Thermoplastic resin composition
The thermoplastic resin composition with composite particles and polymer graft chains addresses the limitations of existing damping materials by enhancing interface strength, resulting in superior vibration damping and noise reduction.
Patent Information
- Application Number
- JP2024162518
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-05-29
- Filing Date
- 2024-09-19
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2040-05-28
AI Technical Summary
Existing damping materials, such as laminated metal plates with vibration-absorbing materials and alloy-type materials, suffer from limited formability, weight, and insufficient vibration damping performance, making them unsuitable for various equipment applications.
A thermoplastic resin composition containing composite particles with polymer graft chains bonded to the particle surface, enhancing the interface between elastomer and filler, thereby improving vibration damping properties.
The composition achieves excellent vibration damping performance with improved strain energy absorption, leading to reduced vibration and noise in molded articles.
Smart Images

Figure 2024169603000001 
Figure 2024169603000002 
Figure 2024169603000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermoplastic resin composition and a method for producing the same, an additive for improving the vibration-damping properties of a thermoplastic resin, and a vibration-damping material containing the thermoplastic resin composition. [Background technology]
[0002] In recent years, there has been a demand for vibration countermeasures for various devices, especially in the fields of automobiles, home appliances, and precision instruments. Generally, materials with high vibration damping properties include composite materials such as metal plates bonded to vibration absorbing materials such as rubber or asphalt, or vibration-damping steel plates in which vibration absorbing materials are sandwiched between metal plates. These vibration-damping materials maintain their shape with high-rigidity metal plates and absorb vibrations with vibration absorbing materials. In addition, there are alloy-type materials that use only metals to convert kinetic energy into thermal energy and absorb vibrations by using twin crystals or ferromagnetism. However, composite-type materials have limitations in formability because different materials are bonded together, and because metal steel plates are used, there is a problem that the product itself is heavy. In addition, alloy-type materials are heavy because they use only metal, and their vibration damping performance is insufficient.
[0003] In response to such conventional techniques, functional resin compositions having vibration suppression functions have been proposed. For example, Patent Document 1 discloses a vibration-damping resin molded article obtained by molding a polypropylene-based resin composition in which a reinforcing inorganic filler is blended with a resin component in which high-density polyethylene (PE) and an aromatic hydrocarbon resin are added and mixed with crystalline polypropylene (PP), and the resin composition is characterized in that a hydrogenated product of an aromatic vinyl-conjugated diene block copolymer is further added and mixed as a resin component. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 5-331329 Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention relates to a new thermoplastic resin composition having excellent vibration-damping properties and a method for producing the same, an additive for improving the vibration-damping properties of a thermoplastic resin, and a vibration-damping material containing the thermoplastic resin composition. [Means for solving the problem]
[0006] The present invention relates to the following [1] to [4]. [1] A thermoplastic resin composition comprising a thermoplastic resin and composite particles having polymer graft chains bonded to the particle surface. [2] A method for producing a thermoplastic resin composition, comprising the step of melt-kneading a thermoplastic resin and composite particles having polymer graft chains bonded to the particle surface. [3] An additive for improving the vibration damping properties of thermoplastic resins, comprising composite particles having polymer graft chains bonded to the particle surface. [4] A vibration-damping material comprising the thermoplastic resin composition according to [1], which comprises a thermoplastic resin and composite particles having polymer graft chains bonded to the particle surface. [5] A vibration-damping material comprising a thermoplastic resin and composite particles having polymer graft chains bonded to the particle surface. [6] A method for producing a vibration-damping material, comprising the step of melt-kneading a thermoplastic resin with composite particles having polymer graft chains bonded to the particle surface. [7] Use of composite particles having polymer graft chains bonded to the particle surface to improve the vibration damping properties of thermoplastic resins. [8] A method for improving the vibration damping properties of thermoplastic resins using composite particles having polymer graft chains bonded to the particle surface. Effect of the Invention
[0007] According to the present invention, it is possible to provide a new thermoplastic resin composition having excellent vibration-damping properties and a method for producing the same, an additive for improving the vibration-damping properties of a thermoplastic resin, and a vibration-damping material containing the thermoplastic resin composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The present inventors have newly discovered that vibration-damping properties can be improved by forming some kind of bond between the elastomer and the filler added to the thermoplastic resin composition and strengthening the interface between them. Although the mechanism is unclear, it is presumed that the strain energy in the elastomer can be increased by strengthening the interface between the elastomer and the filler. The present inventors have also newly discovered that excellent vibration-damping properties can be obtained by using composite particles obtained by the grafting from method, in which a polymer graft chain corresponding to the elastomer is polymerized from the polymerization initiation point on the surface of the particle used as the filler, as a composite particle in which an elastomer and a filler are bonded. It is presumed that this is because the grafting from method allows the polymer graft chain to be bonded to the particle surface at a high density, thereby significantly strengthening the interface between them.
