Semiconductor structures for optoelectronic applications - Patents.com
A semiconductor structure with an intermediate layer having a refractive index close to the first and second layers simplifies the bonding process, reducing costs and defects in VCSEL fabrication, while maintaining optical performance.
Patent Information
- Application Number
- JP2024507100
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-09-22
- Filing Date
- 2022-09-08
- Publication Date
- 2024-10-02
AI Technical Summary
The fabrication of vertical cavity surface emitting lasers (VCSELs) is complicated and costly due to the direct bonding of high-quality thin working layers onto carrier substrates, which requires complex and expensive surface preparation steps.
A semiconductor structure comprising a first layer coupled to a second layer via an intermediate layer with a refractive index close to that of the first and second layers, and a low damping coefficient, facilitating direct bonding without the need for adhesive materials, thereby simplifying the fabrication process.
This approach enhances the bonding quality, reduces the risk of defects, and lowers the overall cost by simplifying the surface preparation and alignment of layers, while maintaining the optical performance of VCSELs.
Smart Images

Figure 2024535671000001_ABST
Abstract
Description
[Technical field]
[0001] FIELD OF THEINVENTION The field of the invention is that of semiconductors, in particular the optoelectronics field.The invention relates to a semiconductor structure comprising a first layer made of a crystalline semiconductor bonded to a second layer through an intermediate layer, the intermediate layer having a refractive index very close to the refractive indexes of the first and second layers. [Background technology]
[0002] (Technical Background of the Invention) Vertical-cavity surface-emitting lasers (VCSELs) are increasingly being developed for emerging mass-market applications, especially in face recognition in the mobile phone sector, and light detection and ranging (lidar) for the automotive industry.
[0003] The VCSEL 100 is manufactured by a stack of III-V semiconductor layers by successive steps of epitaxial growth (FIGS. 1a and 1b). The composition, doping and thickness of each layer are precisely controlled to form, on the one hand, an active region 2 consisting of one or more quantum wells enabling a laser beam to be generated, and, on the other hand, two Bragg mirrors 3a, 3b sandwiching the active region 2 and consisting of alternating layers of high and low refractive index.
[0004] As shown in Fig. 1a, it is known to form a stack of layers of a VCSEL 100 on a bulk substrate 1, for example made of Gallium Arsenide (GaAs) for laser wavelengths between 650 nm and 1300 nm, or made of Indium Phosphide (InP) for laser wavelengths between 1300 nm and 2000 nm. To obtain a high-performance VCSEL 100, the bulk substrate 1 must have good quality to properly play the role of an epitaxial seed and ensure that the stack of layers is of high quality.
[0005] Alternatively, to address the cost issues associated with the use of high-quality bulk substrates, the thin high-quality working layer 10 can be transferred to a carrier substrate 1' (FIG. 1b) whose properties are more moderate and / or tailored to other constraints, such as the integration or packaging of the VCSEL 100. Such a transfer of the working layer to a carrier substrate is notably proposed in document WO 2021 / 125005.
[0006] The transfer of one or more thin layers may also be useful in the context of the manufacture of the VCSEL itself. For example, if the Bragg mirrors 3a, 3b require a very large number of alternating layers due to limitations on composition and doping (due to epitaxial growth techniques), it may be more preferable to transfer a set of thin layers (Bragg mirrors) rather than growing them by epitaxy. See, for example, the article by A. Syrbu et al., "1.5-mW single-mode operation of wafer-fused 1550-nm VCSELs," IEEE Photonics Technology Letters, Vol. 16, No. 5, pp. 1230-1232, May 2004.
[0007] Whenever transfer is adopted, the bond between the thin working layer 10 and the carrier substrate 1' must allow the high quality of said layer 10 to be maintained and to prevent disturbances occurring in the operation of the VCSEL 100. Problems may arise from the fact that direct bonding between the thin working layer 10 and the carrier substrate 1', both made of III-V semiconductors, requires several steps to be performed to chemically prepare the surfaces to be bonded, and these steps may prove to be complex and therefore expensive. Objectives of the invention
[0008] The present invention provides a solution that simplifies the fabrication of VCSELs, and more generally of optoelectronic components, by employing a transfer of a first layer to a second layer. The present invention particularly relates to a semiconductor structure comprising a first layer made of a crystalline semiconductor bonded to a second layer via an intermediate layer, the second layer also made of a crystalline semiconductor, the intermediate layer having a refractive index very close to the refractive index of at least one sublayer of the first layer and to the refractive index of at least one sublayer of the second layer, said sublayers being adjacent to the intermediate layer. The intermediate layer further has a very low extinction coefficient. Summary of the Invention
[0009] BRIEF DESCRIPTION OF THE DRAWINGS The present invention relates to a semiconductor structure for optoelectronic applications, comprising: a first layer made of a crystalline semiconductor, an intermediate layer including or adjacent to a direct bond interface; a second layer made of a crystalline semiconductor, Equipped with The first layer is disposed on an intermediate layer, which is disposed on a second layer.
