Carbon-carbon nanotube hybrid materials and methods of producing the same
The in-situ synthesis of CNT hybrids on carbon particles using surfactants and scalable reactors addresses the challenges of high costs and dispersion issues, achieving enhanced performance and cost-effectiveness by ensuring uniform CNT distribution and high loading.
Patent Information
- Application Number
- JP2024159522
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-04-30
- Filing Date
- 2024-09-13
- Publication Date
- 2024-12-05
AI Technical Summary
The incorporation of carbon nanotubes (CNTs) with carbon particles in existing applications is limited by high production costs, self-assembly issues, and difficulty in dispersion, leading to reduced performance enhancement due to low CNT loading and uneven distribution, which is costly and inefficient.
An in-situ synthesis method using carbon particles as catalyst supports and surfactants in aqueous solutions to disperse metal catalysts, allowing for the growth of CNTs on the particle surface, thereby creating a dense and uniform CNT carpet with controlled reaction conditions in scalable reactors.
This method enables high-quality CNT hybrids with increased CNT loading, improved performance, and reduced manufacturing costs, overcoming the limitations of physical mixtures by ensuring uniform distribution and maintaining the high aspect ratio of CNTs.
Smart Images

Figure 2024169494000001_ABST
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to Provisional Patent Application No. 62 / 841,104, filed April 30, 2019, the entire disclosure of which is incorporated herein by reference.
[0002] The present disclosure relates to carbon-carbon nanotube hybrid materials. [Background technology]
[0003] Carbon nanotubes (CNTs) are tubes of graphene with nanoscale diameters (approximately 1 nm to 10 nm) and high aspect ratios (length to diameter ratios of hundreds to thousands). CNTs are the strongest material per unit weight, yet are also tough and flexible. High-quality CNTs are highly crystalline and have very high chemical and thermal stability (>500°C). CNTs have higher electrical conductivity per unit weight than any other carbon particle, including natural graphite, synthetic graphite, graphene, carbon black, and activated carbon (except for high-quality graphene). In most applications of CNTs, it is highly desirable to incorporate CNTs in combination with carbon particles already used in these applications to further improve performance. There are several successful commercial examples of this, but all use a physical mixture of CNTs and carbon particles. For example, CNTs and natural graphite are used in negative electrodes to extend the cycle life of lithium-ion batteries and improve the charge / discharge rate, CNTs and natural graphite are used in lead-acid batteries to extend the cycle life, and CNTs and carbon black are used in positive electrodes to extend the cycle life of lithium-ion batteries.
[0004] If it were more affordable and practical to effectively incorporate CNTs into these applications, there would be many more commercial examples combining CNTs with carbon particles. Conventional CNT synthesis methods result in CNT production costs per unit weight that are much higher (10-1,000 times) than the carbon particles they are intended to reinforce. Thus, CNTs can only be obtained affordably when using small amounts of CNTs (usually less than 10% of the weight of the carbon particles, more commonly less than 1%). This economic constraint clearly limits the impact of CNTs on performance enhancement. Furthermore, creating a physical mixture of CNTs with carbon particles typically requires creating a dispersion of CNTs in a fluid. However, CNTs are notoriously difficult to disperse, as they self-organize into ropes or become highly entangled in a "bird's nest" structure upon synthesis, which can be costly. Properly dispersing CNTs in a fluid requires significant energy and unconventional processing that can result in significant damage to the CNTs, i.e., sidewall defects (destroying the properties of the CNTs) and / or reduced length of the CNTs (destroying the desired high aspect ratio and the ability of the CNTs to enhance the properties of the carbon particles). Furthermore, the desired high aspect ratio of CNTs increases the viscosity of the fluid mixture so significantly that it severely limits the concentration of CNTs that can be dispersed in the fluid (typically less than 10% of the fluid, more typically less than 1%). This rheological constraint limits the amount of CNTs that can be added to a physical mixture of CNTs and carbon particles, limiting the impact of CNTs on performance.
[0005] There is another notable limitation in creating physical mixtures of CNTs and carbon particles. In many cases, the properties of carbon particles are best achieved when the CNTs are on the surface of the carbon particles. The ideal structure would be a relatively dense coating or "carpet" of CNTs on the surface of the carbon particles, but this structure is difficult to create during physical mixing; many of the CNTs remain agglomerated together and do not come into contact with the carbon particles. Also, due to the practical constraints mentioned above, it is not possible to fully pack the surface of the carbon particles with CNTs to maximize their properties. Summary of the Invention
[0006] New hybrid materials containing carbon particles "carpeted" with carbon nanotubes (CNTs) can be made by in-situ synthesis of CNTs on the surface of carbon particles. The resulting CNT hybrids can have significantly better properties than the carbon particles alone. They also have better properties than physical mixtures of CNTs and carbon particles and can be manufactured at lower cost. The resulting CNT hybrids can also allow higher CNT loadings than physical mixtures of CNTs and carbon particles, resulting in even better properties.
[0007] Our in-situ synthesis method allows the production of a wide range of carbon-CNT hybrid compositions. Carbon-CNT hybrids can be made using carbon particles. In some embodiments, the carbon particles include natural graphite, synthetic graphite, graphene, carbon black, activated carbon, etc. The CNT compositions can be multi-walled, few-walled, double-walled, or single-walled CNTs (MWCNT, FWCNT, DWCNT, SWCNT, respectively).
[0008] Carbon-CNT hybrid materials are used in a wide range of applications including, but not limited to, electrode materials for batteries and supercapacitors; conductive and / or reinforcing additives for inks, coatings, polymers, rubbers, etc.; air and water purification; catalyst supports; refractories; flame retardants; rheology modifiers; RF shielding; and gas and / or energy storage.
[0009] The in-situ synthesis method creates carbon-CNT hybrids that address all of these constraints associated with physical mixtures of CNTs and carbon particles: The CNT loading can be easily increased significantly; CNTs can completely cover the surface of the carbon particles; Expensive dispersion treatments are not required for CNTs; The high aspect ratio of CNTs does not need to be compromised; The cost of synthesizing CNT hybrids can be significantly reduced, making them more affordable for targeted applications.
[0010] The in-situ synthesis method utilizes features that enable high-quality carbon-CNT hybrids to be produced at large scale and at low cost, including the use of scalable, low-cost recipes to prepare well-controlled catalysts, and the achievement of well-controlled reaction conditions (e.g., temperature, gas composition, residence time, uniform mixing, etc.) when the catalyst is contacted with an appropriate carbon-containing feed gas (CCFG) in a commercial-scale reactor.
[0011] In one non-limiting example, an in-situ synthesis method is catalytic chemical vapor deposition (CCVD) using metal-supported catalysts, which is a method commonly used for commercial-scale production of CNTs. Under appropriate reaction conditions, when CCFG comes into contact with the metal-supported catalyst, CCFG decomposes at the catalytic metal sites, providing carbon atoms for CNT growth (via crystallization). Catalyst supports for commercial-scale production of CNTs are typically composed of metal oxide particles. After synthesis, the metal oxide particles are removed (by acid decomposition) to produce CNTs of sufficiently high purity for applications such as energy storage (e.g., battery electrodes). It is important to note that the cost of the metal oxide particles (which constitute more than 95% of the total weight of the catalyst) plus the cost of removing them from the final product (which consumes large amounts of expensive acid, generates hazardous waste, and incurs further costs for waste treatment and disposal) constitutes a significant portion of the overall CNT production cost.
