Laminate for paper cup, and paper cup

A paper cup laminate with a biomass polyethylene resin inner layer addresses interfacial peeling and liquid leakage issues, enhancing strength and environmental sustainability.

JP2024169619AActive Publication Date: 2024-12-05NISSIN FOODS HOLDINGS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024164842
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-12-05
Estimated Expiration
2040-12-28

AI Technical Summary

Technical Problem

Existing paper cups made with biomass-derived polyethylene resin face issues of interfacial peeling during molding and liquid leakage due to differences in properties from general-purpose resins, with no optimal usage mode established for this application.

Method used

A paper cup laminate comprising a paper base layer and an inner layer of biomass polyethylene resin with a density between 0.92 g/cm³ and 0.95 g/cm³, which enhances cup strength and prevents interfacial peeling and liquid leakage.

Benefits of technology

The laminate achieves improved physical properties and reduced environmental impact by preventing interfacial peeling and liquid leakage, while utilizing biomass-derived materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169619000001_ABST
    Figure 2024169619000001_ABST
Patent Text Reader

Abstract

To provide a laminate for paper cup molding that has low environmental load and less troubles such as interfacial peeling during molding and liquid leakage, and to provide a paper cup.SOLUTION: The present inventors have found that the problem can be solved by a laminate for paper cup molding that includes at least a paper substrate layer and an inner surface layer made of a biomass polyethylene resin, and in which, characterized, the density of the biomass polyethylene resin is 0.92 g / cm3 or more and 0.95 g / cm3 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate for forming a paper cup having a biomass-derived polyethylene resin layer, and a paper cup. [Background technology]

[0002] In order to achieve the Sustainable Development Goals (SDGs), it is desirable to move away from fossil fuels, and the use of biomass materials has been proposed as one way to achieve this.

[0003] Polylactic acid (PLA) is known as a biomass resin, but it has not yet come into widespread use because its properties are significantly different from general-purpose resins such as polyolefins and PET. For this reason, efforts are being made to produce ethylene from renewable plant raw materials and use it to synthesize biomass-derived polyethylene resin (hereinafter referred to as "biomass polyethylene resin") (Patent Document 1).

[0004] However, because polyethylene resin has a wide range of uses, the optimal use of biomass polyethylene resin for each use has not been clarified. In particular, in the paper cup application that is the subject of the present invention, no consideration has been given to interfacial peeling that occurs between polyethylene resins during molding and liquid leakage, which are important physical properties for cups (Patent Documents 2 to 4). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Special Publication No. 2011-506628 [Patent Document 2] JP 2014-133338 A [Patent Document 3] JP 2015-214365 A [Patent Document 4] JP 2017-196777 A Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a laminate for paper cups and a paper cup that have a small environmental impact and are less susceptible to interfacial peeling during molding and less likely to leak when liquid is poured into them. [Means for solving the problem]

[0007] The present inventors have discovered a laminate for forming a paper cup, which comprises at least a paper base layer and an inner surface layer made of a biomass polyethylene resin, the density of which is 0.92 g / cm 3 More than 0.95g / cm 3 It has been found that the above problems can be solved by a laminate for forming paper cups, which is characterized by the following: Effect of the Invention

[0008] The completion of the present invention has made it possible to produce a laminate for paper cups and paper cups that have a small environmental impact and excellent physical properties. [Brief description of the drawings]

[0009] [Figure 1] 1 is a cross-sectional view illustrating a configuration of a first embodiment. [Diagram 2] FIG. [Diagram 3] FIG. 13 is a diagram showing a route of liquid leakage. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention relates to a laminate for forming a paper cup, which comprises at least a paper base layer and an inner surface layer made of a biomass polyethylene resin. The details will be described below.

[0011] paper base material The paper substrate constituting the laminate of the present invention is not particularly limited, but uncoated paper, coated paper, etc. can be used. In addition, from the viewpoint of realizing the toughness as a container, the basis weight of the paper substrate is 150 to 400 g / m 2 It is preferable to set the thickness to 250 to 350 g / m 2 It is more preferable to set the above.

