Resin composition, film and multilayer structure
A resin composition with a hydrophilic resin and metal compound forms a layered structure for improved oxygen barrier properties under high humidity, addressing the limitations of existing PVA-based films by enhancing gas barrier performance and maintaining transparency.
Patent Information
- Application Number
- JP2024165372
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-03-29
- Filing Date
- 2024-09-24
- Publication Date
- 2024-12-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing gas barrier films made from hydrophilic resins like polyvinyl alcohol (PVA) lose their barrier properties under high humidity conditions.
A resin composition containing a hydrophilic resin, such as PVA, combined with a metal compound that forms a layered structure with a specific lattice spacing, exhibiting an X-ray diffraction peak at 2θ=2~15° when measured by CuKα radiation, enhancing gas barrier properties, particularly oxygen barrier properties under high humidity.
The resin composition achieves excellent oxygen barrier properties under high humidity conditions, with oxygen permeability as low as 10cc·3μm/m²·day·atm or less, and maintains transparency with a haze of 0.3% or less, making it suitable for packaging materials.
Smart Images

Figure 2024169633000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, and more particularly to a resin composition having high gas barrier properties under high humidity conditions. The present invention relates to a resin composition capable of obtaining a film having the above properties. [Background technology]
[0002] Hydrophilic resins such as polyvinyl alcohol resins have excellent strength, transparency, and gas barrier properties. Therefore, it is necessary to mold it into a film and use it as a packaging material, especially to prevent deterioration caused by oxygen. It is widely used as a packaging material for important foods, medicines, etc. However, hydrophilic resins are highly susceptible to the effects of humidity because they contain many hydroxyl groups. In high humidity environments, the gas barrier properties are significantly reduced.
[0003] For example, Patent Document 1 describes a film with improved gas barrier properties, which has an average particle size of 500 The water-soluble or water-dispersible polymer compound is included in the water-soluble inorganic fine particles. The poorly soluble inorganic fine particles are selected from the group consisting of aluminum, silicon, zinc, zirconium, silver, and tin. Inorganic compounds or their salts containing one or more essential components, organic acids, inorganic acids and their salts A gas barrier is an ionic crystal synthesized by reacting with one or more compounds selected from the salts of Materials for film are disclosed.
[0004] In addition, Patent Document 2 discloses a method for producing a water-soluble polymer, a metal alkoxide, a hydrolyzate thereof, and tin chloride. and at least one of the general formula (R 1 Si(OR 2 )3)n(where R 1 is an organic functional group, R 2 teeth A gas barrier layer forming composition containing a compound represented by the formula (CH3, C2H5, or C2H4OCH3). The composition is disclosed.
[0005] Furthermore, in Patent Document 3, zinc ions are applied to the surface of a substrate film or a laminate containing the same. and a coating material comprising at least one of a metal alkoxide and a hydrolyzate thereof, and a water-soluble polymer. A method for manufacturing a gas barrier laminate comprising the steps of forming a film and forming a gas barrier layer on the surface of the film. A method for manufacturing the body is disclosed. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2002-338821 A [Patent Document 2] JP 2016-221864 A [Patent Document 3] JP 2018-089567 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0007] However, the gas barrier films disclosed in the above Patent Documents 1 to 3 are difficult to withstand high humidity conditions. Therefore, the gas barrier properties are insufficient and further improvement is required.
[0008] In the present invention, under such circumstances, the gas barrier property under high humidity, particularly The object of the present invention is to provide a resin composition having excellent oxygen barrier properties. [Means for solving the problem]
[0009] However, the present inventors have discovered that a resin composition containing a hydrophilic resin and a metal compound When measured by wide-angle X-ray diffraction using CuKα radiation, the X-ray diffraction angle is in the range of 2θ = 2 to 15°. It was found that those having such a peak have excellent gas barrier properties under high humidity conditions.
[0010] That is, the present invention is a method for detecting wide-angle X-rays by using a wide-angle X-ray detector that contains a hydrophilic resin and a metal compound and uses CuKα radiation. The resin composition having an X-ray diffraction peak at 2θ=2 to 15° when measured by X-ray diffraction is called the first resin composition. This is the gist. The present invention also provides, in a second aspect, a film containing the resin composition according to the first aspect, A multilayer structure having at least one layer made of the film according to the second aspect of the present invention is also provided as a third aspect of the present invention. This is what we do. Effect of the Invention
[0011] The resin composition of the present invention contains a hydrophilic resin and a metal compound, and is widely used for the analysis of the composition using CuKα radiation. When measured by angle X-ray diffraction, it has an X-ray diffraction peak at 2θ = 2 to 15 degrees. Therefore, the film containing this resin composition has excellent gas barrier properties under high humidity conditions, particularly This provides excellent oxygen barrier properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, the embodiments of the present invention will be described in detail, but the present invention is not limited to these. It is not something that can be determined.
