Hybrid development of EUV resist

The hybrid development process for EUV photoresists addresses pattern collapse and residue issues by combining wet and dry techniques, achieving precise critical dimensions and reducing EUV radiation dose, thus improving lithographic performance and throughput.

JP2024535798APending Publication Date: 2024-10-02TOKYO ELECTRON LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024515825
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-15
Filing Date
2022-08-25
Publication Date
2024-10-02

AI Technical Summary

Technical Problem

EUV photoresists face challenges in achieving precise critical dimensions due to pattern collapse and residue issues during conventional single development processes, particularly at dimensions below 30 nm, which are exacerbated by capillary forces in wet development and scum generation in dry development.

Method used

A hybrid development process involving a multi-step approach, combining wet and dry development techniques, including a less aggressive initial development followed by a more intensive dry process, with optional thermal or UV treatments to enhance resist structure and control, using apparatuses with integrated chambers for sequential processing.

Benefits of technology

The hybrid method effectively prevents pattern collapse and reduces residue, improving lithographic performance by achieving precise critical dimensions and reducing the EUV radiation dose required, thereby enhancing throughput and reducing defects in EUV photoresist patterns.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024535798000001_ABST
    Figure 2024535798000001_ABST
Patent Text Reader

Abstract

A method of microfabrication includes depositing a photoresist film on a working surface of a semiconductor wafer, the photoresist film being sensitive to extreme ultraviolet light, exposing the photoresist film to a pattern of extreme ultraviolet light, and performing hybrid development of the photoresist film, the hybrid development including performing a first development process to remove a first portion of the photoresist film, stopping development of the photoresist film after the first development process, where after stopping, the photoresist film includes a structure having a first critical dimension that is larger than a target critical dimension, and after stopping development, performing a second development process to remove a second portion of the photoresist film and reduce the critical dimension of the structure from the first critical dimension to a second critical dimension that is smaller than the first critical dimension.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of U.S. Provisional Patent Application No. 63 / 244,309, filed September 15, 2021, which is incorporated herein by reference.

[0002] The present invention relates generally to systems and methods for developing extreme ultraviolet (EUV) photoresist patterns, and in particular embodiments to systems and methods for hybrid development of EUV photoresists. [Background technology]

[0003] Semiconductor manufacturing involves several processing steps that involve forming a pattern on a semiconductor substrate, including, among other things, coating a photoresist onto a dielectric or conductive surface of the substrate, developing the latent pattern, and transferring the pattern to the dielectric or conductive surface of the substrate by etching.

[0004] In a microfabrication process, a layer of photoresist is coated on the working surface (top surface) of a substrate, such as a semiconductor wafer. The photoresist is then patterned by photolithography to define a mask pattern, which is transferred to an underlying layer by etching using the patterned resist as an etch mask. Patterning the photoresist generally involves the steps of coating, exposing, and developing. The working surface of the substrate is coated with a film of photoresist. The photoresist is exposed through a lithographic mask (and associated optics), for example using microlithography. Exposure with the pattern is followed by a development process during which soluble areas of the photoresist are removed using either a wet (solvent) or dry (gaseous) development process. The soluble areas can be exposed or unexposed areas depending on the tone of the photoresist and the developer used.

[0005] Extreme ultraviolet (EUV) photolithography is a photolithography technique that uses photons in the extreme ultraviolet range (124 nm to 10 nm). Typically, a wavelength of 13.5 nm is used. EUV photoresists are generally metal-containing resists. Summary of the Invention [Means for solving the problem]

[0006] In one embodiment, a method of microfabrication includes depositing a photoresist film on a working surface of a semiconductor wafer, the photoresist film being sensitive to extreme ultraviolet light, exposing the photoresist film to a pattern of extreme ultraviolet light, and performing hybrid development of the photoresist film, the hybrid development including performing a first development process to remove a first portion of the photoresist film, stopping development of the photoresist film after the first development process, where after the stopping, the photoresist film includes a structure having a first critical dimension that is larger than a target critical dimension, and after the stopping of development, performing a second development process to remove a second portion of the photoresist film and reduce the critical dimension of the structure from the first critical dimension to a second critical dimension that is smaller than the first critical dimension.