[0009] [Thermoplastic resin composition] The thermoplastic resin composition of the present invention contains a thermoplastic resin and composite particles having polymer graft chains bonded to the particle surface.
[0010] [Thermoplastic resin] Examples of the thermoplastic resin include polyolefin resin, polyester resin, polyamide resin, ABS resin, polystyrene resin, polycarbonate resin, vinyl chloride resin, acrylic resin, etc. Among these, from the viewpoint of ease of handling of the obtained resin composition such as moldability, preferably one or more types selected from the group consisting of polyolefin resin, polyamide resin, and ABS resin, more preferably one or more types selected from the group consisting of polyolefin resin, and even more preferably polypropylene resin.
[0011] The mass average molecular weight of the thermoplastic resin is not particularly limited, but may be from 5,000 to 500,000.
[0012] The amount of the thermoplastic resin in the thermoplastic resin composition of the present invention is preferably 30% by mass or more, more preferably 40% by mass or more, and even more preferably 50% by mass or more, from the viewpoint of obtaining a molded article or a vibration-damping material exhibiting a desired elastic modulus. On the other hand, from the viewpoint of obtaining a molded article or a vibration-damping material exhibiting a desired vibration-damping property, it is preferably 95% by mass or less, more preferably 80% by mass or less, and even more preferably 75% by mass or less. When two or more types of thermoplastic resins are blended, the blending amount is the total amount of the thermoplastic resins.
[0013] [Composite particles] The composite particles are particles having polymer graft chains bonded to the particle surface. A known filler can be used as the particle, and examples thereof include metal oxides, metal oxide salts, metal hydroxides, metal carbonates, and cellulose. The filler is preferably one or more selected from the group consisting of metal oxides, metal oxide salts, metal hydroxides, and metal carbonates, more preferably one or more selected from the group consisting of silicon oxides such as silica, and silicates such as mica and talc, and even more preferably silica. The shape of the particle is not particularly limited, and examples thereof include plate-like, granular, needle-like, and fibrous. In this specification, the term "particle" refers to the particle used in the production of the composite particle. Examples of the polymer graft chain include homopolymers or copolymers of styrene-based monomers, nitrile-based monomers, (meth)acrylic-based monomers, unsaturated olefins, conjugated diene-based monomers, etc., and from the viewpoint of obtaining a molded article or a vibration-damping material exhibiting the desired vibration-damping properties, it is preferably one or more homopolymers or copolymers selected from the group consisting of acrylic acid, methacrylic acid, and derivatives thereof, more preferably one or more homopolymers or copolymers selected from methacrylic acid and its derivatives, and even more preferably polybutyl methacrylate. From the viewpoint of obtaining a molded article or a vibration-damping material exhibiting the desired vibration-damping properties, the bond is preferably a chemical bond, and even more preferably a covalent bond.
[0014] The glass transition temperature (Tg) of the polymer graft chain in the composite particle is preferably -30°C or higher, more preferably -10°C or higher, even more preferably 10°C or higher, and even more preferably 25°C or higher from the viewpoint of vibration damping property expression, and is preferably 80°C or lower, more preferably 50°C or lower, and even more preferably 40°C or lower from the same viewpoint. The polymer graft chain in the composite particle may have two or more glass transition temperatures (Tg), and may have a Tg other than -30°C or higher and 80°C or lower. The glass transition temperature (Tg) of the polymer graft chain in the composite particle can be controlled by the monomer, molecular weight, and molecular weight distribution used in the production of the composite particle. For example, in the case of the composite particle, it is known that Tg increases when the graft density increases and the polymer chain becomes an extended chain. In that case, Tg can be controlled by adjusting the graft density. In the temperature range near Tg, the tan δ of the viscoelasticity of the resin becomes maximum, which is effective in expressing vibration damping property, and by controlling Tg, it is possible to obtain a desired temperature. The glass transition temperature (Tg) can be measured by the method described in the Examples below.
[0015] The graft density of the polymer graft chains in the composite particles is preferably 0.001 chains / nm from the viewpoint of increasing the strain energy in the elastomer. 2 More preferably, 0.01 chains / nm 2 More preferably, 0.1 chains / nm 2 On the other hand, from the viewpoint of ease of grafting of polymer chains, it is preferable to set the number of chains to 5 / nm. 2 Less than or equal to 3 chains / nm, more preferably 2 More preferably, 1 chain / nm or less 2 Less than 0.3 chains / nm, more preferably 0.3 chains / nm 2 The graft density is measured by the method described in the Examples below.
[0016] The thickness of the polymer graft chain in the composite particle is preferably 1 nm or more, more preferably 3 nm or more, and even more preferably 5 nm or more, from the viewpoint of efficiently increasing the strain energy in the elastomer. From the same viewpoint, the thickness is preferably 1 μm or less, more preferably 100 nm or less, more preferably 40 nm or less, and even more preferably 15 nm or less. The thickness of the polymer graft chain is calculated by the method described in the examples below.
