Silicon compound coated-metal fine particle
By controlling the Si-OH and Si-O bond ratios in silicon compound-coated metal fine particles, the invention addresses the issue of uncontrolled properties, improving dispersibility and performance in various applications.
Patent Information
- Application Number
- JP2024159111
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2016-11-07
- Filing Date
- 2024-09-13
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2037-06-01
AI Technical Summary
Existing methods for coating metal fine particles with silicon compounds fail to control the properties effectively, leading to impaired dispersibility and reduced effectiveness in various applications due to uncontrolled coating states and ratios of Si-OH and Si-O bonds.
Control the ratio of Si-OH bonds and Si-OH bonds/Si-O bonds in silicon compound-coated metal fine particles within specific ranges (0.1% to 70% and 0.001 to 700, respectively) by treating the particles with functional group modifications and environmental adjustments.
This control enables precise management of dispersibility and other properties, enhancing the performance of silicon compound-coated metal fine particles in applications such as coatings, magnetic compositions, conductive compositions, and catalyst compositions.
Smart Images

Figure 2024169487000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to silicon compound-coated fine metal particles. [Background technology]
[0002] Metal fine particles are used in a wide variety of applications, such as magnetic materials, conductive materials, coloring materials, and catalysts, and their properties are improved by making them into fine particles of 1 μm or less, making them suitable compositions for use as dispersions, etc. However, in any application, the properties that are generated or improved by making the metal fine particles finer also make them more susceptible to explosive reactions due to sudden oxidation in the atmosphere, and they are more likely to lose the properties expected of metal fine particles due to oxidation or hydroxylation due to contact with moisture, making it difficult to make the most of the properties of the metal fine particles.
[0003] In order to solve these problems, it is effective to coat the surface of metal microparticles with a silicon compound such as silica, as described in Patent Documents 1 and 2. However, in these conventional technologies, it was difficult to control the coating state itself, and the effects originally expected of metal microparticles were compromised by coating with a silicon compound. In addition, metal microparticles coated with a silicon compound with strictly controlled properties had not been obtained, and the factors behind the properties of metal microparticles coated with a silicon compound were not clear.
[0004] Patent document 3 describes a method for producing coated particles in which the coverage rate of the particles is controlled by the amount of silica coating on the surface of the metal particles in order to control the electrical conductivity. However, in order to improve insulation, it is of course necessary to increase the coverage rate. Silicon compound-coated metal microparticles that have been treated in this way to increase the coverage rate can have problems such as a significant decrease in dispersibility in various dispersion media or failure to achieve the expected effects, and there has been a demand from the industry for silicon compound-coated metal microparticles in which the amount of silica coating on the metal microparticles is reduced as much as possible.
[0005] Regarding silica coating, Patent Document 4 describes silica-coated metal oxide particles that are further surface-treated with a hydrophobicity-imparting agent such as dimethylethoxysilane. However, there is no disclosure of silica-coated metal fine particles, and the particles are merely treated with a hydrophobicity-imparting agent to enhance the dispersibility of silica-coated metal oxide particles in oil-based dispersion media such as polyglycerin triisostearate, silicone oil, and squalane for cosmetic purposes. Patent Document 4 also describes silica-coated metal oxide particles that are further surface-treated with a hydrophobicity-imparting agent to enhance the dispersibility of silica-coated metal oxide particles in oil-based dispersion media such as polyglycerin triisostearate, silicone oil, and squalane for cosmetic purposes. -1 It is described that the peak seen in is the absorption of bending vibration of Si-OH, but it should usually be attributed to Si-O bond, and the description of Si-OH is an obvious misprint. In addition, the ratio of the two different peaks in the infrared absorption spectrum described in Patent Document 4 is clearly unrelated to the properties of silica-coated metal fine particles, and therefore Patent Document 4 also does not find any effect of the ratio of Si-OH bonds contained in the silica-coated metal oxide or the ratio of Si-OH bonds to the ratio of Si-O bonds on the properties of the fine particles, and no silicon compound-coated metal fine particles with strictly controlled properties have been obtained.
[0006] Patent Document 5 by the applicant of the present application describes a method for producing uniform metal fine particles by precipitating various nanoparticles such as metal fine particles and magnetic fine particles between relatively rotating processing surfaces that can approach and separate from each other. However, Patent Document 5 describes the production of uniform metal fine particles, but does not describe silicon compound-coated metal fine particles, and of course, does not describe the control of the properties of these silicon compound-coated metal fine particles, particularly the dispersibility of silicon compound-coated metal fine particles by controlling the Si-O bond or Si-OH bond contained in the silicon compound. In other words, there is no description of controlling the properties exhibited by the silicon compound-coated metal fine particles, and silicon compound-coated metal fine particles with strictly controlled properties have been desired. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2008-264611 A [Patent Document 2] JP 2007-088156 A [Patent Document 3] JP 2011-219869 A [Patent Document 4] International Publication No. 2000 / 042112 Brochure [Patent Document 5] International Publication No. 2009 / 008393 Brochure Summary of the Invention [Problem to be solved by the invention]
[0008] In light of these circumstances, the present invention aims to provide silicon compound-coated metal fine particles with controlled properties. That is, the present invention aims to maximize the properties expected of metal fine particles and to compensate for such properties by coating metal fine particles with a silicon compound and controlling the properties. The present invention utilizes the fact that the ratio of Si-OH bonds or the ratio of the Si-OH bonds / Si-O bonds in the coated silicon compound changes in the method of producing the silicon compound-coated metal fine particles or the environmental changes after production. The present inventors have found that the ratio of Si-OH bonds or the ratio of the Si-OH bonds / Si-O bonds contained in the silicon compound-coated metal fine particles can be controlled within a specific range, and that the properties such as dispersibility of the silicon compound-coated metal fine particles can be strictly controlled by controlling the ratio of the Si-OH bonds or the ratio of the Si-OH bonds / Si-O bonds within the specific range, and have completed the present invention. In light of the above circumstances, the present invention also aims to provide various compositions using silicon compound-coated metal fine particles with strictly controlled properties. [Means for solving the problem]
[0009] In other words, the present invention is a silicon compound-coated metal microparticle in which at least a portion of the surface of a metal microparticle consisting of at least one type of metal element or semi-metal element is coated with a silicon compound, and the ratio of Si-OH bonds contained in the silicon compound-coated metal microparticle is controlled to be 0.1% or more and 70% or less.
[0010] The present invention also relates to silicon compound-coated metal microparticles in which at least a portion of the surface of metal microparticles consisting of at least one type of metal element or semi-metal element is coated with a silicon compound, and the ratio of Si-OH bonds / Si-O bonds, which is the ratio of Si-OH bonds to the ratio of Si-O bonds contained in the silicon compound-coated metal microparticles, is controlled to be 0.001 or more and 700 or less.
[0011] In the present invention, the ratio of Si--OH bonds or the ratio of Si--OH bonds / Si--O bonds contained in the silicon compound-coated, fine metal particles is preferably controlled by a treatment for modifying functional groups.
[0012] In the present invention, the treatment for modifying the functional group is preferably at least one reaction selected from a substitution reaction, an addition reaction, an elimination reaction, a dehydration reaction, a condensation reaction, a reduction reaction, and an oxidation reaction.
[0013] In addition, in the present invention, the silicon compound-coated metal microparticles are metal microparticles in which at least a portion of the surface of the metal microparticles is coated with a silicon compound, and it is preferable that the primary particle diameter of the metal microparticles is 1 μm or less and that the primary particle diameter of the silicon compound-coated metal microparticles is 100.5% or more and 190% or less of the primary particle diameter of the metal microparticles.
[0014] In the present invention, the silicon compound-coated fine metal particles are preferably core-shell type silicon compound-coated fine metal particles in which the entire surface of a single metal particle serving as a core is coated with a silicon compound serving as a shell.
[0015] In addition, in the present invention, the silicon compound-coated metal microparticles are formed by coating at least a portion of the surface of an agglomerate of a plurality of metal microparticles with a silicon compound, and it is preferable that the diameter of the agglomerate is 1 μm or less, and that the particle diameter of the silicon compound-coated metal microparticles is 100.5% or more and 190% or less of the diameter of the agglomerate.
[0016] In the present invention, the metal element or metalloid element preferably includes at least one selected from the group consisting of silver, copper, and nickel.
[0017] The present invention also relates to a method for producing a silicon compound-coated metal fine particle having an infrared absorption spectrum of 750 cm in wave number, the infrared absorption spectrum being measured by an attenuated total reflection method (ATR method). -1 From 1300cm -1 It is preferable that the peak is obtained by waveform separation of the peak in the region.
[0018] The present invention also relates to a method for producing a silicon compound-coated metal fine particle having an infrared absorption spectrum of 750 cm in wave number measured by an attenuated total reflection method (ATR method). -1 From 1300cm -1 The peak at wave number 850 cm was obtained by waveform separation. -1 From 980cm -1 The peak having the largest area ratio among the peaks derived from the Si-OH bond separated in the wave number region of 750 cm is assigned to the peak having the largest area ratio. -1 From 1300cm -1 It is preferable that the ratio is the ratio of the area of the peak assigned to the Si-OH bond to the total area of the peaks obtained by waveform separation of the peaks in the region.
[0019] The present invention also relates to a method for producing a silicon compound-coated metal fine particle having an infrared absorption spectrum of 750 cm in wave number measured by an attenuated total reflection method (ATR method). -1 From 1300cm -1The peaks in the region of 1000 cm were separated by waveform separation. -1 More than 1300cm -1 The peaks derived from the Si-O bond are separated into the following regions, and belong to the peak with the largest area ratio. The Si-OH bond is located at a wave number of 750 cm in the infrared absorption spectrum of the silicon compound-coated metal fine particles measured using an attenuated total reflection method (ATR method). -1 From 1300cm -1 The peak at wave number 850 cm was obtained by waveform separation. -1 From 980cm -1 It is preferable that the ratio of Si-OH bonds is the ratio of the area of the peak assigned to the Si-OH bonds to the area of the peak assigned to the Si-O bonds, which is the peak having the largest area ratio among the peaks assigned to the Si-OH bonds that have been waveform-separated in the region.
[0020] In addition, in the present invention, it is preferable that the silicon compound-coated metal microparticles are obtained by precipitating metal microparticles between relatively rotating processing surfaces that can approach and separate from each other, and continuously coating the surfaces of the metal microparticles with a silicon compound following the precipitation.
[0021] In addition, in the present invention, it is preferable that the silicon compound-coated metal microparticles contain silicon inside the metal microparticles at least before being subjected to heat treatment, and that, as a result of being subjected to heat treatment, the silicon has migrated from the inside of the metal microparticles toward the outer periphery compared to before being subjected to heat treatment.
[0022] In addition, in the present invention, it is preferable that the dispersibility of the silicon compound-coated metal microparticles in a solvent is controlled by controlling the ratio of the Si-OH bonds to be 0.1% or more and 70% or less, or the ratio of the Si-OH bonds / Si-O bonds to be 0.001 or more and 700 or less.