[0013] The resin composition of the present invention contains a hydrophilic resin and a metal compound, and is widely used for the analysis of the composition using CuKα radiation. When measured by angle X-ray diffraction, it has a peak at 2θ=2 to 15°. The ingredients will be explained.
[0014] <Hydrophilic resin> Specific examples of the hydrophilic resin used in the present invention include vinyl alcohol resins and polysaccharides. The hydrophilic resins include water-soluble resins such as water-soluble resins, acrylic resins, and polyether resins. The fats may be used alone or in combination of two or more kinds.
[0015] In addition, the hydrophilic resin has the following properties when made into a film: is preferred. A film having a thickness of 30 μm was prepared using the above hydrophilic resin and was left to stand in water at 25° C. for 2 hours. The area change rate when the sample is immersed in water is 105% or more. The area change rate is calculated by the following formula: It can be requested. Area change rate (%) = film area after immersion / film area before immersion × 100 Specific hydrophilic resins will be described in detail below.
[0016] [Vinyl alcohol resin] The vinyl alcohol resin is usually an ethylene-vinyl alcohol copolymer resin (ethylene This excludes resins known to have a polyethylene content of 20 to 60 mol%, e.g., poly Examples include vinyl alcohol (hereinafter, referred to as "PVA")-based resins.
[0017] The PVA resin is preferably an unmodified PVA resin. A resin may also be used.
[0018] The unmodified PVA resin is usually prepared by polymerizing vinyl ester monomers and then kenolizing them. It can be produced by The modified PVA resin is a polymer of vinyl ester monomer and other unsaturated monomer. It can be produced by saponifying copolymers or by post-modifying unmodified PVA resins. Cut.
[0019] Examples of the vinyl ester monomer include vinyl formate, vinyl acetate, and propionate. Vinyl phosphate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, Vinyl phosphate, vinyl laurate, vinyl stearate, vinyl versatate, trifluoroacetate Aliphatic vinyl esters such as vinyl acetate, aromatic vinyl esters such as vinyl benzoate, etc. Among these, preferred are those having 3 to 20 carbon atoms, more preferably those having 4 to 10 carbon atoms, Particularly preferred are aliphatic vinyl esters having 4 to 7 carbon atoms, and particularly preferred is vinyl acetate. These are usually used alone, but multiple types may be used simultaneously as necessary.
[0020] Examples of the other unsaturated monomers include ethylene, propylene, isobutylene, α- Olefins such as octene, α-dodecene, α-octadecene, acrylic acid, methacrylic acid unsaturated acids such as crotonic acid, maleic acid, maleic anhydride, itaconic acid, etc. Salts or mono- or di-alkyl esters, etc., acrylonitrile, methacrylonitrile, etc. nitriles, amides such as acrylamide and methacrylamide, ethylene sulfonic acid, Olefin sulfonic acids such as allyl sulfonic acid and methallyl sulfonic acid or their salts, Alkyl vinyl ethers, N-acrylamidomethyltrimethylammonium chloride , Allyltrimethylammonium chloride, Dimethylallyl vinyl ketone, N-vinyl Pyrrolidone, vinyl chloride, vinylidene chloride, polyoxyethylene (meth)allyl ether , polyoxyalkylene (meth)allyl ether, etc. ether, polyoxyethylene (meth)acrylate, polyoxypropylene (meth) Polyoxyalkylene (meth)acrylates such as acrylates, polyoxyethylene (meth)acrylates, Polyoxyalkylenes such as polyoxypropylene (meth)acrylamide and polyoxypropylene (meth)acrylamide Kylene (meth)acrylamide, Polyoxyethylene (1-(meth)acrylamide-1 ,1-dimethylpropyl) ester, polyoxyethylene vinyl ether, polyoxyprop Propylene vinyl ether, polyoxyethylene allylamine, polyoxypropylene aryl Examples of the vinyl amine include polyoxyethylene vinyl amine and polyoxypropylene vinyl amine. These can be used alone or in combination of two or more. "(Meth)allyl" refers to allyl or methallyl, and "(meth)acrylate" refers to acrylate. "(Meth)acrylic" means acrylic or methacrylate. Each of these refers to a different
[0021] The PVA resin can be obtained by any known polymerization method, saponification method, or post-modification method. can.