[0007] In one embodiment, a method of micro-fabrication includes depositing a photoresist film on a working surface of a semiconductor wafer, the photoresist film being sensitive to extreme ultraviolet radiation; exposing the photoresist film to a pattern of extreme ultraviolet radiation to form an EUV photoresist pattern; performing a wet development process to remove a first portion of the EUV photoresist pattern to obtain a structure having a first critical dimension that is larger than the target critical dimension; and, after performing the wet development process, performing a dry development process to remove a second portion of the EUV photoresist pattern to obtain a structure having the target critical dimension.

[0008] In one embodiment, a semiconductor manufacturing apparatus includes a first developer chamber and a second developer chamber, the apparatus configured to sequentially process a substrate in the first developer chamber and the second developer chamber.

[0009] For a more complete understanding of the present invention, and the advantages thereof, reference is now made to the following descriptions taken in conjunction with the accompanying drawings, in which: [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a block diagram of a semiconductor device for forming an EUV photoresist pattern, according to an embodiment. [Figure 2A] 1A-1D are 3D isometric views of process steps for forming an EUV photoresist pattern, according to an embodiment. [Figure 2B] 1A-1D are 3D isometric views of process steps for forming an EUV photoresist pattern, according to an embodiment. [Figure 2C] 1A-1D are 3D isometric views of process steps for forming an EUV photoresist pattern, according to an embodiment. [Figure 2D] 1A-1D are 3D isometric views of process steps for forming an EUV photoresist pattern, according to an embodiment. [Figure 2E] 1A-1D are 3D isometric views of process steps for forming an EUV photoresist pattern, according to an embodiment. [Figure 2F] 1A-1D are 3D isometric views of process steps for forming an EUV photoresist pattern, according to an embodiment. [Figure 3A] 1A-1D are plan views of process steps for forming an EUV photoresist pattern, according to an embodiment. [Figure 3B] 1A-1D are plan views of process steps for forming an EUV photoresist pattern, according to an embodiment. [Figure 3C] 1A-1D are plan views of process steps for forming an EUV photoresist pattern, according to an embodiment. [Figure 3D] 1A-1D are plan views of process steps for forming an EUV photoresist pattern, according to an embodiment. [Figure 3E] 1A-1D are plan views of process steps for forming an EUV photoresist pattern, according to an embodiment. [Figure 3F] 1A-1D are plan views of process steps for forming an EUV photoresist pattern, according to an embodiment. [Figure 4] FIG. 1 is a flow diagram illustrating formation of an EUV photoresist pattern using hybrid development, according to an embodiment. [Diagram 5] FIG. 1 is a flow diagram illustrating formation of an EUV photoresist pattern using hybrid development, according to an embodiment. [Figure 6] FIG. 1 is a flow diagram illustrating a method for reducing the dose of EUV radiation required to expose a pattern in an EUV photoresist, according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Although the present invention has been described with reference to exemplary embodiments, this specification is not intended to be construed in a limiting sense. Various modifications and combinations of those exemplary embodiments, as well as other embodiments of the present invention, will become apparent to those skilled in the art upon reference to this specification. Therefore, it is intended that the appended claims cover any such modifications or embodiments.

[0012] EUV radiation and EUV photoresists behave differently than traditionally used deep ultraviolet (DUV) radiation and DUV photoresists. Therefore, different techniques are used in EUV photolithography. EUV photoresists are typically metal-containing resists instead of DUV carbon-containing photoresists, and are less transparent to the exposure radiation. EUV resists are typically thinner (20 nm to 40 nm) than DUV resists (2000 nm to 4000 nm), making it more difficult to fully expose the photoresist layer and more difficult to develop, especially at critical dimensions below 30 nm.

[0013] EUV photoresists can be wet photoresists (wet deposited) or dry photoresists (dry deposited). Wet photoresists are typically deposited by spin-on deposition techniques, i.e., the wafer is rapidly spun and liquid resist is deposited onto the rotating wafer, causing the photoresist to spread and coat the surface of the wafer. Dry photoresists are deposited in gaseous or molecular form by any number of dry deposition techniques, including chemical vapor deposition, molecular layer deposition, physical vapor deposition, sputter deposition, etc.

[0014] EUV resist can be wet developed using a solvent or dry developed using a gas. Conventional EUV photoresist development processes use a single wet development (or a single dry development) process to resolve the exposed latent image in the EUV photoresist.