[0017] The number average molecular weight of the polymer graft chain in the composite particle is preferably 10,000 or more, more preferably 20,000 or more, and even more preferably 30,000 or more, from the viewpoint of controlling the film thickness of the polymer graft chain. From the same viewpoint, it is preferably 1,000,000 or less, more preferably 500,000 or less, and even more preferably 200,000 or less. The number average molecular weight of the polymer graft chain is measured by the method described in the examples below.
[0018] The amount of the composite particles in the thermoplastic resin composition of the present invention is preferably 1% by mass or more, more preferably 10% by mass or more, even more preferably 20% by mass or more, and even more preferably 25% by mass or more, from the viewpoint of vibration-damping property expression. On the other hand, from the viewpoint of obtaining a molded body or a vibration-damping material exhibiting a desired elastic modulus, it is preferably 75% by mass or less, more preferably 60% by mass or less, even more preferably 55% by mass or less, and even more preferably 50% by mass or less. When two or more types of composite particles are contained, the amount is the total amount of the composite particles.
[0019] The amount of the composite particles in the thermoplastic resin composition of the present invention is preferably 1 part by mass or more, more preferably 20 parts by mass or more, even more preferably 30 parts by mass or more, and even more preferably 40 parts by mass or more, relative to 100 parts by mass of the thermoplastic resin, from the viewpoint of vibration damping property expression. On the other hand, from the viewpoint of obtaining a molded body or a vibration damping material exhibiting a desired elastic modulus, it is preferably 300 parts by mass or less, more preferably 200 parts by mass or less, even more preferably 100 parts by mass or less, and even more preferably 90 parts by mass or less. The content of the polymer graft chain of the composite particles in the thermoplastic resin composition of the present invention is preferably 1 part by mass or more, more preferably 5 parts by mass or more, and even more preferably 10 parts by mass or more, relative to 100 parts by mass of the thermoplastic resin, from the viewpoint of vibration damping property expression. On the other hand, from the viewpoint of obtaining a molded body or a vibration damping material exhibiting a desired elastic modulus, it is preferably 100 parts by mass or less, more preferably 50 parts by mass or less, and even more preferably 40 parts by mass or less.
[0020] The dispersed particle size of the composite particles in the thermoplastic resin composition of the present invention is preferably 10 nm or more, more preferably 100 nm or more, and even more preferably 1 μm or more from the viewpoint of vibration damping property expression, and is preferably 200 μm or less, more preferably 100 μm or less, and even more preferably 10 μm or less from the same viewpoint. The composite particles may exist alone or as aggregates. The dispersed particle size of the composite particles is measured by the method described in the examples below.
[0021] [Method of manufacturing composite particles] The composite particles are obtained by bonding a polymer graft chain to the particle surface. The method of bonding a polymer graft chain to the particle surface is not particularly limited as long as it is a method that can perform grafting of a polymer chain, but the grafting from method in which the polymer graft chain is polymerized from the polymerization initiation point on the particle surface is preferred. The polymerization method is not particularly limited, but examples thereof include radical polymerization, anionic polymerization, cationic polymerization, etc. Among these, from the viewpoint of easy control of the molecular weight and molecular weight distribution of the polymer chain and the viewpoint of easy grafting of various copolymers, living radical polymerization, living anionic polymerization, and living cationic polymerization are preferred, and living radical polymerization is more preferred from the viewpoint of application to a wide range of monomers. As the living radical polymerization method, atom transfer radical polymerization method (ATRP method), reversible addition fragmentation chain transfer polymerization method (RAFT method), and living radical polymerization method mediated by nitroxide (NMP method) can be used, and from the same viewpoint, atom transfer radical polymerization method (ATRP method) is preferred.