[0022] The amount of the other unsaturated monomer introduced and the amount of modification by post-modification depend on the type of monomer. The amount of introduction and the amount of the aryl group are appropriately set, but are usually 15 mol % or less, and particularly 10 mol % or less. If the amount of modification is too large, the crystallinity of the PVA resin decreases, and the gas barrier properties of the film are deteriorated. tends to decrease.
[0023] The average saponification degree of the PVA resin is usually 70 to 100 mol %, preferably 80 to 10 0 mol %, particularly preferably 85 to 100 mol %, and further preferably 90 to 99.99 mol %. If the average saponification degree is less than 70 mol %, the oxygen permeability becomes large under high humidity conditions. The above average saponification degree is based on JIS K 6726 3.5. To be measured.
[0024] The average degree of polymerization of the PVA resin is usually 100 to 4,000, and preferably 200 The average degree of polymerization is preferably from 300 to 2,500, and more preferably from 300 to 2,500. If the concentration is too high, the mechanical properties such as film strength tend to decrease, and if the concentration is too high, it becomes difficult to form an aqueous solution. The above average degree of polymerization is based on JIS K 6726 It is measured in accordance with.
[0025] In addition, PVA resins are available in a wide range of types and amounts of modification, average saponification degree, average polymerization degree, etc. Two or more types may be used in combination.
[0026] The hydrophilic resin is preferably the main component of the resin composition of the present invention, and the entire resin composition The content of the hydrophilic resin in the body is usually 80% by weight or more, preferably 90% by weight or more, particularly The upper limit is usually 99.99% by weight.
[0027] [Polysaccharide] Examples of the polysaccharides include starch and cellulose. Examples of the starch include natural starches such as corn starch and potato starch, and etherified starches. Starch, esterified starch, cross-linked starch, grafted starch, roasted dextrin, enzyme-modified dextrin Examples of modified starches include thorin, pregelatinized starch, oxidized starch, and the like. Examples of the cellulose include carboxymethyl cellulose, methyl cellulose, Ethyl cellulose, hydroxymethyl cellulose, hydroxypropyl methyl cellulose , Hydroxyethyl cellulose, Hydroxyethyl methyl cellulose, Hydroxypropyl cellulose, nitrocellulose, cationic cellulose, etc., and their sodium salts Examples of such salts include
[0028] [Acrylic resin] Examples of the acrylic resin include polyacrylamide, polyacrylic acid, and the like. and metal salts such as the sodium salt of the above.
[0029] [Polyether resin] Examples of the polyether resin include polyethylene glycol and polypropylene. glycol, etc.
[0030] Among the above hydrophilic resins, those with excellent gas barrier properties, especially oxygen barrier properties under high humidity conditions, are From this viewpoint, vinyl alcohol resins and polysaccharides are preferred, and PVA resins and polysaccharides are particularly preferred. It is preferably cellulose, and most preferably unmodified PVA resin.
[0031] <Metal compounds> The metal compound used in the present invention has a structure in which metal complexes are layered with a specific interplanar spacing. For example, a metal-containing layered compound such as a layered compound containing Zn as a metal species is used. Some examples include:
[0032] Examples of the metal species contained in the metal compound include Zn, Co, Ni, and Si. These metal species may be contained alone or in combination. In view of its excellent gas barrier properties, particularly oxygen barrier properties, Zn is preferred.
[0033] The metal compound is, for example, at least one metal selected from Zn, Co, Ni, and Si. The metal-containing compound is a compound having a metal group (hereinafter referred to as a "metal-containing compound"). It is obtained by the method. Examples of the metal-containing compound include organic acid salts of metals and inorganic salts of metals. .
[0034] Examples of the organic acid constituting the organic acid salt of the metal include monovalent carboxylic acids such as acetic acid, Dicarboxylic acids such as succinic acid, oxalic acid, and tartaric acid, citric acid, and ethylenediaminetetraacetic acid These may be used alone or in combination of two or more. Good too. The organic acid salt of the metal may be a hydrate or an anhydride. The organic acid salts of the above metals have excellent gas barrier properties, particularly oxygen barrier properties, under high humidity conditions. From this viewpoint, a monovalent metal carboxylate is preferred, and particularly preferred is zinc acetate or a hydrate thereof. It is an object.
[0035] Examples of inorganic salts of the above metals include fluorides, chlorides, bromides, iodides, etc. of metals. These may be used alone or in combination of two or more. The inorganic acid salts of the above metals are excellent in gas barrier properties, particularly oxygen barrier properties, under high humidity conditions. From this viewpoint, metal chlorides are preferred, and zinc chloride or its hydrate is particularly preferred.