[0015] Wet development processes inherently suffer from capillary forces caused by the surface tension of the liquid, which can lead to pattern distortion, pattern collapse, and other defects, especially at critical dimensions below 30 nm.

[0016] Gas phase chemical etch development, referred to as dry development, does not suffer from such capillary forces. This provides some advantages in patterning in terms of reducing pattern collapse and increasing process tunability. Unfortunately, dry development processes suffer from scumming and residue that may remain after the dry development process, especially in areas with lower EUV exposure, e.g., near the bottom of the EUV photoresist layer. Attempts to solve this residue problem include attempts to mitigate the residue using sputtering and other processes. Dry development can be performed with or without plasma assistance.

[0017] Disclosed embodiments include a multi-step hybrid development process for developing EUV photoresist. The hybrid development process can include a wet development process followed by one or more dry development processes, or a first, less aggressive dry development process followed by a second, more aggressive dry development process. Typically, a mild first development step is followed by a more aggressive development step. Intermediate thermal or UV treatments can be used to strengthen the photoresist structure and change the development rate before the next development step.

[0018] This multi-step hybrid development method can be applied to wet- or dry-deposited photoresist. In wet-developed EUV photoresist embodiments, the hybrid development process prevents pattern collapse. In dry-developed EUV photoresist embodiments, the hybrid development process reduces scumming / residue. The result is improved lithographic performance of features printed with EUV photoresist patterns.

[0019] An apparatus for forming an EUV pattern on a semiconductor substrate according to an embodiment will be described using Figure 1. Where appropriate, a process flow will be described using Figure 4 in conjunction with Figures 2A-2F and 3A-3F.

[0020] FIG. 1 is a block diagram of a semiconductor device for patterning EUV photoresist using a hybrid development procedure, according to an embodiment.

[0021] Embodiments of the present disclosure are enabled by the apparatus described herein that allows for hybrid development within a common tool or tool platform.

[0022] The hybrid developer 130 includes a hybrid dry developer tool 131 that enables an embodiment of a dry / dry hybrid development process to be performed. The hybrid developer 130 may also include additional manufacturing tools, such as a wet developer track 148, that enable a wet / dry hybrid development process.

[0023] 1 includes a load lock 140 for transferring a substrate / wafer from outside the hybrid dry develop tool 131 to inside the transfer chamber 132. The transfer chamber 132 is fitted with a dry develop chamber 152 capable of dry developing the exposed EUV photoresist at less aggressive development conditions and a second dry develop chamber 154 capable of developing the EUV photoresist pattern at more aggressive process conditions. The exemplary hybrid dry develop tool 131 also includes an optional bake chamber 156 for optionally baking the substrate after development, and an optional UV exposure chamber 158 for optionally blanket exposing the substrate to UV radiation prior to the dry develop process.

[0024] 1, in various embodiments, the hybrid dry developer 120 may additionally include a wet development track 148 that enables implementation of the hybrid wet / dry development procedure of the embodiments. The hybrid developer 130 may also include other processing tools related to EUV processing, such as a photoresist coat track 144 for depositing photoresist on a substrate, an EUV scanner 146 for exposing the photoresist to EUV radiation through a photolithography mask, and a critical dimension measurement tool 150, such as a scanning electron microscope (SEM) or a transmission electron microscope (TEM). A wafer / substrate transport system 145, such as a robotic system, may transfer wafers / substrates between the various processing tools in the hybrid developer 130 and transport them to / from the hybrid dry developer tool 131.

[0025] An embodiment dry / dry hybrid development process can be performed in the dry development tool 131. An embodiment hybrid dry / dry development process can be performed by first partially developing the EUV pattern in one of the dry development chambers 152 or 154 using a less aggressive dry development process, stopping the development, and then performing a second development step in the same chamber using a second, more aggressive development process. Alternatively, a first, less aggressive dry development process can be performed in the dry development chamber 152 and a second, more aggressive dry development process can be performed in the dry development chamber 154. In one or more embodiments, the dry development tool 131 is configured to process substrates sequentially in the dry development chamber 152 and then in the dry development chamber 154, for example, without the need to pass through a load lock.