[0012] In the CNT hybrids described in this disclosure, carbon particles are used as catalyst supports. Since the carbon support is an integral part of the CNT hybrid product, it leads to significant cost savings compared to traditional CNT production using metal oxides as catalyst supports. First, the cost of the "catalyst support" is no longer an "extra" cost. Also, the cost of removing the catalyst support by acid decomposition is no longer necessary.
[0013] However, because carbon particles are hydrophobic, it is difficult to prepare carbon-supported catalysts using conventional methods of impregnating metal oxide particles with aqueous metal salt solutions. In the present disclosure, this challenge is addressed by incorporating a surfactant into the catalyst recipe, which allows for uniform dispersion of catalytic metals on the surface of hydrophobic carbon particles, even when aqueous metal salt solutions are used. The uniform dispersion of small metal catalytic sites allows for the selective synthesis of CNTs and other (non-CNT) forms of carbon (e.g., carbon nanofibers) that may grow if the metal catalytic sites are too large.
[0014] The disclosed method also allows for complete removal of the surfactant from the catalyst surface without extra processing steps and without damaging the carbon particles. This can be achieved by pyrolyzing the surfactant when the catalyst particles are typically heated in the reactor immediately prior to in-situ CNT synthesis. Removing the surfactant prior to in-situ synthesis avoids contamination of the metal catalyst sites. Also, because the surfactant is removed by pyrolysis, the carbon particles are not damaged (e.g., oxidized) during surfactant removal. This is helpful since the carbon particles are an integral part of the CNT hybrid product.
[0015] The method of the present invention also utilizes scalable reactor platforms, such as fluidized bed reactors and rotary kiln reactors, which can be operated in batch or continuous flow modes. These reactor platforms have been successful in commercial scale production of CNTs, today at hundreds of tons per year. However, CNT hybrid applications may require production scales of 10,000 tons per year or more. All of the CNT hybrid examples described in the literature utilize non-scalable reactor platforms (suitable for producing CNT hybrids at scales of less than 0.1 tons per year). Furthermore, these examples appear to be limited to natural graphite or graphene (exfoliated natural graphite) as catalyst supports, to the synthesis of larger diameter (low quality) MWCNTs, and to the production of CNT carpets that do not adequately cover the surface of the carbon particles to maximize performance.
[0016] This disclosure is distinguished from the "CNT hybrid" prior art in at least the following ways: The catalyst composition and preparation method allows for the formation of uniformly distributed tiny (nanoscale) metal catalytic sites on the surface of carbon particles using aqueous solutions of metal salts with specific surfactants; The use of scalable reactor platforms, such as fluidized bed reactors and rotary kiln reactors, that allow precise control of reaction conditions; The ability to create CNT carpets on various types of carbon particles; The ability to synthesize a wide variety of CNTs (MWCNTs to SWCNTs); The ability to synthesize small diameter CNTs (<20 nm) with superior properties to larger diameter CNTs (usually >20 nm, more commonly >50 nm); The ability to achieve a more uniform and more substantial (higher areal density) CNT carpet on carbon particles.
[0017] Prior art teaches the deposition of active metals onto carbon support materials using organic solvents, electrochemical or chemical vapor deposition (CVD) techniques, which are more costly than the method of the present invention, produce large, non-uniform metal catalytic sites, and do not allow for well-controlled, selective synthesis of small diameter CNTs.
[0018] The use of certain surfactants for the aqueous impregnation of metal salts has several advantages compared to other impregnation methods of the prior art using organic solvents. These advantages are: Most metal salts are more soluble in water than in organic solvents. The surfactants can prevent the precipitation of metal salts. The surfactants control the formation of metal nanoparticles with a predetermined size distribution and improve their deposition on the surface of the highly hydrophobic carbon material. The surfactants disperse the carbon particles well during the impregnation step, allowing these particles to adsorb the active metal on their surface. The surfactants also aid in the formation of a homogeneous paste with improved rheology, especially at high solids concentrations. The surfactants separate the solid particles from each other during the drying process. No grinding or sieving steps are required before adding the supported catalyst to the reactor for in-situ synthesis.
[0019] All embodiments and features described below can be combined in any manner which is technically possible.
[0020] In one embodiment, a carbon-carbon nanotube (CNT) hybrid material includes carbon particles and CNTs on the surfaces of the particles, in some embodiments, the CNTs comprise greater than about 3.2 weight percent of the hybrid material.
[0021] Some embodiments include one of the above and / or the following features, or any combination thereof. In one embodiment, the CNTs comprise at least about 10 weight percent of the hybrid material. In one embodiment, the CNTs comprise at least about 12 weight percent of the hybrid material. In one embodiment, the CNTs comprise at least one of multi-walled, few-walled, double-walled, and single-walled CNTs. In one embodiment, the carbon particles comprise at least one of natural graphite, synthetic graphite, graphene, carbon black, and activated carbon. In one embodiment, the CNTs have a length in the range of about 3 microns to about 10 microns, a diameter of about 10 nm to about 50 nm, and a length-to-diameter aspect ratio of about 60 to about 1000.
[0022] In another aspect, a method for producing a carbon-carbon nanotube (CNT) hybrid material includes providing carbon particles, dispersing a metal catalyst on the surface of the carbon particles using an aqueous metal salt solution, and exposing the catalyzed carbon particles to a carbon-containing gas to grow carbon nanotubes (CNTs) at the catalyst sites.
[0023] Some embodiments include one of the above and / or the following features, or any combination thereof. In one embodiment, the CNTs comprise greater than about 3.2 weight percent of the hybrid material. In one embodiment, the CNTs comprise at least about 10 weight percent of the hybrid material. In one embodiment, the CNTs comprise at least about 12 weight percent of the hybrid material. In one embodiment, the carbon particles comprise at least one of natural graphite, synthetic graphite, graphene, carbon black, and activated carbon.
[0024] Some embodiments include one of the above and / or the following features, or any combination thereof. In one embodiment, the metal salt solution includes a surfactant. In one embodiment, the surfactant is non-ionic. In one embodiment, the surfactant is removed by pyrolysis before CNT growth begins. In one embodiment, a fluidized bed reactor or a rotary kiln reactor is used to grow the CNTs. In one embodiment, the method is effective in converting graphite flakes into a more spheroidized structure. In one embodiment, the CNTs have a length in the range of about 3 microns to about 10 microns, a diameter of about 10 nm to about 50 nm, and a length-to-diameter aspect ratio of about 60 to about 1000.