[0036] As described above, the metal compound used in the present invention is a compound in which the metal complex is layered with a specific interplanar spacing. Therefore, the metal compound is surrounded by hydrophilic resin molecules and water molecules. When the metal complex is present, the layers of the metal compound are peeled off, and the peeled fine metal complex molecules are As a result of interacting with hydrophilic resins at the molecular level, it has excellent gas barrier properties, especially oxygen barrier properties. is assumed to be obtained.
[0037] The interlayer distance (distance between layers) of the above metal compounds is determined by the interaction with the hydrophilic resin molecules and water molecules. From the viewpoint of function, the thickness is preferably 0.01 to 50 nm, and more preferably 0.1 to 30 nm. is more preferred.
[0038] The molecular weight of the metal complex peeled off from the metal compound is determined by the molecular level interaction with the hydrophilic resin. From the viewpoint of the above, it is preferable that the number of the molecules is 100 to 10,000, and more preferably 200 to 2,000. It is particularly preferred that:
[0039] In addition, the metal complex is hydrophilic in terms of the interaction with the hydrophilic resin molecules. It is preferable that there is. Furthermore, the above metal complexes were not observed even after being left to stand for 1,000 hours at 23°C and 80% RH. It is preferable not to solve the problem.
[0040] The content of the compound having the metal in terms of the metal is 0.01 to 20 parts by weight based on the resin composition. % by weight, more preferably 0.1 to 8% by weight, and particularly preferably 0.2 to 10% by weight. If the content of the metal compound is too low, the gas barrier property under high humidity, In particular, oxygen barrier properties tend to decrease, and if the metal compound content is too high, the film, etc. When the temperature is increased, the film tends to become white and the transparency decreases. In addition, when the resin composition contains a plurality of metal compounds with different metal species, The total amount of metal compounds contained in the material is taken as the content. The content of the above metal compounds is determined by the standard addition method using ICP-MS. can be done.
[0041] [Other ingredients] The resin composition of the present invention generally contains a hydrophilic resin within a range that does not impair the effects of the present invention. Additives to be added to fats, such as heat stabilizers, antioxidants, antistatic agents, colorants, and UV absorbers agents, lubricants, plasticizers, light stabilizers, surfactants, antibacterial agents, drying agents, antiblocking agents, Flame retardant, crosslinking agent, hardener, foaming agent, crystal nucleating agent, anti-fogging agent, biodegradable additive, silane coupling agent The composition may contain a blocking agent, an oxygen absorber, etc. These may be used alone or in combination of two or more kinds. There can be.
[0042] <<Resin composition>> The resin composition of the present invention contains the above-mentioned hydrophilic resin and a metal compound, and is irradiated with CuKα radiation. When measured by wide-angle X-ray diffraction using The peaks appearing on the low angle side of 2θ=2 to 15° are due to the addition of metal-containing compounds. is converted to a metal compound, and this peak is derived from the metal compound.
[0043] In the present invention, the gas barrier property, particularly the oxygen barrier property, is excellent under high humidity conditions. When measured by wide-angle X-ray diffraction using CuKα radiation, the X-ray diffraction peak was observed at 2θ = 2 to 15 °. It is further preferred that the peak is at 2θ=2 to 9°, and more preferably at 2θ=3 to 8°. It is particularly preferable that the peak is at 10°.
[0044] When measured by wide-angle X-ray diffraction using CuKα radiation, X-ray diffraction peaks are observed at 2θ = 2 to 15°. It is presumed that the presence of such a metal compound indicates that a layered structure is formed. The layered structure of the metal compound interacts with the hydrophilic resin, forming a resin composition. By increasing the polarity of the material, the gas barrier properties, especially the oxygen barrier properties, are excellent under high humidity conditions. It is assumed that the following effects will be obtained.
[0045] The above X-ray diffraction is measured under the following conditions. [Measurement conditions] Equipment used: D8 DISCOVER (manufactured by Bruker Japan) Detector: 2D detector VANTEC-500 (manufactured by Bruker Japan) Voltage: 50kV Current: 100mA Camera length: 100mm Measurement method: Reflection method Accumulation time: 30 minutes Wavelength: CuKα radiation (Kα1 and Kα2 are not separated) Detector position: 2θ=10° X-ray incident angle: θ=0.3° Conditions for one-dimensionalization in the 2θ direction: 2θ=1 to 35°, azimuth angle (chi)=-95 to -85° One-dimensional azimuth direction: 2θ=3.5~4.5°, azimuth angle (chi)=-180~0° The sample used for the wide-angle X-ray diffraction was a resin composition in the form of a film. In addition, when the resin composition is laminated with another substrate, the resin composition layer may be If peeling is possible, peel off the resin composition layer and perform the measurement. If peeling is not possible, use another substrate. The measurement can be performed while the resin composition is still laminated. The thickness of the layer (film) is preferably 30 μm or more. If necessary, a film may be laminated.
