Nonflammable surface protection structure
A nonflammable surface protection structure using a flammable resin layer with ammonium polyphosphate and adhesion layers addresses the combustibility of resin-based paints and complexity of metal lining, ensuring non-combustibility and quick construction.
Patent Information
- Application Number
- JP2024084136
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2024-05-23
- Publication Date
- 2024-12-06
AI Technical Summary
Existing resin-based paints are combustible, making them unsuitable for applications requiring non-combustibility, such as certain structures and buildings, and metal lining methods are cumbersome and require skilled labor.
A nonflammable surface protection structure comprising a flammable resin layer with added ammonium polyphosphate, providing a second protective layer to ensure non-combustibility, along with adhesion layers for improved bonding and resistance to peeling.
The structure achieves non-combustibility, ensures waterproofness, and allows for quick construction on complex shapes, reducing construction time and costs while maintaining durability and resistance to abrasion, corrosion, and heat.
Smart Images

Figure 2024170310000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a non-flammable surface protection structure for protecting the surface of an object to be protected, such as a structure. [Background technology]
[0002] Most resin-based paints are organic and therefore basically treated as combustible materials. Therefore, there are places where painting is not possible, such as structures and buildings that require non-combustibility from the perspective of fire protection. For example, water can seep in through joints and cracks in concrete structures, hazardous materials storage facilities, block walls, etc. Normally, waterproofing paint is used to prevent this, but in places where the Building Standards Act requires that the building be non-flammable, general waterproofing paint is classified as flammable and cannot meet the requirement.
[0003] One example of currently used construction methods that fulfills the requirements for surface protection such as fireproofing is the metal lining method using stainless steel or the like (see, for example, Patent Document 1). Stainless steel is a metal and therefore a fireproof material, and by lining up and welding the stainless steel together to make one seamless steel material, fireproofing and other effects are achieved. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2004-324230 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the metal lining method has disadvantages such as the need for skilled special welders, a very long construction period, and difficulty in dealing with complex shapes. Resin coating has the advantage that the work can be done by waterproofing workers (there are more waterproofing workers in total than the welders used by stainless steel lining workers), the construction period can be shortened, and even complex shapes can be handled with the simple task of painting. Under these circumstances, there has been a demand for the development of a surface protection structure that can at least meet the requirement of being non-combustible.
[0006] The present invention has been made in consideration of the above circumstances, and has an object to provide a surface protection structure that can satisfy the requirement of non-combustibility by using a resin-based coating. [Means for solving the problem]
[0007] In order to achieve the above object, the present invention provides a flame-retardant surface protective structure for protecting a surface of an object to be protected, comprising: A first protective layer formed of a flammable resin layer and directly or indirectly applied to the surface of the object to be protected; A second protective layer is formed on the surface of the first protective layer directly or indirectly, and is a resin layer containing a resin to which ammonium polyphosphate has been added; The present invention is characterized by comprising:
[0008] Here, the object to be protected may be, for example, a structure. The structure may be made of, for example, concrete, metal, resin, wood, etc., but is not limited thereto, and may be a composite material containing at least two of these. Furthermore, the object to be protected is not limited to a structure, and may be any object that is required to be non-flammable.
[0009] The first protective layer is usually waterproof since it is painted and formed of a flammable resin layer. In addition to waterproofness, the first protective layer may have rust resistance, corrosion resistance, abrasion resistance, chemical resistance, salt damage resistance, insulating properties, heat insulation properties, etc. When the resin layer (first protective layer) is formed by applying a coating material to the surface, the layer may be formed from a polyurethane resin containing an isocyanate component and a polyol component. In addition, a synthetic resin paint other than polyurethane resin may be applied to the surface to form a resin layer (first protective layer). Examples of synthetic resin paint other than polyurethane resin include epoxy resin, urea resin, methacrylic resin, polyester resin, vinyl ester resin, and acrylic resin paints. These paints form a flammable resin layer (coating).
[0010] In addition, a surface strengthening agent may be applied to the surface of the object to be protected instead of the first protective layer. Examples of such surface strengthening agents include silica-based, silicofluoride-based, and epoxy resin-based surface strengthening agents for the purpose of strengthening the concrete base when the surface of the object to be protected is formed of concrete. When used as an inorganic material or in combination with an inorganic material, cement-based, polymer cement-based, SBR-based, or EVA-based reinforcing materials may be used.
[0011] Furthermore, when a plate material is fixed to the surface instead of the first protective layer, the plate material may be attached and fixed with an adhesive, or may be fixed mechanically with screws, nails, or the like. Examples of board materials that can be used primarily for waterproofing or insulation purposes include inorganic board materials such as glass wool and rock wool, wood fiber board materials such as cellulose fiber, natural material board materials such as wool breath and carbonized cork, and foamed plastic board materials such as polystyrene foam, rigid urethane foam, and phenol foam.
[0012] Furthermore, when a sheet is attached to the surface instead of the first protective layer, a sheet made of vulcanized rubber, non-vulcanized rubber, PVC resin, EVA resin, polyethylene resin, polypropylene resin, glass fiber, vinylon fiber, aramid fiber, or polymer cement mortar may be used, mainly for the purpose of waterproofing or preventing peeling.
[0013] The second protective layer is formed, for example, by a resin layer containing a urethane-based composite polymer, a curing agent containing aminosilane, and a base material containing ammonium polyphosphate. Ammonium polyphosphate is a chain inorganic phosphate compound containing ammonium.