[0026] The wet / dry hybrid development procedure of the embodiments can be performed in the hybrid developer 130 by performing a wet development step on the wet developer track 148 and then transferring the substrate / wafer to the hybrid dry developer tool 131. The dry development portion of the hybrid wet / dry development procedure of the embodiments can be performed in the dry developer chambers 152 or 154. The dry development process can be a chemical vapor development process or a plasma etch development process. If desired, the CD can be measured in the CD measurement tool 150 after the wet development and before the dry development. In one or more embodiments, the hybrid developer 130 is configured to process the substrate sequentially in the wet developer track 148 followed by the dry developer chambers 152 or 154.

[0027] An advanced process control system 160 (APC) may be coupled to some or all of the chambers and fabrication tools in the hybrid developing apparatus 130. The APC system 160 may include computers and servers that collect large amounts of data 162 from the processing chambers and fabrication tools, analyze the data, compare the analysis results to specifications, and send instructions 164 to microprocessors in the processing chambers and fabrication tools to adjust the process recipes to produce structures with the target specifications. For example, a critical dimension (CD) measurement tool 150 can measure the CD of the structures in the EUV photoresist pattern after a first development process and send data 162 to the APC system 160. The APC system 160 can then calculate the difference between the target CD specification and the measured CD and send instructions 164 to a microprocessor in the dry developing chamber 152 to adjust the dry developing recipe to produce structures with the target CD after a dry developing process.

[0028] 4 is a flow diagram illustrating the formation of an EUV photoresist pattern using hybrid development, according to an embodiment. Figures 2A-2F show three-dimensional isometric views, while Figures 3A-3F show top views of the EUV photoresist pattern at various stages of a hybrid development procedure.

[0029] 2A and 3A, and with reference to block 100 of FIG. 4, an EUV photoresist 124 is deposited on a hard mask material 122 overlying a semiconductor substrate 120 in a photoresist coat track 144 of FIG.

[0030] Substrate 120 contains the layer to be etched and, in various embodiments, may include device regions formed in the layer. The substrate may be a semiconductor wafer, such as a silicon wafer or a gallium arsenide wafer, a chrome or other layer on a lithographic reticle, or a layer such as silicon dioxide, silicon nitride, titanium, titanium nitride, or copper overlying a base substrate structure.

[0031] In general, as used herein, "substrate" refers generally to an object being processed. The substrate may include any material portion of a device, particularly a semiconductor device or other electronic device structure, such as a base substrate structure, such as a semiconductor wafer, a lithographic reticle, or a layer on or overlying the base substrate structure, such as a thin film. Thus, the substrate is not limited to any particular base structure, underlying layer, or overlying layer, whether patterned or not, but is intended to include such layers or base structures, as well as any combination of layers and / or base structures. Although particular types of substrates may be referred to herein, this is for illustrative purposes only.

[0032] The hard mask material 122 may be a dielectric material such as silicon dioxide, silicon nitride, or aluminum oxide, or may be a conductive material such as titanium nitride or tantalum nitride. The hard mask material 122 is selected to have high etch selectivity with respect to the wet and dry development chemistries and with respect to the substrate 120 being etched. The substrate may be a dielectric material such as silicon dioxide, silicon nitride, a semiconductor material such as undoped single crystal silicon, or a conductive material such as titanium, titanium nitride, aluminum, copper, or doped single crystal silicon.

[0033] The EUV photoresist 124 can be an organometallic EUV resist. The organometallic EUV resist 124 includes a metal oxide core surrounded by organic alkyl groups covalently bonded to the metal oxide core. The metal oxide core can be, for example, tin oxide, hafnium oxide, zinc oxide, and zirconium oxide. The metal atoms in the metal oxide core absorb EUV radiation more strongly than the carbon and oxygen atoms in the organic polymer resist. The metal atoms make the organometallic EUV resist more sensitive to EUV radiation.

[0034] In block 102 of Figure 4, a pattern is exposed in the EUV photoresist layer 124 using EUV radiation transmitted through a lithographic reticle, as shown in Figures 2B and 3B. The EUV exposure may be performed in an EUV scanner 146 shown in Figure 1.

[0035] The EUV photoresist pattern comprises exposed regions 126 and unexposed regions 124. For purposes of illustration, a positive EUV photoresist is used, where exposure to EUV radiation renders the EUV photoresist 124 insoluble to form exposed regions 126. To form minimum width features in the semiconductor substrate 120, the EUV photoresist 124 is exposed to a dose of EUV radiation necessary to expose a minimum width line having a target critical dimension 125.