[0046] In addition, the resin composition of the present invention has a second virial value obtained by static light scattering measurement. coefficient (A2) and the second virial coefficient (A 2,0 ) is calculated using the following formula: It is preferable that (1) is satisfied. ΔA2=A2-A 2,0 >0 (1)
[0047] The second virial coefficient (A2) of the resin composition and the second virial coefficient of the hydrophilic resin in the resin composition coefficient (A 2,0 ) and the difference (A2-A2,0 ) is preferably greater than 0, more preferably A2-A 2,0 >0.00005, and particularly preferably A2-A 2,0 >0.0001 , particularly preferably A2-A 2,0 >0.0005. The upper limit is usually 0.01. , preferably 0.1. 2,0 When the value is 0 or less, the gas barrier property under high humidity is As a result, the barrier properties, especially the oxygen barrier properties, tend to decrease.
[0048] Above A2 and A 2,0 is determined by the following: The resin composition was mixed in hexafluoroisopropanol as a solvent to a solids concentration of 0.1 Five levels of measurement solutions were prepared in the range of up to 1mg / mL, and static light scattering measurements were performed at a temperature of 25°C. The second virial coefficient A2 and weight average of the resin composition obtained from the Zimm plot are Molecular weight Mw b Request. In addition, the second virial coefficient A of the hydrophilic resin was calculated using the same method. x and weight average molecular weight Mw a Ask for . The hydrophilic resin is the same as the hydrophilic resin contained in the resin composition, i.e., The resin composition is a hydrophilic resin before containing a metal compound. The resin composition of the present invention contains a hydrophilic resin and a metal compound. The weight average molecular weight of the hydrophilic resin is the apparent weight average molecular weight (Mw a ) and different The second virial coefficient A obtained by static light scattering measurement of the hydrophilic resin is x in the resin composition Second virial coefficient A of hydrophilic resin 2,0 Therefore, the following procedure can be used Second virial coefficient A of hydrophilic resin in resin composition 2,0 Request. 1) Calculate the constant q from the following equation (2). q=A X / Mw a ν (2) A x : Second virial coefficients of hydrophilic resins obtained by static light scattering measurements Mw a : Weight average molecular weight of hydrophilic resin obtained by static light scattering measurement ν :-0.25 Here, since ν in a good solvent is usually -0.25, calculations are performed assuming ν = -0.25. . 2) The constant q thus obtained and the weight average molecular weight Mw obtained by static light scattering measurement of the resin composition b Using The second virial coefficient A of the hydrophilic resin is calculated from the following formula (3). 2,0 The following ν is calculated. , -0.25 is used as in equation (2). A 2,0 =q × Mw b ν (3)
[0049] The resin composition of the present invention having the above-mentioned characteristics can be prepared, for example, by the following preparation method (i) etc. You can get more.
[0050] <Preparation method (i)> (i-1) a step of mixing a hydrophilic resin, a metal-containing compound, and a solvent, and heating and stirring the mixture; (i-2) A step of forming a film from the heated solution and drying it to obtain a film; (i-3) A step of leaving the film at rest under high humidity. Each step will be described in detail below.
[0051] [Step (i-1)] In the above step (i-1), the metal-containing compound reacts in the solvent and undergoes a structural change. This produces a metal compound.
[0052] The amount of the metal-containing compound is usually 0.01 to 0.01 parts by weight, calculated as the metal, per 100 parts by weight of the hydrophilic resin. The amount is from 0.01 to 20 parts by weight, preferably from 0.1 to 8 parts by weight, and particularly preferably from 0.2 to 5 parts by weight. It is a quantitative part.
[0053] The solvent is not particularly limited as long as it dissolves the hydrophilic resin, but water is usually used. In order to shorten the drying time after the film formation, for example, methanol, ethanol, etc. Lower alcohols having 1 to 5 carbon atoms, such as propanol, n-butanol, and isopropanol etc. may be used as long as the hydrophilic resin can be dissolved therein. The amount of the solvent is usually 100 to 9,900 parts by weight per 100 parts by weight of the hydrophilic resin. parts by weight, and preferably 400 to 1,900 parts by weight.