[0012] Uncoated paper can be produced by adding fillers such as clay, talc, titanium dioxide, calcium carbonate, aluminum hydroxide powder, etc. to the raw pulp, and, if necessary, adding sizing agents, paper strength agents, fixing agents, etc. In addition, to improve the paper surface strength, chemicals such as styrene resin, styrene-maleic acid resin, starch, carboxymethyl cellulose, polyvinyl alcohol, polyacrylamide, etc. may be coated on the surface.

[0013] Coated paper can be obtained by preparing a coating liquid containing pigments such as calcium carbonate, titanium dioxide, and aluminum hydroxide, and adhesives such as polyvinyl alcohol, styrene-butadiene latex, and methyl methacrylate-butadiene latex, and applying the liquid to the surface.

[0014] Inner layer In the present invention, it is necessary to provide an inner layer made of biomass polyethylene resin. Although the detailed mechanism is not clear, it has become clear that the cup strength and laminate strength are improved by using biomass polyethylene resin for the inner layer. Note that cup strength refers to the adhesive strength between the body and the bottom, and increasing the cup strength can prevent liquid leakage when water or the like is poured into the cup. Furthermore, laminate strength refers to the laminate strength between the paper base material and the inner layer, and increasing the laminate strength can prevent problems during molding such as interfacial peeling.

[0015] Here, biomass polyethylene resin refers to polyethylene resin synthesized from plant-derived ethylene. Plant-derived ethylene can be produced by a well-known method using ethanol obtained by fermenting plants (corn, sugarcane, tapioca, etc.) as a raw material. In the present invention, polyethylene resin derived from fossil fuels is referred to as petrochemical polyethylene resin and is distinguished from biomass polyethylene resin.

[0016] In addition, the "biomass degree" (concentration of biomass-derived carbon in polyolefin resin) is a value obtained by measuring the amount of biomass-derived carbon by radioactive carbon (C14) measurement, and more specifically, it refers to the amount of biomass-derived carbon (mass%) in total carbon calculated by measurement according to the biobased concentration test standard "ASTM-D6866-20". Carbon dioxide in the atmosphere contains a certain amount of C14, and the amount of C14 in plants that grow by absorbing carbon dioxide from the atmosphere is also about the same. On the other hand, fossil fuels contain almost no C14. Therefore, the biomass-derived carbon concentration in polyolefin resin, the "biomass degree", can be calculated by measuring the proportion of C14 contained in the polyolefin resin.

[0017] In the present invention, the biomass content does not need to be 100%, and polyethylene resin with a biomass content of 5% or more is called biomass polyethylene resin. This is because the objective of reducing the amount of fossil fuel used can be achieved by replacing part of the polyethylene resin with a material derived from biomass.

[0018] In the present invention, the biomass polyethylene resin has a density of 0.93 g / cm 3 More than 0.97g / cm 3 It is preferred that the resin contains a high density biomass polyethylene resin having a molecular weight of 0.945 g / cm 3 More than 0.960g / cm 3 It is more preferable that the cup contains the following high density biomass polyethylene resin. By containing the high density biomass polyethylene resin, the strength of the cup is improved, and leakage when liquid is poured into the cup can be prevented.

[0019] In addition, as a biomass polyethylene resin, it has a density of 0.90 g / cm 3 More than 0.93g / cm 3 Preferably, the biomass polyethylene resin has a low density of less than 0.910 g / cm 3 More than 0.925g / cm 3 It is more preferable that the low-density biomass polyethylene resin contains the following low-density biomass polyethylene resin. By containing the low-density biomass polyethylene resin, the laminate strength is improved and interfacial peeling can be prevented.

[0020] In addition to containing high-density biomass polyethylene resin and low-density biomass polyethylene resin, the biomass polyethylene resin (a mixture of high-density biomass polyethylene resin and low-density biomass polyethylene resin) that constitutes the inner layer has an average density of 0.92 g / cm 3 More than 0.95g / cm 3 It must be less than 0.935g / cm 3 More than 0.945g / cm 3 By adjusting the average density of the biomass polyethylene resin constituting the inner surface layer to be within this range, liquid leakage and interfacial peeling can be prevented.

[0021] Furthermore, it is preferable not to provide an intermediate layer between the paper base layer and the inner surface layer. This is because providing an intermediate layer increases the amount of materials used and increases the environmental load. If it is unavoidable to provide an intermediate layer, polylactic acid film, PET film, CPP film, OPP film, nylon film, etc., and barrier films obtained by depositing aluminum oxide or the like on these films can be appropriately selected and used. These films can be used regardless of whether they are made from raw materials derived from biomass or fossil fuels.