[0023] The silicon compound-coated metal fine particles of the present invention can be used as a coating composition, a transparent material composition, a magnetic composition, a conductive composition, a coloring composition, a reaction composition, or a catalyst composition. Effect of the Invention
[0024] According to the present invention, by controlling the ratio of Si-OH bonds or the ratio of Si-OH bonds / Si-O bonds contained in the silicon compound-coated metal fine particles, it is possible to provide silicon compound-coated metal fine particles with controlled properties such as dispersibility. By controlling the ratio of Si-OH bonds or the ratio of Si-OH bonds / Si-O bonds, it is possible to easily design compositions that are more suitable than ever for the diversifying uses and desired properties of the silicon compound-coated metal fine particles. [Brief description of the drawings]
[0025] [Figure 1] 1 shows the results of STEM mapping of the silicon compound-coated silver fine particles obtained in Example 1-1. [Diagram 2] 1 shows the results of line analysis of the silicon compound-coated silver particles obtained in Example 1-1. [Diagram 3] 1 shows the results of waveform separation in the wavenumber region of 750 cm −1 to 1300 cm −1 in the FT-IR measurement results of the silicon compound-coated silver fine particles obtained in Example 1-7. [Figure 4] 1 shows the results of XRD measurement of the silicon compound-coated silver fine particles obtained in Example 1-1. [Diagram 5] 1 is a TEM photograph taken using a collodion film prepared from the aqueous dispersion of silicon compound-coated silver particles obtained in Example 1-1. [Figure 6] 1 shows the results of STEM mapping of the silicon compound-coated silicon aluminum-doped iron microparticles obtained in Example 5-5. [Figure 7] 1 shows the results of XRD measurement of the silicon compound-coated silicon aluminum-doped iron fine particles obtained in Example 5-5. [Figure 8]FIG. 5 is a diagram showing an enlarged area where peaks were confirmed in the XRD measurement results of the silicon compound-coated silicon aluminum-doped iron microparticles obtained in Example 5-5, and comparing the peak list with the peaks of Fe (Metal) in the database. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Note that the present invention is not limited to the embodiment described below.
[0027] (Silicon compound coated metal fine particle composition-1) The silicon compound-coated metal fine particles according to the present invention are silicon compound-coated metal fine particles whose properties such as dispersibility are controlled by controlling the ratio of Si-OH bonds or the ratio of Si-OH bonds / Si-O bonds contained in the silicon compound-coated metal fine particles. The silicon compound-coated metal fine particles according to the present invention are particularly suitable for coating compositions used for coating coating films or coated bodies, transparent material compositions used for kneading or coating transparent agents such as glass, films, and transparent resins, magnetic compositions used for adding to magnetic fluids, magnetic materials, etc., conductive compositions used for adding to electronic materials, semiconductor materials, etc., coloring compositions used for coloring coating films, coated bodies, or transparent agents, and reaction compositions or catalyst compositions used as materials for various chemical reactions.
[0028] (Silicon compound coated metal fine particle composition-2) The silicon compound-coated metal fine particles according to the present invention are silicon compound-coated metal fine particles in which the ratio of Si-OH bonds contained in the silicon compound-coated metal fine particles is controlled within a range of 0.1% to 70%, or in particular, the ratio of Si-OH bonds / Si-O bonds is controlled within a range of 0.001 to 700. This makes it possible to strictly control the dispersibility in hydrophilic or lipophilic dispersion media when used in the various compositions. For example, by using silicon compound-coated metal fine particles in which the ratio of Si-OH bonds or the ratio of Si-OH bonds / Si-O bonds contained in the silicon compound-coated metal fine particles is controlled for the octanol / water partition coefficient of different dispersion media, the dispersibility in the dispersion media is strictly controlled, so that when used as a target composition, it becomes possible to fully exhibit the properties required as silicon compound metal fine particles. The present inventors have found that although it is difficult to control the ratio of Si-OH bonds or the ratio of Si-OH bonds / Si-O bonds contained in the silicon compound-coated metal fine particles when they are outside the above range, they can be very easily controlled when they are within the above range. In order to obtain a good dispersion state, silicon compounds that are usually coated are treated with various functional groups according to the dispersion medium used, and the functional groups are selected depending on whether the dispersion medium is aqueous or non-aqueous. For example, silicon compounds to which various functional groups such as phenolic hydroxyl groups, carboxyl groups, carbonyl groups, amino groups, nitro groups, sulfo groups, and alkyl groups are added are used, but the smaller the particle size, the worse the dispersion state becomes due to aggregation, and it is difficult to achieve the purpose by selecting the functional group alone. Under such circumstances, it was found that the desired dispersion state can be obtained by controlling the ratio of Si-OH bonds / Si-O bonds even when various functional groups are selected, and the present invention was completed. That is, information on various bonds can be obtained by FT-IR spectra, and in particular, the information on the bonds at wavenumbers of 750 cm -1 From 1300cm -1The desired dispersion state can be achieved by controlling the ratio of the peak areas attributable to Si-OH bonds and Si-O bonds obtained by waveform separation of the peaks in the region. It has been found that the silicon compound-coated metal fine particles can be produced with strictly controlled dispersibility in various solvents, and that the stability of the silicon compound-coated metal fine particles themselves and the storage stability in the powder state can be controlled, so that the silicon compound-coated metal fine particles can be suitably used in the various compositions described above.
[0029] (Silicon compound coated metal fine particle composition-3) In the silicon compound-coated metal fine particles according to the present invention, the ratio of Si-OH bonds contained in the silicon compound-coated metal fine particles is controlled to a range of 0.1% to 70%, or the ratio of Si-OH bonds / Si-O bonds is controlled to a range of 0.001 to 700. In addition to the dispersibility and stability, the absorption characteristics, transmission characteristics, or reflection characteristics, and plasmon characteristics for electromagnetic waves such as ultraviolet rays, visible light, and near infrared rays are controlled, so that the silicon compound-coated metal fine particles can be suitably used as a transparent agent composition for use in glass, films, transparent resins, etc., and as a coating composition such as a coating film or a coated body. In addition, when the silicon compound-coated metal fine particles, in which the surface of metal fine particles made of at least one metal element or semimetal element is coated with a silicon compound, are used as a magnetic composition, the magnetic anisotropy can be controlled in an isolated manner because they are formed of nano-sized magnetic domains insulated by the silicon compound, and as a result, the coercive force can also be controlled. In other words, it is more suitable than ever before as a magnetic composition. It is also suitable as an internal electrode for electronic components. For example, when used for the internal electrodes of multilayer ceramic capacitors, the dispersion is processed into a laminated coating film and then fired in a reducing atmosphere, during which the silicon compound migrates to the surface of the electrode and forms a thin insulating film at the boundary between the electrode layer and the dielectric layer, greatly improving the performance of the multilayer ceramic capacitor. Whether the silicon compound-coated metal fine particles are used as the magnetic composition or as an internal electrode material, slurrying is an important factor, and it is essential to make the particles in a suitable dispersion medium in a slurry state without aggregation, and the ratio of Si-OH bonds / Si-O bonds affects the state of the coating film formation and the state after firing depending on the firing conditions. Si-O bonds have a tendency to be water-repellent or lipophilic, while Si-OH bonds have a tendency to be hydrophilic, so the ratio is also a dominant factor in dispersion, and the firing temperature and firing atmosphere are also important factors in controlling the progress of water evaporation and reduction, as well as insulation.
[0030] Furthermore, in the case of silicon compound-coated metal fine particles having semiconducting properties, the semiconductor properties such as conductivity, insulation, or their temperature dependence are controlled, so that they can be suitably used in semiconductor compositions. Although the factors that enable these controls are unclear, the inventors of the present application believe that each of the Si-OH bonds or Si-O bonds contained in the surface of the particles has the property of absorbing different energy waves by vibrating, and that by controlling the ratio of Si-OH bonds or the ratio of Si-OH bonds / Si-O bonds contained in the silicon compound-coated metal fine particles, it is possible to control the type of different energy absorbed by the vibration of each of the Si-OH bonds or Si-O bonds. In addition, at the end portion of a bond where free electrons are thought to move freely between atoms, such as Si-Si between silicon elements, which are semimetals, or Si-M between silicon element (Si) and another metal element or semimetal element M, that is, at the surface of the particles, the free electrons are in an activated state because they have nowhere to go, and can always be said to be in a state where new bonds can be created. The inventors of the present application believe that metal elements containing activated electrons or metalloid elements such as silicon form bonds with, for example, surrounding oxygen, and the resulting silicon-oxygen bonds (Si-O bonds) or metal-oxygen bonds (MO bonds) further react with other elements or functional groups to change into the most stable bonds in the environment in which the particles are placed, such as silicon-oxygen bonds (Si-OH bonds) or metal-hydroxyl bonds (M-OH bonds). That is, since the Si-O bonds or MO bonds and the Si-OH bonds or M-OH bonds on the particle surfaces are in an equilibrium state, the ratio of Si-OH bonds / Si-O bonds or the ratio of M-OH bonds / MO bonds can be controlled by treating the particles in a specific environment, and since the effect of these ratios on the particle properties increases as the particles become smaller, it has been found that the properties of silicon compound-coated metal fine particles can be strictly controlled by strictly controlling the ratio of Si-OH bonds / Si-O bonds.
[0031] When the silicon compound-coated metal fine particles of the present invention are used as a catalyst, in addition to controlling the dispersibility, it is also possible to control the catalytic activity by controlling the coating state of the silicon compound-coated metal fine particles. For example, when used in a liquid, the coverage rate is controlled by dissolving at least a portion of the silicon compound coating the surface during use, and the surface active sites of the coated metal fine particles are exposed by dissolving the silicon compound coating, thereby exerting or improving the catalytic activity of the metal fine particles. In this case, in order to control the catalytic activity, the ratio of Si-OH bonds or the ratio of Si-OH bonds / Si-O bonds contained in the silicon compound-coated metal fine particles can be controlled to control the solubility or dissolution rate in the liquid of the silicon compound coating at least a portion of the surface of the metal fine particles, and the properties of the catalyst can be controlled and improved, so that the catalyst composition can also be suitably used. Similarly, when the silicon compound-coated metal microparticles of the present invention are used as reaction materials such as oxidizing agents or reducing agents, the solubility or dissolution rate of the silicon compound that coats at least a portion of the surface of the metal microparticles in liquid can be controlled to control the desired reaction between the metal microparticles contained in the silicon compound-coated metal microparticles and the reactant, thereby improving the yield and selectivity of the reaction product, and therefore the silicon compound-coated metal microparticles can also be suitably used in reaction compositions.
[0032] (Morphology of silicon compound-coated metal particles-1) The silicon compound-coated metal fine particles according to the present invention are metal fine particles in which at least a part of the surface of the metal fine particles is coated with a silicon compound, and the metal is a metal fine particle containing a single or multiple different elements of a metal element or a metalloid element on the chemical periodic table. The metal element in the present invention is not particularly limited, but preferably includes metal elements such as Ag, Cu, Fe, and Al. The metalloid element in the present invention is not particularly limited, but preferably includes metalloid elements such as Si, Ge, As, Sb, Te, and Se. These metals and metalloids may be metal fine particles made of a single metal element, alloy fine particles made of multiple metal elements, or alloy fine particles containing a metal element and a metalloid element.
[0033] (Morphology of silicon compound-coated metal particles-2) The metal fine particles in the silicon compound-coated metal fine particles according to the present invention are not limited to those composed only of metal. They may also be implemented as those containing compounds other than metals to the extent that they do not affect the present invention. For example, they may be implemented as silicon compound-coated metal fine particles in which at least a part of the surface of metal fine particles or alloy fine particles containing compounds other than metals is coated with a silicon compound. Examples of the compound other than the metal include oxides, hydroxides, nitrides, carbides, various salts such as nitrates, sulfates, or carbonates, as well as hydrates and organic solvates.
