth of the silicon oxide film can be suppressed. EXAMPLES

[0060] The present invention will be described in more detail below with reference to examples of the above-mentioned composition for etching silicon nitride film, but the technical scope of the present invention is not limited to the following examples.

[0061] [Production of silicon nitride film etching composition] (Examples 1 to 10) Methyltrimethoxysilane (alkoxysilane) and 3-aminopropyltriethoxysilane (aminosilane) were dissolved in deionized water (DIW), and the solution was decompressed to reduce the concentration of the alkoxysilane. Phosphoric acid was then added to prepare a composition for etching silicon nitride film according to the embodiment. The specific contents of deionized water, alkoxysilane, aminosilane, and phosphoric acid and 1 H-NMR of Si-CH 3 The area of ​​the peak due to Si-OR a (where R a The area ratio of the peaks derived from the group (wherein is a substituted or unsubstituted alkyl group) is shown in Table 1 below. 1 The H-NMR spectrum is shown in Figure 1.

[0062] In addition, 1 The measurement conditions for H-NMR are as follows: Si-CH 3 The chemical shift of the peak due to Si-OR appears at 0.2 ppm. a The chemical shifts of the peaks originating from the above appear at 3.8 ppm, 3.5 ppm, 3.4 ppm, 3.2 ppm, and 0.9 ppm.

[0063] < 1 H-NMR measurement conditions> NMR instrument: AVANCE III 300 (Bruker) Resonance frequency: 300MHz Total: 16 times Measurement solvent: CDCl 3 Reference substances and chemical shifts of reference peaks: Tetramethylsilane (TMS), 0 ppm Sample concentration: [CDCl 3 :sample = 1:1 (mass ratio)].

[0064] (Comparative Examples 1 to 4) The composition according to Comparative Example 1 was an aqueous phosphoric acid solution, and the compositions according to Comparative Examples 2 to 4 contained phosphoric acid, alkoxysilane, aminosilane, and DIW in the following amounts, as shown in Table 1 below.

[0065] [Table 1]

[0066] [Evaluation 1: Evaluation of reduction in air bubble volume] 15 g of the silicon nitride film etching compositions according to Comparative Examples 1 to 4 and Examples 1 to 10 were placed in a 20 mL vial and shaken up and down in the same way 40 times. The vial was then placed on a piece of paper with text written on it to check whether the text could be seen. When the composition was shaken, air bubbles were generated in the composition due to physical friction, and the degree to which the air bubbles remained over time after shaking, that is, the degree to which the text could be seen, was observed to evaluate the degree to which the air bubbles were removed. The results are shown in Table 2 below. In Table 2 below, "○" means that there were no or a small amount of air bubbles and the characters were clearly distinguishable, "△" means that there were some air bubbles and only some of the characters could be distinguished, and "×" means that there were a large amount of air bubbles or the solution was frozen, making it difficult to distinguish the characters.

[0067] [Table 2]

[0068] Referring to Table 2 above, it can be seen that the compositions according to Examples 1 to 9 either had a small amount of bubbles or no bubbles, and even if bubbles were generated, the amount of bubbles decreased within one minute. On the other hand, the compositions according to Comparative Examples were either had a large amount of bubbles or crystallized. The composition according to Comparative Example 4 was confirmed to have agglomerated silane compounds.

[0069] [Evaluation 2: Etching rate, etching selectivity, and etching by-products] The silicon nitride film etching compositions produced in Examples 1 to 10 and Comparative Examples 1 to 4 were placed in a beaker and heated to the etching temperature (165°C). Then, a silicon nitride film (LP-SiN film) or a silicon oxide film (PE-SiO film) was placed in the beaker and etched for 30 minutes at the above etching temperature. The thickness of the LP-SiN film or the PE-SiO film before and after etching was measured using an ellipsometer to determine the etching rate. The ratio of the etching rate (A) of the silicon nitride film to the etching rate (B) of the silicon oxide film (etching selectivity = A / B) was calculated, and the presence or absence of by-products generated after the etching progressed was confirmed with the naked eye, and the results are shown in Table 3 below.

[0070] [Table 3]

[0071] Referring to Table 3 above, it can be seen that the compositions according to Examples 1 to 10 have excellent etching rates and etching selectivities, and do not generate by-products after the etching process.