[0022] outer layer In the present invention, an outer layer may be provided on the opposite side of the paper base material to the inner layer. By providing the outer layer, waterproofing and heat insulation properties can be improved.

[0023] In the present invention, a foam layer may be provided as the outer surface layer. In this case, the foam layer has a density of 0.91 g / cm 3 More than 0.93g / cm 3 By using a low-density polyolefin resin having a low melting point for the foam layer, it is possible to foam only the outer surface layer without foaming the inner surface layer during foaming processing.

[0024] When the outer layer is used as a waterproof layer, there are no particular limitations on the material of the outer layer, and polyethylene resin, polypropylene resin, polyester resin, etc. can be used as appropriate.

[0025] Manufacturing method The method for forming the inner and outer layers is not particularly limited, but extrusion lamination or the like can be used.

[0026] Extrusion Lamination Conditions The extrusion lamination method can be appropriately selected from the single lamination method, the tandem lamination method, the sandwich lamination method, the coextrusion lamination method, and the like.

[0027] The temperature of the polyethylene resin (directly below the T-die) during lamination is preferably 260 to 350° C., more preferably 280 to 330° C. Within this range, the laminate strength between the polyethylene resin layer and the paper substrate can be made suitable. The surface temperature of the cooling roll is preferably controlled within the range of 10 to 50° C.

[0028] The thickness of the polyethylene resin layer after lamination is not particularly limited, but is preferably 30 to 150 μm, more preferably 40 to 100 μm, in which case sufficient cup strength can be achieved after the cup is molded.

[0029] Furthermore, if the take-up speed is too slow, the productivity is poor, so the take-up speed is preferably 40 m / min or more, and more preferably 60 m / min or more. On the other hand, if the take-up speed is too fast, the polyethylene resin is likely to neck in and the productivity is likely to decrease. Therefore, the pulling speed is preferably 130 m / min or less, and more preferably 110 m / min or less.

[0030] Next, the air gap will be described. Here, the air gap refers to the distance from the extrusion opening of the T-die to the nip roll.

[0031] If the air gap during lamination is too wide, the polyethylene resin will neck in and productivity will decrease, so the air gap is preferably 250 mm or less, and more preferably 200 mm or less.

[0032] In the present invention, the polyethylene resin is preferably surface-treated with ozone gas and / or oxygen gas while passing through the air gap. By surface-treating with ozone gas and / or oxygen gas, it is possible to promote the formation of an oxide film and improve the laminate strength between the substrate layer and the polyethylene resin. There is no particular limitation on the amount of ozone gas and / or oxygen gas to be treated, but from the viewpoint of promoting the oxidation of the polyethylene resin, 0.5 mg / m 2 The above is preferred. EXAMPLES

[0033] Prototype example 1 (Step 1) A polyethylene resin (SBC818:SHC7260LS-L=90:10) was extrusion laminated on one side of a paper substrate to provide an inner layer with a thickness of 40 μm to produce a laminate (Prototype 1). The processing conditions were as follows:

[0034] (Lamination conditions) Paper base material: moisture content 23g / m 2 , basis weight 320g / m 2 Extrusion temperature (T die exit temperature): 320℃ Take-off speed (lamination speed): 60m / min Air gap: 80mm

[0035] Prototype examples 2-24 The polyethylene resin used in the inner layer was changed as shown in Tables 1-1 and 1-2, and laminates (Prototype Examples 2 to 24) were manufactured under the same lamination conditions as those of Prototype Example 1. The polyethylene resin used in this example is shown in Table 2. In Tables 1 to 3, "LDPE" refers to low-density polyethylene resin, and "HDPE" refers to high-density polyethylene resin. Biomass polyethylene resin is abbreviated as "bio", and petrochemical polyethylene resin is abbreviated as "petrochemical".