[0022] More specifically, the method for producing the composite particles includes, for example, a production embodiment including the following step 2, and if necessary, the following step 1 may be carried out. The following steps 1 and 2 can be carried out under known conditions for living radical polymerization. Step 1: Attaching a polymerization initiating group to the particle surface Step 2: contacting particles having polymerization initiation groups on their surfaces with a monomer under living radical polymerization conditions
[0023] The particles having a polymerization initiating group on the surface in step 2 are not particularly limited as long as they have a binding group that bonds the particle surface and the polymer chain. The polymerization initiating group is a living radical polymerization initiating group from the viewpoint of binding a polymer graft chain to the particle surface, and is preferably an atom transfer radical polymerization initiating group, more preferably a haloacyl group, even more preferably an α-haloacyl group, even more preferably an α-bromoacyl group, and even more preferably a 2-bromoisobutyryl group. The compound that is the raw material of the binding group includes a compound having a group and a polymerization initiating group that are bound to the particle surface, and a compound having a group or a polymerization initiating group that are bound to the particle surface. Step 1 includes a step of introducing an amino group or a hydroxy group to the particle surface and a step of introducing a polymerization initiating group, and from the viewpoint of binding a polymer graft chain to the particle surface, preferably includes a step of introducing a polymerization initiating group to the particle surface after a step of introducing an amino group or a hydroxy group to the particle surface. The compound used in the step of introducing an amino group or a hydroxyl group to the particle surface is a compound having a group that bonds to the particle surface and an amino group or a hydroxyl group, and from the viewpoint of easy availability, it is preferably a silane compound, more preferably an aminoalkylsilane compound, and even more preferably 3-aminopropyltrimethoxysilane. The compound used in the step of introducing a polymerization initiator group to the particle surface is a compound having a functional group that reacts with a polymerization initiator group and an amino group or a hydroxyl group, and from the viewpoint of bonding a polymer graft chain to the particle surface, it is preferably a haloalkanoic acid derivative, more preferably a bromoalkanoic acid derivative, even more preferably a 2-bromo-2-methylpropionic acid derivative, and even more preferably 2-bromoisobutyl bromide. For example, when the particle originally has a polymerization initiation site or is formed as a result of surface treatment by plasma treatment or the like, it has a polymerization initiator group, so step 1 is not necessary, but when silica, mica, talc, glass filler, etc. that does not have a polymerization initiator group are used, step 1 may be performed. Note that, from the viewpoint of graft density adjustment, in step 1, a silane coupling agent that does not contain a polymerization initiator group may be added to the polymerization initiator group-containing silane coupling agent and used. In the step 1, in which the polymerization initiating groups are bonded to the particle surface, a method in which the particles are dispersed in a dispersion medium is preferred from the viewpoint of preventing the particles from agglomerating.
[0024] The monomer in step 2 can be a monomer constituting a thermoplastic elastomer known as a vibration-damping elastomer. Examples of the monomer constituting such a thermoplastic elastomer include styrene-based monomers, nitrile-based monomers, (meth)acrylic monomers, unsaturated olefins, conjugated diene monomers, and other monomers having specific groups in their side chains can also be used. In the step of contacting the particles having polymerization initiation groups on the surface with the monomer under living radical polymerization conditions in step 2, a method in which the particles, monomers, and composite particles are dispersed in a dispersion medium and polymerized is preferred from the viewpoint of preventing aggregation of the particles, monomers, and composite particles.
[0025] After polymerization, the composite particles may be optionally purified. In the purification step of the composite particles, in order to prevent the composite particles from agglomerating, it is preferable to disperse the composite particles in a polymer with a dispersion medium and remove the solvent. Furthermore, it is preferable to remove the metal catalyst used in the polymerization step.
[0026] The thermoplastic resin composition of the present invention may contain, as components other than those described above, a chain extender, a plasticizer, an organic crystal nucleating agent, an inorganic crystal nucleating agent, a hydrolysis inhibitor, a flame retardant, an antioxidant, a lubricant such as a hydrocarbon wax or an anionic surfactant, an ultraviolet absorber, an antistatic agent, an antifogging agent, a light stabilizer, a pigment, an antifungal agent, an antibacterial agent, a foaming agent, other polymer materials, and the like.
[0027] [Method of producing thermoplastic resin composition] The method for producing the thermoplastic resin composition of the present invention includes a production method including a step of melt-kneading a thermoplastic resin and a composite particle having a polymer graft chain bonded to the particle surface. For melt-kneading, a known kneading machine such as an internal kneader, a single-screw or twin-screw extruder, or an open roll type kneader can be used. After melt-kneading, the melt-kneaded product may be dried or cooled according to a known method. In addition, the raw materials may be mixed uniformly in advance using a Henschel mixer, a super mixer, or the like, and then subjected to melt-kneading. The melt-kneading temperature and the melt-kneading time are not necessarily set depending on the type of raw materials used, but are preferably 170 to 240°C and 15 to 900 seconds.
[0028] In the process of melt-kneading a thermoplastic resin and composite particles having polymer graft chains bonded to their particle surfaces, the amount of composite particles having polymer graft chains bonded to their particle surfaces added is, from the viewpoint of expressing vibration damping properties, preferably 1 part by mass or more, more preferably 30 parts by mass or more, and even more preferably 40 parts by mass or more, per 100 parts by mass of the thermoplastic resin; and from the same viewpoint, it is preferably 200 parts by mass or less, more preferably 100 parts by mass or less, and even more preferably 90 parts by mass or less.
[0029] [Additives] The additive of the present invention includes composite particles having polymer graft chains bonded to the particle surface. The additive of the present invention may optionally contain a chain extender, a plasticizer, an organic crystal nucleating agent, an inorganic crystal nucleating agent, a hydrolysis inhibitor, a flame retardant, an antioxidant, a lubricant such as a hydrocarbon wax or an anionic surfactant, an ultraviolet absorber, an antistatic agent, an antifogging agent, a light stabilizer, a pigment, an antifungal agent, an antibacterial agent, a foaming agent, and the like. Furthermore, the additive of the present invention may contain a part of the resin (for example, 0.1 to 50.0 mass % of the additive) that is melt-kneaded together. The additive of the present invention is used as an additive for improving the vibration damping property of a thermoplastic resin. Therefore, the present invention also discloses a method of using composite particles having polymer graft chains bonded to the particle surface for improving the vibration damping property of a thermoplastic resin.