[0036] After a pattern is formed in the EUV photoresist 124, a post-exposure bake (PEB) may be performed in bake chamber 156 of Figure 1. The PEB is typically a 1-3 minute bake in air or nitrogen at a temperature between 50°C and 250°C. The EUV post-exposure bake conditions are selected to promote a degree of crosslinking in the exposed EUV photoresist 126 to improve structural strength, improve contrast, and reduce line edge roughness (LER).

[0037] 2C and 3C show the semiconductor device under construction after a first development process, with FIG. 2C showing a three-dimensional isometric view while FIG. 3C shows a plan view.

[0038] Referring to block 104 of FIG. 4 in conjunction with FIGS. 2C and 3C, a first development step in a hybrid development sequence is performed according to various embodiments. The hybrid development sequence includes two or more development processes. The first development process is a less aggressive development process that removes a first portion of the unexposed EUV photoresist 124. The first development step forms a structure, e.g., a line, having a critical dimension 127 larger than the target critical dimension 125. A subsequent more aggressive dry development process in the hybrid development sequence further shrinks the line laterally. Some height of the EUV photoresist may be removed, but the primary removal is lateral because the EUV exposure is concentrated over the entire line.

[0039] The first development step can be performed by wet development, by dry chemical vapor development, or by dry plasma development. Dry development can be performed in a separate dry development tool 131 or in a track module. Thus, the hybrid development apparatus 130 can include a wet development track 148 and dry development chambers 152 and 154.

[0040] The wet development process uses a solvent in which the unexposed EUV photoresist 124 is soluble. The wet development process can be performed on the wet development track 148 of FIG.

[0041] Alternatively, the first development process may be a dry development process having less aggressive development conditions that partially develops the EUV photoresist pattern leaving minimum width features with CDs larger than the target critical dimension. The dry development process may be performed in the dry development chamber 152 of FIG.

[0042] The wet development solvent may include organic solvents, water, acids or bases, or combinations thereof. The wet development solvent may include aromatics (e.g., xylene, toluene), ethers (e.g., anisole, tetrahydrofuran), esters (e.g., propylene glycol monomethyl ether acetate, or PGMEA), alcohols (e.g., isopropanol, 4-methyl 3-propanol, ketones, 2-heptaone, water, n-butyl acetate, acetic acid, or methyl isobutyl carbinol (MIBC). The acetic acid concentration in water or PGMEA may range from 0% to 10% for most hybrid wet development applications.

[0043] The dry development process may be either a chemical vapor etch development process or a plasma etch development process. The chemical vapor etch development process is typically carried out in a chamber having a showerhead above the substrate for distributing the vapor etch gas uniformly across the substrate. The chemical vapor etch chamber may also have a substrate chuck that rotates to additionally improve the uniformity of the development. The dry plasma etch development process is typically carried out in a plasma etch chamber having a showerhead above the substrate for distributing the etch gas uniformly across the substrate. An RF oscillator coupled to an antenna in the dry plasma etch development chamber generates and maintains the plasma. The plasma development chamber may also have a substrate chuck that rotates to additionally improve the uniformity of the vapor etch development. The substrate chuck may be biased with a voltage to add a sputter etch component to the plasma etch development process.

[0044] The dry chemical vapor development chemistry may depend on the composition of the corresponding EUV photoresist. Exemplary chemical vapor development chemistry may include a halide, hydrogen halide, hydrogen gas, halogen gas, organic halide, acyl halide, carbonyl halide, or thionyl halide, including mixtures thereof. More specific examples include hydrogen fluoride, hydrogen chloride, hydrogen bromide, or hydrogen iodide. In one example, the chemical vapor development gas is hydrogen bromide.

[0045] The dry plasma etch development chemistry may depend on the composition of the corresponding resist. Exemplary dry plasma etch development chemistry may include halides such as hydrogen halides, organic halides, acyl halides, carbonyl halides, or thionyl halides, hydrogen gas, nitrogen gas, or halogen gas, or may include mixtures of these gases. In an exemplary dry plasma etch development process, the etching gas may include hydrogen chloride, hydrogen bromide, argon, or helium. In one example plasma etch development process, the etching gas may include hydrogen bromide and argon.