[0054] The order in which the hydrophilic resin, the metal-containing compound, and the solvent are mixed is not particularly limited. They may be mixed together at once or sequentially. It is preferable to incorporate the containing compound from the viewpoint of reactivity.
[0055] The heating temperature is usually 20 to 100°C, preferably 40 to 95°C, and particularly preferably 80 to 100°C. 0 to 95°C. If the heating temperature is too low, the hydrophilic resin tends not to dissolve completely. If the heating temperature is too high, the metal-containing compound tends to decompose.
[0056] The reaction time is usually 0.5 to 5 hours, preferably 1 to 4 hours, and particularly preferably 2 to 3 hours. If the reaction time is too short, the reaction tends not to proceed sufficiently, and if the reaction time is too long, However, the reaction yield does not improve and the economic efficiency tends to decrease. The pressure during heating may be normal pressure.
[0057] A metal compound is obtained by the above step (i-1). Hydrogen bonds are formed between the groups and the hydroxyl groups of the hydrophilic resin, or between the metal species of the metal compound and the hydrophilic resin. The interaction with fats provides excellent gas barrier properties, especially oxygen barrier properties, under high humidity conditions. It is expected that this will produce positive results.
[0058] [Step (i-2)] The above-mentioned step (i-2) is a step of forming a film from a solution containing a hydrophilic resin and a metal compound. This is the process of obtaining the
[0059] The solid concentration of the solution containing the hydrophilic resin and the metal compound when forming the membrane is usually 0.5 to 1.0 μm. The content is 30% by weight, preferably 5 to 20% by weight.
[0060] The film-forming method may be a known method such as a melt extrusion method, a casting method, or a coating method. Any method suitable for forming a film from the hydrophilic resin to be used may be used. For example, when the hydrophilic resin is a PVA-based resin, the coating method is preferable in terms of the accuracy of the film thickness. The coating method and the casting method are preferred. In addition, the film after the film formation may be stretched uniaxially or biaxially as necessary. It is also possible.
[0061] Examples of the coating method include bar coating, roll coating, die coating, etc. Examples of the coating method include known methods such as coating, gravure coating, comma coating, and screen printing. can be.
[0062] The film may be a single-layer structure film or a multi-layer structure film. The layer structure preferably has at least one layer made of the above-mentioned film. The multilayer structure may be formed by laminating the formed film or by laminating it with another base resin. stomach.
[0063] Examples of the base resin include linear low-density polyethylene, low-density polyethylene, ultra-low-density polyethylene, and Low density polyethylene, medium density polyethylene, high density polyethylene, ethylene-propylene (Block and random) copolymers, ethylene-α-olefins (α- Polyethylene resins such as propylene-α-olefin copolymers, polypropylene, propylene-α-olefin copolymers, etc. Polypropylene resins such as polyolefin (α-olefin with carbon number of 4 to 20) copolymers, Polypentene, polycyclic olefin resins (cyclic olefin structures in the main chain and side chains) (Unmodified) polyolefin resins such as those having at least one of the following properties: Unsaturated carboxylic acids are graft-modified olefins with unsaturated carboxylic acids or their esters. Polyolefin resins in the broad sense, including modified olefin resins such as acid-modified polyolefin resins Fatty acids, ionomers, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, Styrene-acrylic acid ester copolymer, polyester resin, polyamide resin (copolymer (including polyamide), polyvinyl chloride, polyvinylidene chloride, acrylic resin, polystyrene Polyethylene, vinyl ester resin, polyester elastomer, polyurethane elastomer Polystyrene elastomers, chlorinated polyethylene, chlorinated polypropylene and other halogenated and substituted polyolefins, aromatic or aliphatic polyketones. The base resin may be subjected to a surface treatment such as a corona treatment.
[0064] The thickness of the film is usually 1 to 200 μm, preferably 1 to 100 μm, and particularly preferably In addition, when the film formed above is a multi-layer structure, the hydrophilic The total thickness of all films obtained by casting a solution containing a reactive resin and a metal compound was calculated. The result is the thickness of the film.
[0065] [Step (i-3)] The above step (i-3) is a step of leaving the film obtained above at rest under high humidity. This process provides excellent gas barrier properties, especially oxygen barrier properties, under high humidity conditions. The principle by which such an effect is obtained is not clear, but By leaving the film in a high humidity environment, the metal compounds dispersed in the film are converted to hydrophilic resin. It is speculated that this is due to interaction with the fat or localization at the surface of the film.