[0030] [Vibration-damping materials] The thermoplastic resin composition of the present invention can be suitably used as a vibration-damping material for products such as audio equipment, electrical products, buildings, industrial equipment, automobile parts, motorcycle parts, containers, and the like, or for parts or housings thereof, by using various molding processing methods such as injection molding, extrusion molding, and thermoforming.
[0031] For example, when a part or a housing containing the thermoplastic resin composition of the present invention is produced by injection molding, pellets of the thermoplastic resin composition of the present invention are filled into an injection molding machine and then injected into a mold for molding.
[0032] For injection molding, a known injection molding machine can be used. For example, there can be mentioned a machine having a cylinder and a screw inserted therein as main components (J75E-D, J110AD-180H (manufactured by Japan Steel Works, Ltd.), etc.). Although the raw materials of the thermoplastic resin composition of the present invention may be supplied to a cylinder and melt-kneaded as is, it is preferable to fill the injection molding machine with the materials melt-kneaded in advance.
[0033] When a molding method other than injection molding is used, the molding may be performed according to a known method, and there are no particular limitations.
[0034] The molded article of the thermoplastic resin composition of the present invention can be suitably used as a vibration-damping material for products such as audio equipment, electrical products, buildings, industrial equipment, automobile parts, motorcycle parts, containers, etc., or their parts or housings. The application to these can be appropriately set depending on the manufacturing method, application location, and desired purpose of the parts, housings, devices, and equipment, and can be used according to the usual methods in the technical field. EXAMPLES
[0035] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples in any way.
[0036] <Glass transition temperature of polymer graft chains in composite particles> Measurement was performed according to the method of JIS K 7121. Using a differential scanning calorimeter (DSC7020 manufactured by Hitachi High-Tech Science), the composite particles were heated from 40°C to 200°C at a rate of 10°C / min, and the thermal capacity was The midpoint glass transition temperature Tmg (°C) was determined as the temperature at the point where a straight line equidistant in the vertical direction from the extended straight line of each baseline intersects with the curve of the step-like change in the glass transition in the DSC thermogram.
[0037] <Number average molecular weight of polymer graft chains in composite particles> The number average molecular weight of the polymer graft chains in the composite particles was measured by taking the number average molecular weight of the polymer chains not bonded to the composite particles, which were simultaneously produced in the process of producing the composite particles, as the number average molecular weight of the polymer graft chains. The number average molecular weight was measured by gel permeation chromatogram (GPC) using GMHHR-H+GMHHR-H (cation) as a column, chloroform as a solvent, a flow rate of 1.0 mL / min, and a column temperature of 40°C, using polystyrene as a molecular weight standard.
[0038] <Graft density of polymer chains in composite particles> Graft density (chains / nm 2 ) was calculated by measuring the graft amount (W) and the number average molecular weight (Mn) of the graft chains and using the following formula. The graft amount was calculated by thermal weight loss measurement (TG). More specifically, the temperature was raised from 40°C to 500°C at a rate of 10°C / min in air, and the weight loss rate at that time was measured. The number average molecular weight of the graft chains was calculated by the gel permeation chromatography (GPC) method shown below. Graft density (chains / nm 2 ) = Graft amount (g / nm 2 ) / number average molecular weight of grafted chains × (Avogadro's number)
[0039] <Film thickness of polymer graft chains in composite particles> The film thickness was calculated from the following formula. The polymer density of the polymer chains that are not bonded to the composite particles and are generated simultaneously in the process of producing the composite particles was taken as the polymer density of the polymer graft chains. It was measured by the pycnometer method according to JIS K 7112.
[0040]
number
[0041] <Dispersion particle size of composite particles> The composite particles in the thermoplastic resin were observed by observing the fracture surface of a test piece of the thermoplastic resin composition with a scanning electron microscope (SEM). From the image observed with the SEM, the cross sections of 30 composite particles were selected, and the major axis of each was visually read, and the average value was taken as the dispersed particle diameter. conditions Equipment: Field emission scanning electron microscope (S-4000, Hitachi, Ltd.) Acceleration magnification: 10kV Spot diameter: 8mm Magnification: 400x~5000x
[0042] [Preparation of composite particle 1] a) A step of bonding a polymerization initiating group to the particle surface a-1) Introduction of amino groups onto the surface of silica particles 40 g of silica particles (SILFIL NSS-3N, Tokuyama Corp., average particle size 120 nm) and 2 g of 3-aminopropyltrimethoxysilane (KBM-903, Shin-Etsu Chemical Co., Ltd.) were added to 200 mL of ethanol. The mixture was stirred at room temperature for 12 hours. After that, it was washed with ethanol, and the silica particles were collected by a centrifuge, and then heated at 110°C for 1 hour to obtain amino group-introduced silica particles.