[0025] In another embodiment, a method for producing a carbon-carbon nanotube (CNT) hybrid material includes providing carbon particles, dispersing a metal catalyst on the surface of the carbon particles using an aqueous solution of a metal salt and a surfactant, and exposing the catalyzed carbon particles to a carbon-containing gas to grow carbon nanotubes (CNTs) at the catalytic sites, the CNTs comprising greater than about 3.2% by weight of the hybrid material. In one embodiment, the surfactant is non-ionic. In one embodiment, the surfactant is removed by pyrolysis before CNT growth begins. [Brief description of the drawings]
[0026] [Figure 1] Illustrates a graphite-CNT hybrid material and the basic method by which it is produced. [Diagram 2] FIG. 1 is a block diagram of a system that can be used to produce carbon-CNT hybrid materials. [Diagram 3] 1 illustrates steps in a method for producing carbon-CNT hybrid materials. [Figure 4] 1 is a prior art SEM image of a carbon nanotube-graphite hybrid material. [Figure 5A]1 is a SEM image at low magnification corresponding to a carbon nanotube-graphite hybrid material of the present disclosure. [Figure 5B] 1 is a SEM image at high magnification corresponding to a carbon nanotube-graphite hybrid material of the present disclosure. [Figure 6] Thermogravimetric analysis of the carbon nanotube-graphite hybrid material disclosed herein. The signals at approximately 550 °C and 650 °C correspond to CNTs and graphite, respectively. In all gravimetric analyses herein, the plot lines are associated with the correct axes with arrows pointing to the axes. [Figure 7A] FIG. 2 is a SEM image of the carbon nanotube-graphite hybrid material obtained when the catalyst was prepared using a surfactant solution. [Figure 7B] 1 is a SEM image of the carbon nanotube-graphite hybrid material obtained when the catalyst is prepared without the use of a surfactant solution. [Figure 8] This shows the results of thermogravimetric analysis of the carbon nanotube-graphite hybrid material obtained when the catalyst was prepared without using a surfactant solution. [Figure 9A] Comparison of the discharge rates of CNT-graphite hybrid and commercial graphite at 22°C. [Figure 9B] Comparison of discharge rates between CNT-graphite hybrid and commercial graphite at 0°C and 30°C. [Figure 10] Figures 10A and 10B are SEM images of the carbon nanotube-graphite hybrid materials obtained with reaction times of 3 and 30 minutes, respectively. [Figure 11] SEM image of natural graphite flakes with an average particle size of about 5 μm. [Figure 12] 12A and 12B are the thermogravimetric analysis results corresponding to the carbon nanotube-graphite hybrid materials obtained using a rotary tube reactor for reaction times of 3 and 30 minutes, respectively. [Figure 13]1 shows the results of thermogravimetric analysis of carbon nanotube-graphite hybrid materials synthesized in a fluidized bed reactor. [Figure 14A] This is an SEM image of conductive carbon. [Figure 14B] 1 is a SEM image of a carbon nanotube-conductive carbon hybrid material. [Figure 15] 1 is a SEM image of a carbon nanotube-activated carbon hybrid material. [Figure 16] 1 is a SEM image showing SWCNT bundles in a graphite hybrid material. [Figure 17] 1 shows the results of thermogravimetric analysis of SWCNT-graphite hybrid materials. [Figure 18] 1 shows the optical absorption spectrum of a SWCNT-graphite hybrid material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] Described herein are carbon-CNT hybrid materials and methods for producing such materials. Aspects of the disclosure relate to catalyst preparation methods and processes for producing CNT-carbon hybrid materials (materials sometimes referred to herein as "hairy carbon"). In particular, the disclosure describes novel catalyst preparation methods and synthesis conditions for making uniform CNT-carbon hybrid materials. CNT-carbon hybrid materials are suitable for applications such as energy storage (lithium ion, lead acid, supercapacitor, electrode manufacturing), high performance tires and rubber products (racing cars, belts, gaskets, construction equipment, trucks), additives for plastics, electrostatic discharge compounds, high performance coatings, and other industrial applications.
[0028] One of the main challenges in the preparation of heterogeneous catalysts using hydrophobic supports such as carbon materials with different morphologies, specific surface areas, and porosities is to finely control the deposition and dispersion of active metals on the carbon surface during the catalyst impregnation and drying steps. Due to poor wettability and weak interactions of metal ions with the carbon surface, the deposition of active metals is nonuniform and poorly controlled. For these reasons, many of the works published in the literature use organic solvents such as polyethylene glycol, ethanol, and isopropyl alcohol to enhance the wettability of the solids instead of using aqueous metal solutions. Other prior art metal deposition methods include chemical vapor deposition of iron pentacarbonyl in the gas phase or ferrocene in aerosols, and electrochemical deposition of metals on carbon electrodes. In contrast to the prior art, the present disclosure allows for the fabrication of different types of CNT-carbon hybrid materials such as single-walled CNTs, few-walled CNTs, and multi-walled CNTs. Prior art has reported CNT-graphite materials with large diameter MWCNTs (>60 nm diameter) and carbon fiber materials with low surface coverage.
[0029] The use of organic solvents as in the prior art brings about a series of disadvantages when producing catalysts on a large scale. For example, some metal salts have limited solubility in these solvents. Also, even if the use of organic solvents improves the wettability of the surface, the metal still exhibits weak interactions with the surface. Therefore, the deposition of the active metals cannot be well controlled. Most of the active metals are preferentially deposited on the edge parts sandwiched between the lamellar sheets of graphite, and fewer metal atoms are deposited on the surface of the basal plane. When the active metals aggregate, the cluster particle size increases, which leads to the formation of large MWCNTs and carbon fibers. The diameter of the carbon nanotubes is highly dependent on the size of the metal clusters, due to the low selectivity of the reaction. In addition, organic solvents are volatile, flammable, and hazardous, so special equipment is required for operation and safety. Finally, the high price of organic solvents has a negative impact on the production cost of the catalyst.
[0030] These technical limitations have been overcome by using surface modifiers (so-called surfactants) together with aqueous metal solutions to improve the wettability properties of the solid and to control the adsorption and dispersion of metals on the carbon particle surface. These surface modifiers form ad-micelles by interaction of their hydrophobic tails with the carbon surface, which change the surface roughness and hydrophilic properties of the carbon substrate. The active metal is deposited uniformly on the exposed hydrophilic surface of the ad-micelles. It may also be located surrounding the outer surface of the surfactant micelles formed in solution. The metal-surfactant micelles can be deposited on the carbon surface during the impregnation and drying process. In this case, the metal particle size depends on the amount of active metal surrounding the micelles, the type of micelles, and their size and aggregation number.
[0031] In some examples, for the synthesis of CNT-carbon hybrid materials, an aqueous solution containing a soluble metal salt (nitrate, acetate, ammonium salt, or citrate salt) of cobalt, nickel, iron, or molybdenum and a non-ionic surfactant (Triton X-100 "Polyethylene glycol p-(1,1,3,3-tetramethylbutyl)-phenyl ether" (available from Sigma-Aldrich Corp., St. Louis, Missouri, USA) is used. , alcohol ethoxylates, polyethylene glycols, polypropylene glycols and mixtures thereof (e.g., Pluronic p123, also available from Sigma-Aldrich Corp., etc.) can be employed. The total amount of metal will depend on the maximum content allowed for the particular application.