[0014] In the present invention, the first protective layer is provided on the surface of the object to be protected by a resin-based coating, so that waterproofing can be easily and reliably obtained. Furthermore, if this first protective layer has adhesion, rust prevention, corrosion resistance, abrasion resistance, chemical resistance, salt damage resistance, insulation, heat insulation, etc., it is also possible to easily impart adhesion, waterproofing, rust prevention, corrosion resistance, abrasion resistance, chemical resistance, salt damage resistance, insulation, and heat insulation to the surface. Furthermore, by forming a second protective layer made of a resin layer containing a resin to which ammonium polyphosphate has been added by painting on the surface of the first protective layer made of a flammable resin layer, it is possible to ensure non-flammability through the resin coating, which was not previously possible. As described above, in the present invention, the first protective layer and the second protective layer are formed by resin-based coating, so that the construction period can be shortened and it is easy to apply the protective layer to objects having complex shapes. In addition, since the resin layer containing the resin to which ammonium polyphosphate has been added is formed by painting, waterproofness is usually ensured, and thus waterproofness can be ensured by the second protective layer in addition to the waterproofness of the first protective layer.
[0015] In the above-mentioned configuration of the present invention, a first adhesive layer for improving adhesion to the first protective layer may be applied to the surface.
[0016] The first adhesion layer is formed by an adhesion improving coating (primer), and the coating that forms this first adhesion layer uses at least one type of paint such as epoxy-based resin, urethane-based resin, urea-based resin, methacrylic resin, polyester-based resin, vinyl ester-based resin, acrylic resin, chlorinated rubber-based resin, inorganic paint, etc.
[0017] According to this configuration, a first adhesion layer is applied to the surface of the object to be protected to improve adhesion with the first protective layer, thereby improving adhesion between the surface and the first protective layer and suppressing peeling of the first protective layer.
[0018] In the above-mentioned configuration of the present invention, a second adhesive layer may be applied to the surface of the first protective layer in order to improve adhesion to the second protective layer.
[0019] The second adhesion layer is formed by an adhesion improving coating (primer), and like the first adhesion layer, the coating used to form this second adhesion layer is at least one type of paint selected from epoxy-based resins, urethane-based resins, urea-based resins, methacrylic resins, polyester-based resins, vinyl ester-based resins, acrylic resins, chlorinated rubber-based resins, inorganic paints, etc.
[0020] According to this configuration, a second adhesion layer is coated on the surface of the first protective layer to improve adhesion with the second protective layer, thereby improving adhesion between the surface of the first protective layer and the second protective layer and suppressing peeling of the second protective layer.
[0021] In the above-described configuration of the present invention, the second protective layer preferably has a thickness of 0.6 mm or more. If the thickness of the second protective layer is less than 0.6 mm, the second protective layer becomes too thin, making it difficult to ensure non-combustibility.
[0022] Therefore, by setting the thickness of the second protective layer to 0.6 mm or more, non-combustibility can be reliably ensured.
[0023] In the above-described configuration of the present invention, the object to be protected may be a structure. According to this configuration, the surface of the structure is protected by the first protective layer and the second protective layer, thereby ensuring non-combustibility of the surface. Effect of the Invention
[0024] According to the present invention, a surface protection structure that can satisfy the requirement of non-combustibility by using a resin-based coating can be provided. [Brief description of the drawings]
[0025] [Figure 1] 1 is a cross-sectional view showing a surface protection structure according to a first embodiment of the present invention. [Diagram 2] FIG. 4 is a cross-sectional view showing a surface protection structure according to a second embodiment of the present invention. [Diagram 3] FIG. 11 is a cross-sectional view showing a surface protection structure according to a third embodiment of the present invention. [Figure 4] FIG. 11 is a cross-sectional view showing a surface protection structure according to a fourth embodiment of the present invention. [Diagram 5] FIG. 11 is a cross-sectional view showing a surface protection structure according to a fifth embodiment of the present invention. [Figure 6] FIG. 11 is a cross-sectional view showing a surface protection structure according to a sixth embodiment of the present invention. [Figure 7] FIG. 13 is a cross-sectional view showing a surface protection structure according to a seventh embodiment of the present invention. [Figure 8] FIG. 13 is a cross-sectional view showing a surface protection structure according to an eighth embodiment of the present invention. [Figure 9] FIG. 13 is a cross-sectional view showing a surface protection structure according to a ninth embodiment of the present invention. [Figure 10] FIG. 23 is a cross-sectional view showing a surface protection structure according to a tenth embodiment of the present invention. [Figure 11] 1 is a graph showing the total amount of heat generated and the rate of heat generation over time in a heat generation test of the surface protection structure of the present invention. [Figure 12] 1 is a graph showing the total amount of heat generated and the rate of heat generation over time in a heat generation test of a conventional surface protection structure. [Figure 13] 1 is a graph showing the total amount of heat generated and the heat generation rate over time in a heat generation test when the layer thickness of the second protective layer is 0.6 mm, which is the lower limit value. [Figure 14] 1 is a graph showing the total amount of heat generated and the heat generation rate over time in a heat generation test when the layer thickness of the second protective layer is 0.5 mm, which is less than the lower limit. [Figure 15] 1 is a graph showing the total amount of heat generated and the heat generation rate over time in a heat generation test when the layer thickness of the second protective layer is 1.0 mm, which is the upper limit value. [Figure 16] 1 is a graph showing the total amount of heat generated and the heat generation rate over time in a heat generation test when the layer thickness of the second protective layer is 1.2 mm, which exceeds the upper limit value. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, embodiments of a non-flammable surface protection structure according to the present invention will be described with reference to the drawings. It should be noted that the embodiments described below are merely examples of embodiments of the present invention, and the present invention is not limited to the configurations of these embodiments, and can be modified as appropriate without departing from the gist of the present invention.
[0027] (First embodiment) Fig. 1 is a cross-sectional view showing a surface protection structure according to a first embodiment. As shown in Fig. 1, the surface protection structure protects a surface 10a of a structure 10, which is an object to be protected 10, and a first adhesive layer 11, a first protective layer 12, a second adhesive layer 13, and a second protective layer 14 are laminated on the surface 10a in this order from the bottom in Fig. 1.