[0043] a-2) Introduction of polymerization initiator groups onto the surface of amino group-introduced silica particles In a 500 mL eggplant flask, 40 g of the above amino group-introduced silica microparticles, 200 mL of anhydrous THF, 1 mL of anhydrous triethylamine (Tokyo Chemical Industry Co., Ltd.), and 1 mL of 2-bromoisobutyl bromide (BIBB, Tokyo Chemical Industry Co., Ltd.) were placed and stirred at room temperature for 2 hours. After that, the particles were washed with THF and methanol, and the polymerization initiator group-introduced silica microparticles into which 2-bromoisobutyryl groups were introduced as polymerization initiator groups were collected by a centrifuge and then stored as a polymerization initiator group-introduced silica microparticle methanol solution.
[0044] b) contacting particles having polymerization initiating groups on their surfaces with a monomer under living radical polymerization conditions; A methanol solution containing 40 g of the prepared silica microparticles having polymerization initiator groups, 160 mL of methanol, 40 mL of water, and 35 g of butyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.) were placed in a 500 mL eggplant-shaped flask, and nitrogen bubbling was performed for 1 hour. Then, a methanol solution in which 11 mg of Cu(II)Br (manufactured by Tokyo Chemical Industry Co., Ltd.) and 90 mg of pentamethyldiethylenetriamine (manufactured by Tokyo Chemical Industry Co., Ltd.) were stirred in 2 mL of methanol in advance was poured in. After sufficient stirring, a 90 mg aqueous solution of ascorbic acid (manufactured by Tokyo Chemical Industry Co., Ltd.) was poured in to initiate polymerization. Then, the temperature was raised to 40°C and the mixture was stirred for 4 hours. Then, the mixture was washed with methanol, and the silica microparticles grafted with polybutyl methacrylate were collected by a centrifuge. The content of polymer graft chains was 35.5% by mass.
[0045] [Preparation of composite particle 2] b) contacting particles having polymerization initiating groups on their surfaces with a monomer under living radical polymerization conditions; In a 500 mL eggplant-shaped flask, an anisole solution containing 40 g of silica microparticles having a polymerization initiator group prepared in the same process as in step a) of the preparation of composite particle 1, 20 mL of anisole, and 60 g of butyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.) were placed, heated to 60 ° C., thoroughly stirred, and then nitrogen bubbling was performed for 1 hour. Then, an anisole solution in which 144 mg of Cu (I) Br (manufactured by Tokyo Chemical Industry Co., Ltd.) and 346 mg of pentamethyldiethylenetriamine (manufactured by Tokyo Chemical Industry Co., Ltd.) were stirred in 2 mL of anisole in advance was poured, and polymerization was started. Then, the mixture was stirred for 10 hours. Then, the mixture was dispersed in chloroform, washed with methanol and ammonia water, and dried with the solvent to obtain silica microparticles grafted with polybutyl methacrylate. The content of polymer graft chains was 32.0 mass%.
[0046] [Preparation of composite particle 3] This was prepared in the same manner as Composite Particle 2, except that the amount of silica microparticles added was 6 g, the amount of anisole added was 60 mL, the amount of butyl methacrylate added was 180 g, the polymerization temperature was 80°C, the amount of Cu(I)Br stirred in 2 mL of anisole was 431 mg, the amount of pentamethyldiethylenetriamine was 1040 mg, and the polymerization time was 5 minutes.
[0047] [Preparation of composite particle 4] Composite particles were prepared in the same manner as for Composite Particle 3, except that the polymerization time was changed to 15 minutes.
[0048] [Preparation of Composite Particle 5] Composite particles were prepared in the same manner as for Composite Particle 3, except that the polymerization time was changed to 30 minutes.
[0049] [Preparation of Composite Particle 6] Composite particles 2 were prepared in the same manner as Composite particles 2, except that the amount of silica fine particles added was changed to 20 g, the amount of anisole added to 3 mL, the amount of butyl methacrylate added to 100 g, and the polymerization temperature to 80°C.
[0050] [Preparation of Composite Particle 7] Composite particles were prepared in the same manner as for composite particles 3, except that the silica fine particles were changed to Nipsil AQ and the polymerization time was changed to 20 minutes.
[0051] [Preparation of Composite Particle 8] Composite particles were prepared in the same manner as in Composite Particle 3, except that the silica fine particles were replaced by mica fine particles A-21S and the polymerization time was changed to 20 minutes.
[0052] [Preparation of Composite Particle 9] This was prepared in the same manner as composite particle 3, except that the amount of silica microparticles added was 12 g, the amount of Cu(I)Br added was 861 mg, the amount of pentamethyldiethylenetriamine added was 2080 mg, the polymerization time was 10 minutes, and butyl methacrylate was changed to hexyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.).