[0032] CNT-carbon hybrid materials are developed by growing carbon nanotubes on conventional carbon substrates such as graphite powder, carbon black, graphene, carbon fibers, and glassy carbon. A catalyst is used to initiate the growth of CNTs in the presence of a carbon source (ethylene, acetylene, methane, carbon monoxide, etc.). The reaction is carried out using catalytic chemical vapor deposition (CCVD) at temperatures between 300 and 1000 °C in reactors such as fluidized beds, moving beds, and rotary kilns. Catalytically active metals consist of combinations of transition elements from groups VIII and / or VIB of the periodic table. Catalyst supports are based on graphite, graphene, carbon black, and activated carbon. The preparation of the catalyst consists of impregnating the catalyst support in the presence of an aqueous solution containing the above metals and a surfactant. As surfactants, mainly nonionic surfactants are used, but other types of surfactants such as zwitterionic surfactants, catanionic surfactants, and amphoteric surfactants can also be used. This catalyst preparation method provides a high density of CNT surface coverage with long tubular shape and narrow diameter distribution through better control of metal deposition on carbon support particles. The type of carbon nanotubes synthesized depends on the type of active metal, the carbon source used, and the reaction temperature. The resulting MWCNT-graphite hybrid materials exhibit superior battery performance compared to conventional carbon materials when used as electrodes in lithium-ion batteries, lead-acid batteries, and supercapacitors.
[0033] FIG. 1 illustrates a graphite-CNT hybrid material 18 and a basic process 10 by which it can be produced. As described elsewhere herein, the same basic process steps can be used to produce hybrid materials from carbons other than graphite. The starting carbon material 12 (graphite flakes in this non-limiting example) is mixed with an aqueous solution containing a metal salt (of the catalytic metal(s)) and a suitable surfactant. An active metal 16 is then present on the carbon surface. CNTs are then synthesized using this catalyst. If the process involves graphite flakes, the flakes can be spheroidized by the growth of CNTs to produce spherical graphite-CNT hybrid material 18, with the carbon surface covered with CNTs. Further details on the exemplary process are described herein.
[0034] FIG. 2 is a block diagram of a system 20 that can be used to produce carbon-CNT hybrid materials, and FIG. 3 provides steps of a method 30 for producing carbon-CNT hybrid materials using the system 20. A high-speed mixer 22 can be used to contact carbon powder or flakes with an aqueous solution containing metal salts and surfactants. In some examples, a paste is formed in the mixer, and the materials are kept under controlled moisture and temperature for the desired contact time. The sample is then dried, for example using a vacuum dryer 23, leaving a fine powder. The metal salts are then decomposed in an oven 24, which typically operates at less than 200° C. This forms precursors of the metal oxide catalyst on the surface of the carbon particles. The sample is then placed in a reactor 25. In some examples, the reactor 25 is a fluidized bed reactor or a rotary kiln reactor, although other reactors can be used. The surfactant is removed by pyrolysis (under a flow of inert gas from an inert gas source 27) at moderate temperatures. Pyrolysis can be performed during the normal heat-up of the sample. The carbon catalyst is then exposed to CNT growth conditions in a reactor 25 using a carbon-containing gas source 26. Once CNT growth is complete, the sample is cooled under non-oxidizing conditions, which can be assisted by an inert gas source 27. Specific process details are described below.
[0035] In some embodiments, the carbon-CNT hybrid material includes carbon particles and greater than about 3.2 weight percent CNTs on the surface of the particles. In one embodiment, the carbon particles include at least one of natural graphite, synthetic graphite, graphene, carbon black, and activated carbon. In one embodiment, the CNTs comprise at least about 10 weight percent of the hybrid material. In another embodiment, the CNTs comprise at least about 12 weight percent of the hybrid material. The CNTs can be of any morphology, and in some embodiments, include at least one of multi-walled, few-walled, double-walled, and single-walled CNTs. In some embodiments, the CNTs have lengths ranging from about 3 microns to about 10 microns. In some embodiments, the CNTs have diameters ranging from about 10 nm to about 50 nm. In some embodiments, the CNTs have length-to-diameter aspect ratios ranging from about 60 to about 1000.
[0036] In some embodiments, the metal salt solution includes a surfactant. In one embodiment, the surfactant is non-ionic. In some embodiments, the surfactant is removed by pyrolysis before CNT growth begins. In some embodiments, a fluidized bed reactor or a rotary kiln reactor is used to grow the CNTs. In one embodiment, this method is effective in converting graphite flakes into a more spheroidized structure.
[0037] In the examples described herein, the metal oxide composition in the catalyst varies between 2 and 7 wt.%, as determined by ash method and TGA analysis. Typical values are in the range of 3.5 to 5.5 wt.%. In one example, the atomic ratio of Co(Ni) / Fe or Co+Ni / Fe is about 1:2. In the examples, the purity of the graphite catalyst support is 96.0 wt.% or higher, with typical values being 99.0 wt.% or higher, and most preferably 99.5 wt.% or higher. After metal deposition, the surface area of the catalyst does not change significantly with respect to the value obtained with the graphite support.
[0038] In some embodiments, the surfactant concentration varies from about 0.1 to about 5.0 wt.%, with typical values ranging from 0.5 to 2.0 wt.%, and most preferably from 0.5 to 1.0 wt.%. The removal of the surfactant is carried out in an inert atmosphere, typically under nitrogen flow in a fluidized bed reactor or rotary tube reactor, at least at the decomposition temperature of the surfactant. For Triton X-100 surfactant, this temperature is about 300C.
[0039] In some embodiments, the decomposition of the metal salt is carried out in two successive steps in an oven under air flow at 60° C. for about 2 hours and then at 180° C. for about 2 hours.
[0040] For growing MWCNTs, catalyst particle sizes range from about 10 to about 15 nm, as determined by SEM. In the case of Pt supported on carbon black, it is possible to determine the catalyst particle size and dispersion using chemisorption techniques and electron microscopy. Pt / carbon black is reduced to metal, which becomes the active and stable phase during the reaction. In the case of CNTs, the oxide precursor is activated by a reduction-carbonization reaction to form metal clusters, which are aggregates of supported metal carbides, followed immediately by CNT growth. A method for measuring the active phase particle size of CNTs is to observe the metal particles attached to the tubes with a TEM.
[0041] In some examples, the reactor process conditions depend on the carbon source and the type of CNTs being synthesized. In the example of MWCNT synthesis using ethylene, the reaction temperature varies from 600 to 800 C, with typical values being 650 C to 730 C. For SWCNT production from CO, the reaction temperature varies from 650 to 800 C, with typical values being 680 to 760 C. For FWCNT synthesis from methane, the reaction temperature varies from 900 to 1000 C, with typical values being 950 to 975 C.
[0042] The gas composition varies depending on the type of CNT to be synthesized. In the MWCNT embodiment, a C2H4 / H2 ratio of 100 / 0 to 70 / 30 V / V% is used, with a typical composition of 70 / 30 to 80 / 20 V / V%. The N2 composition can vary from 0 to 40 V%, with a typical value in the range of 20 to 35 V%. In the SWCNT embodiment, the CO / inert gas (e.g., N2, Ar) ratio is 100 / 0 V / V% to 60 / 40 V%, with a typical value of 100 / 0 to 80 / 20 v / v%. In the FWCNT embodiment, the CH4 / H2 ratio is in the range of 30 / 70 V / V% to 10 / 90 v / v%, with a typical value of 15 / 85 to 25 / 75 v / v%.