[0066] In the present invention, "high humidity" means 20±5° C. and 90±10% RH. The standing time is usually 70 hours or more, preferably 300 hours or more, and more preferably 6 The upper limit of the standing time is usually 1,000 hours.
[0067] By going through the above process, the 2θ The resin composition of the present invention (film made of the resin composition) has an X-ray diffraction peak at 2 to 15°. The result is a 300 rpm. The method for preparing the resin composition is not limited to the above-mentioned preparation method (i), and may be, for example, the following preparation method (i-1 In the process of catalysis, a metal organic acid salt and a strong base (e.g., an alkali metal, an alkaline earth metal The metal compound is first generated by reacting with the hydroxide of the metal, and then the hydrophilic compound is reacted with the hydroxide of the metal. Resin may also be blended.
[0068] The oxygen permeability of the film containing the obtained resin composition was evaluated as a gas barrier property, particularly an oxygen barrier property. From the viewpoint of adhesiveness, 80cc·3μm / m 2 ·day·atm or less is preferable, and 70 cc·3μm / m 2 ·day·atm or less is preferable, and 55cc·3μm / m 2 ·day·atm or less is more preferable, and 40cc·3μm / m 2 ·da y·atm or less is more preferable, and 35cc·3μm / m 2 ·day·atm More preferably, it is 30cc·3μm / m or less. 2 ·day·atm or less More preferably, 25cc·3μm / m 2 ·day·atm or less It is preferable for 20cc·3μm / m 2 It is even more preferable that the temperature is less than 1000°C. , 10cc·3μm / m 2 It is particularly preferable that the above-mentioned The oxygen permeability was measured under an environment of 23°C and 80% RH. The lower limit of the oxygen permeability is , usually 0cc·3μm / m 2 The oxygen permeability is calculated based on the oxygen permeability. It can be determined using a transient measuring device.
[0069] The film containing the resin composition of the present invention is very transparent. It is far superior to films containing organic layer compounds or fillers. The film containing the resin composition of the present invention preferably has a haze of 1% or less. More preferably, it is 0.6% or less, even more preferably, it is 0.3% or less, and particularly preferably, it is 0. The haze is 2% or less. The haze is measured in accordance with the JIS K7361-1 standard. For example, ten test pieces of 50 mm x 50 mm are cut from a film. The haze was measured using a haze meter (NDH-4000, manufactured by Nippon Denshoku Co., Ltd.) and the average of 10 sheets was The average value is taken as the haze (%).
[0070] The resin composition of the present invention and a film containing the resin composition are useful as packaging materials. It can be particularly suitably used as a packaging material for food, medicines, etc. EXAMPLES
[0071] The present invention will be described in more detail below with reference to examples, but the present invention will not go beyond the gist of the invention. The present invention is not limited to the following examples unless otherwise specified. In the following, "parts" are based on weight. It means standard.
[0072] Prior to the examples, the following hydrophilic resins were prepared.
[0073] [Hydrophilic resin] PVA-1 (unmodified PVA resin, average degree of polymerization 300, average degree of saponification 99 mol%)
[0074] <Example 1> Add 100 parts of PVA-1 and 0.3 parts of zinc acetate (metal equivalent) to 900 parts of water and stir. The mixture was then heated to 90°C while stirring to dissolve the mixture. The temperature was then maintained at 90°C for 3 hours. After that, it was cooled to room temperature (23°C) to prepare a solution containing a hydrophilic resin and a metal compound. Ta. The solution prepared above was applied to a corona-treated PET film with a thickness of 38 μm using a bar coater. The coated film was dried in a hot air dryer at 120°C for 5 minutes. The coating film was left to stand for 72 hours under an environment of 23°C and 80% RH to obtain the resin composition of Example 1. A resin composition film (thickness: 3 μm) was obtained.
[0075] The resin composition film obtained above is peeled off from the PET film, and the thickness is reduced to 30 μm or less. The samples were stacked so that the top was facing up. X-ray diffraction measurement of this sample was carried out under the following conditions, and the results are shown in Table 1 below. [Measurement conditions] Equipment used: D8 DISCOVER (manufactured by Bruker Japan) Detector: 2D detector VANTEC-500 (manufactured by Bruker Japan) Voltage: 50kV Current: 100mA Camera length: 100mm Measurement method: Reflection method Accumulation time: 30 minutes Wavelength: CuKα radiation (Kα1 and Kα2 are not separated) Detector position: 2θ=10° X-ray incident angle: θ=0.3° Conditions for one-dimensionalization in the 2θ direction: 2θ=1 to 35°, Chi=-95 to -85° One-dimensional azimuth direction: 2θ=3.5~4.5°, azimuth angle (chi)=-180~0° If a peak is observed in the range of 2θ=3~10° when the data is converted into one dimension in the 2θ direction, the azimuth angle If no peak is observed when the peak is linearized in the 2θ direction, = 3.5 to 4.5°, the azimuth angle is converted to one dimension in the range of -180 to 0°, and The azimuth angle dependence of the diffraction strength was confirmed. At this time, a diffraction peak was observed at an azimuth angle of -90°. If so, it was determined that a complex was present in the resin composition.