[0028] The structure 10 is, for example, a concrete structure 10, and a first adhesion layer 11 is applied to the surface 10a so as to cover the entire surface 10a. The first adhesion layer 11 is formed by an adhesion improving coating (primer) for improving adhesion with the first protective layer 12. Note that if the surface 10a and the resin forming the first protective layer 12 are compatible with each other and adhesion can be ensured, the first adhesion layer 11 may be omitted.
[0029] The coating that forms the first adhesion layer 11 is composed of at least one type of paint, such as epoxy-based resin, urethane-based resin, urea-based resin, methacrylic resin, polyester-based resin, vinyl ester-based resin, acrylic resin, chlorinated rubber-based resin, inorganic paint, etc. When the surface 10a of the concrete structure 10 is not rough, the first adhesive layer 11 is formed directly on the surface 10a by painting, as shown in FIG.
[0030] Furthermore, if the surface 10a is rough, cross-section repair and surface preparation of the surface 10a are performed. Cross-section repair refers to correcting defects (such as craters, pockmarks, unevenness, etc.) that occur on the surface 10a of the concrete structure 10. In general, scratches and irregularities on the concrete surface of 1 mm or more are repaired. In this repair (restoration) process, weak areas on the surface 10a are removed → glue is applied → mortar or resin is poured in and the surface is smoothed with a trowel or the like. The surface preparation is to remove small holes in the surface 10a after the cross section is repaired. Basically, a surface preparation material is applied to the entire surface 10a with a trowel. This surface preparation is a pinhole prevention process when forming (painting) the first adhesive layer 11 and the first protective layer 12.
[0031] The first protective layer 12 is provided indirectly on the surface 10a via the first adhesive layer 11 so as to cover the entire surface of the first adhesive layer 11, and may have waterproof properties. The first protective layer 12 may have rust resistance, corrosion resistance, abrasion resistance, chemical resistance, salt damage resistance, insulation, heat insulation, etc. in addition to waterproof properties, and is formed by applying paint to the surface of the first adhesive layer 11. When formed by painting in this way, waterproof properties are usually ensured. When a resin layer (first protective layer 12) is formed by applying paint to the surface, for example, the paint is formed of a polyurethane resin containing an isocyanate component and a polyol component.
[0032] Moreover, a synthetic resin paint other than polyurethane resin may be used as the resin applied to the first protective layer 12. For example, the first protective layer 12 may be formed using paint such as epoxy resin, urea resin, methacrylic resin, polyester resin, vinyl ester resin, and acrylic resin. Such a first protective layer 12 is a flammable resin layer.
[0033] Furthermore, the thickness of the first protective layer 12 is set to be 0.5 mm or more and less than 5.0 mm, but may be 0.5 mm or more and less than 3.0 mm, or 0.5 mm or more and less than 2.0 mm. The thickness of the first protective layer 12 is set to 0.5 mm or more and less than 5.0 mm because, if the thickness is less than 0.5 mm, the first protective layer 12 becomes too thin, making it difficult to ensure waterproofness and other performance properties, while if the thickness is 5.0 mm or more, the first protective layer 12 becomes too thick, resulting in increased material costs and laborious construction.
[0034] The second adhesion layer 13 is applied to the surface 12a of the first protective layer 12 so as to cover the entire surface 12a. The second adhesion layer 13 is intended to improve adhesion with the second protective layer 12, and is formed by an adhesion improving coating (primer). The coating for forming the second adhesive layer 13 is similar to that for the first adhesive layer 11, and is made of one of the following paints: epoxy resin, urethane resin, urea resin, methacrylic resin, polyester resin, vinyl ester resin, acrylic resin, chlorinated rubber resin, inorganic resin, etc.
[0035] The second protective layer 14 is indirectly applied to the first protective layer 12 via the second adhesive layer 13 so as to cover the entire surface of the second adhesive layer 13. The second protective layer 14 is formed of a resin layer containing a urethane composite polymer, a curing agent containing aminosilane, and a base material containing ammonium polyphosphate. Ammonium polyphosphate is a chain inorganic phosphate compound containing ammonium, and is a flame retardant. An example of the paint used to form the second protective layer 14 is Nullifier Hybrid Basecoat SC902 (manufactured by Nullifier Ltd., UK).
[0036] Furthermore, when forming the second protective layer 14, it is preferable to add compounds such as boron compounds, molybdenum compounds, tin compounds, antimony compounds, zirconium compounds, phosphorus compounds, silicon compounds, hydrated compounds, hydrated metal compounds, nitrogen compounds, ceramic compounds, bromine compounds, and chlorine compounds as diluents (additives) to a resin containing a urethane composite polymer, a curing agent containing aminosilane, and a base containing ammonium polyphosphate. The diluent (additive) is preferably added at a concentration of 30 wt % in a weight ratio of 50 to 400% relative to the resin of the second protective layer 14. By adding a diluent, the viscosity of the resin of the second protective layer 14 is reduced, making it easier to apply.
[0037] The thickness of the second protective layer 14 is set to 0.6 mm or more, but may be set to 0.6 mm or more and less than 5.0 mm, preferably 0.6 mm or more and 2.0 mm or less, and more preferably 0.6 mm or more and 1.0 mm or less. The reason why the thickness of the second protective layer 14 is set to 0.6 mm or more is that if the thickness is less than 0.6 mm, the second protective layer 14 becomes too thin and it becomes difficult to ensure non-combustibility. On the other hand, if the thickness exceeds 1.0 mm, the second protective layer 14 becomes too thick, which increases the material cost and the construction work, and in addition, the amount of resin forming the resin layer (second protective layer) becomes too large, which may actually decrease the non-combustibility, so the thickness is preferably 1.0 mm or less.