[0043] In the obtained carbon-CNT hybrid materials, it is observed by SEM that most of the CNTs grow according to the base mode mechanism, where the CNTs are bonded to the substrate.
[0044] In one embodiment, high purity graphite (carbon content about 99.8 wt) with an average size of about 20 μm was contacted with a solution containing 0.042 g / cc cobalt acetate, 0.137 g / ml ferric nitrate, and 0.01 g / ml Triton X-100 surfactant. A thin paste was obtained using a standard industrial high speed mixer, which was then left under moisture and temperature controlled conditions for about 12 hours before drying. Drying was performed using a freeze dryer at 77° K under vacuum or a rotavapor at T≧60° C under vacuum. Drying can also be done using a double-cone tumbling dryer machine. The obtained graphite catalyst powder sample was loaded into a fluidized bed reactor. Surfactants, acetates, and nitrates were decomposed and removed during heating of the reactor from room temperature to 675 °C under N2 flow. Then, a mixture of 80% V ethylene, 20% Ar, and 5% H2 was introduced into the reactor (total gas flow rate 2 L / min) to grow CNTs. The system was maintained under the same conditions for about 30 min. The reactor was cooled to room temperature under N2 flow (2 L / min). A dense carpet of MWCNTs with a thickness of about 0.38 μm, diameter of about 10–20 nm, and length of about 5–10 μm was formed on the graphite surface. The graphite particles were completely covered by CNTs. Thermogravimetric analysis (TGA) results showed that the estimated amount of MWCNTs in the hybrid material was about 12 wt.%, with residual metal oxides less than 1 wt.%.
[0045] The same graphite catalyst was prepared using the same procedure, but without the use of a surfactant, which resulted in a low density MWCNT carpet and partial particle coverage, with most of the CNTs growing on the edge faces of the graphite particles and fewer on the basal faces. TGA analysis confirmed that less MWCNTs were produced without the use of a surfactant.
[0046] The hybrid material was used to fabricate a lithium ion anode. Battery performance tests were performed at different temperatures. The hybrid material had a larger energy capacity at different discharge rate capabilities at various temperatures. For example, at C / 5 and 22C, at a discharge rate of 5, the graphite-CNT hybrid material had about 1.5 times the percentage of total capacity (about 90% vs. about 60% for graphite). In another example, at 0°C and a discharge rate of 1, the capacity of the graphite-CNT hybrid material increased by about 40% (about 85% vs. about 60% for graphite). In another example, at -30°C, the capacity of graphite was zero, while the graphite-CNT hybrid material had more than 50% of the total capacity at a discharge capacity of about 0.2.
[0047] In another example, graphite material with an average particle size of about 5μ was used as the catalyst support. The catalyst was prepared by the same procedure as described above. The synthesis of CNTs was carried out in a rotary tube reactor. About 1 gram of catalyst was contacted with a gas flow of 2L / min of ethylene-H2 mixture (75% V ethylene) at 675C for reaction times of 3 and 30 minutes. SEM images of the hybrid materials obtained at reaction times of 3 and 30 minutes show a high density of CNT carpet in both samples. The density of this carbon carpet is higher than that of the hybrid material synthesized using a catalyst with a graphite particle size of 20μ. Also, the particles of the hybrid material show a spherical shape, even though the starting graphite particles are not uniform. This is probably due to the graphite becoming more spherical during the CNT growth process. The relative percentage CNT / graphite ratio composition increases with increasing reaction time.
[0048] Decreasing the graphite particle size from 20μ to 5μ increases the surface area by approximately 3 times and the pore volume by approximately 1.8 times. As MWCNTs grow on the surface of the graphite, both the surface area and the pore volume increase. This increase is more significant when smaller sized graphite particles are used. For a reaction time of 3 minutes, a significant increase in the surface area (361% increase) and pore volume (122% increase) is observed, and the amount of MWCNTs deposited on the graphite surface (~22 wt.%) is also significantly higher.
[0049] In one embodiment, the CNT-graphite hybrid material is synthesized from two different graphite materials. The difference lies in the average particle size. The use of graphite with a particle size of 5 microns increases the surface area and pore volume. The increased surface area improves the surface dispersion of the active metals. Hence, higher CNT coverage is obtained. TGA analysis of the CNT-graphite hybrid material obtained in a rotary tube reactor with graphite with a particle size of about 5 microns at reaction times of 3 and 10 minutes, respectively, confirmed that the CNT content increases dramatically with reaction time.
[0050] When this catalyst was loaded into a fluidized bed reactor and the synthesis conditions described above were used (graphite with a particle size of approximately 5 microns, reaction time of 10 minutes), TGA analysis confirmed that the reactor produced similar material.
[0051] In one example, the CoFe surfactant solution described above was contacted with a conductive carbon black support. In this case, 5 grams of carbon catalyst support was impregnated with excess solution (1 gram solid / 10 ml solution) at 55°C for 2 hours, after which the solvent was removed from the solid using a freeze-drying device. The resulting dry powder was charged into a rotary kiln reactor, after which a N2 gas flow was introduced to remove the air in the system. After heating to 675°C with N2 gas, ethylene was introduced into the reactor at 1.5 L / min. The system was maintained at the same conditions for about 30 minutes. The reactor was cooled to room temperature with N2 flow (2 L / min). SEM analysis corresponding to the starting carbon black material and the resulting carbon black-CNT hybrid material confirmed that the carbon black is composed of chains of elementary spherical particles with diameters ranging from 30 to 60 nm and particle sizes ranging from 5 to 20 μ. Upon initiating the growth of CNTs, the spherical carbon chains start to separate from each other, forming a carpet of MWCNTs with diameters of 10 to 20 nm.
[0052] In one example, CoFe supported on activated carbon was prepared following the same procedure as described above. The catalyst support had a BET surface area of about 1649 m. 2 / g, pore volume 0.91cc / g, and maximum oxidation rate at 620℃. About 60% of the pores are smaller than 2nm in diameter. This is about 1000m 2 The micropore area is expressed as 1.0 μm / g (0.54 cc / pore volume). The outer diameter of the MWCNTs is approximately 10-20 nm. The growth of MWCNTs occurs at the outer surface region of the carbon particles. This is evidenced by the SEM images which clearly show the formation of MWCNTs at the outer surface of the carbon particles.
[0053] In one embodiment, 5μ of graphite material was dissolved in cobalt nitrate, ammonium heptamolybdate (Mo:Co molar ratios of 1:1 and 2:0) and 0.5 wt.% Triton. The mixture was contacted with a solution containing X-100 surfactant aqueous solution. It was mixed in a high-speed mixer apparatus to form a smooth paste. After aging for 6 hours, it was dried in a freeze-drying apparatus. The synthesis of SWCNTs was carried out using a rotary kiln reactor. The catalyst was activated by reduction of the metal under H2 flow at 550 °C for 30 min. After the activation step, the temperature of the reactor was increased to 700 °C under nitrogen flow, and then a flow of CO was introduced to carry out SWCNT synthesis for 30 min. SEM images show SWCNT bundles with diameters ranging from 2 to 9 nm. Thermogravimetric analysis confirmed graphite and SWCNT-graphite hybrid materials. The appearance of a second signal around 550 °C is attributed to the presence of CNTs. Near-infrared fluorescence (NIRF) analysis was carried out to confirm the presence of SWCNTs in the hybrid materials as suggested by SEM, TGA, and optical absorption spectra. As a result, when using 532nm, 638nm, 671nm, and 785nm lasers, the range was 8,000 to 11,000cm -1 High-intensity emission peaks were observed in the optical frequency region of (6,5), (7,5), (9,4), and (8,3). By integrating these signals, it was found that the hybrid material mainly contained semiconducting SWCNTs of (6,5), (7,5), (9,4), and (8,3) with proportions of 41%, 17%, 15%, and 13%, respectively.