[0034] (Morphology of silicon compound-coated metal particles-3) The silicon compound-coated metal fine particles of the present invention are silicon compound-coated metal fine particles in which the ratio of Si-OH bonds contained in the silicon compound-coated metal fine particles or the ratio of Si-OH bonds to Si-O bonds, i.e., the ratio of Si-OH bonds / Si-O bonds, is controlled. Therefore, the silicon compound-coated metal fine particles of the present invention contain at least silicon (Si) and oxygen (O). As a method for evaluating the inclusion of silicon (Si) and oxygen (O), a method is preferable in which a transmission electron microscope (TEM) or a scanning electron microscope (STEM) is used to observe a plurality of particles, and an energy dispersive X-ray analyzer (EDS) is used to confirm the abundance ratio and the location of silicon relative to elements other than silicon in each particle. As an example, a method is exemplified in which the abundance ratio (molar ratio) of elements other than silicon and silicon contained in one silicon compound-coated metal fine particle is specified, and the average value and the coefficient of variation of the molar ratio in a plurality of silicon compound-coated metal fine particles are calculated to evaluate the uniformity, and a method is exemplified in which the location of silicon contained in the silicon compound-coated metal fine particles is specified by mapping. In the present invention, the silicon compound-coated metal fine particles are preferably those in which silicon and oxygen are detected in the vicinity of the surface layer of the silicon compound-coated metal fine particles in STEM mapping or line analysis. By coating the surface of the metal fine particles with a silicon compound, there is an advantage in that chemical stability such as water resistance and acid / alkali resistance can be imparted to the metal fine particles.
[0035] (Explanation of Si-OH and Si-O bonds-1) In the present invention, various properties such as dispersibility of the silicon compound-coated metal fine particles are controlled by controlling the ratio of Si-OH bonds contained in the silicon compound-coated metal fine particles, or the ratio of Si-OH bonds to Si-O bonds, i.e., the ratio of Si-OH bonds / Si-O bonds, and the ratio of the Si-OH bonds or the Si-OH bonds / Si-O bonds can be determined, for example, from the results of FT-IR measurement. Here, IR is an abbreviation for infrared absorption spectroscopy. (Hereinafter, simply referred to as IR measurement.) The ratio of the Si-OH bonds or the Si-OH bonds / Si-O bonds may be measured by a method other than IR measurement, and examples of such methods include X-ray photoelectron spectroscopy (XPS), solid-state nuclear magnetic resonance (solid-state NMR), and electron energy loss spectroscopy (EELS).
[0036] (Explanation of Si-OH and Si-O bonds-2) In the present invention, the ratio of Si-OH bonds or the ratio of Si-OH bonds / Si-O bonds contained in the silicon compound-coated metal fine particles is determined by measuring the infrared absorption spectrum of the silicon compound-coated metal fine particles at a wave number of 750 cm. -1 From 1300cm -1 It is preferable to obtain the peak in the region of 850 cm by waveform separation. -1 From 980cm -1 Among the peaks derived from Si-OH bonds separated in the waveform region, the peak that is assigned to the peak with the largest area ratio is preferably the peak derived from Si-OH bonds, and the peak at a wave number of 1000 cm -1 More than 1300cm -1 Of the peaks derived from Si-O bonds that are separated into the following regions, it is preferable to determine the peak that is assigned to the peak with the largest area ratio as the peak derived from the Si-O bond. -1 From 1300cm -1 The ratio of the area of the peak assigned to the Si-OH bond to the total area of the peaks obtained by waveform separation of the peaks in the wave number region of 750 cm is preferably taken as the ratio of the area of the peak assigned to the Si-OH bond to the total area of the peaks, and the ratio of the Si-O bond is preferably taken as the ratio of the area of the peak assigned to the Si-O bond to the total area of the peaks,-1 From 1300cm -1 It is preferable to calculate the ratio of Si-OH bonds / Si-O bonds from the ratio of Si-OH bonds to the ratio of Si-O bonds obtained by waveform separation of the peaks in the region. That is, the ratio of bonds of functional groups different from the types of bonds described in at least Patent Document 4 is controlled.
[0037] (Explanation of amorphous silicon compounds) In the present invention, the silicon compound that covers at least a part of the surface of the metal fine particles preferably contains amorphous silicon oxide, since it is easy to control the ratio of the Si-OH bond or the ratio of the Si-OH bond / Si-O bond. The method for evaluating whether the silicon compound contains amorphous silicon oxide is not particularly limited, but includes a method of evaluating by combining the confirmation of the presence of Si and O by the STEM mapping and the confirmation of the presence of silicon oxide by infrared absorption spectrum, and a method of confirming that no peak derived from crystalline silica (SiO2) is observed in XRD measurement, and a method of confirming that no crystal lattice is observed in the site where Si and O are detected in TEM observation or STEM observation.
[0038] (Method for controlling the ratio of Si-OH bonds or Si-OH bonds / Si-O bonds-1) In the present invention, the method for controlling the ratio of the Si-OH bond or the Si-OH bond / Si-O bond is not particularly limited, but it is preferable to control the ratio of the Si-OH bond or the Si-OH bond / Si-O bond by modifying the functional group contained in the silicon compound-coated metal fine particles. The modification of the functional group can control the ratio of the Si-OH bond or the Si-OH bond / Si-O bond by a method of performing a conventionally known substitution reaction, addition reaction, elimination reaction, dehydration reaction, condensation reaction, reduction reaction, or oxidation reaction on the functional group contained in the silicon compound-coated metal fine particles. The modification of the functional group can control the ratio of the Si-OH bond or the Si-OH bond / Si-O bond to a high value or a low value. As an example, a method of controlling the ratio of Si-OH bonds or Si-OH bonds / Si-O bonds by esterification achieved by a dehydration-condensation reaction in which OH is eliminated from the carboxyl group (-COOH) and H is eliminated from the hydroxyl group (-OH) in the Si-OH group by acting a carboxylic acid such as acetic anhydride on the Si-OH bonds contained in the silicon compound-coated metal fine particles can be mentioned, and in addition to a method using an acid anhydride, a method using a dehydrating agent such as a mixed acid anhydride, an acid halide, or a carbodiimide can also be used in the esterification. In addition to the above esterification, it is also possible to control the ratio of Si-OH bonds or the ratio of Si-OH bonds / Si-O bonds by a method of causing an alkyl halide, an aryl halide, or a heteroaryl halide to act on the Si-OH group, preferably in the presence of an acid catalyst, to generate an ether bond between the alkyl halide or other substance and Si by dehydration, or a method of causing an isocyanate or a thioisocyanate to act on the Si-OH to generate a (thio)urethane bond.
[0039] The substance acting on the Si-OH bond may be a substance containing a functional group containing fluorine or a functional group having hydrophilicity or lipophilicity, etc., to control the ratio of Si-OH bonds or the ratio of Si-OH bonds / Si-O bonds contained in the silicon compound-coated metal fine particles. In the present invention, it is not limited to directly acting other substances or functional groups on the Si-OH bonds or Si-O bonds to generate new bonds, and it is also possible to control the ratio of Si-OH bonds or the ratio of Si-OH bonds / Si-O bonds by, for example, acting carbodiimide on carboxylic acid or the like contained in the particles, or by acting ethylene oxide or the like on the Si-OH bonds to generate bonds such as Si-O-(CH2)2-OH, or by acting epihalohydrin. In addition, the ratio of Si-OH bonds or the ratio of Si-OH bonds / Si-O bonds can also be controlled by acting hydrogen peroxide or ozone on the silicon compound-coated metal fine particles. In addition, when the silicon compound-coated metal fine particles are precipitated in a liquid, the ratio of the Si-OH bonds or the ratio of the Si-OH bonds / Si-O bonds can be controlled by controlling the pH or the formulation of the metal raw material liquid or the metal precipitation solvent when precipitating the silicon compound-coated metal fine particles. As an example of a dehydration reaction, the ratio of the Si-OH bonds or the ratio of the Si-OH bonds / Si-O bonds can also be controlled by a method of heat-treating the silicon compound-coated metal fine particles. When the ratio of the Si-OH bonds or the ratio of the Si-OH bonds / Si-O bonds is controlled by a method of heat-treating the silicon compound-coated metal fine particles, it can be performed by a dry heat treatment or by heat-treating the silicon compound-coated metal fine particles in a dispersion state in which the silicon compound-coated metal fine particles are dispersed in a dispersion medium.
[0040] (Method of controlling the ratio of Si-OH bonds or Si-OH bonds / Si-O bonds-2) As the functional group modification treatment of the silicon compound-coated metal fine particles according to the present invention, in addition to reactions such as dehydration, the silicon compound-coated metal fine particles can be treated in a reducing atmosphere or an oxidizing atmosphere to control the ratio of Si-OH bonds or Si-OH bonds / Si-O bonds by reduction reactions or oxidation reactions. For example, the powder of silicon compound-coated metal fine particles is treated in a furnace with reducing gases such as hydrogen, ammonia, hydrogen sulfide, sulfur dioxide, and nitrogen monoxide, or oxidizing gases such as oxygen, ozone, and nitrogen dioxide, thereby changing the oxidation number of Si or M contained in the silicon compound-coated metal fine particles in which at least a part of the surface of the metal fine particles is coated with a silicon compound, thereby controlling the ratio of Si-OH bonds or Si-OH bonds / Si-O bonds. The functional group modification treatment including the above-mentioned oxidation treatment or reduction treatment may be performed in combination, for example, by simultaneously performing a heat treatment and a reduction treatment.
[0041] (Method of controlling the ratio of Si-OH bonds or Si-OH bonds / Si-O bonds-3) As described later, the silicon compound-coated metal fine particles may be dispersed in a target solvent, a substance containing a functional group is added to the dispersion liquid, and a process such as stirring is performed to control the ratio of the Si-OH bonds or the ratio of the Si-OH bonds / Si-O bonds, or the metal raw material liquid, metal deposition solvent, and silicon compound raw material liquid are mixed to precipitate a dispersion liquid containing silicon compound-coated metal fine particles, and the dispersion liquid is continuously stirred to control the ratio of the Si-OH bonds or the ratio of the Si-OH bonds / Si-O bonds. Furthermore, a device in which a dispersion device and a filtration membrane are connected is constructed, and impurities are removed from a slurry containing silicon compound-coated metal fine particles by a dispersion process for particles and a process using a cross-flow membrane filtration, and the like, and the like. In this case, a uniform modification treatment can be performed on the primary particles of the silicon compound-coated metal microparticles, particularly on the surface of each primary particle, which has the advantage that it is possible to more strictly and uniformly control the ratio of Si-OH bonds or the ratio of Si-OH bonds / Si-O bonds contained in the silicon compound-coated metal microparticles of the present invention, and to control properties such as dispersibility.
[0042] The pH adjustment when precipitating the above-mentioned silicon compound-coated metal microparticles may be adjusted by adding a pH adjuster such as an acidic substance or a basic substance to at least one of the various solutions and solvents in the present invention, or by changing the flow rate when mixing a fluid containing the metal raw material liquid and a fluid containing the metal precipitating solvent.
[0043] The method for changing the functional group contained in the silicon compound-coated metal fine particles according to the present invention is not particularly limited. It may be carried out by dispersing the silicon compound-coated metal fine particles in a target solvent, adding a substance containing a functional group to the dispersion liquid, and carrying out a treatment such as stirring, or by mixing a fluid containing the silicon compound-coated metal fine particles and a fluid containing a substance containing a functional group using the microreactor described in Patent Document 5.