[0038] To paint the surface 10a of the structure 10, that is, to construct the surface protection structure of this embodiment, first, a first adhesive layer 11 is provided on the surface 10a. In this case, a resin composed of at least one type of paint such as epoxy resin, urethane resin, urea resin, methacrylic resin, polyester resin, vinyl ester resin, acrylic resin, chlorinated rubber resin, and inorganic paint is applied to the surface 10a so as to cover the entire surface (primer coating). If the surface 10a is rough, the cross section is repaired as described above, and the surface is adjusted as necessary, and then the primer coating is applied. The thickness of the first adhesive layer 11 formed by the primer coating is about 0.02 mm.
[0039] Next, after the primer coating, and after sufficient curing (for example, 3 hours or more and 48 hours or less), the first protective layer 12 is provided. In this case, the first protective layer 12 is provided on the surface of the first adhesive layer 11 by applying paint to cover the entire surface. The coating material is formed from a polyurethane resin containing an isocyanate component and a polyol component. The first adhesive layer 11 not only repairs small scratches on the surface 10a of the structure 10 and allows the first protective layer 12 to be formed smoothly by painting, but also improves adhesive strength. Furthermore, even if cracks or the like occur in the structure 10, the first protective layer 12 can impart high durability to the structure 10 due to its conformability.
[0040] Next, the first protective layer 12 is provided by painting, and after sufficient curing (for example, within 24 hours), the second adhesive layer 13 is provided. In this case, a resin composed of at least one type of paint such as epoxy resin, urethane resin, urea resin, methacrylic resin, polyester resin, vinyl ester resin, acrylic resin, chlorinated rubber resin, inorganic resin, etc. is painted (primer painted) on the surface 12a of the first protective layer 12 so as to cover the entire surface. The layer thickness of the second adhesive layer 13 by the primer painting is about 0.02 mm.
[0041] Next, after the primer coating is applied and sufficient curing (for example, 1 hour or more and 48 hours or less), the second protective layer 14 is provided. In this case, the second protective layer 14 is provided on the surface of the second adhesive layer 13 by applying paint to cover the entire surface of the second adhesive layer 13. The paint forming the second protective layer 14 is formed from a resin containing a urethane composite polymer, a curing agent containing aminosilane, and a base material containing ammonium polyphosphate, to which the above-mentioned diluent (additive) has been added. By applying such paint, the durability of the structure 10 can be improved and the surface 10a can be made non-flammable.
[0042] Table 1 shows the steps, paint material, coating amount, layer thickness, and coating interval when constructing an example of the surface protection structure of this embodiment described above. The coating interval is the time interval between the next steps. In Table 1, the layer thickness of the second protective layer is set to 0.6 to 1.0 mm.
[0043] [Table 1]
[0044] According to this embodiment, the following effects are obtained. (1) A first protective layer 12 is provided on the surface 10a of the object to be protected (concrete structure) 10, and since this first protective layer 12 is formed by painting, waterproofing is usually ensured. Also, since the first protective layer 12 has rust resistance, corrosion resistance, abrasion resistance, chemical resistance, salt damage resistance, insulation, heat insulation, etc. in addition to waterproofing, the rust resistance, corrosion resistance, abrasion resistance, chemical resistance, salt damage resistance, insulation, and heat insulation of the surface 10a can be easily ensured. (2) Furthermore, by forming a second protective layer 14 made of a resin layer containing a resin to which ammonium polyphosphate has been added by painting on the surface of the first protective layer 12 made of a flammable resin layer, it is possible to ensure non-flammability using a resin coating film, which was not previously possible. As described above, in the present invention, the first protective layer 12 and the second protective layer 14 are formed by resin-based coating, which can shorten the construction period and can easily be applied to objects to be protected having complex shapes. (3) Moreover, since the second protective layer 14 is formed by painting a resin layer, waterproofness is usually ensured. As a result, waterproofness can be ensured by the second protective layer 14 in addition to the waterproofness of the first protective layer 12.
[0045] (4) A first adhesion layer 11 for improving adhesion with the first protective layer 12 is applied to the surface 10a of the object to be protected (concrete structure) 10, thereby improving adhesion between the surface 10a and the first protective layer 12 and suppressing peeling of the first protective layer 12. (5) Since the second adhesion layer 13 is coated on the surface 12a of the first protective layer 12 to improve adhesion with the second protective layer 14, the adhesion between the surface 12a of the first protective layer 12 and the second protective layer 14 is improved, and peeling of the second protective layer 14 can be suppressed.
[0046] In the first embodiment, the first adhesion layer 11, the first protective layer 12, the second adhesion layer 13, and the second protective layer 14 are formed in sequence on the surface 10a of the object to be protected 10, and before forming the first adhesion layer 11, cross-sectional repair and surface preparation are performed on the surface 10a. In other words, the steps of (1) cross-sectional repair → (2) surface preparation → (3) first adhesion layer 11 (primer) → (4) first protective layer 12 → (5) second adhesion layer 13 (primer) → (6) second protective layer 14 are performed. In the present invention, the steps of forming the first protective layer 12 and the second protective layer 14 are essential, but the other steps are performed as necessary. Therefore, when the surface protective structure according to the present invention is constructed, there are a total of 16 different patterns, and the structure has 16 different cross-sectional structures.
[0047] Furthermore, when the base material preparation and the formation of the first adhesion layer 11 are integrated, the steps are (1) cross-section repair → (2) base material preparation + first adhesion layer 11 (primer) → (3) first protective layer 12 → (4) second adhesion layer 13 (primer) → (5) second protective layer 14, which means a total of eight steps and eight different cross-sectional structures. Furthermore, when the cross-sectional repair, surface preparation, and formation of the first adhesion layer are integrated, the steps are (1) cross-sectional repair + surface preparation + first adhesion layer 11 (primer) → (2) first protective layer 12 → (3) second adhesion layer 13 (primer) → (4) second protective layer 14, which means there are four steps in total and four different cross-sectional structures. Therefore, when constructing the surface protection structure according to the present invention, there are a total of 28 different cross-sectional structures (16 + 8 + 4).