[0010] The semiconductor structure has an intermediate layer made of a material different from the materials of the first and second layers, and the refractive index of the intermediate layer is the refractive index of at least one sublayer of the first layer adjacent to the intermediate layer, and the refractive index of at least one sublayer of the second layer adjacent to the intermediate layer It is noteworthy that the difference is less than 0.3.
[0011] The intermediate layer further has a damping coefficient of less than 100.
[0012] According to some advantageous features of the invention, which may be implemented alone or in any feasible combination, the damping coefficient of the intermediate layer is less than 10, or even less than 1, or in practice even more preferably as close to 0 as possible; The material of the intermediate layer is amorphous. The material of the first layer is monocrystalline with high crystal quality so as to form a seed for epitaxy; the first layer forms all or part of a vertical cavity surface emitting laser (VCSEL); the second layer is a carrier substrate having a light transmittance of more than 30%, The semiconductor of the first layer is gallium arsenide, the semiconductor of the second layer is gallium arsenide, and the material of the intermediate layer is silicon; the first layer is an active region of a vertical cavity surface emitting laser (VCSEL) and the second layer is a multi-layer Bragg mirror of said laser; The semiconductor of the first layer is indium phosphide, the semiconductor of at least one sublayer of the second layer adjacent to the intermediate layer is gallium arsenide, and the material of the intermediate layer is zinc germanium phosphide or boron carbide or zinc silicon arsenide.
[0013] Other features and advantages of the present invention will become apparent from the following detailed description, taken in conjunction with the accompanying drawings. [Brief description of the drawings]
[0014] [Figure 1a] 1 shows a semiconductor structure for fabricating a VCSEL according to the prior art. [Figure 1b] 1 shows a semiconductor structure for fabricating a VCSEL according to the prior art. [Diagram 2] 1 shows a semiconductor structure according to the present invention. [Diagram 3] 1 shows a semiconductor structure according to a first embodiment of the invention; [Figure 4a] 1 illustrates process steps for fabricating a semiconductor structure according to a first embodiment of the invention; [Figure 4b] 1 illustrates process steps for fabricating a semiconductor structure according to a first embodiment of the invention; [Figure 4c] 1 illustrates process steps for fabricating a semiconductor structure according to a first embodiment of the invention; [Figure 4d] 1 illustrates process steps for fabricating a semiconductor structure according to a first embodiment of the invention; [Figure 4e] 1 illustrates process steps for fabricating a semiconductor structure according to a first embodiment of the invention; [Figure 4f] 1 illustrates process steps for fabricating a semiconductor structure according to a first embodiment of the invention; [Figure 4g] 1 illustrates process steps for fabricating a semiconductor structure according to a first embodiment of the invention; [Figure 5a] 5A-5D show process steps for fabricating a semiconductor structure according to a variant of the first embodiment of the invention. [Figure 5f] 5A-5D show process steps for fabricating a semiconductor structure according to a variant of the first embodiment of the invention. [Figure 6a] 2 shows a semiconductor structure according to a second embodiment of the present invention. [Figure 6b] 2 shows a semiconductor structure according to a second embodiment of the present invention. [Figure 6c] 2 shows a semiconductor structure according to a second embodiment of the present invention. Detailed Description of the Invention
[0015] The figures are schematic and not drawn to scale for ease of reading, in particular the layer thicknesses along the z-axis are not to scale relative to the lateral dimensions along the x- and y-axes.
[0016] In the figures, the same reference numbers may be used for elements of the same nature.
[0017] The present invention relates to a semiconductor structure 150 that is specifically tailored for optoelectronic applications.