[0044] The substance containing a functional group is not particularly limited, and may be a substance containing a functional group that can be substituted for a hydroxyl group contained in the silicon compound-coated metal fine particles, and may include acylating agents such as acetic anhydride and propionic anhydride; methylating agents such as dimethyl sulfate and dimethyl carbonate; and silane coupling agents such as chlorotrimethylsilane and methyltrimethoxysilane. Other examples of substances containing a CF bond, which is a hydrophobic group, include compounds containing fluorine such as trifluoroacetic acid, trifluoromethanesulfonic acid, or their anhydrides, silane coupling agents containing fluorine such as triethoxy-1H,1H,2H,2H-heptadecafluorodecylsilane and trimethoxy(3,3,3-trifluoropropyl)silane, or fluorine compounds such as trifluoromethane and trifluoroethane. Furthermore, it is also possible to control the ratio of Si-OH bonds or the ratio of Si-OH bonds / Si-O bonds contained in the silicon compound-coated oxide particles by a method in which gas such as trifluoromethane or trifluoroethane is applied to the silicon compound-coated oxide particles. Specifically, when a substance containing a functional group capable of substituting these hydroxyl groups is used, it is possible to control the ratio of Si-OH bonds.
[0045] As described above, the ratio of the Si-OH bonds or the ratio of the Si-OH bonds / Si-O bonds can also be controlled by a method of reacting hydrogen peroxide or ozone with oxide particles. The method of reacting hydrogen peroxide or ozone with silicon compound-coated metal fine particles is not particularly limited. The method may be carried out by dispersing the silicon compound-coated metal fine particles in a target solvent, adding hydrogen peroxide or ozone or a solution containing them to the dispersion, and performing a treatment such as stirring, or by mixing a fluid containing the silicon compound-coated metal fine particles and a fluid containing hydrogen peroxide or ozone using a microreactor described in Patent Document 5.
[0046] The above-mentioned dispersion can be implemented as a liquid dispersion in which silicon compound-coated metal fine particles are dispersed in a liquid dispersion medium such as water, an organic solvent, or a resin, or as a dispersion in the form of a coating film prepared using a dispersion liquid containing silicon compound-coated metal fine particles.When heat-treated in the state of a dispersion containing silicon compound-coated metal fine particles, the aggregation of particles can be suppressed compared to dry heat treatment, and when the silicon compound-coated metal fine particles of the present invention are used for a coating film, the silicon compound-coated metal fine particles are made into a coating film, and then the ratio of the Si-OH bond or the Si-OH bond / Si-O bond contained in the silicon compound-coated metal fine particles is controlled by a method such as heat treatment, so that the characteristics of the silicon compound-coated metal fine particles can be controlled, which is suitable for reducing the number of steps and controlling the characteristics strictly.
[0047] In addition to the above-mentioned coating film applications, for example, in compositions for transparent materials used in glass or film of buildings, transparent resins, etc., silicon compound-coated metal fine particles can be dispersed in glass or resin, etc., and can be suitably used for shielding against electromagnetic waves such as ultraviolet rays and near infrared rays, and can also be suitably used as a silicon compound-coated metal fine particle composition for ultraviolet protection or near infrared protection. In addition, similar to the above-mentioned coating film, silicon compound-coated metal fine particles are dispersed in glass or transparent resin to form a film, and then subjected to a functional group modification treatment such as heat treatment to control the ratio of Si-OH bonds or the ratio of Si-OH bonds / Si-O bonds contained in the silicon compound-coated metal fine particles, thereby controlling the properties of the silicon compound-coated metal fine particles, which is suitable for reducing the number of steps and strictly controlling the properties, similar to the above-mentioned coating film.
[0048] In the present invention, the primary particle diameter of the metal fine particles in the silicon compound-coated metal fine particles is preferably 1 μm or less, more preferably 1 nm or more and 1 μm or less. The primary particle diameter of the coated silicon compound-coated metal fine particles is also preferably 1 μm or less, more preferably 1 nm or more and 0.5 μm or less. It is assumed that the Si-OH bond or Si-O bond contained in the silicon compound-coated metal fine particles is mainly present on the surface of the particles, which makes it possible to strictly control the properties of the silicon compound-coated metal fine particles. Therefore, the silicon compound-coated metal fine particles having a primary particle diameter of 1 μm or less have a larger surface area than the silicon compound-coated metal fine particles having a primary particle diameter of more than 1 μm, and it is considered that the effect of controlling the ratio of Si-OH bonds or the ratio of Si-OH bonds / Si-O bonds of the silicon compound-coated metal fine particles on the properties such as dispersibility of the silicon compound-coated metal fine particles is large. Therefore, in the case of silicon compound-coated metal microparticles having a primary particle diameter of 1 μm or less, by controlling the ratio of Si-OH bonds or the ratio of Si-OH bonds / Si-O bonds contained in the silicon compound-coated metal microparticles, there is an advantage in that it is possible to suitably exhibit specified properties (in particular properties suitable for use in coating compositions intended for use in coating films or painted bodies, etc., or transparent material compositions intended for use in coated bodies, glass, transparent resins or films where transparency is required, magnetic compositions intended for use in magnetic bodies such as magnetic fluids, semiconductor compositions intended for use in semiconductors, etc., conductive compositions intended for use as conductive materials, reaction compositions intended for use as reaction materials, etc., or catalyst compositions intended for use as catalyst materials).
[0049] In the silicon compound-coated metal fine particles according to the present invention, the ratio of the average primary particle diameter of the silicon compound-coated metal fine particles to the average primary particle diameter of the metal fine particles before coating with the silicon compound is preferably 100.5% or more and 190% or less. If the silicon compound coating on the metal fine particles is too thin, the effects related to the properties of the silicon compound-coated metal fine particles may not be exhibited, so the average primary particle diameter of the silicon compound-coated metal fine particles is preferably 100.5% or more of the average primary particle diameter of the metal fine particles. If the coating is too thick or if coarse aggregates are coated, it becomes difficult to control the properties, and if the coating thickness exceeds 1 μm, the peak derived from the Si-OH bond and the peak derived from the Si-O bond may overlap in the IR measurement results, so the average primary particle diameter of the silicon compound-coated metal fine particles is preferably 190% or less of the average primary particle diameter of the metal fine particles. Various compositions according to the present invention include metal fine particles having at least a part of the surface coated with a silicon compound, that is, the silicon compound-coated metal fine particles themselves. The silicon compound-coated metal fine particles according to the present invention may be core-shell type silicon compound-coated metal fine particles in which the entire surface of the core metal fine particles is uniformly coated with a silicon compound. The silicon compound-coated metal fine particles are preferably silicon compound-coated metal fine particles in which at least a part of the surface of a single metal fine particle, in which a plurality of metal fine particles are not aggregated, is coated with a silicon compound, but may be silicon compound-coated metal fine particles in which at least a part of the surface of an aggregate of a plurality of metal fine particles is coated with a silicon compound. However, in this case, silicon compound-coated metal fine particles in which the aggregates exceeding a certain size are coated with a silicon compound are not preferred because the effect of the above-mentioned characteristics such as dispersibility is difficult to obtain compared to silicon compound-coated metal fine particles in which at least a part of the surface of a single metal fine particle is coated with a silicon compound. Here, the above-mentioned aggregates exceeding a certain size refer to, for example, aggregates having a size of more than 1 μm. The particle diameter of the silicon compound-coated metal fine particles, in which at least a portion of the surface of an aggregate of a plurality of metal fine particles is coated with a silicon compound, is preferably 100.5% or more and 190% or less of the diameter of the aggregate.The diameter of the aggregates is defined as the distance between the maximum outer circumferences of the aggregates.
[0050] (Method of Producing Silicon Compound-Coated Metal Fine Particles: Preferred Method) As an example of the method for producing the silicon compound-coated metal fine particles according to the present invention, a metal raw material liquid containing at least the raw material of the metal fine particles to be coated with a silicon compound and a metal precipitating solvent containing at least a metal precipitating material for precipitating the metal fine particles are prepared, and in a mixed fluid obtained by mixing the metal raw material liquid and the metal precipitating solvent, the metal fine particles are precipitated by a method such as reaction, crystallization, precipitation, coprecipitation, etc., and the mixed fluid containing the precipitated metal fine particles is mixed with a silicon compound raw material liquid containing at least the raw material of the silicon compound, which is the compound to be coated, to produce a method for producing the silicon compound-coated metal fine particles by coating at least a part of the surface of the metal fine particles with a silicon compound. In addition, when the metal fine particles are alloy fine particles and the purpose is to produce alloy fine particles coated with a silicon compound, the different metal elements or semimetal elements contained in the metal fine particles may be contained together in the metal raw material liquid, may be contained in the metal raw material liquid and the metal precipitating solvent, or may be contained in both the metal raw material liquid and the metal precipitating solvent or the silicon compound raw material liquid.
[0051] The raw material of the silicon compound-coated metal fine particles in the present invention is not particularly limited. Any method that can produce silicon compound-coated metal fine particles by reaction, crystallization, precipitation, coprecipitation, or the like can be used. In the present invention, compounds of metal elements or metalloid elements are collectively referred to as compounds. The compounds are not particularly limited, but examples include salts, oxides, hydroxides, hydroxide oxides, nitrides, carbides, complexes, organic salts, organic complexes, organic compounds, or hydrates and organic solvates of metals or metalloids containing metal elements or metalloid elements. It is also possible to use a single metal or metalloid. The salts of metals or metalloids are not particularly limited, but include nitrates, nitrites, sulfates, sulfites, carbonates, formates, acetates, phosphates, phosphites, hypophosphites, chlorides, oxysalts, acetylacetonate salts, or hydrates and organic solvates of metals or metalloids, and organic compounds include alkoxides of metals or metalloids. As described above, these metal or metalloid compounds may be used alone or as a mixture of more than one. In the present invention, when the metals constituting the silicon compound-coated metal microparticles are multiple different metal elements or metalloid elements, where the main metal element is M1 and the secondary metal element or metalloid element is M2, it is preferable that the molar ratio of M2 to M1 (M2 / M1) is 0.01 or more and 1.00 or less.
[0052] In addition, the raw material of the silicon compound according to the present invention includes oxides and hydroxides of silicon, other compounds such as silicon salts and alkoxides, and hydrates thereof. Although not particularly limited, silicates such as sodium silicate, phenyltrimethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-trifluoropropyl-trimethoxysilane, methacryloxypropyltriethoxysilane, tetramethoxysilane (TMOS), tetraethoxysilane (TEOS), and oligomer condensates of TEOS, such as ethyl silicate 40, tetraisopropylsilane, tetrapropoxysilane, tetraisobutoxysilane, tetrabutoxysilane, and similar substances. Furthermore, other siloxane compounds, bis(triethoxysilyl)methane, 1,9-bis(triethoxysilyl)nonane, diethoxydichlorosilane, triethoxychlorosilane, etc. may be used as the raw material of the silicon compound.
[0053] In addition, when the raw materials of the metal fine particles or the silicon compound for coating are solid, it is preferable to use each raw material in a molten state or in a state where it is mixed or dissolved in a solvent described later (including a molecularly dispersed state).Even when each raw material is liquid or gas, it is preferable to use it in a state where it is mixed or dissolved in a solvent described later (including a molecularly dispersed state).