[0036] [Table 1]

[0037] [Table 2]

[0038] [Table 3]

[0039] A body member and a bottom member were cut out from Prototype 1, and a paper cup (Example 1) was produced using a known paper cup forming machine. Furthermore, paper cups (Examples 2 to 16, Comparative Examples 1 to 8) were produced from Prototypes 2 to 24 in the same manner as in Example 1. The shape of the paper cup is as follows: Height: 107mm (leg height: 9mm) Caliber: 95mm (with green mouth) Bottom diameter: 64mm Taper angle: 6.5°

[0040] Rating: Density The measurements were made according to the standard test method for density of plastics by density gradient method (ASTM D1505-10). In addition, the test specimen (made from the pellet sample) was left to stand at 23°C for 40 hours in advance to stabilize the temperature of the test specimen.

[0041] Evaluation: Laminate strength A cross-shaped cut (size: approximately 30 mm per side, depth: approximately 50 μm (*the cut reaches the paper base material but does not penetrate the base material) was made with a cutter on the inner layer (resin layer side) of the prototype, and adhesive tape (50 mm cloth tape, 25 mm roll 121-50, Nichiban Co., Ltd.) was applied to cover the area, and the adhesive tape was then peeled off vigorously. The peeled interface at this time was evaluated as follows. In addition, compared to when the paper is peeled off, when interfacial peeling occurs, the laminate strength is lower and defects are more likely to occur during molding. ○(Good): Paper has peeled off completely. *Paper peeling: A condition in which the paper base material is damaged. ○△: Paper peeling and interfacial peeling between the paper base material and resin were mixed, and the area of ​​paper peeling was large. △: Paper peeling and interfacial peeling between the paper base material and resin are mixed, and the area of ​​interfacial peeling is large. × (Poor): Interfacial peeling between the paper base material and the resin has occurred over the entire surface.

[0042] Rating: Leaking 50 paper cups each (Examples 1 to 16, Comparative Examples 1 to 8) were prepared, and 300 mL of the score roll liquid was filled therein. After leaving the cups to stand for 30 minutes, the number of paper cups from which liquid leakage had occurred was counted. Scoroll solution: 1000mL of water, 1mL of Scoroll Concentrate (Scoreroll 700, Kitahiro Chemical), 0.5g of Eriochrome Black T

[0043] According to this example, it can be seen that biomass polyethylene resin has a tendency to be less prone to liquid leakage. In the course of studying the present invention, it was found that the decrease in cup strength and liquid leakage occur for the following reasons. First, when the legs are formed, heat and pressure are applied, causing the polyethylene resin to flow to some extent. If the thickness of the polyethylene resin is only slightly reduced, this does not affect liquid leakage, but if the fluidity is high, there will be areas where the polyethylene resin is almost absent locally, resulting in pinholes where the paper base materials face each other. If liquid is poured into a paper cup with pinholes and allowed to stand for a while, the liquid will penetrate the paper base material through the pinholes, causing liquid leakage. Note that the more pinholes there are, the lower the cup strength tends to be, so there is a correlation between cup strength and liquid leakage.

[0044] [Table 4]

[0045] [Table 5] [Explanation of symbols]

[0046] 1...Paper base material 2. Inner layer 11...Paper base material for body 12....Inner body layer 21...Bottom paper base material 22...bottom inner layer 31 Leakage route

Claims

1. A laminate for forming a paper cup, comprising an outer layer including a foam layer containing low-density polyolefin, a paper base layer, and an inner layer containing a biomass polyethylene resin, The inner surface layer is Density 0.945g / cm 3 More than 0.960g / cm 3 The following high density polyethylene resins: Density 0.910g / cm 3 More than 0.925g / cm 3 It is composed of a mixture of the following low density polyethylene resins: The mixing ratio of the high density polyethylene resin to the low density polyethylene resin is 10:90 to 61:

39. Laminate for forming paper cups.

2. A paper cup comprising the laminate for forming paper cups according to claim 1.

Citation Information

Patent Citations

  • Resin laminate including plant-derived polyethylene and resin made multilayer container

    JP2014030942A

  • Paper cup

    JP2015214365A

  • Laminate for packaging product having biomass-derived resin layer

    JP2019043145A

  • Laminate for paper cup, and paper cup

    JP2022104378A

  • Integrated method for the production of ethylene-butylene copolymer, ethylene-butylene copolymer and use of ethylene and 1-butylene as comonomers supplied from renewable natural raw materials.

    JP2011506628A