[0018] The semiconductor structure 150 comprises a first layer 10 made of a crystalline semiconductor, said layer being arranged on an intermediate layer 50, itself arranged on a second layer 40 made of a crystalline semiconductor. As shown in Fig. 2, these layers 10, 40, 50 lie parallel to a major plane (x, y) and have a thickness along the z-axis. By convention, the front side 150a of the semiconductor structure 150 lies on the side of the first layer 10 and the back side 150b of the semiconductor structure 150 lies on the side of the second layer 40.
[0019] The semiconductor structure 150 may take the form of a wafer, e.g., 50 mm to 200 mm in diameter, intended to accommodate a number of optoelectronic components that may then be separated, or alternatively, the semiconductor structure 150 may take the form of a smaller sized die corresponding to a single optoelectronic component or group of components.
[0020] The crystalline semiconductors forming the first layer 10 and the second layer 40, respectively, may be of the same or different nature. For the purpose of manufacturing optoelectronic components, the crystalline semiconductors are suitably selected from III-V semiconductor compounds such as gallium nitride, gallium arsenide, indium phosphide, and other binary, ternary, or quaternary III-V compounds. It is noted that the first layer 10 (and / or the second layer 40) may consist of a stack of sublayers of different doping or composition, or may have a uniform composition.
[0021] The semiconductor structure 150 according to the invention further comprises a direct bonding interface 51, said interface 51 being contained within or adjacent to the intermediate layer 50. By direct bonding is meant bonding based on molecular adhesion between the surfaces to be bonded, without the need for adhesive materials. There are several types of direct bonding, differing in particular in temperature conditions, pressure conditions, atmospheres or treatments carried out before bringing the surfaces into contact: room temperature direct bonding with or without prior plasma activation of the surfaces to be bonded, atomic diffusion bonding (ADB), surface activated bonding (SAB) etc.
[0022] Because semiconductor structure 150 is intended for optoelectronic applications, all or some of the constituent layers of semiconductor structure 150 are intended to pass optical signals, and typically, optoelectronic components fabricated on structure 150 may transmit or receive optical signals through either the front surface 150a or the back surface 150b of semiconductor structure 150, depending on the type of optoelectronic component and the nature of the optoelectronic component.
[0023] In order for the semiconductor structure 150 to have general properties and be compatible with a wide variety of optoelectronic components, the refractive index of the intermediate layer 50 is the refractive index of at least one sublayer of the first layer, said sublayer being adjacent to the intermediate layer 50; and the refractive index of at least one sublayer of the second layer 40, said sublayer being adjacent to the intermediate layer 50; is a difference of less than 0.3, or even less than 0.2.
[0024] In other words, if the first layer 10 (respectively the second layer 40) is formed from stacked sublayers, the difference in refractive index between the sublayer in contact with the intermediate layer 50 and said intermediate layer 50 is less than 0.3, or even less than 0.2. If the first layer 10 (respectively the second layer 40) has a uniform composition, the difference in refractive index between the first layer 10 (respectively the second layer 40) and the intermediate layer 50 is less than 0.3, or even less than 0.2.
[0025] Furthermore, the intermediate layer 50 has an attenuation coefficient k less than 100, or even less than 10, or indeed even less than 1, and preferably also as close as possible to 0, in order to limit the attenuation of the optical signal intended to pass through said layer 50. This means that the physicochemical and mechanical properties of the intermediate layer 50 are selected to ensure a low attenuation coefficient.
[0026] It will be recalled that the refractive index of a material can be considered to be a complex number (n+ik), having a real part n (the aforementioned refractive index) and an imaginary part k (the extinction coefficient).
[0027] The intermediate layer 50 of the structure 150 is further composed of a material different from the materials of the first and second layers 10, 40, in particular because this layer serves an additional role, namely, to promote bonding between the first layer 10 and the second layer 40.
[0028] For example, when the refractive index of the first layer 10 is equal to 3, the refractive index of the second layer 40 is between [3+0.3=3.30] and [3-0.3=2.70], as is the refractive index of the intermediate layer 50. The extinction coefficient of the intermediate layer 50 is less than 100, less than 10, or less than 1 for the portion of the intermediate layer 50.