[0046] As non-limiting examples, the first development step may be a wet development process using PGMEA, 5% acetic acid, a mixture of acetic acid and PGMEA, or MIBC, and the second development step may be a dry chemical vapor development step using HBr.

[0047] Referring to block 106 of Figure 4, an optional first post-development bake (PDB) may be performed in the bake chamber 126 of Figure 1. The PDB is a 1-3 minute bake in air or nitrogen at a temperature between 50°C and 250°C. The PDB bake conditions may be selected to promote a degree of cross-linking in the exposed EUV photoresist pattern 126 to alter development rate, improve structural strength, improve contrast, and reduce line edge roughness (LER).

[0048] 2D and 3D, one or more second dry development processes may be performed to complete full development of the EUV photoresist pattern. The dry development process may be performed in either the second dry development chamber 154 or the first dry development chamber 152, or both. The dry development process may additionally remove unexposed EUV photoresist 124. The width of the minimum width feature in the EUV photoresist pattern after the second dry etch development is smaller than the width after the first development process. The width of the minimum width feature after the second dry etch development may be equal to the critical dimension specification 125.

[0049] The steam etch chemistry for the second development process may be the same or different than that for the first steam etch development. The process conditions for the second steam etch development may be the same or different than that for the first steam etch development. For example, the second steam etch development process may have a different temperature, different chemical concentrations and flow rates, and different pressure than that in the first steam etch development process.

[0050] In block 110 of Figure 4, after the EUV photoresist pattern is fully developed, an optional second post-development bake or hard bake may be performed in the bake chamber 156 of Figure 1. The post-development bake is typically performed to increase the thermal and mechanical stability of the EUV photoresist pattern 166 to withstand the harsh conditions of subsequent processing steps. This hard bake may usually be omitted because the EUV photoresist pattern 166 is removed after the hard mask etch.

[0051] 2E and 3E are three-dimensional isometric and plan views of the semiconductor structure after the hardmask material 122 has been etched using the EUV photoresist pattern as an etch mask. In various embodiments, the hardmask material 122 is etched using an anisotropic plasma etch process that transfers the photoresist pattern into the hardmask layer to form the hardmask pattern 123.

[0052] 2F and 3F are three-dimensional isometric and plan views of mask pattern 123 after the EUV photoresist pattern has been removed. In an embodiment, the EUV photoresist pattern is removed by ashing in an oxygen plasma or a halide plasma.

[0053] FIG. 5 is a flow diagram illustrating the main steps of an embodiment of a wet / dry hybrid development method for forming a pattern in an EUV photoresist. The hybrid development method in this embodiment may use a first wet development process followed by a second dry development process. One advantage of these embodiments is that the critical dimension (CD) can be measured after wet development and CD feedback correction can be provided for each wafer during the dry development process. The CD measurement can be wafer-wide or location-dependent to monitor CD uniformity (CDU). The CD measurement can be performed in-line on the track or with an offline CD metrology tool.

[0054] The critical dimension data can be sent to the APC system 160 coupled to the dry development chamber 152 and other modules, and the critical dimension data can be used to adjust the dry development process recipe and other process recipes to produce the target critical dimensions and improve uniformity across the wafer. Modifications to the thermal treatment can be location (i.e., wafer zone temperature) dependent. Modified dry development process conditions can include process variables such as wafer temperature, flow rate, time, dilution, or parallel flow. CD monitoring can have environmental factors that change from day to day.

[0055] The methods herein can have two or more development steps and any number of bake steps. For example, the bake steps can include a first pre-develop post-exposure bake (PEB), a first post-develop bake (PDB1), and a second post-develop hard bake (PEB2). These bake steps are optional. These bake steps may be performed to improve structural stability, alter development rate, improve contrast, and reduce line edge roughness.

[0056] As can be appreciated, there are numerous alternative embodiments contemplated herein. The development or developer may be sensitive to the dose. In one embodiment, the second developer may have a higher development rate compared to the first developer. The higher development rate may be the result of using different developer chemistries or the same chemistries at different times / temperatures during processing.