[0072] Although specific embodiments of the present invention have been described and illustrated above, the present invention is not limited to the described embodiments, and various modifications and variations can be made without departing from the spirit and scope of the present invention, as will be apparent to those skilled in the art. Therefore, such modifications or variations should not be understood individually from the technical spirit and perspective of the present invention, and the modified embodiments should be considered to belong to the scope of the claims of the present invention.

Claims

1. A composition for etching a silicon nitride film, comprising phosphoric acid, a compound represented by the following chemical formula 1, a compound represented by the following chemical formula 2, and water, The content of the water is 11% by mass to 16% by mass based on the total mass of the composition for etching a silicon nitride film, 1 Si—CH measured by H-NMR spectrum 3 The area of ​​the peak derived from Si-OR a (Here, R a a silicon nitride film etching composition, wherein the ratio of the area of ​​the peak derived from the group consisting of 1 to 2 is 2 to 16: [Formula 1] In the above Chemical Formula 1, R 1 and R 2 are each independently a hydrogen atom, a deuterium atom, or a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, R 3 are each independently a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a and b are each independently an integer from 0 to 2, and 0≦a+b≦2; [chemical 2] In the above Chemical Formula 2, R 5 and R 6 are each independently a hydrogen atom, a deuterium atom, an unsubstituted alkyl group having 1 to 10 carbon atoms, or at least one hydrogen atom is -NR c R d or at least one -CH 2 - is -NR e is an alkyl group having 2 to 10 carbon atoms substituted with -; R 7 teeth, (i) at least one hydrogen atom is -NR f R g an alkyl group having 1 to 10 carbon atoms substituted with (ii) at least one -CH 2 - is -NR h is an alkyl group having 2 to 10 carbon atoms substituted with -; At this time, R c ~R h each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 5 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 10 carbon atoms, a substituted or unsubstituted aryl group having 6 to 10 carbon atoms, or a combination thereof; R 8 is a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, c and d each independently represents an integer of 0 to 2, provided that 0≦c+d≦2.

2. R in Formula 1 1 ~R 3 The silicon nitride film etching composition according to claim 1, wherein each of the groups is independently a substituted or unsubstituted alkyl group having 1 to 5 carbon atoms.

3. R in Formula 1 3 The silicon nitride film etching composition according to claim 1 , wherein is a methyl group, an ethyl group, or a propyl group.

4. The composition for etching a silicon nitride film according to claim 1 , wherein a+b in Formula 1 is 0.

5. R in Formula 2 5 ~R 7 are each independently (i) at least one hydrogen atom is -NR f R g an alkyl group having 1 to 10 carbon atoms substituted with (ii) at least one -CH 2 - is -NR h 2. The silicon nitride film etching composition according to claim 1, wherein the alkyl group is an alkyl group having 2 to 10 carbon atoms and substituted with -.

6. R that may be included in the above Chemical Formula 2 c ~R hand each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 5 carbon atoms, or a combination thereof.

7. The composition for etching a silicon nitride film according to claim 1 , wherein c+d in the formula (2) is 0.

8. 2. The silicon nitride film etching composition according to claim 1, wherein the content of the water is 12 mass % to 15 mass % based on the total mass of the silicon nitride film etching composition.

9. The Si—CH 3 The area of ​​the peak derived from Si-OR a (Here, R a 2. The silicon nitride film etching composition according to claim 1, wherein the ratio of the area of ​​the peak derived from the group (a) to the area of ​​the peak derived from the group (b) is 2 to 10.

10. The silicon nitride film etching composition according to claim 1, wherein the content of the compound represented by Chemical Formula 1 is 0.3 mass % to 10 mass % based on the total mass of the silicon nitride film etching composition.

11. The content of the compound represented by the chemical formula 2 is 0.5 mass% to 30 mass% based on the total mass of the composition for etching silicon nitride film.

12. A method for etching a silicon nitride film, comprising contacting a surface of the silicon nitride film with the silicon nitride film etching composition according to any one of claims 1 to 11.

Citation Information

Patent Citations

  • Chemical etching composition and application thereof

    CN115584263A

  • Selective etching solution of silicon nitride / silicon oxide 3D NAND structural sheet

    CN115873599A

  • Etchant for silicon nitride

    JP2012099550A

  • Composition for silicon nitride film etching

    JP2018182312A