[0048] In addition, in this embodiment, the first protective layer 12 is formed from a polyurethane resin, but instead of the first protective layer 12 made of this polyurethane resin, the first protective layer 12A may be formed from a first adhesive layer 11 and / or a second adhesive layer 13 (see Figure 10). In this case, there is no need to form both the first adhesion layer 11 and the second adhesion layer 13; it is sufficient to form either one of the adhesion layers, so the steps are (1) cross-section repair →(2) base material adjustment →(3) first protective layer (first adhesion layer 11 or second adhesion layer 13) →(4) second protective layer 14, which means there are a total of four steps and four different cross-sectional structures. Therefore, by adding 4 to the 28 mentioned above, there are a total of 32 possible cross-sectional structures.
[0049] Next, examples of surface protection structures having some of the 32 cross-sectional structures described above will be described. Second embodiment 2 is a cross-sectional view showing a surface protection structure according to a second embodiment. The surface protection structure according to the second embodiment is different from the first embodiment in that the second adhesive layer 13 is omitted, and other configurations are the same as those of the first embodiment, so the same configurations are denoted by the same reference numerals and the description thereof will be omitted.
[0050] In this embodiment, when the second protective layer 14 can be formed (painted) immediately after the first protective layer 12 is formed by painting (within the recoating interval time), the second protective film 14 is formed directly by painting without forming a second adhesion layer 13 on the surface 12a of the first protective layer 12.
[0051] According to this embodiment, in addition to obtaining the effects (1) to (4) in the first embodiment, the second adhesion layer 13 is omitted, so that construction time and construction costs can be reduced accordingly.
[0052] (Third embodiment) 3 is a cross-sectional view showing a surface protection structure according to a third embodiment. The surface protection structure according to the third embodiment differs from the first embodiment in that the coating of the first adhesive layer 11, the cross-sectional repair of the surface 10a of the concrete structure 10, and the base preparation are omitted, and other configurations are the same as those of the first embodiment, so that the same configurations are denoted by the same reference numerals and the description thereof is omitted.
[0053] In this embodiment, when the surface condition of the surface 10a of the concrete structure 10 is suitable for forming (painting) the first protective layer 12, the surface 10a is compatible with the resin that forms the first protective layer 12, and the adhesion of the first protective layer 12 is high, the first protective layer 12 is formed (painted) directly on the surface 10a.
[0054] According to this embodiment, in addition to obtaining the effects (1) to (3) and (5) in the first embodiment, painting of the first adhesion layer 11, cross-sectional repair of the surface 10a of the concrete structure 10 and base preparation are omitted, so that construction time and construction costs can be shortened accordingly.
[0055] (Fourth embodiment) 4 is a cross-sectional view showing a surface protection structure according to a fourth embodiment. The surface protection structure according to the fourth embodiment differs from the first embodiment in that the coating of the first adhesion layer 11 and the second adhesion layer 12, and the cross-sectional repair and base preparation of the surface 10a of the concrete structure 10 are omitted, and other configurations are the same as those of the first embodiment, so that the same configurations are denoted by the same reference numerals and their description is omitted.
[0056] In this embodiment, if the surface 10a of the concrete structure 10 and the resin forming the first protective layer 12 are compatible and have high adhesion, and if the second protective layer 14 can be formed (painted) immediately after forming (painting) the first protective layer 12 (within the recoating interval time), the first protective layer 12 is formed (painted) directly on the surface 10a without performing cross-sectional repair and base adjustment, and further, the second protective layer 14 is formed (painted) directly on the first protective layer 12.
[0057] According to this embodiment, in addition to obtaining the effects (1) to (3) in the first embodiment, the painting of the first adhesion layer 11 and the second adhesion layer 12, and the cross-sectional repair and base preparation of the surface 10a of the concrete structure 10 are omitted, so that the construction time and construction costs can be shortened accordingly.
[0058] Fifth embodiment 5 is a cross-sectional view showing a surface protection structure according to a fifth embodiment. The surface protection structure according to the fifth embodiment differs from the first embodiment in that cross-section repair is performed when the surface 10a of the concrete structure 10 is rough, and other configurations are the same as those of the first embodiment, so the same components are denoted by the same reference numerals and their description will be omitted.
[0059] In this embodiment, the cross-section repair of the surface 10a is a full and / or partial repair of the surface 10a (usually repair of unevenness of 1 mm or more). As shown in Fig. 5, the surface 10a is provided with a cross-section repair layer 20 formed by the repair. In addition, if the object to be protected 10 is not a concrete structure but is formed of a metal plate, repair of the metal plate with putty is also included.
[0060] According to this embodiment, in addition to obtaining the effects (1) to (5) in the first embodiment, the first adhesion layer 11 is formed (painted) after cross-sectional repair of the surface 10a of the concrete structure 10, so that the first adhesion layer 11 can be reliably formed on the surface 10a.
[0061] Sixth embodiment 6 is a cross-sectional view showing a surface protection structure according to a sixth embodiment. The surface protection structure according to the sixth embodiment differs from the first embodiment in that a surface preparation is performed on the surface 10a of the concrete structure 10 before forming (painting) the first adhesive layer 11. Since the other configurations are the same as those of the first embodiment, the same components are denoted by the same reference numerals and the description thereof is omitted.
[0062] In this embodiment, the surface conditioning of the surface 10a is performed on the entire surface 10a by applying a surface conditioning material to the entire surface 10a. As shown in Fig. 6, the surface 10a is provided with a surface conditioning layer 21 formed by the surface conditioning.
[0063] According to this embodiment, in addition to obtaining the effects (1) to (5) of the first embodiment, the first adhesion layer 11 is formed (painted) after the surface 10a of the concrete structure 10 is prepared, so that the first adhesion layer 11 can be formed uniformly and pinholes that tend to occur in the first adhesion layer 11 and the first protective layer 12 can be suppressed.