[0054] The metal precipitating material is not particularly limited as long as it can precipitate the raw material of the silicon compound-coated metal fine particles contained in the metal raw material liquid as silicon compound-coated metal fine particles, and for example, it is preferable to use a reducing agent that can reduce the ions of metal or metalloid contained in the metal raw material liquid. The reducing agent is not particularly limited, but all reducing agents that can reduce the metal elements or metalloid elements that constitute the silicon compound-coated metal fine particles can be used. Examples include hydride reducing agents such as sodium borohydride and lithium borohydride, aldehydes such as formalin and aldehyde, sulfites, carboxylic acids or lactones such as formic acid, oxalic acid, succinic acid, ascorbic acid, and citric acid, monoalcohols such as aliphatic monoalcohols such as methanol, ethanol, butanol, isopropyl alcohol, and octanol, and alicyclic monoalcohols such as terpineol, aliphatic diols such as ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, triethylene glycol, and tetraethylene glycol, polyhydric alcohols such as glycerin and trimethylolpropane, and polyethylene glycol. Examples of suitable solvents include polyethers such as alcohol and polypropylene glycol, alkanolamines such as diethanolamine and monoethanolamine, phenols such as hydroquinone, resorcinol, and aminophenol, sugars such as glucose and fructose, sodium citrate, hypochlorous acid or a salt thereof, transition metal ions (e.g., titanium and iron ions), hydrazines, amines such as triethylamine, triethanolamine, dimethylaminoethanol, octylamine, and dimethylaminoborane, and pyrrolidones (polyvinylpyrrolidone, 1-vinyl-2-pyrrolidone, and methylpyrrolidone). Reducing gases such as hydrogen gas and ammonia gas can also be used.
[0055] The metal source liquid and the metal deposition solvent may contain an acidic or basic substance, such as metal hydroxides, such as sodium hydroxide and potassium hydroxide, metal alkoxides, such as sodium methoxide and sodium isopropoxide, amine compounds, such as triethylamine, diethylaminoethanol and diethylamine, and ammonia.
[0056] Examples of the acidic substance include inorganic acids such as aqua regia, hydrochloric acid, nitric acid, fuming nitric acid, sulfuric acid, and fuming sulfuric acid, and organic acids such as formic acid, acetic acid, chloroacetic acid, dichloroacetic acid, oxalic acid, trifluoroacetic acid, trichloroacetic acid, and citric acid. The basic substances and acidic substances can also be used to precipitate silicon compound-coated metal fine particles or compounds for coating.
[0057] (solvent) Examples of the solvent used for the metal source liquid, metal precipitation solvent, or silicon compound source liquid include water, organic solvents, or mixed solvents consisting of a plurality of them. Examples of the water include tap water, ion-exchanged water, pure water, ultrapure water, RO water (reverse osmosis water), and examples of the organic solvent include alcohol compound solvents, amide compound solvents, ketone compound solvents, ether compound solvents, aromatic compound solvents, carbon disulfide, aliphatic compound solvents, nitrile compound solvents, sulfoxide compound solvents, halogen compound solvents, ester compound solvents, ionic liquids, carboxylic acid compounds, and sulfonic acid compounds. Each of the above solvents may be used alone, or a plurality of them may be used in combination. Examples of the alcohol compound solvent include monohydric alcohols such as methanol and ethanol, and polyols such as ethylene glycol and propylene glycol.
[0058] (Dispersants, etc.) Various dispersants and surfactants may be used according to the purpose and necessity as long as they do not adversely affect the preparation of the silicon compound-coated metal fine particles according to the present invention. Although not particularly limited, various commonly used commercial products, products, or newly synthesized ones can be used as dispersants and surfactants. Examples include dispersants such as anionic surfactants, cationic surfactants, nonionic surfactants, and various polymers. These may be used alone or in combination of two or more. The above surfactants and dispersants may be contained in at least one of the fluids of the metal source liquid and the metal deposition solvent. In addition, the above surfactants and dispersants may be contained in a different fluid that is different from the metal source liquid and the metal deposition solvent.
[0059] (Method for producing silicon compound-coated metal particles: method overview) In the step of coating at least a part of the surface of the metal fine particles with a silicon compound, it is preferable to coat the metal fine particles with the silicon compound before they aggregate. When mixing the silicon compound raw material liquid with the fluid containing the metal fine particles, it is important to add the silicon compound raw material liquid at a speed faster than the rate at which the metal fine particles precipitate and then aggregate to precipitate the silicon compound on the surface of the metal fine particles. Furthermore, by adding the silicon compound raw material liquid to the fluid containing the metal fine particles, the pH of the fluid containing the metal fine particles and the concentration of the silicon compound raw material gradually change, and if the silicon compound for coating the surface of the particles precipitates after the particles change from a state in which they are easy to disperse to a state in which they are easy to aggregate, it may be difficult to coat them before they aggregate to such an extent that the characteristics of the present invention cannot be exhibited. It is preferable to act on the silicon compound raw material contained in the silicon compound raw material liquid immediately after the metal fine particles are precipitated. It is preferable to obtain silicon compound-coated metal fine particles by a method in which metal fine particles are precipitated between relatively rotating processing surfaces that can approach and separate as described in Patent Document 5, and the surfaces of the metal fine particles are continuously coated with a silicon compound following the precipitation of the metal fine particles. By changing the temperature, pH, and formulation conditions when obtaining the silicon compound-coated metal fine particles, there is an advantage that the silicon compound-coated metal fine particles of the present invention can be produced, and the ratio of Si-OH bonds or the ratio of Si-OH bonds / Si-O bonds, and the properties of the silicon compound-coated metal fine particles can be strictly controlled. By setting the temperature when obtaining the silicon compound-coated metal fine particles to a certain level or higher, it is possible to produce silicon compound-coated metal fine particles having a hollow layer between the metal fine particles in the silicon compound-coated metal fine particles and the layer of the silicon compound that coats them. The surface of the metal fine particles precipitated in an environment of a certain temperature or higher is coated with a silicon compound at the same temperature, and then cooled to a low temperature such as room temperature, utilizing the fact that the shrinkage rate of the metal fine particles in the silicon compound-coated metal fine particles is smaller than that of the silicon compound. In the present invention, the temperature for obtaining the silicon compound-coated, fine metal particles having a hollow layer is preferably 150° C. or higher, more preferably 200° C. or higher.
[0060] (Method and apparatus for producing silicon compound-coated metal particles) An example of the method for producing the silicon compound-coated metal fine particles according to the present invention is a method for producing the silicon compound-coated metal fine particles by using a microreactor or by carrying out a reaction in a dilute system in a batch container, etc. In addition, in order to produce the silicon compound-coated metal fine particles, an apparatus and method such as those proposed by the applicant of the present application and described in JP 2009-112892 A may be used. The device described in JP 2009-112892 A has a stirring tank having an inner peripheral surface with a circular cross section, and a stirring tool attached to the inner peripheral surface of the stirring tank with a small gap therebetween, the stirring tank has at least two fluid inlets and at least one fluid outlet, a first treated fluid containing one of the reactants among the treated fluids is introduced into the stirring tank from one of the fluid inlets, and a second treated fluid containing one of the reactants different from the reactant is introduced into the stirring tank from a flow path different from that of the first treated fluid from the other of the fluid inlets, at least one of the stirring tank and the stirring tool rotates at high speed relative to the other to make the treated fluid into a thin film state, and reactants contained in at least the first treated fluid and the second treated fluid react with each other in this thin film, and it is described that three or more introduction pipes may be provided as shown in Figures 4 and 5 of the same publication in order to introduce three or more treated fluids into the stirring tank. An example of the above-mentioned microreactor is a device based on the same principle as the fluid treatment device described in Patent Document 5.
[0061] As a method for producing silicon compound-coated metal fine particles according to the present invention, which is different from the above method, there is a method of treating fine particles of a material that can be a precursor of the metal contained in the metal fine particles in a reducing atmosphere. Specifically, the method is a method of preparing silicon compound-coated precursor fine particles in which at least a part of the surface of fine particles containing the precursor is coated with a silicon compound, or silicon-doped precursor fine particles in which fine particles containing the precursor are doped with silicon, and treating the silicon compound-coated precursor fine particles or the silicon-doped precursor fine particles in a reducing atmosphere. Examples of the precursor include oxides or hydroxides, nitrides, carbides, various salts such as nitrates, sulfates, or carbonates containing metal elements or semimetal elements that constitute the metal fine particles, as well as hydrates and organic solvent solvates. For example, silicon compound-coated precursor fine particles such as silicon compound-coated iron oxide particles can be reduced to silicon compound-coated iron particles by heat treating them in a hydrogen atmosphere, which is a reducing atmosphere. In addition, by treating the silicon compound-coated precursor fine particles in a reducing atmosphere, even if the silicon compound is reduced to silicon, it can be converted into a silicon compound such as silicon oxide by treating in an atmospheric atmosphere such as air, so that the silicon compound-coated metal fine particles can be obtained in the same manner as above. In this way, by treating the silicon compound-coated precursor fine particles containing the precursor of the metal fine particles in a reducing atmosphere, not only can the production of the silicon compound-coated metal fine particles and the ratio of the Si-OH bond or the ratio of the Si-OH bond / Si-O bond be performed substantially simultaneously, but also the ratio of the Si-OH bond or the ratio of the Si-OH bond / Si-O bond can be more strictly controlled.
[0062] The silicon compound-coated metal fine particles according to the present invention can also be obtained by treating silicon-doped precursor fine particles, the precursor of which contains silicon, in a reducing atmosphere. For example, first, silicon-doped iron oxide particles, which are silicon-doped precursor particles, are heat-treated in a reducing atmosphere, thereby reducing both silicon and iron to obtain silicon-iron alloy particles. Next, the silicon-iron alloy particles obtained are treated in an oxidizing atmosphere such as air to oxidize the silicon contained in the surface of the silicon-iron alloy particles to form silicon compounds such as silicon oxides, thereby making it possible to produce silicon compound-coated metal fine particles such as silicon compound-coated iron particles or silicon compound-coated silicon-iron alloy particles.
[0063] The inventors of the present application have also found that the silicon contained in the metal particles or precursor particles such as oxides undergoes a change in which the silicon is moved from the inside of the particles to the outside by heat treatment. Even when the particles are fused together, the fused part between the particles can be reduced to a state in which it does not contain silicon and silicon compounds, and the surface of the particles whose particle diameter has been increased by fusion can be covered with silicon compounds. The silicon compound-coated metal fine particles produced by using these methods contain silicon inside the metal fine particles at least before heat treatment, and the silicon has migrated from the inside of the metal fine particles to the outer periphery direction compared to before heat treatment by heat treatment, and have the advantage that the reduction or particle diameter of the precursor particles, the ratio of the Si-OH bonds, or the ratio of the Si-OH bonds / Si-O bonds can be controlled simultaneously. However, the present invention is not limited to simultaneously performing the reduction and the control of the ratio of the Si-OH bonds or the ratio of the Si-OH bonds / Si-O bonds. In addition, for example, when the silicon compound-coated metal fine particles according to the present invention are used for conductive wiring materials, the metal element contained in the silicon compound-coated metal fine particles can form conductive wiring, and the outer periphery of the wiring can be coated with the silicon compound, so that the metal forming the wiring can be protected from moisture and prevented from oxidation by the silicon compound on the outer periphery of the wiring. In addition, in the present invention, the reduction treatment of the silicon compound-coated precursor fine particles or silicon-doped precursor fine particles may be performed by a dry method or a wet method.