[0054] Some examples are given below. Example 1: Comparison of the catalyst preparation methods of the prior art and the present disclosure
[0055] Prior Art: Catalyst Preparation and CNT-Graphite Material Synthesis Conditions
[0056] Approximately 2.4 g of natural graphite with an average particle size of about 25 μm was dispersed in 50 ml of alcohol, and an aqueous solution of nickel nitrate was added dropwise. The composition of carbon and nickel was 400:1 to 100:1 in molar ratio. The solution was then heated under vigorous magnetic stirring until the solvent was completely evaporated. The sample was then dried at 110 °C under vacuum for 10 h to remove moisture. The nickel-supported graphite catalyst was spread on a quartz boat and transferred to the right side of a tubular furnace. Another boat containing 2 g of carbon source (2,3 dipicolinic acid (C7H5NO4)) was placed in the left zone of the furnace. After cooling to room temperature, the resulting CNT-coated graphite was treated with 10% HNO3 for 2 h to remove traces of Ni nanoparticles dispersed on the graphite surface, and then vacuum dried at 110 °C for 10 h.
[0057] Figure 4 (prior art, taken from "Hairy Graphite of High Electrochemical Performance Prepared Through In-Situ Decoration of Carbon Nanotubes", Huiyuan Zheng, Guobin Zhu, Qunting Qu, Siming Yang, Honghe Zheng. Electrochimica Acta 233 (2017) 229-236 ) shows the SEM image corresponding to the hairy graphite (HG) material obtained under the best catalyst formulation (C / Ni molar ratio 200:1). MWCNTs with diameters of about 60-80 nm were observed, with some tubes showing lengths of about 10 μm. Some parts of the graphite material were not completely covered by CNTs, and amorphous carbon was observed on the surface. The estimated amount of MWCNTs in the sample was about 3.2 wt.%.
[0058] Zhao et al. ("Carbon Nanotube growth in the pores of expanded graphite by chemical vapor deposition", J. Zhao, Q. Guo, J. Shi, L. Liu, J. Jia, Y. Liu, H. Hang., Carbon 47 (2009) 1747-1751) studied the growth of carbon nanotubes in the pores of expanded graphite by CCVD. They impregnated the expanded graphite particles with an aqueous metal solution containing nitrates of Co, Fe, or Ni. The optimal catalyst formulation was obtained with an aqueous Co concentration of 0.025 mol / L. The synthesis of MWCNTs was carried out in a boat reactor at 850 °C for 30 min using acetylene as the carbon source. The average diameter of MWCNTs is about 70 nm. A carpet of CNTs was observed on some of the graphite particles. The hairy graphite composite showed improved tensile strength properties (15.2 MPa CNT / flexible graphite vs. 10 MPa flexible graphite).
[0059] Tour et al. ("Graphen-Carbon Nanotube Hybrid Materials and Use as Electrodes" JM Tour, Y. Zhu, L. Li, Z. Yan, J. Lin., US Patent 9455094, 27 September 2016) describe a method for the preparation of graphene-carbon nanotube hybrid materials and their use as electrodes for supercapacitors. The preparation of the catalyst consists of the steps of i) associating a graphene film with a substrate (copper foil), ii) applying a catalyst based on Fe supported on alumina and a carbon source to the graphene film, and iii) growing CNTs on the graphene film. The deposition of the metal and the alumina support on the graphene film is both carried out using an electron beam method. Methane, ethane, ethylene, etc. are used as carbon sources. The reaction temperature is 550-1100 °C, and ultra-short SWCNT or MWCNT tubes are obtained.
[0060] Takeuchi et al. ("Carbon Electrode for a Nonacoustic Secondary ElectroChemical Cell", ES Takeuchi; RA Leising, U.S. Pat. No. 5,443,929, Aug. 22, 2019) disclose a method for the manufacture of an electrode based on carbon filaments (carbon fibers) supported on a conventional carbon substrate (carbon black, graphite, carbon fiber, glassy carbon). The carbon filaments have a diameter of 50-200 nm. The catalyst comprises a combination of cobalt oxide and iron complexes such as ferrocene and / or iron pentacarbonyl. This carbon-carbon fiber hybrid material is said to be suitable for the manufacture of anodes for rechargeable alkali metal electrochemical cells.
[0061] This disclosure
[0062] Approximately 40 g of high purity graphite (99.8% wt carbon content) with an average size of approximately 20 μm was contacted with 30 ml of a solution containing 0.042 g / cc cobalt acetate, 0.137 g / ml ferric nitrate, and 0.01 g / ml Triton X-100 surfactant. A thin paste was obtained using a typical industrial high speed mixer, which was then left under moisture and temperature controlled conditions for approximately 12 hours before drying. Drying was performed using a freeze dryer at 77° K under vacuum or a rotavapor at T > 60° C under vacuum. It can also be dried using a double cone tumbling dryer machine.
[0063] About 20 g of the obtained graphite catalyst powder was loaded into a fluidized bed reactor. Surfactants, acetates, and nitrates were decomposed and removed during heating of the reactor from room temperature to 675 °C under N2 flow. Subsequently, a mixture of 5% H2 in 20% Ar in 80% V ethylene (total gas flow rate 2 L / min) was introduced into the reactor, after which the system was maintained at the same conditions for about 30 min. The reactor was cooled to room temperature under N2 flow (2 L / min).
[0064] Figures 5A and 5B show SEM images taken at 4,000x and 7,000x, respectively, corresponding to the HG material obtained by this process. A dense carpet of MWCNTs with a thickness of about 0.38μ, a diameter of 10-20 nm (vs. 60-80 nm in the prior art) and a length of about 5-10μ is formed on the graphite surface. The graphite particles are completely covered by the CNTs. Thermogravimetric analysis (TGA), shown in Figure 6, clearly shows two very well differentiated signals corresponding to MWCNTs and graphite, respectively. The estimated amount of MWCNTs in the HG material is about 12 wt.% (vs. 3.2 wt.% in the prior art) and residual metal oxides are less than 1 wt.%.
[0065] Example 2: Comparison of catalyst preparation with and without surfactant
[0066] A second Co-Fe / graphite catalyst was prepared following the same procedure as described in Example 1, but in this case without the use of Triton X-100 surfactant. SEM images in Figures 7A and 7B show a comparison of hairy graphite (HG) material obtained when the catalyst was prepared with and without surfactant in the metal solution, respectively. In Figure 7A, the graphite is substantially covered with CNTs when surfactant was used. On the other hand, in Figure 7B, a low density carpet of MWCNTs and partial particle coverage can be seen when the catalyst was prepared without surfactant. Most of the tubes grow on the edge faces of the graphite particles, with fewer on the basal faces. TGA analysis in Figure 8 shows that the HG material prepared without surfactant produces less MWCNTs compared to Figure 6.