[0053] [Preparation of Thermoplastic Resin Composition] Examples 1 to 3, Comparative Example 1 c) Melting and kneading the composite particles with a thermoplastic resin Using a Labo Plastomill (manufactured by Toyo Seiki Seisakusho), the components shown in Table 1 were mixed in the amounts shown in Table 1 and melt-kneaded at 200° C. to obtain a thermoplastic resin composition.
[0054] Examples 4 to 13, 15 to 17 Thermoplastic resin compositions were obtained in the same manner as in Examples 1 to 3, except that the formulations were changed as shown in Tables 2 and 3.
[0055] Example 14 Thermoplastic resin compositions were obtained in the same manner as in Examples 1 to 3, except that the formulation was changed as shown in Table 3, the melt kneading temperature was changed to 240°C, the melting temperature for press molding was changed to 240°C, and the cooling temperature was changed to 80°C.
[0056] <Loss factor> Using an auto press molding machine (manufactured by Toyo Seiki Seisakusho), the material was melted at 200°C, cooled at 30°C, and a loss factor test piece (127mm x 12.7mm x 1.6mm) was molded. For this test piece, the loss factor was calculated by the half-width method from the peak of the secondary resonance of the frequency response function measured by the central excitation method based on JIS K7391. A system consisting of an oscillator Type 3160, an amplifier Type 2718, an exciter Type 4810, and an acceleration sensor Type 8001 (all manufactured by B&K) was used, and loss factor measurement software MS18143 was used. The measurement environment was controlled by a thermostatic chamber (manufactured by Espec Corporation, PU-3J), and measurements were made in the temperature range from 0°C to 80°C. The results at 20°C and 80°C are shown in Tables 1 to 3.
[0057] [Table 1]
[0058] [Table 2]
[0059] [Table 3]
[0060] Details of each component shown in Tables 1 to 3 are as follows. Polypropylene: MA03 (Japan Polypropylene) PBMA: Polybutyl methacrylate (Sigma-Aldrich) SiO2: SILFIL NSS-3N (Tokuyama Corporation) GF:T-480 (manufactured by Nippon Electronic Glass Co., Ltd.) Composite particle 7 SiO2: Nipsil AQ (manufactured by Tosoh Silica Corporation) Composite particle 8: Mica A-21S (manufactured by Yamaguchi Mica Co., Ltd.) Polyamide: Amilan CM1017 (manufactured by Toray Industries, Inc.) ABS: Toyolac 7000-314 (Toray)
[0061] The thermoplastic resin compositions of Example 3 and Comparative Example 1 were injection molded, and the following plate vibration test, fan vibration test, and fan rotation noise test were carried out. The results are shown in Tables 4 and 5.
[0062] <Plate vibration test> Using an injection molding machine (Japan Steel Works, J11AD-180H), the thermoplastic resin compositions of Example 3 and Comparative Example 1 were injection molded to mold flat plate test pieces (100 mm x 100 mm x 2 mm). The cylinder temperature was set to 200°C from the nozzle tip side to the 5th unit, 170°C for the remaining unit, and 45°C below the hopper. The mold temperature was set to 50°C. For the vibration test, a system consisting of an oscillator Type 3160, an amplifier Type 2718, a vibrator Type 4810, an acceleration sensor Type 8001, and a sound level meter 4189-A-029 was used (all manufactured by B&K). The center part of the flat plate molded was attached to a contact tip and fixed to an acceleration sensor, and then random vibration was applied, and the vibration level was calculated from the ratio of the vibration acceleration detected by the acceleration sensor in the range of 20 Hz to 12,000 Hz to the vibration force. The noise level was calculated from the ratio of the sound pressure detected by a sound level meter at a center height of 100 mm on the plate to the excitation force. The measurement environment was controlled at 20°C or 80°C in a thermostatic chamber (PU-3J, manufactured by Espec Corporation). The smaller the value, the more the vibration and noise have been reduced.
[0063] <Fan vibration test> Using an injection molding machine (SE180D manufactured by Sumitomo Heavy Industries, Ltd.), the thermoplastic resin compositions of Example 3 and Comparative Example 1 were injection molded to mold a plate fan molded body having the same shape as a plate fan manufactured by Fantech Co., Ltd. (PLF125-18, diameter 150 mm, 8 blades). The cylinder temperature was set to 200°C from the nozzle tip side to the 5th unit, 170°C for the remaining unit, and 45°C below the hopper. The mold temperature was set to 50°C. For the vibration test, a system consisting of an oscillator Type 3160, an amplifier Type 2718, a vibrator Type 4810, an acceleration sensor Type 8001, and a sound level meter 4189-A-029 was used (all manufactured by B&K Co., Ltd.). The center part of the plate fan was attached to a contact tip and fixed to an acceleration sensor, and then random vibration was applied, and the vibration level was calculated from the ratio of the vibration acceleration detected by the acceleration sensor in the range of 20Hz to 12000Hz to the vibration force. The measurement environment was controlled at 80°C using a thermostatic chamber (PU-3J, manufactured by Espec Corporation). A smaller value indicates greater reduction in vibration.