[0029] Thus, the intermediate layer 50 of the semiconductor structure 150 does not or only little interfere with the optical signal when it has to pass through said intermediate layer 50. Moreover, the intermediate layer 50 promotes a direct bond between the first layer 10 and the second layer 40, thereby simplifying the surface preparation step carried out before the first layer 10 and the second layer 40 are bonded, the material of the intermediate layer 50 being selected in particular to facilitate the preparation of the surface preparation step, said material further allowing the arrangement of atoms at low temperatures favorable for bond formation while limiting the stress between the layers 10 and 40. It is also noted that the lower the attenuation coefficient (i.e. the closer it is to 0), the greater the freedom in the choice of the thickness of the intermediate layer 50; in other words, with a very low attenuation coefficient, a thicker intermediate layer 50 can be employed, which may prove to be an advantageous way of enhancing the quality of the direct bond.
[0030] In the semiconductor structure 150, the interface roughness between the various layers 10, 50, 40, or sublayers is preferably kept below about 5 nm RMS (measured by Atomic Force Microscope (AFM) in a 10 micron x 10 micron scan) to limit scattering of the optical signal at said interfaces.
[0031] Preferably, the material of the intermediate layer 50 is amorphous so as to limit the stress fields associated with the joining of two materials whose crystal lattices are misaligned and / or whose lattice parameters differ, and to avoid the formation of nanobubbles at the joining interface.
[0032] According to a first embodiment of the present invention, the semiconductor structure 150 is intended to accommodate a VCSEL in a configuration in which the laser signal is emitted through the back surface 150b.
[0033] The material of the first layer 10 is a high-quality single crystal intended to form a seed for the epitaxial growth of a stack of layers comprising an active region 2 sandwiched between two Bragg mirrors 3a, 3b. The second layer 40 is a carrier substrate 40 with high optical transparency (potentially better than that of the first layer 10), typically higher than 30%. Preferably, for essentially economic reasons, the carrier substrate 40 has a lower crystalline quality than the first layer 10 (FIG. 3).
[0034] Typically, the semiconductor of the first layer 10 is gallium arsenide (GaAs) with a crystalline quality that allows for defect-free growth, typically tailored for the intended application, and with a density of 500 / cm 2 n-type GaAs with a dislocation density of less than about 10 18 at / cm 3 The first layer 10 has a thickness of 50 to 1500 nm.
[0035] The semiconductor of the second layer 40 is gallium arsenide, which has a lower absorbance (good optical transparency) than the material of the first layer 10 in the working length of the target component. The second layer 40, which forms the carrier substrate 40 of the semiconductor structure 150, does not require high crystal quality, in that it essentially plays the role of a mechanical carrier. The thickness of the second layer 40 is, for example, 200 to 2000 microns. Considering the passage of the optical signal through the carrier substrate 40, which is required for the VCSEL to emit through the back surface 150b, the gallium arsenide of the carrier substrate 40 is further selected to be semi-insulating, in order to limit the absorption of the optical signal and thus increase the efficiency of the VCSEL.
[0036] For a wavelength of the optical signal of about 900 nm, the first layer 10 and the carrier substrate 40 have a refractive index equal to 3.52.
[0037] The material of the intermediate layer 50 is silicon (Si), in particular amorphous silicon. The thickness of the intermediate layer 50 can vary from 1 nm to 100 nm. For a wavelength of the optical signal of about 900 nm, the intermediate layer 50 has a refractive index equal to 3.6 and an extinction coefficient very close to 0.
[0038] The semiconductor structure 150 according to this first embodiment may be manufactured using known prior art processes for transferring layers by bonding and thinning, in particular the Smart Cut™ process, which is particularly suitable for transferring very thin layers.
[0039] The first step a) consists of providing a donor substrate 11 from which the first layer 10 is to be derived (FIG. 4a). The donor substrate 11 may consist of a bulk GaAs substrate having the qualities and properties expected of the first layer 10. Alternatively, the donor substrate 11 may comprise an initial substrate 11a and one or more high-quality surface layers 11b formed, for example by epitaxy, on the initial substrate 11a, from which the first layer 10 is then to be derived.
[0040] A second step b) consists of providing a carrier substrate 40 intended for forming the second layer 40 of the semiconductor structure 150 (FIG. 4b). The quality and characteristics of the GaAs carrier substrate 40 are, as mentioned above, tailored to the intended application.