[0064] When obtaining silicon compound-coated metal fine particles by reducing the silicon compound-coated precursor fine particles or silicon-doped precursor particles, the particle diameter of the silicon compound-coated precursor fine particles is preferably 100 nm or less. By being 100 nm or less, a uniform reduction process to the silicon compound-coated metal fine particles is possible, and there is an advantage that the ratio of the Si-OH bonds or the ratio of the Si-OH bonds / Si-O bonds can be controlled simultaneously, and even base metals that have been difficult to reduce only by methods such as electric reduction using large energy such as electricity can be reduced to metal fine particles. There is no particular limitation on the method for producing the silicon compound precursor particles, but similar to the silicon compound-coated metal fine particles, precursor fine particles may be produced by using a method of producing them using an apparatus described in Patent Document 5 or a pulverization method such as a bead mill, and then a process of coating the precursor particles with the silicon compound using a reaction vessel or the microreactor may be performed after the production.
[0065] (Correspondence with priority applications) The present inventors have found that the properties of silicon compound-coated metal fine particles, such as dispersibility, can be controlled by controlling the ratio of Si-OH bonds or the ratio of Si-OH bonds / Si-O bonds contained in the silicon compound-coated metal fine particles, and have completed the present invention. Coating the surfaces of various fine particles with silicon compounds, and obtaining silicon compound-coated metal oxide fine particles in which the silicon compound is a silicon oxide, which can be a precursor of silicon compound-coated metal fine particles, are also disclosed in Japanese Patent Application No. 2016-111346, which is the basic application of this application, and have found that this can be reduced to metal in a reducing atmosphere. The present inventors have further found that the properties of silicon compound-coated metal fine particles, such as dispersibility, can be controlled by controlling the Si-OH bonds contained in the silicon compound-coated metal fine particles in a specific atmosphere, as disclosed in PCT / JP2016 / 83001, which is another basic application of this application. EXAMPLES
[0066] The present invention will be further described below with reference to examples, but the present invention is not limited to these examples. In the following examples, unless otherwise specified, pure water with a conductivity of 0.84 μS / cm (measurement temperature: 25° C.) was used.
[0067] (Preparation of specimens for TEM observation and STEM observation) The silicon compound-coated metal particles obtained in the examples were dispersed in a dispersion medium, and the resulting dispersion was dropped onto a collodion film and dried to prepare a sample for TEM observation or a sample for STEM observation.
[0068] (Transmission electron microscope and energy dispersive X-ray analyzer: TEM-EDS analysis) A transmission electron microscope, JEM-2100 (manufactured by JEOL Ltd.), equipped with an energy dispersive X-ray analyzer, JED-2300 (manufactured by JEOL Ltd.), was used for the observation and quantitative analysis of the silicon compound-coated metal fine particles by TEM-EDS analysis. The observation conditions were an acceleration voltage of 80 kV and an observation magnification of 25,000 times or more. The particle size was calculated from the distance between the maximum outer circumferences of the silicon compound-coated metal fine particles observed by TEM, and the average value (average primary particle size) of the results of measuring the particle size of 100 particles was calculated. The molar ratio of the elemental components constituting the silicon compound-coated metal fine particles was calculated by TEM-EDS, and the average value of the results of calculating the molar ratio for 10 or more particles was calculated.
[0069] (Scanning transmission electron microscope and energy dispersive X-ray analyzer: STEM-EDS analysis) For mapping and quantification of elements contained in the silicon compound-coated metal microparticles by STEM-EDS analysis, an atomic resolution analytical electron microscope, JEM-ARM200F (manufactured by JEOL Ltd.), equipped with an energy dispersive X-ray analyzer, Centurio (manufactured by JEOL Ltd.) was used. The observation conditions were an acceleration voltage of 80 kV, an observation magnification of 50,000 times or more, and a beam diameter of 0.2 nm.
[0070] (X-ray diffraction measurement) For the X-ray diffraction (XRD) measurement, a powder X-ray diffraction measuring device EMPYREAN (manufactured by Spectris Corporation, PANalytical Division) was used. The measurement conditions were: measurement range: 10 to 100 [°2θ] Cu anticathode, tube voltage 45 kV, tube current 40 mA, scanning speed 0.3° / min. XRD measurement was performed using the dried powder of the silicon compound-coated metal fine particles obtained in each example.
[0071] (FT-IR measurement) For the FT-IR measurement, a Fourier transform infrared spectrophotometer, FT / IR-6600 (manufactured by JASCO Corporation) was used. The measurement conditions were an ATR method under a nitrogen atmosphere with a resolution of 4.0 cm. -1 The number of integrations is 1024. The wave number in the IR spectrum is 750 cm -1 From 1300cm -1 The waveform separation of the peaks was performed by curve fitting using a spectrum analysis program attached to the control software of the FT / IR-6600 so that the residual sum of squares was 0.01 or less. The measurement was performed using the dry powder of the silicon compound-coated metal fine particles obtained in the examples.
[0072] (Particle size distribution measurement) For the particle size distribution measurement, a particle size distribution meter UPA-UT151 (manufactured by Nikkiso Co., Ltd.) was used. The measurement conditions were as follows: the dispersion medium in which the silicon compound-coated metal particles obtained in the examples were dispersed was used as the measurement solvent; and the particle refractive index and density were the values of the main metal element or metalloid element constituting the metal fine particles in the silicon compound-coated metal fine particles obtained in the examples.
[0073] Example 1 In Example 1, a silicon compound-coated metal fine particle was prepared using an apparatus based on the principle described in Patent Document 5, and the dispersibility in various dispersion media was controlled by controlling the ratio of Si-OH bonds or the ratio of Si-OH bonds / Si-O bonds contained in the silicon compound-coated metal fine particle. A metal source liquid (liquid A), a metal deposition solvent (liquid B), and a silicon compound source liquid (liquid C) were prepared using a Clearmix (product name: CLM-2.2S, manufactured by M-Technique Co., Ltd.), which is a high-speed rotary dispersion and emulsification apparatus. Specifically, based on the formulation of the metal source liquid shown in Example 1 of Table 1, each component of the metal source liquid was homogeneously mixed by stirring at a preparation temperature of 50°C and a rotor rotation speed of 20,000 rpm for 30 minutes using Clearmix to prepare the metal source liquid. Also, based on the formulation of the metal deposition solvent shown in Example 1 of Table 2, the components of the metal deposition solvent were mixed homogeneously by stirring for 30 minutes at a preparation temperature of 25°C and a rotor rotation speed of 8000 rpm using a Clearmix to prepare a metal deposition solvent. Furthermore, based on the formulation of the silicon compound raw material liquid shown in Example 1 of Table 3, the components of the silicon compound raw material liquid were mixed homogeneously by stirring for 10 minutes at a preparation temperature of 20°C and a rotor rotation speed of 6000 rpm using a Clearmix to prepare a silicon compound raw material liquid. For the substances represented by the chemical formulas or abbreviations in Tables 1 to 3, MeOH was methanol (manufactured by Mitsubishi Chemical Corporation), EG was ethylene glycol (manufactured by Kishida Chemical Co., Ltd.), KOH was potassium hydroxide (manufactured by Nippon Soda Co., Ltd.), NaOH was sodium hydroxide (manufactured by Kanto Chemical Co., Ltd.), TEOS was tetraethyl orthosilicate (manufactured by Wako Pure Chemical Industries, Ltd.), AgNO3 was silver nitrate (manufactured by Kanto Chemical Co., Ltd.), NaBH4 was sodium tetrahydroborate (manufactured by Wako Pure Chemical Industries, Ltd.), HMH was hydrazine monohydrate (manufactured by Kanto Chemical Co., Ltd.), PVP was polyvinylpyrrolidone K = 30 (manufactured by Kanto Chemical Co., Ltd.), DMAE was 2-dimethylaminoethanol (manufactured by Kanto Chemical Co., Ltd.), and H2SO4 was concentrated sulfuric acid (manufactured by Kishida Chemical Co., Ltd.).
[0074] Next, the prepared metal source liquid, metal deposition solvent, and silicon compound source liquid were mixed using a fluid treatment device described in Patent Document 5 by the applicant of the present application. Here, the fluid treatment device described in Patent Document 5 is the device described in FIG. 1(B) of the same publication, in which the openings d20 and d30 of the second and third introduction parts are concentrically annular surrounding the central opening of the processing surface 2, which is a disk formed in a ring shape. Specifically, the metal source liquid or the metal deposition solvent was introduced as the A liquid from the first introduction part d1 between the processing surfaces 1 and 2, and while the processing part 10 was operated at a rotation speed of 1130 rpm, the other liquid of the metal source liquid or the metal deposition solvent, which is different from the liquid sent as the A liquid, was introduced as the B liquid from the second introduction part d2 between the processing surfaces 1 and 2, and the metal source liquid and the metal deposition solvent were mixed in the thin film fluid, and silver fine particles as the core were precipitated between the processing surfaces 1 and 2. Next, a silicon compound raw material liquid was introduced as liquid C from the third introduction part d3 between the processing surfaces 1 and 2, and mixed with a mixed fluid containing silver particles that would become cores in the thin film fluid. A silicon compound was precipitated on the surface of the silver particles that would become cores, and a discharge liquid containing the silicon compound-coated silver particles (hereinafter, silicon compound-coated silver particle dispersion liquid) was discharged from between the processing surfaces 1 and 2 of the fluid processing device. The discharged silicon compound-coated silver particle dispersion liquid was collected in a beaker b via a vessel v.
[0075] Table 4 shows the operating conditions of the fluid treatment device, and the molar ratio of Si / M (Si / Ag in Example 1) calculated by TEM-EDS analysis calculated from the TEM observation results of the obtained silicon compound-coated silver microparticles, together with the calculated values calculated from the formulations and introduction flow rates of liquid A, liquid B, and liquid C. The introduction temperatures (liquid delivery temperatures) and introduction pressures (liquid delivery pressures) of liquid A, liquid B, and liquid C shown in Table 4 were measured using a thermometer and a pressure gauge installed in the sealed introduction paths (first introduction part d1, second introduction part d2, and third introduction part d3) leading between the processing surfaces 1 and 2. The introduction temperature of liquid A shown in Table 2 is the actual temperature of liquid A under the introduction pressure in the first introduction part d1, the introduction temperature of liquid B is the actual temperature of liquid B under the introduction pressure in the second introduction part d2, and the introduction temperature of liquid C is the actual temperature of liquid C under the introduction pressure in the third introduction part d3.
[0076] For the pH measurement, a pH meter of Model D-51 manufactured by Horiba, Ltd. was used. Before introducing the A, B and C solutions into the fluid treatment device, their pH was measured at room temperature. In addition, since it is difficult to measure the pH of the mixed fluid immediately after mixing the metal raw material liquid with the metal deposition solvent, and the pH immediately after mixing the fluid containing the silver particles as the core with the silicon compound raw material liquid, the pH of the silicon compound-coated silver particle dispersion discharged from the device and collected in beaker b was measured at room temperature.
[0077] A dry powder and a wet cake sample were prepared from the silicon compound-coated silver fine particle dispersion discharged from the fluid processing device and collected in a beaker b. The preparation method was performed according to a conventional method for this type of treatment, the discharged silicon compound-coated silver fine particle dispersion was collected, the silicon compound-coated silver fine particles were allowed to settle, and the supernatant liquid was removed. After that, washing and settling were repeated with 100 parts by mass of pure water, and washing was repeated until the conductivity of the washing liquid containing the silicon compound-coated silver fine particles became 10 μS / cm or less. A part of the wet cake of the silicon compound-coated silver fine particles finally obtained was dried at -0.10 MPaG at 25 ° C. for 20 hours to obtain a dry powder. The remaining portion was used as a wet cake sample.