[0067] The HG samples obtained with Triton X-100 surfactant were used to fabricate lithium ion negative electrodes. Battery performance tests were conducted at different temperatures. Figures 9A and 9B show the performance results obtained for HG and the conventional graphite material used as a reference. As observed, the HG material exhibited higher energy capacity at different discharge rate capabilities at various temperatures.
[0068] Example 3: Effect of graphite particle size on MWCNT content and surface coverage, BET surface area, and pore volume
[0069] In this example, graphite material with an average particle size of about 5μ was used as the catalyst support. The catalyst was prepared by the same procedure as described in Example 1. The synthesis of CNTs was carried out in a rotary tube reactor. About 1 gram of catalyst was contacted with a gas flow of 2 L / min of ethylene-H2 mixture (75% V ethylene) at 675°C and reacted for 3 and 30 minutes. Figures 10A and 10B show SEM images of the HG material obtained at reaction times of 3 and 30 minutes, respectively.
[0070] A dense CNT carpet can be observed in both samples. The density of this carbon carpet is higher than that of the HG material synthesized using a catalyst with a graphite particle size of 20μ. The HG particles show a spherical shape, despite the non-uniformity of the starting graphite particles (Figure 11). This represents another competitive advantage compared to conventional graphite materials, which require a step to spheronize the graphite before using it in electrode fabrication, which increases the production cost. Figures 12A and 12B show the thermogravimetric analysis results (using a rotary tube reactor) of the carbon nanotube-graphite hybrid material obtained with reaction times of 3 min (Figure 12A) and 30 min (Figure 12B). The signals at about 600 C and about 700 C correspond to CNT and graphite, respectively. The longer the reaction time, the higher the composition of the relative CNT / graphite ratio.
[0071] Table 1 shows the BET surface area, pore volume, and MWCNT content of different graphite and HG-synthesized hybrid materials. Decreasing the graphite particle size from 20μ to 5μ increases the surface area by about 3 times and the pore volume by about 1.8 times, respectively. When MWCNTs grow on the graphite surface, both the surface area and the pore volume increase significantly. This increase is more significant when smaller sized graphite particles are used. For a reaction time of 3 min, a significant increase in the surface area (361% increase) and pore volume (122%) is observed, and the amount of MWCNTs deposited on the graphite surface (~22 wt.%) is also quite high. This provides a new competitive advantage for the commercial production of these materials in a continuously operated reactor.
[0072] Table 1 below shows the properties of CNT-graphite hybrid materials synthesized from two different graphite materials. The difference is in the average particle size. When graphite with a particle size of 5 microns is used, the surface area and pore volume are increased. The increased surface area allows for better surface dispersion of the active metals. Therefore, higher CNT coverage is obtained as shown in Table 1.
[0073] [Table 1]
[0074] Figures 12A and 12B show the TGA analysis results corresponding to the CNT-graphite hybrid materials obtained in a rotary tube reactor with graphite particles of about 5 microns for reaction times of 3 and 10 minutes. The CNT content increases dramatically with reaction time.
[0075] Example 4: Comparison of fluidized bed reactor and rotary reactor
[0076] In this example, the catalyst prepared in Example 3 was loaded into a fluidized bed reactor and the synthesis conditions were the same as those described in Example 1. Figure 13 shows the TGA analysis obtained for a fluidized bed CNT-graphite hybrid material with a graphite particle size of about 5 microns and a reaction time of 10 minutes. This TGA analysis is comparable to that in Figure 12B. Thus, both reactors yielded materials with similar TGA patterns (MWCNT content and thermal stability), demonstrating the flexibility of the manufacturing process that can be used here.
[0077] Example 5: Hairy Carbon Black
[0078] In this example, the CoFe surfactant solution of Example 1 was contacted with a conductive carbon black support. In this case, 5 grams of carbon catalyst support was impregnated with excess solution (1 g solid / 10 ml solution) at 55°C for 2 hours, after which the solvent was removed from the solid using a freeze-drying device. The resulting dry powder was charged into a rotary kiln reactor, after which a N2 gas flow was introduced to remove the air in the system. After heating to 675°C under N2 gas, an ethylene flow (1.5 L / min) was introduced into the reactor. The system was maintained at the same conditions for about 30 minutes. The reactor was cooled to room temperature under N2 flow (2 L / min).
[0079] FIG. 14A shows the results of an SEM analysis corresponding to a carbon black material (Carbon Super-P material). FIG. 14B is an SEM of a carbon black-CNT hybrid material prepared from the carbon black of FIG. 14A as described above. This carbon black consists of elementary spherical particles arranged in chains with diameters of 30-60 nm and particle sizes ranging from 5-20 μm. Upon initiating CNT growth, the spherical carbon chains start to separate from one another and a carpet of MWCNTs with diameters of 10-20 nm is formed.
[0080] Example 6: Woollen Activated Carbon
[0081] In this example, CoFe supported on activated carbon (CEP21KS from Power Carbon Technology Co. Ltd., Korea) was prepared using the same procedure as described in Example 1. The catalyst support had a BET surface area of approximately 1649 m 2 / g, pore volume 0.91cc / g, and maximum oxidation rate at 620℃. About 60% of the pores are smaller than 2nm in diameter. This is about 1000m 2 The micropore area is expressed as 1.0 μm / g (0.54 cc / pore volume). The outer diameter of the MWCNTs is approximately 10-20 nm. The growth of MWCNTs occurs at the outer surface region of the carbon particles. This is evident from the SEM image shown in Figure 15, which clearly shows the formation of MWCNTs at the outer surface of the carbon particles.
[0082] Example 7: SWCNT-graphite hybrid
[0083] In this example, 5μ of graphite material was contacted with a solution containing cobalt nitrate, ammonium heptamolybdate (1:1 and 2:0 molar ratios of Mo:Co) and 0.5 wt.% of Triton X-100 surfactant in water. It was mixed in a high-speed mixer to form a smooth paste. After aging for 6 hours, it was dried in a freeze-drying apparatus. The synthesis of SWCNTs was carried out using a rotary kiln reactor. The catalyst was activated by reduction of the metal under flowing H2 at 550 °C for 30 min. After the activation step, the temperature of the reactor was increased to 700 °C under flowing nitrogen, and then CO flow was introduced to carry out SWCNT synthesis for 30 min.
[0084] The SEM image in Figure 16 shows bundles of SWCNTs with diameters ranging from 2 to 9 nm. The thermogravimetric analysis in Figure 17 shows graphite and SWCNT-graphite hybrid materials. A second signal appears around 550 °C, which is due to the presence of CNTs. Near-infrared fluorescence (NIRF) analysis was performed to confirm the presence of SWCNTs in the hybrid materials, as suggested by the SEM, TGA, and optical absorption spectra in Figures 16 to 18, respectively. The results showed that the 8,000-11,000 cm-wavelength peaks were observed when using 532 nm, 638 nm, 671 nm, and 785 nm lasers. -1 High-intensity emission peaks were observed in the optical frequency region of (6,5), (7,5), (9,4), and (8,3). By integrating these signals, it was found that the hybrid material mainly contained semiconducting SWCNTs of (6,5), (7,5), (9,4), and (8,3), with the proportions of 41%, 17%, 15%, and 13%, respectively.