[0041] Then, in a third step c), a bonding layer 5 made of amorphous Si is deposited on the donor substrate 11 and / or on the carrier substrate 40 (FIG. 4c) and, after the two substrates 11, 40 are bonded, this (or these) bonding layer 5 will be embedded in the structure to form the intermediate layer 50. The Si bonding layer 5 can be formed using known techniques employing chemical vapor deposition (CVD) (such as, for example, plasma-enhanced chemical vapor deposition (PECVD)) or epitaxy or even physical vapor deposition (PVD). The deposition is typically carried out at temperatures between 200° C. and 700° C. A typical thickness of the bonding layer 5 is between 1 nm and 20 nm.
[0042] The fourth step d) consists in introducing light ions into the donor substrate 11 so as to form a buried weakened plane 12, visually representing the layer to be transferred, i.e. the first layer 10, against the front surface of the donor substrate 11 (FIG. 4d). Typically, with a GaAs donor substrate, helium or hydrogen or both ions are introduced at 1000 nm to the donor substrate 11, so as to form a buried weakened plane 12, visually representing the layer to be transferred, i.e. the first layer 10 (FIG. 4d). E +16at / cm 2 ~5 E +17at / cm 2 Ion implantation at a dose of 0.1 μm and an energy of about 100 keV allows the formation of a buried weakened plane 12 which makes it possible to transfer a first layer 10 with a thickness of 500 nm (700 nm, respectively) in the case of implantation of helium ions (hydrogen ions, respectively). It is noted that surface preparation and cleaning can be performed before and / or after implantation to remove potential organic or metallic particle contamination.
[0043] The fifth step e) consists in bonding the donor substrate 11 to the carrier substrate 40 so as to form a bonded assembly along the bonding interface 51 (Figure 4e). This bonding step consists in bringing the two substrates 11, 40 into intimate contact via the front side of the substrate 11, 40 provided with one or more bonding layers 5. As mentioned above, room temperature direct bonding, or alternatively direct bonding under ambient and controlled temperature (ADB or SAB) may be adopted. Of course, a surface cleaning or activation (for example using plasma) carried out before the sides to be bonded come into contact may be provided. These surface preparations are easier than those involving III-V materials, since the cleaning and / or activation required prior to the bonding of silicon require conventional steps and equipment that are more well understood in the semiconductor industry.
[0044] As an example, ADB may be performed under ultra-high vacuum after a bonding layer 5 made of amorphous silicon is deposited on the substrates 11 and 40 .
[0045] The bonded assembly may suitably be subjected to a heat treatment to strengthen the bond interface 51, typically at a temperature between 150° C. and 600° C. for a period of a few minutes to a few hours.
[0046] 4e shows a bonding interface 51 located within the intermediate layer 50, which may alternatively be located between the first layer 10 and the intermediate layer 50 if the bonding layer 5 is deposited only on the carrier substrate 40, or between the carrier substrate 40 and the intermediate layer 50 if the bonding layer 5 is deposited only on the donor substrate 11. Even if the bonding layer 5 is deposited only on one of the donor and carrier substrates 11, 40, direct bonding is facilitated.
[0047] The sixth step f) involves separation along the embedded weakened plane 12, which results from the presence and / or growth of cavities and microcracks in said plane (FIG. 4f). As known per se, such separation occurs, for example, during a heat treatment designed to develop cavities, to place under pressure and to bring about the spontaneous propagation of splitting waves through the embedded weakened plane 12. The separation heat treatment typically corresponds to an annealing at 200° C. for 120 minutes. Instead of or in conjunction with the heat treatment, separation may also be induced by a mechanical stress applied to the embedded weakened plane 12.
[0048] At the end of step f), the following is obtained: on the one hand, a semiconductor structure 150 having a first layer 10 arranged on an intermediate layer 50, which intermediate layer 50 is itself arranged on a carrier substrate 40 (or on a second layer 40), and on the other hand, the remaining part 11' of the donor substrate.
[0049] Step f) may then comprise a surface treatment (cleaning, polishing, etching) or other smoothing treatment with the aim of improving the surface quality of the first layer 10 .
[0050] The structure 150 according to the invention is advantageous with respect to structures in which the first layer 10 and the second layer 40 are directly bonded without an intermediate layer, since it greatly facilitates the step of preparing the surface before the first layer 10 and the second layer 40 are bonded, ensuring an excellent bonding quality, and furthermore eliminating the risk of dislocations forming between the crystals of the first layer 10 and the second layer 40. It will be recalled that bonding defects such as nanobubbles and crystal defects (such as dislocations) can disrupt optical signals passing through the bonding interface 51, which is potentially detrimental for certain optoelectronic components that may be manufactured on the semiconductor structure 150.