[0078] [Table 1]
[0079] [Table 2]
[0080] [Table 3]
[0081] [Table 4]
[0082] In Examples 1-1 to 1-3, the treatment temperature was changed when metal fine particles were precipitated and a fluid containing a silicon compound (silicon compound raw material liquid) was allowed to act on the metal fine particles in order to change the ratio of Si-OH bonds or the ratio of Si-OH bonds / Si-O bonds. In Examples 1-4 to 1-6, the concentration of sulfuric acid contained in the fluid containing a silicon compound was changed from that in Example 1-1 to change the pH when metal fine particles were precipitated and a fluid containing a silicon compound was allowed to act on the metal fine particles. In Examples 1-7 to 1-9, the formulations of the metal raw material liquid, metal precipitation solvent, and silicon compound raw material liquid were changed, and the treatment temperature was changed.
[0083] As a further example of the modification of the functional group contained in the silicon compound-coated silver fine particles, hydrogen peroxide was applied to the silicon compound-coated silver fine particles obtained in Example 1-1. Specifically, the silicon compound-coated silver fine particles obtained in Example 1-1 were added to propylene glycol so that the silicon compound-coated silver fine particles were 0.1% by mass, and the silicon compound-coated silver fine particles were homogeneously mixed and dispersed by stirring for 30 minutes at a preparation temperature of 30°C and a rotor rotation speed of 20000 rpm using a high-speed rotary dispersion emulsification device Clearmix (product name: CLM-2.2S, manufactured by M-Technique Co., Ltd.) to prepare a silicon compound-coated silver fine particle dispersion liquid. While stirring the above dispersion at 20000 rpm using Clearmix, 35% by mass hydrogen peroxide water (manufactured by Kanto Chemical Co., Ltd.) was added, and the treatment was continued for 30 minutes while maintaining the rotation speed of Clearmix at 20000 rpm and the treatment temperature at 30°C to 35°C. After the treatment, a dry powder and wet cake sample of the silicon compound-coated silver microparticles were prepared in the same manner as in Examples 1-1 to 1-9. The amount of hydrogen peroxide added was 0.005 mol times the amount of hydrogen peroxide relative to the silver contained in the silicon compound-coated silver microparticles in Example 1-10, 0.01 mol times in Example 1-11, and 0.1 mol in Example 1-12.
[0084] The silicon compound-coated silver particles of Example 1-1 were heat-treated using an electric furnace as a treatment to change the functional group contained in the silicon compound of the silicon compound-coated silver particles. The heat treatment conditions were as follows: Example 1-1: untreated, Example 1-13: 100°C for 30 minutes, Example 1-14: 200°C for 30 minutes, and Example 1-15: 300°C for 30 minutes.
[0085] The silicon compound-coated silver particles of Example 1-1 were treated in a desiccator in a fuming sulfuric acid atmosphere in order to introduce sulfo groups by reacting sulfonic acid with the Si-OH groups contained in the silicon compound-coated silver particles as a treatment for changing the functional groups contained in the silicon compound of the silicon compound-coated silver particles. The heat treatment conditions were as follows: Example 1-1: untreated, Example 1-16: room temperature (25°C) for 120 minutes, Example 1-17: warm (25°C) for 480 minutes.
[0086] FIG. 1 shows the results of mapping using STEM of the silicon compound-coated silver microparticles obtained in Example 1-1, and FIG. 2 shows the results of line analysis at the position indicated by the dashed line in the HAADF image in FIG. 1. In FIG. 1, (a) is a dark field image (HAADF image), (b) is the mapping result of oxygen (O), (c) is silicon (Si), and (d) is the mapping result of silver (Ag). FIG. 2 shows the results of line analysis at the position indicated by the dashed line in the HAADF image in FIG. 1, and shows the atomic % (mol %) of elements detected in the line portion from one end of the particle to the other. As can be seen in FIG. 2, oxygen and silicon were detected up to both ends of the analysis range in the line analysis, but silver was not detected up to about several nm inside from the end of the particle, and it can be seen that the surface of the silver microparticles is coated with a silicon compound containing silicon oxide. As can be seen in FIG. 1 and FIG. 2, the silicon compound-coated silver microparticles obtained in Example 1-1 were observed as silver microparticles whose entire particles were covered with a silicon compound. The silicon compound-coated oxide particles obtained in Examples 1-2 to 1-17 also obtained the same STEM mapping and line analysis results as in Example 1-1. However, in Example 1-6, the silver fine particles were not entirely covered with a silicon compound, and a silicon compound-coated silver fine particle was also confirmed in which a part of the surface of the silver fine particles was coated with a silicon compound containing silicon oxide. In the present invention, at least a part of the surface of the metal fine particles can be coated with a silicon compound to form a silicon compound-coated metal fine particle. In addition, in Examples 1-9, 1-14, and 1-15, a hollow layer was observed between the silver fine particles and the silicon compound coating the surface.
[0087] FIG. 3 shows the FT-IR measurement results for the silicon compound-coated silver particles obtained in Examples 1-7 at a wave number of 750 cm. -1 From 1300cm -1 As shown in FIG. 3, in this embodiment, the results of waveform separation for the wave number 750 cm -1 From 1300cm -1 As a result of waveform separation of the peak in the region of wave number 850 cm -1 From 950cm -1Among the peaks derived from Si-OH bonds separated in the waveform region, the peak that is assigned to the peak with the largest area ratio is determined as the peak derived from Si-OH bonds, and the wave number is 1000 cm. -1 More than 1300cm -1 Among the peaks derived from Si-O bonds separated into the following regions, the peak with the largest area ratio was determined as the peak derived from Si-O bonds, and the wavenumber was 750 cm -1 From 1300cm -1 The ratio of the area of the peak assigned to the Si-OH bond to the total area of the peaks obtained by waveform separation of the peaks in this region was defined as the ratio of the Si-OH bond, and the ratio of the area of the peak assigned to the Si-O bond was defined as the ratio of the Si-O bond, thereby calculating the ratio of the Si-OH bond and the ratio of the Si-OH bond / Si-O bond.
[0088] FIG. 4 shows the XRD measurement results of the silicon compound-coated silver microparticles obtained in Example 1-1. As shown in FIG. 4, only peaks derived from Ag were detected in the XRD measurement. That is, it was confirmed that the silicon compound containing silicon oxide confirmed in the above STEM and IR measurements was an amorphous silicon compound. In addition, similar XRD measurement results were obtained for Examples 1-2 to 1-15.
[0089] Table 5 shows the average primary particle size, Si-OH bond ratio (Si-OH bond ratio), Si-O bond ratio (Si-O bond ratio), Si-OH bond / Si-O bond ratio (Si-OH bond / Si-O bond ratio) of the silicon compound-coated silver fine particles obtained in Examples 1-1 to 1-15, and the dispersed particle size of the dispersion liquid obtained by dispersing the silicon compound-coated silver fine particles obtained in each Example in pure water or toluene (manufactured by Kanto Chemical Co., Ltd.) as a dispersion medium, using the volume average particle size obtained by particle size distribution measurement. In this Example, dispersibility is evaluated as one of the characteristics of the silicon compound-coated metal fine particles, and dispersibility is evaluated by the dispersed particle size and the dispersed particle size relative to the average primary particle size (dispersed particle size / average primary particle size). To prepare the dispersions, silicon compound-coated silver microparticles were added to each dispersion medium so that the content was 0.1 mass %, and the mixture was mixed and dispersed homogeneously by stirring for 30 minutes at a preparation temperature of 30°C and a rotor rotation speed of 20,000 rpm using a Clearmix to prepare a silicon compound-coated silver microparticle particle dispersion.
[0090] [Table 5]
[0091] As shown in Table 5, by increasing the Si-OH bond ratio and the Si-OH bond / Si-O bond ratio, the dispersed particle size and the dispersed particle size / average primary particle size tend to become smaller when pure water and ethanol are used as the dispersion medium, and by decreasing the Si-OH bond / Si-O bond ratio, the dispersed particle size and the dispersed particle size / average primary particle size tend to become smaller when toluene is used as the dispersion medium. In addition, in Examples 1-16 and 1-17, the sulfo group, which is a hydrophilic functional group, was confirmed in the IR measurement results, but the dispersibility in pure water decreased and the dispersibility in toluene improved by decreasing the Si-OH bond ratio or the Si-OH bond / Si-O bond ratio. Figure 5 shows a TEM photograph observed using a collodion film made from the aqueous dispersion of the silicon compound-coated silver fine particles obtained in Example 1-1.
[0092] In the following Examples 2 to 4, the metal particles coated with a silicon compound were produced by changing the metal element in the metal particles coated with a silicon compound (Example 2, Example 3) or the processing equipment (Example 4). Although the metal elements or processing equipment were different, conditions with the same sub-number in each Example are conditions in which the purpose in producing the metal particles coated with a silicon compound is the same and the silicon compound-coated metal particles were produced or processed under similar conditions. The same is true for the list of analysis results and evaluation results for each Example (Example 2: [Table 10], Example 3: [Table 15], Example 4: [Table 16]).
[0093] Example 2 Hereinafter, in Example 2, silicon compound-coated copper microparticles in which at least a portion of the surface of copper microparticles is coated with a silicon compound will be described as metal microparticles. Except for the preparation conditions shown in Tables 6 to 9, the microparticles were prepared under the same conditions as in Example 1. Table 10 shows the analysis and evaluation results of the obtained silicon compound-coated copper microparticles. Note that, for the substances shown by the chemical formulas and abbreviations in Tables 6 to 8, copper nitrate trihydrate (manufactured by Wako Pure Chemical Industries, Ltd.) was used as Cu(NO3)2·3H2O, which is different from the substances shown in Tables 1 to 3, and the same substances as in Example 1 were used otherwise.
[0094] Example 3 Hereinafter, in Example 3, silicon compound-coated nickel microparticles in which at least a portion of the surface of nickel microparticles is coated with a silicon compound will be described as metal microparticles. Except for the preparation conditions shown in Tables 11 to 14, the preparation was carried out under the same conditions as in Example 1. Table 15 shows the analysis and evaluation results of the obtained silicon compound-coated nickel microparticles. Note that, for the substances shown by the chemical formulas and abbreviations in Tables 11 to 13, nickel nitrate hexahydrate (manufactured by Kanto Chemical Co., Ltd.) was used as Ni(NO3)2·6H2O, which is different from the substances shown in Tables 1 to 3 or Tables 6 to 8, and the same substances as in Example 1 or Example 2 were used for the rest.
[0095] In Examples 2 and 3, the results of STEM mapping and line analysis and the results of XRD measurement were similar to those of Example 1. In the XRD measurement result of Example 2, only a peak derived from Cu was detected, and in the XRD measurement result of Example 3, only a peak derived from Ni was detected.
[0096] As seen in Tables 10 and 15, the same results were obtained for the silicon compound-coated copper microparticles and the silicon compound-coated nickel microparticles as in Example 1. It was found that even if the metal microparticles in the silicon compound-coated metal microparticles are different types of metal, the dispersibility of the silicon compound-coated metal microparticles can be controlled when the Si-OH bond ratio is in the range of 0.1% or more and 70% or less, and when the Si-OH bond / Si-O bond ratio is in the range of 0.001 or more and 700 or less.