[0076] [Oxygen Barrier Properties] The oxygen permeability of the obtained resin composition film was measured using an oxygen permeability measuring device (OX-TRAN1 The measurements were taken at 23°C and 80% RH using a 00A thermocouple (MOCON). The details are shown in Table 1.
[0077] <Example 2> In Example 1, the same procedure was repeated except that the amount of Zn acetate added was 1 part in terms of metal. A resin composition film of Example 2 was obtained in the same manner as in Example 1. The X-ray diffraction of the composition film was measured in the same manner as in Example 1. The oxygen barrier property was evaluated, and the results are shown in Table 1 below.
[0078] <Example 3> In Example 1, the same procedure was repeated except that the amount of Zn acetate added was 5 parts in terms of metal. A resin composition film of Example 3 was obtained in the same manner as in Example 1. The X-ray diffraction of the composition film was measured in the same manner as in Example 1. The oxygen barrier property was evaluated, and the results are shown in Table 1 below.
[0079] <Comparative Example 1> A comparative example was prepared in the same manner as in Example 1, except that Zn acetate was not added. The hydrophilic resin film of 1 was obtained. Then, X-ray diffraction of the obtained hydrophilic resin film was performed. Measurement was carried out in the same manner as in Example 1. Furthermore, the oxygen barrier property was evaluated in the same manner as in Example 1. The results are shown in Table 1 below.
[0080] <Comparative Example 2> In Example 1, Zn oxide was added in place of Zn acetate so that the amount was 1 part in terms of metal. Other than that, the same procedure as in Example 1 was carried out to obtain a resin composition film of Comparative Example 2. In addition, the X-ray diffraction of the resin composition film was measured in the same manner as in Example 1. The oxygen barrier properties were evaluated using the test pieces, and the results are shown in Table 1 below.
[0081] <Comparative Example 3> In Example 1, Zn chloride was added in place of Zn acetate so that the amount was 1 part in terms of metal. Other than that, the same procedure as in Example 1 was carried out to obtain a resin composition film of Comparative Example 3. In addition, the X-ray diffraction of the resin composition was measured in the same manner as in Example 1. The oxygen barrier property was evaluated, and the results are shown in Table 1 below.
[0082] [Table 1]
[0083] As can be seen from Table 1 above, the hydrophilic resin and the metal compound are contained, and the low angle X-ray diffraction measurement Examples 1 to 3, which have a peak on the side (2θ=2 to 15°), show an oxygen barrier effect under high humidity. It was excellent. On the other hand, in Comparative Examples 1 to 3, which do not have a peak on the low angle side in the X-ray diffraction measurement, all of them have oxygen barriers. It was inferior in quality. [Industrial Applicability]
[0084] The resin composition of the present invention has excellent gas barrier properties, particularly oxygen barrier properties, under high humidity conditions. Therefore, it is useful as a packaging material, and is particularly suitable for use as a packaging material for food, medicines, etc. This can be done.
Claims
1. It contains a hydrophilic resin and a metal compound, and when measured by wide-angle X-ray diffraction using CuKα radiation, The resin composition is characterized by having an X-ray diffraction peak at 2θ=2 to 15°.
2. 2. The method according to claim 1, wherein the hydrophilic resin is a polyvinyl alcohol resin. A resin composition.
3. The content of the metal compound in terms of metal is 0.01 to 20% by weight based on the resin composition. The resin composition according to claim 1 or 2,
4. A film comprising the resin composition according to any one of claims 1 to 3. 。
5. The oxygen permeability of the above film under an environment of 23°C and 80% RH is 80cc / 3μm / m 2 5. The film according to claim 4, characterized in that it has a viscosity of not more than 1.times.day.atm.
6. A multilayer structure having at least one layer made of the film of claim 4 or 5.
Citation Information
Patent Citations
Material for gas barrier film
JP2002338821A
Gas barrier laminate
JP2016221864A
Gas barrier laminate and production method of the same
JP2018089567A