[0085] Although a number of embodiments have been described, it will nevertheless be understood that additional modifications may be made without departing from the scope of the inventive concepts described herein, and accordingly, other embodiments are within the scope of the following claims. The present invention can be carried out in the following configurations (1) to (20). (1) A carbon-carbon nanotube (CNT) hybrid material, Carbon particles; CNTs on the surface of the carbon particles, A carbon-carbon nanotube (CNT) hybrid material, characterized in that the CNTs comprise greater than about 3.2 weight percent of the hybrid material. (2) The hybrid material according to (1) above, characterized in that the CNTs account for at least about 10% by weight of the hybrid material. (3) The hybrid material according to (1) above, wherein the CNTs account for at least about 12% by weight of the hybrid material. (4) The hybrid material according to (1) above, wherein the CNTs include at least one of multi-walled, few-walled, double-walled and single-walled CNTs. (5) The hybrid material according to (1) above, wherein the carbon particles include at least one of natural graphite, synthetic graphite, graphene, carbon black, and activated carbon. (6) The hybrid material described in (1) above, wherein the CNTs have a length in the range of about 3 microns to about 10 microns, a diameter of about 10 nm to about 50 nm, and a length-to-diameter aspect ratio of about 60 to about 1000. (7) A method for producing a carbon-carbon nanotube (CNT) hybrid material, comprising: Providing carbon particles; dispersing a metal catalyst on the surface of carbon particles using an aqueous metal salt solution; and exposing the catalyst-treated carbon particles to a carbon-containing gas to grow carbon nanotubes (CNTs) at the catalyst sites. (8) The method according to (7) above, wherein the CNTs account for more than about 3.2% by weight of the hybrid material. (9) The method according to (7) above, wherein the CNTs account for at least about 10% by weight of the hybrid material. (10) The method according to (7) above, wherein the CNTs account for at least about 12% by weight of the hybrid material. (11) The method according to (7) above, wherein the carbon particles include at least one of natural graphite, synthetic graphite, graphene, carbon black, and activated carbon. (12) The method according to (7) above, wherein the metal salt solution contains a surfactant. (13) The method according to (12) above, wherein the surfactant is nonionic. (14) The method according to (12) above, characterized in that the surfactant is removed by pyrolysis before the CNT growth begins. (15) The method according to (7) above, characterized in that the CNTs are grown using a fluidized bed reactor or a rotary kiln reactor. (16) The method according to (7) above, characterized in that it is effective in converting graphite flakes into a more spheroidized structure. (17) The method according to (7) above, wherein the CNTs have a length in the range of about 3 microns to about 10 microns, a diameter of about 10 nm to about 50 nm, and a length-to-diameter aspect ratio of about 60 to about 1000. (18) A method for producing a carbon-carbon nanotube (CNT) hybrid material, comprising the steps of: Providing carbon particles; dispersing a metal catalyst on the surface of carbon particles using an aqueous solution containing a metal salt and a surfactant; and exposing the catalytically treated carbon particles to a carbon-containing gas to grow carbon nanotubes (CNTs) at the catalytic sites, wherein the CNTs comprise greater than about 3.2% by weight of the hybrid material. (19) The method according to (18) above, characterized in that the surfactant is nonionic. (20) The method according to (19) above, characterized in that the surfactant is removed by pyrolysis before the start of CNT growth.
Claims
1. A carbon-carbon nanotube (CNT) hybrid material, comprising: Carbon particles having a starting BET surface area; CNTs on the surface of the carbon particles; A hybrid material, wherein the CNTs comprise at least 10 weight percent of the hybrid material, the hybrid material having a BET surface area that is increased by at least 200% over the starting BET surface area.
2. 10. The hybrid material of claim 1, wherein the CNTs include at least one of multi-walled, few-walled, double-walled and single-walled CNTs.
3. 10. The hybrid material of claim 1, wherein the CNTs have a length ranging from about 3 microns to about 10 microns, a diameter from about 10 nm to about 50 nm, and a length-to-diameter aspect ratio of about 60 to about 1000.
4. 10. The hybrid material of claim 1, wherein the hybrid material has a BET surface area that is at least 300% increased over the starting BET surface area.
5. 10. The hybrid material of claim 1, wherein the hybrid material has a BET surface area that is at least 500% increased over the starting BET surface area.
6. 10. The hybrid material of claim 1, wherein the carbon particles have a starting pore volume, and the hybrid material has a pore volume that is at least 100% increased from the starting pore volume.
7. 10. The hybrid material of claim 1, wherein the carbon particles have a starting pore volume, and the hybrid material has a pore volume that is at least 300% increased from the starting pore volume.
8. 10. The hybrid material of claim 1, wherein the CNTs comprise 12 to 70 weight percent of the hybrid material.
9. 9. The hybrid material of claim 8, wherein the carbon particles are made more spherical with 12-70 weight percent of the CNTs on the surface of the carbon particles.
10. The hybrid material of claim 9, wherein the carbon particles are graphite flakes.
11. The hybrid material of claim 10, wherein the graphite flakes have an average particle size of about 5 microns to about 20 microns.
12. 1. A method for producing a carbon-carbon nanotube (CNT) hybrid material, comprising: Providing carbon particles having a starting BET surface area; catalytically treating the carbon particles by dispersing a metal catalyst on the surface of the carbon particles using an aqueous metal salt solution and a surfactant; removing the surfactant from the carbon particles by pyrolysis in a stream of inert gas; and exposing the catalytically treated carbon particles to a carbon-containing gas to grow carbon nanotubes (CNTs) at the catalytic sites, thereby creating a carbon-CNT hybrid material, wherein the CNTs comprise at least 10 weight percent of the hybrid material, and the hybrid material has a BET surface area that is increased by at least 200% over the starting BET surface area.
13. 13. The method of claim 12, wherein the CNTs comprise at least one of multi-walled, few-walled, double-walled and single-walled CNTs.
14. 13. The method of claim 12, wherein the CNTs have lengths ranging from about 3 microns to about 10 microns, diameters from about 10 nm to about 50 nm, and length-to-diameter aspect ratios of about 60-100.
15. 13. The method of claim 12, wherein the hybrid material has a BET surface area that is at least 300% increased over the starting BET surface area.
16. 13. The method of claim 12, wherein the hybrid material has a BET surface area that is at least 500% increased over the starting BET surface area.
17. 13. The method of claim 12, wherein the carbon particles have a starting pore volume and the hybrid material has a pore volume that is at least 100% increased from the starting pore volume.
18. 13. The method of claim 12, wherein the carbon particles have a starting pore volume and the hybrid material has a pore volume that is at least 300% increased from the starting pore volume.
19. The method of claim 12, wherein the CNTs comprise 12 to 70 weight percent of the hybrid material.
20. 20. The method of claim 19, wherein the carbon particles are rendered more spherical with 12 to 70 weight percent of the CNTs on the surface of the carbon particles.
Citation Information
Patent Citations
Carbon-carbon nanotube hybrid material and its manufacturing method
JP2022530905A