[0051] Successive epitaxial growth steps g) aimed at manufacturing one or more optoelectronic components, in this case one or more VCSELs, can then be applied to the semiconductor substrate 150, the first layer 10 being used as an epitaxial seed (FIG. 4g). These steps, known in the prior art, lead in particular to the formation of the active region 2 of a VCSEL, this region being sandwiched between two Bragg mirrors 3a, 3b based on gallium arsenide.
[0052] According to one variant of the first embodiment of the semiconductor structure 150, the first layer 10 forms all or part of a VCSEL and the second layer 40 is a carrier substrate 40 of high optical transparency at the nominal operating wavelength of the optical component and optionally of low crystalline quality. Thus, in this variant, the first layer 10 comprises a number of sublayers.
[0053] In step a), a donor substrate 11 is provided with an active layer 2 and two Bragg mirrors, for example as shown in Figure 5a, or some of this stack. Thus, all or part of the VCSEL is transferred as a first layer 10 at the end of step f) (Figure 5f).
[0054] In the first embodiment and its variations, the fact that the intermediate layer 50 has a very low attenuation coefficient (close to zero) and a refractive index close to the refractive index of the first layer 10 (or the refractive index of a sublayer of the first layer 10 adjacent to the intermediate layer 50) and the carrier substrate 40 allows the laser signal of the VCSEL to be emitted through the back surface 150b of the semiconductor structure 150 without obstruction and attenuation of the signal as a result of passing through the intermediate layer 50 and the carrier substrate 40.
[0055] Of course, the semiconductor structure 150 according to this first embodiment is also suitable for other types of optoelectronic components that transmit or receive optical signals, whether the optical signals are transmitted or received through the front surface 150a or through the back surface 150b.
[0056] According to a second embodiment of the invention, the semiconductor structure 150 is again intended to correspond to a VCSEL. However, this time the first layer 10 forms the active region 2 of the VCSEL and the second layer 40 forms the multi-layer Bragg mirror 3a (FIG. 6a).
[0057] Typically, the semiconductor of the first layer 10 has a dopant density of 5000 / cm 2 The first layer 10 comprises at least one layer of indium phosphide (InP) having a dislocation density of less than 10 nm. The thickness of the first layer 10 is between 10 and 1500 nm. For a wavelength of an optical signal of about 1.55 microns, the first layer 10 has a refractive index equal to 3.1.
[0058] The second layer 40 is formed of a number of stacked sublayers having compositions such as (the reader is particularly referred to the paper by A. Syrbu cited in the introduction) that include gallium arsenide, are doped and form a Bragg mirror for optical signals of a wavelength of 1.55 microns. The sublayers are formed, for example, of GaAs (refractive index of about 3.37 at the wavelength of interest), aluminum arsenide (AlAs) (refractive index of about 2.89), and ternary AlGaAs compounds. The thickness of the second layer 40 is between 1 and 6 μm.
[0059] The material of the intermediate layer 50 is zinc germanium phosphide (ZnGeP2) or boron carbide (B4C) or zinc silicon arsenide (ZnSiAs2). For a wavelength of an optical signal of about 1.55 microns, an intermediate layer 50 made of ZnGeP2, B4C or ZnSiAs2 has a refractive index equal to 3.17, 3.25 or 3.26, respectively, and an extinction coefficient less than 10.
[0060] The thickness of the intermediate layer 50 can vary from 1 nm to 100 nm.
[0061] The sublayer of the second layer 40 having the refractive index closest to that of the first layer 10 (i.e., the difference in refractive index is less than 0.3) is selected to be positioned closest to the first layer 10, i.e., adjacent to the intermediate layer 50.
[0062] In the second embodiment, the semiconductor structure 150 preferably comprises a carrier substrate 41 arranged under the second layer 40 (FIG. 6b). The carrier substrate 41 does not need to have high crystal quality, in that it essentially plays the role of a mechanical carrier. The carrier substrate 41 may be formed from InP or GaAs. The thickness of the carrier substrate 41 is, for example, 250 to 1000 microns depending on the diameter of the carrier substrate 41. If the carrier substrate 41 has to be passed by an optical signal, for example if the VCSEL has to emit through the back surface 150b, the carrier substrate 41 is selected to have an optical extinction k (or attenuation coefficient) as low as possible and ideally equal to 0, in order to limit the absorption of the optical signal and thus promote the efficiency of the VCSEL.