[0064] Seventh embodiment 7 is a cross-sectional view showing a surface protection structure according to a seventh embodiment. The surface protection structure according to the seventh embodiment differs from the first embodiment in that cross-section repair and base preparation are performed on the surface 10a of the concrete structure 10 before forming (painting) the first adhesive layer 11. Since the other configurations are the same as those of the first embodiment, the same reference numerals are used for the same configurations and their description is omitted.
[0065] In this embodiment, after the surface 10a is subjected to cross-section repair, the surface is further subjected to surface conditioning. The cross-section repair is a partial repair of the surface 10a, and the surface conditioning is a whole surface (the whole surface 10a). As shown in FIG. 7, the surface 10a is provided with a cross-section repair layer 20 formed by the cross-section repair and a surface conditioning layer 21 formed by the surface conditioning.
[0066] According to this embodiment, in addition to obtaining the effects (1) to (5) in the first embodiment, the first adhesion layer 11 is formed (painted) after cross-sectional repair of the surface 10a of the concrete structure 10, so that the first adhesion layer 11 can be reliably formed on the surface 10a, and further, the first adhesion layer 11 is formed (painted) after surface preparation, so that the first adhesion layer 11 can be formed uniformly and pinholes that tend to occur in the first adhesion layer 11 and the first protective layer 12 can be suppressed.
[0067] Eighth embodiment 8 is a cross-sectional view showing a surface protection structure according to an eighth embodiment. The surface protection structure according to the eighth embodiment differs from the first embodiment in that a surface 10a of a concrete structure 10 is integrally subjected to a base preparation and a first adhesive layer 11, and other configurations are the same as those of the first embodiment, so that the same configurations are denoted by the same reference numerals and their description will be omitted.
[0068] In this embodiment, the resin forming the surface adjustment material and the first adhesion layer is the same resin, and the first adhesion layer 11A including the surface adjustment layer is formed (painted) with the resin as shown in Fig. 8. Therefore, the first adhesion layer 11A is thicker than the first adhesion layer 11 of the first embodiment.
[0069] According to this embodiment, in addition to obtaining the effects (1) to (5) in the first embodiment, the base material adjustment layer on the surface 10a of the concrete structure 10 is formed simultaneously with the first adhesion layer 11A, so that the formation (painting) of the first adhesion layer 11A and the base material adjustment can be carried out simultaneously, which makes construction easier.
[0070] Ninth embodiment 9 is a cross-sectional view showing a surface protection structure according to a ninth embodiment. The surface protection structure according to the ninth embodiment differs from the first embodiment in that the surface 10a of the concrete structure 10 is integrally subjected to base preparation and the first adhesive layer 11, and the second adhesive layer 13 is omitted. Since the other configurations are the same as those of the first embodiment, the same configurations are denoted by the same reference numerals and their description is omitted.
[0071] In this embodiment, similarly to the eighth embodiment, the resin forming the surface adjustment material and the first adhesion layer is the same resin, and the first adhesion layer 11A including the surface adjustment layer is formed (painted) with the resin, as shown in Fig. 9. Therefore, the first adhesion layer 11A is thicker than the first adhesion layer 11 of the first embodiment. Furthermore, in this embodiment, when the second protective layer 14 can be formed (painted) immediately after the first protective layer 12 is formed by painting (within the recoating interval time), the second protective film 14 is formed directly by painting without forming a second adhesion layer 13 on the surface 12a of the first protective layer 12.
[0072] According to this embodiment, in addition to obtaining the effects (1) to (4) in the first embodiment, the base material adjustment layer on the surface 10a of the concrete structure 10 is formed simultaneously with the first adhesion layer 11A, so that the formation (painting) of the first adhesion layer 11A and the base material adjustment can be carried out simultaneously, which makes construction easier. Furthermore, since the second adhesive layer 13 is omitted, construction time and costs can be reduced accordingly.
[0073] Tenth embodiment 10 is a cross-sectional view showing a surface protection structure according to a tenth embodiment. The surface protection structure according to the tenth embodiment differs from the first embodiment in that a surface 10a of a concrete structure 10 is subjected to a base preparation, and a first protective layer 12A is formed by a first adhesive layer and / or a second adhesive layer instead of the first protective layer 12 made of a polyurethane resin. Since the other configurations are the same as those of the first embodiment, the same configurations are denoted by the same reference numerals and the description thereof is omitted.
[0074] In this embodiment, as shown in FIG. 10, a first protective layer 12A made of a first adhesive layer and / or a second adhesive layer is formed on the surface of the base material adjustment layer 21.
[0075] According to this embodiment, in addition to obtaining the effects (1) and (3) in the first embodiment, the first protective layer 12A is formed by a first adhesion layer and / or a second adhesion layer instead of a first protective layer made of polyurethane resin, which makes construction easier and does not use polyurethane resin, which is considered to be relatively difficult to handle (requiring appropriate surface preparation, selection of primer, and careful prior investigation and verification of chemical resistance and heat resistance), thereby making construction easier.
[0076] Next, heat generation tests (cone calorimeter tests) were conducted on the surface protection structure of the present invention and a conventional surface protection structure having only a resin layer (first protective layer) formed from a polyurethane resin, and the results of the heat generation tests will be described.
[0077] The test specimen, which is the object to be protected in the surface structure of the present invention, is a rectangular concrete. A first protective layer made of polyurethane resin was formed (painted) on the surface of the concrete. On the surface of this first protective layer, a second protective layer was formed (painted) on the surface of this first protective layer, made of a resin layer (Narifire's hybrid base coat SC902) containing a urethane composite polymer, a hardener containing aminosilane, and a base agent containing ammonium polyphosphate. The first protective layer has a thickness of 2.0 mm, and the second protective layer has a thickness of 1.0 mm. The rectangular specimen had long and short sides measuring 99 mm x 100 mm, a thickness of 35.0 mm, and a weight (mass) of 729.0 g.