[0057] In some embodiments, an optional blanket UV exposure of the EUV photoresist pattern can replace the first post-develop bake (PDB1). The optional UV exposure can aid in the second development by strengthening the exposed EUV photoresist and making it less susceptible to pattern collapse during the second development. The UV exposure can be a blanket exposure in various embodiments. In certain embodiments, the UV exposure can be location dependent in that certain coordinate locations on the wafer receive more UV treatment compared to other coordinate locations on the wafer. The UV exposure can enable the use of a stronger developer for the second development step.

[0058] To explain the blocks in the flow diagram of FIG. 5, the three-dimensional isometric views of the EUV photoresist patterns in FIGS. 2A-2F and the top views of the EUV photoresist patterns in FIGS. 3A-3F are used.

[0059] Figures 2A and 3A illustrate block 170 of Figure 5. In the photoresist coat module 114 of Figure 1, a DUV photoresist 124 is coated onto a hard mask material 122 overlying a semiconductor substrate 120.

[0060] In block 172 of FIG. 5, shown in FIGS. 2B and 3B, the EUV scanner 146 projects EUV radiation through a lithographic reticle to expose a pattern in the EUV photoresist layer 124.

[0061] In block 174 of Figure 5, shown in Figures 2C and 3C, a wet development step in a hybrid development sequence is performed according to an embodiment. The wet development process may be performed on the wet development track 148 of Figure 1. The wet development process may be a less aggressive development process that removes a first portion of the EUV photoresist 124 that is not exposed to light. After wet development, a minimum width feature in the EUV photoresist pattern may have a critical dimension 127 that is larger than the target critical dimension 125.

[0062] The wet development solvent may include an organic solvent, water, an acid, or a base. The wet development solvent may include an aromatic compound, an ether, an ester, an alcohol, a ketone, 2-heptaone, water, n-butyl acetate, propylene glycol methyl ether acetate (PGMEA), acetic acid, or methyl isobutyl carbinol (MIBC), or a combination thereof. In an exemplary wet development process, the solvent is a 5% acetic acid solution. In another exemplary wet development process, the solvent is PGMEA or MIBC.

[0063] In block 176 of FIG. 5, an optional wet post-develop bake (PDB) may be performed in the bake chamber 156 of FIG.

[0064] In block 178 of Figure 5, the critical dimension of the minimum width feature of the partially developed EUV photoresist pattern may be measured with CD metrology tool 150 of Figure 1. The measured critical dimension 127 after the wet development process is larger than the target critical dimension 125.

[0065] In block 180 of Figure 5, the critical dimension data 162 after wet development is optionally sent to a controller, such as the advanced process control (APC) system 160 shown in Figure 1. The APC system 160 can compare the critical dimension data after wet development to target critical dimension specifications. The APC system 160 can then send instructions 164 to a microprocessor in the dry development chamber 152 to adjust the dry development process recipe to form structures having the target critical dimensions after dry development.

[0066] In block 182 of FIG. 5, the EUV photoresist pattern 126 may be optionally exposed to blanket UV radiation in a UV exposure chamber 158. The blanket UV radiation additionally exposes the exposed EUV photoresist 126 and the unexposed EUV photoresist 124. Typically, when the EUV photoresist pattern is blanket exposed to UV radiation, no wet post-develop bake is performed. The blanket UV radiation may have a uniform intensity across the substrate 120, or may vary in intensity across the substrate 120 to improve post-develop uniformity. In various embodiments, the wavelength of the UV radiation during the optional blanket exposure is in the range of about 130 nm to 300 nm, such as 150 nm to 200 nm in one embodiment. The EUV photoresist 124 is transparent to longer wavelength UV radiation. The UV radiation exposes the EUV photoresist 124 uniformly from the top to the bottom. The blanket UV radiation additionally crosslinks the exposed EUV resist 126, increasing its strength and rendering it insoluble. The UV-induced crosslinking in the previously unexposed EUV resist 124 is insufficient to significantly affect development. An advantage of this embodiment is that the blanket UV exposure reduces the dose of EUV radiation required to pattern the EUV photoresist 124. This increases throughput through the EUV scanner.