[0063] A second intermediate layer 52 of the same nature as the intermediate layer 50 may be inserted between the carrier substrate 41 and the second layer 40; this option is particularly advantageous since the second intermediate layer 52 limits the disturbance and attenuation of the optical signal when it has to pass through the carrier substrate 41. The second bonding interface 51' is located within or adjacent to the second intermediate layer 52.
[0064] The semiconductor structure 150 according to this second embodiment may be manufactured using known prior art processes for transferring layers by bonding and thinning, in particular the Smart Cut™ process detailed with reference to the first embodiment.
[0065] Similar steps as those described above are performed and potentially repeated for the second bond interface 51'.
[0066] In this second embodiment, the successive epitaxial growth step g) aimed at producing one or more VCSELs consists of forming a second Bragg mirror 3b on the first layer 10 (consisting of the active region 2 of the VCSEL). Alternatively, the epitaxial growth step is replaced by the transfer of the layer forming the second Bragg mirror 3b via a third intermediate layer 53 of the same nature as the intermediate layer 50 (FIG. 6c). A third bonding interface 51″ is located in or adjacent to the third intermediate layer 53.
[0067] The semiconductor structure 150 according to the second embodiment makes it possible to produce a VCSEL emitting at a wavelength of about 1.55 μm, while simplifying the production of the Bragg mirrors 3 a, 3 b, which typically require a large number of successive epitaxial InP layers. The transfer of the GaAs Bragg mirror (which requires a smaller stack of layers) to the InP active region via an intermediate layer 50, which has a low attenuation coefficient and a refractive index that differs from that of the active region 2 (first layer 10) by less than 0.3, makes it possible to efficiently manufacture the VCSEL.
[0068] More generally, the semiconductor structure 150 according to this second embodiment is compatible with VCSELs emitting through the front surface 150a or the back surface 150b, since it uses a second intermediate layer 52 or even a third intermediate layer 53 having a refractive index that differs from the refractive index of the first layer 10 (or active region 2) by less than 0.3 and has a low extinction coefficient.
[0069] Of course, the invention is not limited to the described embodiments, and variants of the embodiments can be implemented without departing from the scope of the invention as defined by the claims.
[0070] In particular, the semiconductor structure 150 according to the present invention may be tailored for other optoelectronic applications, such as, for example, photodetectors.
Claims
1. A semiconductor structure (150) for optoelectronic applications, comprising: a first layer (10) made of a crystalline semiconductor; an intermediate layer (50) including or adjacent to the direct bond interface; a second layer (40) made of a crystalline semiconductor; Equipped with the first layer is disposed on the intermediate layer (50), and the intermediate layer is disposed on the second layer (40); The semiconductor structure (150), wherein the intermediate layer (50) is made of a material different from the materials of the first and second layers (10, 40), and the intermediate layer (50) has an attenuation coefficient of less than 100; the refractive index of at least one sublayer of the first layer (10) adjacent to the intermediate layer (50); and The refractive index of at least one sublayer of the second layer (40) adjacent to the intermediate layer (50). and characterized by having a refractive index difference of less than 0.3; the semiconductor of the first layer (10) is gallium arsenide, the semiconductor of the second layer (40) is gallium arsenide, and the material of the intermediate layer (50) is silicon; A semiconductor structure (150).
2. The semiconductor structure (150) of claim 1, wherein said material of said intermediate layer (50) is amorphous.
3. The semiconductor structure (150) of claim 1 or 2, wherein said material of said first layer (10) is monocrystalline with high crystalline quality so as to form a seed for epitaxy.
4. The semiconductor structure (150) of claim 1 or 2, wherein said first layer (10) forms all or part of a vertical cavity surface emitting laser (VCSEL).
5. 10. The semiconductor structure (150) according to one of the preceding two claims, wherein said second layer (40) is a carrier substrate having an optical transparency higher than 30%.
6. The semiconductor structure (150) of any one of claims 1 to 5, wherein the attenuation coefficient of the intermediate layer (50) is less than 1.
Citation Information
Patent Citations
Surface emitting semiconductor laser element and its manufacturing method
JP2004207536A