[0064] <Fan rotation noise test> The same plate fan molded body as above was used. The fan molded body was attached to the rotating shaft of a motor (AC motor manufactured by Kusatsu Denki) and rotated at various rotation speeds. The noise generated at that time was collected by a sound level meter (4189-A-029 manufactured by B&K) at a position 100 mm to the side and 200 mm below the fan, and FFT analysis was performed. The measurement time was 60 seconds, the average number of times per frequency was 358 points, and the frequency weighting characteristic was A-characteristic. The measurement environment was controlled at 80°C in a thermostatic chamber (manufactured by Espec, PU-3J). In the FFT analysis of the fan noise at each rotation speed, the frequency and noise level of the rotation noise peak corresponding to F=2NZ / 60 were measured. It can be judged that the smaller the value, the more the rotation noise is reduced.
[0065] [Table 4]
[0066] [Table 5]
[0067] As can be seen from Table 1, the thermoplastic resin composition of Example 3, which contains composite particles with polymer graft chains bonded to the particle surface, had a higher loss factor at both 20°C and 80°C and was excellent in vibration damping properties, compared to the thermoplastic resin composition of Comparative Example 1, in which the same amount of filler and elastomer were added without being bonded. This confirmed that vibration and noise could be further reduced even in injection-molded samples, as shown in Tables 4 and 5. Furthermore, as shown in Tables 1 to 3, Examples 1, 2, 4 to 13, 16, and 17, which contain composite particles with polymer graft chains bonded to the particle surface, Example 14, which uses a polyamide resin, and Example 15, which uses an ABS resin, also showed high loss factors. The loss coefficient was high and the vibration damping properties were excellent. [Industrial Applicability]
[0068] The thermoplastic resin composition of the present invention can be suitably used in products such as audio equipment, electrical products, buildings, industrial equipment, automobile parts, motorcycle parts, and containers.
Claims
1. The composite particle includes a thermoplastic resin and a polymer graft chain bonded to the particle surface, and the graft density of the polymer graft chain is 0.001 chain / nm 2 More than 5 chains / nm 2 A thermoplastic resin composition, which is:
2. The thermoplastic resin composition according to claim 1, wherein the amount of the composite particles blended in the thermoplastic resin composition is 1 part by mass or more and 300 parts by mass or less per 100 parts by mass of the thermoplastic resin.
3. The thermoplastic resin composition according to claim 1 or 2, wherein the content of the thermoplastic resin in the thermoplastic resin composition is 30% by mass or more and 95% by mass or less.
4. The thermoplastic resin composition according to any one of claims 1 to 3, wherein the thermoplastic resin is one or more resins selected from the group consisting of polyolefin resins, polyamide resins, and ABS resins.
5. The thermoplastic resin composition according to any one of claims 1 to 4, wherein the particles are a metal oxide, a metal oxide salt, a metal hydroxide or a metal carbonate.
6. The thermoplastic resin composition according to any one of claims 1 to 5, wherein the polymer graft chain is a polymer composed of one or more monomers selected from the group consisting of styrene-based monomers, nitrile-based monomers, (meth)acrylic-based monomers, unsaturated olefins, and conjugated diene-based monomers.
7. The thermoplastic resin composition according to any one of claims 1 to 6, wherein the glass transition temperature of the polymer graft chains is -30°C or higher and 80°C or lower.
8. The thermoplastic resin composition according to any one of claims 1 to 7, wherein the content of the polymer graft chain of the composite particle in the thermoplastic resin composition is 1 part by mass or more and 100 parts by mass or less per 100 parts by mass of the thermoplastic resin.
9. The method includes a step of bonding polymer graft chains to particle surfaces, and a step of melt-kneading a thermoplastic resin with composite particles having polymer graft chains bonded to their particle surfaces, A method for producing a thermoplastic resin composition, comprising the following steps 1 and 2: Step 1: A step of bonding a polymerization initiating group to the particle surface Step 2: A step of contacting particles having a polymerization initiating group on the surface with a monomer under living radical polymerization conditions.
10. The method for producing the thermoplastic resin composition according to claim 9, further comprising a molding process.
Citation Information
Patent Citations
Polymerization initiator, method for producing polymeric modified material using the same, and molded body containing polymeric modified material
JP2010024263A
Reinforcing agent for rubber or plastic, method of producing the same, and rubber composition and plastic composition
JP2013213144A
Particle, composition, molding, and printed matter
JP2020094091A
Butadiene-Derived Polymers Grafted Nanoparticles and Their Methods of Manufacture and Use
US20150197593A1
Rubber composition for tires, and pneumatic tire manufactured using same