[0078] Table 2 shows the results of a heat generation test of an example of the surface protection structure according to the present invention.
[0079] [Table 2]
[0080] Figure 11 shows the total heat release (MJ / m) over time. 2 ) and heat release rate (kW / m 2 ) is a graph showing The criteria for determining whether a material is non-flammable, that is, whether it is suitable for being non-flammable, are as follows: <Judgment criteria> (1) Total calorific value: 8.0 MJ / m 2 It is less than or equal to. (2) Maximum heat generation rate: 200KW / m 2 The duration must be 10 seconds or less. (3) There are no through holes on the back surface of the test specimen. To be suitable as non-flammable, it is necessary to satisfy all of the above criteria (1) to (3), and it is most important that the criteria (1) is satisfied.
[0081] As shown in Table 2 and Figure 11, the total heat generation after 20 minutes (1200 seconds) was 5.7 (MJ / m 2 In the heat generation test, the criterion for non-flammability was 8.0 (MJ / m 2 ) or less, the above judgment criterion (1) is satisfied. As shown in Table 2 and Figure 11, the maximum heat generation rate was 140.7 (kW / m 2 ), but the heat generation rate is 200 (kW / m 2 In the heat generation test, the criterion for non-flammability was a heat generation rate of 200 (kW / m 2 ) in less than 10 seconds, whereas the surface protection structure of the present invention has a heat generation rate of 200 (kW / m 2 ) and therefore satisfies the judgment criterion (2) above. Furthermore, there were no holes penetrating the first and second protective layers and reaching the rear surface of the test specimen, and no deformation, so the above judgment criterion (3) was met. As described above, the surface protection structure according to the present invention satisfies all of the criteria (1) to (3) above, and is therefore suitable as a non-combustible material.
[0082] On the other hand, the test specimen, which was the object to be protected in the conventional surface protection structure, was a rectangular concrete body, as in the case of the present invention, and a first protective layer made of polyurethane resin was formed (painted) on the surface of the concrete. The first protective layer had a thickness of 2.0 mm. The rectangular specimen has an area of 0.008840 m 2 It has a thickness of 7.27 mm and a weight (mass) of 70.87 g.
[0083] Table 3 shows the results of heat generation tests on conventional surface protection structures.
[0084] [Table 3]
[0085] Figure 12 shows the total heat release (MJ / m) over time. 2 ) and heat release rate (kW / m 2 ) is a graph showing As shown in Table 3 and Figure 12, the total heat generation after 20 minutes was 24.43 (MJ / m 2 ) Therefore, it is clear that the above criterion (1) is not met. As shown in Table 3 and Figure 12, the maximum heat release rate (highest heat release rate) is 129.70 (kW / m 2 ) and the heat generation rate is 200 (kW / m 2 ) and therefore satisfies the judgment criterion (2) above. Furthermore, since there was no hole penetrating the first protective layer and reaching the rear surface of the test specimen, the above judgment criterion (3) was met. However, although the conventional surface protection structure satisfies the above criteria (2) and (3), it does not meet the most important criterion (1), and therefore is not suitable as a non-combustible material.
[0086] Next, in the surface protection structure according to the present invention, the layer thickness of the second protection layer is set to 0.6 mm or more, and may be set preferably to 0.6 mm or more and 1.0 mm or less. Heat generation tests were conducted when the thickness of the second protective layer was the lower limit of 0.6 mm and when it was 0.5 mm, which is less than the lower limit, and when it was the upper limit of 1.0 mm and when it was 1.2 mm, which is greater than the upper limit. The results of the heat generation tests are described below.
[0087] The test specimen, which is the object to be protected in the surface structure of the present invention, is a rectangular concrete body. A first protective layer made of polyurethane resin is formed (painted) on the surface of the concrete body. A second protective layer (fire-resistant coating) is formed (painted) on the surface of this first protective layer, made of a resin layer containing a urethane composite polymer, a curing agent containing aminosilane, and a base agent containing ammonium polyphosphate.
[0088] (1) When the thickness of the second protective layer is the lower limit of 0.6 mm The rectangular specimen has an area of 0.008840 m 2 It has a thickness of 6.06 mm and a weight (mass) of 52.20 g.
[0089] Table 4 shows the results of the heat build-up test when the thickness of the second protective layer was the lower limit of 0.6 mm.
[0090] [Table 4]
[0091] Figure 13 shows the total heat generation (MJ / m) over time when the thickness of the second protective layer is the lower limit of 0.6 mm. 2 ) and heat release rate (kW / m 2 ) is a graph showing As shown in Table 4 and Figure 13, the total heat generation after 20 minutes was 5.91 (MJ / m 2 ) was. As mentioned above, in the heat generation test, the criterion for non-flammability (1) is 8.0 (MJ / m 2 ) or less, it can be seen that the surface protection structure in which the thickness of the second protective layer is 0.6 mm is appropriately non-combustible. As shown in Table 4 and Figure 13, the maximum heat release rate (highest heat release rate) is 76.12 (kW / m 2 ) and the heat release rate of the judgment criterion (2) is 200 (kW / m 2 ) and so it is deemed suitable as non-flammable. Furthermore, since there were no holes penetrating the first and second protective layers and reaching the rear surface of the test specimen, and no deformation, the test specimen satisfies the judgment criterion (3). Therefore, it is understood that when the thickness of the second protective layer is the lower limit of 0.6 mm, it is suitable as a non-combustible material.
[0092] (2) When the thickness of the second protective layer is less than the lower limit of 0.5 mm The rectangular specimen has an area of 0.008840 m 2 It has a thickness of 5.68 mm and a weight (mass) of 59.51 g.
[0093] Table 5 shows the results of the heat build-up test when the thickness of the second protective layer was 0.5 mm, which is less than the lower limit.