[0097] [Table 6]
[0098] [Table 7]
[0099] [Table 8]
[0100] [Table 9]
[0101] [Table 10]
[0102] [Table 11]
[0103] [Table 12]
[0104] [Table 13]
[0105] [Table 14]
[0106] [Table 15]
[0107] Example 4 In Example 4, silicon compound-coated silver microparticles were produced under the same conditions as in Example 1, except that the apparatus and the method of mixing and reacting the A, B, and C liquids described in JP 2009-112892 A were used. Here, the apparatus described in JP 2009-112892 A was the apparatus described in FIG. 1 of the same publication, with the inner diameter of the stirring vessel being 80 mm, the gap between the outer end of the stirring tool and the inner circumferential side surface of the stirring vessel being 0.5 mm, and the rotation speed of the stirring blade being 7200 rpm. In addition, the A liquid was introduced into the stirring vessel, and the B liquid was added to the thin film of the A liquid pressed against the inner circumferential side surface of the stirring vessel, mixed, and reacted.
[0108] The results of STEM mapping, line analysis and XRD measurement were similar to those of Example 1.
[0109] Table 16 shows the analysis and evaluation results for the silicon compound-coated silver microparticles obtained in Example 4. As seen in Table 16, in Example 4, which was performed using an apparatus different from that described in Patent Document 5, it was found that dispersibility can be controlled by controlling the Si-OH bond ratio or the Si-OH bond / Si-O bond ratio contained in the silicon compound-coated metal microparticles, as in Examples 1 to 3.
[0110] [Table 16]
[0111] Example 5 Example 5 shows an example of producing silicon compound-coated metal microparticles using silicon compound-coated precursor particles and controlling the ratio of Si-OH bonds or the ratio of Si-OH bonds / Si-O bonds. Silicon compound-coated silicon aluminum-doped iron oxide microparticles were produced as silicon compound-coated precursor microparticles. The production conditions were based on the prescription conditions shown in Tables 17 to 19, and the silicon compound-coated silicon aluminum-doped iron oxide microparticles were produced in the same manner as in Example 1, except that the processing conditions shown in Table 20 were used. In the initial stage of Example 5, in order to produce oxide particles, the metal source liquid is described as the oxide source liquid, and the metal deposition solvent is described as the oxide deposition solvent. In addition, with regard to the substances indicated by the chemical formulas or abbreviations in Tables 17 to 19, the substances different from those shown in Tables 1 to 13 are as follows: Fe(NO3)3·9H2O was iron nitrate nonahydrate (manufactured by Kanto Chemical Co., Ltd.), and Al(NO3)3·9H2O was aluminum nitrate nonahydrate (manufactured by Kanto Chemical Co., Ltd.); otherwise, the same substances as in Examples 1 to 4 were used.
[0112] [Table 17]
[0113] [Table 18]
[0114] [Table 19]
[0115] [Table 20]
[0116] The silicon compound-coated silicon aluminum-doped iron oxide fine particles obtained in Example 5 were heat-treated in the reduction furnace by flowing argon gas containing hydrogen in the reduction furnace as a reducing atmosphere. Table 21 shows the hydrogen concentration in the gas flowing in the reduction furnace, the treatment temperature, the treatment time, the average primary particle size of the obtained silicon compound-coated metal fine particles, the ratio of Si-OH bonds (Si-OH bond ratio), the ratio of Si-O bonds (Si-O bond ratio), the ratio of Si-OH bonds / Si-O bonds (Si-OH bond / Si-O bond ratio), and the results of the dispersion particle size of the dispersion liquid in which the silicon compound-coated metal fine particles obtained in each Example were dispersed in pure water and toluene (manufactured by Kanto Chemical Co., Ltd.) as a dispersion medium, which is described using the volume average particle size obtained by particle size distribution measurement. (Note that the results for silicon compound-coated metal fine particles are Examples 5-1 to 5-10.)
[0117] [Table 21]
[0118] FIG. 6 shows the STEM mapping results of the silicon compound-coated silicon aluminum doped iron microparticles obtained in Example 5-5. As can be seen from FIG. 5, the surface of the silicon aluminum doped iron microparticles is coated with a silicon compound containing silicon oxide. Similar STEM mapping results were obtained for Examples 5-1 to 5-4 and Examples 5-6 to 5-8. It was also confirmed that the silicon contained in the silicon aluminum doped iron microparticles migrates toward the vicinity of the surface layer of the particles as the treatment temperature increases or the treatment time extends.
[0119] From the XRD measurement results, the silicon compound-coated silicon aluminum doped iron fine particles obtained under the conditions of Example 5-1 to Example 5-3 also showed peaks of oxides such as magnetite, but the silicon aluminum doped iron fine particles obtained in Example 5-4 to Example 5-8 did not show oxide peaks, but showed peaks close to the peak of only iron. As a representative, the measurement results of Example 5-5 are shown in FIG. 7. In FIG. 8, the peak positions of iron (Fe:Metal) in the database for the peak list of the measurement results shown in FIG. 7 are shown by enlarging the vicinity of each peak. As can be seen in FIG. 8, the XRD measurement results of the silicon aluminum doped iron fine particles obtained in Example 5-5 show peaks close to iron, but the peak positions are shifted from iron itself. It is considered that the above XRD measurement results were obtained because the silicon aluminum doped iron fine particles are formed of a solid solution of iron, silicon, and aluminum.
[0120] As seen in Table 21, it was found that silicon compound-coated metal microparticles can be obtained by treating the silicon compound-coated precursor microparticles in a reducing atmosphere, and the dispersibility of the silicon compound-coated metal microparticles can also be controlled by controlling the Si-OH bond / Si-O bond ratio contained in the silicon compound-coated metal microparticles.
Claims
1. A silicon compound-coated metal microparticle, in which at least a portion of the surface of a metal microparticle made of at least one metal element or semi-metal element is coated with a silicon compound, characterized in that the ratio of Si-OH bonds contained in the silicon compound-coated metal microparticle is controlled to be 0.1% or more and 70% or less.
2. The silicon compound-coated metal microparticles are metal microparticles made of at least one metal element or semi-metal element, at least a portion of the surface of which is coated with a silicon compound, and the silicon compound-coated metal microparticles are characterized in that the ratio of Si-OH bonds to Si-O bonds contained in the silicon compound-coated metal microparticles, i.e., the ratio of Si-OH bonds / Si-O bonds, is controlled to be 0.001 or more and 700 or less.
3. The silicon compound-coated metal fine particles described in claim 1 or 2, characterized in that the ratio of Si-OH bonds or the ratio of Si-OH bonds / Si-O bonds contained in the silicon compound-coated metal fine particles is controlled by a functional group modification treatment.
4. The silicon compound-coated metal particles according to any one of claims 1 to 3, characterized in that the functional group modification treatment is at least one reaction selected from substitution reactions, addition reactions, elimination reactions, dehydration reactions, condensation reactions, reduction reactions, and oxidation reactions.
5. The silicon compound-coated metal microparticles according to any one of claims 1 to 4, characterized in that at least a portion of the surface of a single metal microparticle is coated with a silicon compound, the metal microparticle has a primary particle diameter of 1 μm or less, and the primary particle diameter of the silicon compound-coated metal microparticles is 100.5% or more and 190% or less of the primary particle diameter of the metal microparticles.
6. The silicon compound-coated metal microparticles described in claim 5 are characterized in that the silicon compound-coated metal microparticles are core-shell type silicon compound-coated metal microparticles in which the entire surface of a single metal microparticle serving as a core is covered with a silicon compound serving as a shell.
7. The silicon compound-coated metal microparticles are characterized in that at least a portion of the surface of an agglomerate of a plurality of metal microparticles is coated with a silicon compound, the agglomerate has a diameter of 1 μm or less, and the particle diameter of the silicon compound-coated metal microparticles is 100.5% or more and 190% or less of the diameter of the agglomerate.
8. 8. The silicon compound-coated metal fine particles according to claim 1, wherein the metal element or metalloid element includes at least one element selected from the group consisting of silver, copper and nickel.
9. The ratio of the Si—OH bonds or the ratio of the Si—OH bonds / Si—O bonds is a ratio of a wave number of 750 cm in an infrared absorption spectrum of the silicon compound-coated metal fine particles measured by an attenuated total reflection method (ATR method). -1 From 1300cm -1 9. The silicon compound-coated, fine metal particles according to claim 1, which are obtained by waveform separation of peaks in the region of
10. The Si—OH bond is at a wave number of 750 cm in the infrared absorption spectrum of the silicon compound-coated metal fine particles measured using an attenuated total reflection method (ATR method). -1 From 1300cm -1 The peak in the region of 850 cm -1 From 980cm -1 The ratio of the Si-OH bonds is the peak having the largest area ratio among the peaks derived from the Si-OH bonds separated in the wave number region of 750 cm. -1 From 1300cm -1 10. The silicon compound-coated metal microparticle according to claim 1, wherein the ratio is the ratio of the area of the peak assigned to the Si-OH bond to the total area of the peaks obtained by waveform separation of the peaks in the region.
11. The Si—O bond is at a wave number of 750 cm in the infrared absorption spectrum of the silicon compound-coated metal fine particles measured using an attenuated total reflection method (ATR method). -1 From 1300cm -1 The peak in the region of 1000 cm -1 More than 1300cm -1 The Si—OH bond is the peak with the largest area ratio among the peaks derived from the Si—O bond that are separated into the following regions, and the Si—OH bond is the peak with the largest area ratio among the peaks derived from the Si—O bond that are separated into the following regions, and the Si—OH bond is the peak with the largest area ratio among the peaks derived from the Si—O bond that are separated into the following regions, -1 From 1300cm -1 The peak in the region of 850 cm -1 From 980cm -1 11. The silicon compound-coated metal microparticle according to claim 1, characterized in that the Si-OH bond / Si-O bond ratio is the ratio of the area of the peak assigned to the Si-OH bond to the area of the peak assigned to the Si-O bond, which is assigned to the peak with the largest area ratio among the peaks assigned to the Si-OH bond that have been waveform-separated in the region.
12. The silicon compound-coated metal microparticles described in any one of claims 1 to 11, characterized in that the silicon compound-coated metal microparticles are obtained by precipitating metal microparticles between relatively rotating processing surfaces that can approach and separate from each other, and continuously coating the surfaces of the metal microparticles with a silicon compound following the precipitation.
13. A silicon compound-coated metal microparticle described in any one of claims 1 to 12, characterized in that the silicon compound-coated metal microparticle contains silicon inside the metal microparticle at least before being subjected to heat treatment, and after being subjected to heat treatment, the silicon has migrated from the inside of the metal microparticle toward the outer periphery compared to before being subjected to heat treatment.
14. The ratio of the Si—OH bonds is controlled to 0.1% or more and 70% or less, or the ratio of the Si—OH bonds / Si—O bonds is controlled to 0.001 or more and 700 or less, 14. The silicon compound-coated metal fine particles according to claim 1, characterized in that the dispersibility of the silicon compound-coated metal fine particles in a solvent is controlled.
15. A coating composition, a transparent material composition, a magnetic composition, a conductive composition, a coloring composition, a reaction composition, or a catalyst composition, comprising the silicon compound-coated metal fine particles according to claim 1 .
Citation Information
Patent Citations
Silica-coated gold particulates, manufacturing method therefor and red pigment
JP2003342496A
Silica-coated aluminum pigment and its production method as well as application thereof
JP2004124069A
Gold coloring pigment and method for manufacturing the same
JP2009102607A
Method for producing silica-coated metal composite powder
JP4644390B2
Nickel metal powder and process for producing nickel metal powder
WO2013151172A1