[0094] [Table 5]
[0095] Figure 14 shows the total heat generation (MJ / m) over time when the thickness of the second protective layer is 0.5 mm, which is less than the lower limit. 2 ) and heat generation rate (kW / m 2 ) is a graph showing As shown in Table 5 and Figure 14, the total heat generation after 20 minutes was 9.31 (MJ / m 2 ) was. As mentioned above, in the heat generation test, the criterion for non-flammability (1) is 8.0 (MJ / m 2 ) or less, it can be seen that a surface protection structure in which the thickness of the second protective layer is 0.5 mm is not suitable as a non-combustible material. As shown in Table 5 and Figure 14, the maximum heat release rate (highest heat release rate) is 254.02 (kW / m 2 ) and the heat release rate of the judgment criterion (2) is 200 (kW / m 2 ), it is clear that it is not suitable as a non-flammable material. Furthermore, since there were no holes penetrating the first and second protective layers and reaching the rear surface of the test specimen, and no deformation, the test specimen satisfies the judgment criterion (3). However, since it does not satisfy any of the criteria (1) and (2) above, it is clear that it is not suitable as a non-flammable material.
[0096] (3) When the thickness of the second protective layer is the upper limit of 1.0 mm The rectangular specimen has an area of 0.008840 m 2 It has a thickness of 6.31 mm and a weight (mass) of 57.31 g.
[0097] Table 6 shows the results of the heat build-up test when the thickness of the second protective layer was the upper limit of 1.0 mm.
[0098] [Table 6]
[0099] Figure 15 shows the total heat generation (MJ / m) over time when the thickness of the second protective layer is the upper limit of 1.0 mm. 2 ) and heat generation rate (kW / m 2 ) is a graph showing As shown in Table 6 and Figure 15, the total heat generation after 20 minutes was 6.08 (MJ / m 2 ) was. As mentioned above, in the heat generation test, the criterion for non-flammability (1) is 8.0 (MJ / m 2 ) or less, it can be seen that the surface protection structure in which the thickness of the second protective layer is 1.0 mm is appropriately non-flammable. As shown in Table 6 and Figure 15, the maximum heat release rate (highest heat release rate) is 131.81 (kW / m 2 ) and the heat release rate of the judgment criterion (2) is 200 (kW / m 2 ) and so it is deemed suitable as non-flammable. Furthermore, since there were no holes penetrating the first and second protective layers and reaching the rear surface of the test specimen, and no deformation, the test specimen satisfies the judgment criterion (3). Therefore, it is understood that when the layer thickness of the second protective layer is the upper limit value of 1.0 mm, it is suitable as a non-combustible material.
[0100] (4) When the thickness of the second protective layer is 1.2 mm, which exceeds the upper limit The rectangular specimen has an area of 0.008840 m 2 It has a thickness of 5.29mm and a weight (mass) of 56.88g.
[0101] Table 7 shows the results of the heat generation test when the layer thickness of the second protective layer was 1.2 mm, which exceeds the upper limit.
[0102] [Table 7]
[0103] Figure 16 shows the total heat generation (MJ / m) over time when the thickness of the second protective layer is 1.2 mm, which exceeds the upper limit. 2 ) and heat generation rate (kW / m 2 ) is a graph showing As shown in Table 7 and Figure 16, the total heat generation after 20 minutes was 10.14 (MJ / m 2 ) was. As mentioned above, in the heat generation test, the criterion for non-flammability (1) is 8.0 (MJ / m 2 ) or less, it can be seen that a surface protection structure in which the thickness of the second protective layer is 1.2 mm is not suitable as a non-combustible material. As shown in Table 7 and Figure 16, the maximum heat release rate (highest heat release rate) is 237.58 (kW / m 2 ) and the heat release rate of the judgment criterion (2) is 200 (kW / m 2 ) and therefore it is not suitable as a non-flammable material. Furthermore, since there were no holes penetrating the first and second protective layers and reaching the rear surface of the test specimen, and no deformation, the test specimen satisfies the judgment criterion (3). However, since it does not satisfy the criteria of (1) and (2) above, it is clear that it is not suitable as a non-combustible material. In addition, in the case of a surface protection structure in which the thickness of the second protective layer was 1.2 mm, which exceeded the upper limit, ignition occurred 18 seconds after the start of the test, and the radiation intensity reached 8.0 (MJ / m) in approximately 3 minutes. 2 ) was reached. Therefore, it was found that if the thickness of the second protective layer is 1.2 mm, the second protective layer becomes too thick and the amount of resin forming the resin layer (second protective layer) becomes excessive, which in turn reduces non-flammability. [Explanation of symbols]
[0104] 10 Concrete structures (protected objects) 10a surface 11, 11A First adhesive layer 12,12A 1st protection layer 13 Second Adhesive Layer 14 Second protective layer
Claims
1. A surface protection structure for protecting a surface of an object to be protected, A first protective layer formed of a flammable resin layer, which is directly or indirectly painted on the surface of the object to be protected; a second protective layer formed of a resin layer containing a resin to which ammonium polyphosphate has been added, the second protective layer being directly or indirectly applied to a surface of the first protective layer; A non-flammable surface protection structure comprising:
2. The non-flammable surface protection structure according to claim 1, characterized in that a first adhesion layer is painted on the surface of the object to be protected to improve adhesion with the first protective layer.
3. The non-flammable surface protection structure according to claim 1, characterized in that a second adhesion layer is coated on the surface of the first protective layer to improve adhesion with the second protective layer.
4. 2. The non-combustible surface protection structure according to claim 1, wherein the second protective layer has a thickness of 0.6 mm or more.
5. The non-flammable surface protection structure according to any one of claims 1 to 4, characterized in that the object to be protected is a structure.
Citation Information
Patent Citations
Panel cover for covering side surface and undersurface of structure, and installation method therefor
JP2004324230A