[0067] In block 184 of FIG. 5, shown in FIG. 2D and FIG. 3D, one or more dry development processes using a hybrid development procedure of an embodiment are performed to complete the EUV photoresist pattern development. The dry development process can be performed in either dry development chamber 152 or 154. The dry development process additionally removes unexposed EUV photoresist 124. The width of the structures in the EUV photoresist pattern after the dry etch development process is smaller than the width of the same structures after the wet development process. The width of the minimum width structure after the dry etch development may be equal to the critical dimension specification 125. The APC controller of the APC system 160 can adjust the dry etch development recipe based on the fed back critical dimension data to ensure that the structure width meets the critical dimension specification 125 after the dry etch development.

[0068] The dry development process may be a chemical vapor etch development process, a plasma etch development process, or a sequence of chemical vapor etch development process and plasma etch development process. In an exemplary chemical vapor etch development process, the vapor etch gas is hydrogen bromide. In an exemplary plasma etch development process, the plasma development gas is hydrogen bromide and argon.

[0069] As previously mentioned, the hybrid development process can reduce the dose of EUV radiation required to form a target critical dimension (reducing EUV dose vs. size).

[0070] 6 is a block flow diagram illustrating the main steps of a method for reducing the required EUV radiation dose when using a hybrid development process according to embodiments. The hybrid development process may be wet / dry or dry / dry, according to embodiments. To illustrate these embodiments, a wet development / dry chemical vapor development hybrid process is used. An advantage of these embodiments is that the throughput of wafers passing through an EUV scanner can be increased and cycle time can be reduced.

[0071] In block 200 of FIG. 6, shown in FIGS. 2A and 3A, the wafer is coated with EUV photoresist 124.

[0072] In block 202 of Figure 6, a first dose of EUV radiation required to form a target critical dimension is determined. The EUV pattern is developed using a one-step wet development process. In an exemplary wet development process, the solvent is PGMEA with 5% acetic acid.

[0073] In block 204 , a series of wafers are coated with EUV photoresist 124 .

[0074] In block 206, the series of wafers are exposed in an EUV scanner through a lithographic mask with a series of doses of EUV radiation that decrease from a first dose of EUV radiation.

[0075] In block 208, the wafers are developed using a hybrid development procedure that includes a wet development process followed by a dry development process. For each EUV exposure dose, a design of experiments (DOE) can be performed where the variables are wet developer type and wet developer time, and dry developer type and dry developer time. The hybrid development conditions can be selected to produce structures that meet the critical dimension specifications after development. In one example, two wafers are exposed to equal doses of EUV radiation (73 mJ / cm2). 2 ) when the pattern is developed using a standard wet development process (acetic acid), the width of the features is 18.5 nm. When the pattern is developed using an embodiment hybrid wet / dry development process consisting of a reduced time standard wet development process and chemical vapor development using hydrogen bromide, the width of the same features is 14.5 nm. A target of 18.5 nm can be formed with an embodiment hybrid development process using a low dose of EUV radiation.

[0076] In block 210 of FIG. 6, a second EUV dose is selected with a corresponding hybrid development process. The second EUV dose is selected as an EUV dose (lower than the first EUV dose) that still produces an EUV pattern with a target CD and sufficient manufacturing window. In one example, the second EUV dose is lower than the first EUV dose by more than 15%. In another example, the second EUV dose is lower than the first EUV dose by about 20%. The lower second EUV dose reduces the cycle time through the bottleneck EUV scanner. This allows for significant cost savings by reducing the number of EUV steppers required.

[0077] It should be understood that the order of consideration of the different steps described herein is presented for clarity. In general, these steps can be performed in any suitable order. In addition, although each of the various features, techniques, configurations, etc. herein may be described in various places in this disclosure, it is intended that each of these concepts can be performed independently of each other or in combination with each other. Thus, the present invention can be embodied and viewed in many different ways.

[0078] As will be appreciated, there are many combinations of multi-step hybrid EUV photoresist development methods contemplated herein. In one embodiment, an EUV-sensitive photoresist is coated on a wafer, then exposed, then a post-exposure bake is performed, followed by a first development process, followed by an optional post-development bake, followed by a second development process with an optional final hard bake. In another embodiment, an EUV-sensitive photoresist is coated on a wafer, then exposed, then a post-exposure bake is performed, followed by a first development process, followed by an optional blanket UV exposure, followed by a second development process with an optional final hard bake.

[0079] The hybrid multi-step development process herein, with multiple development and / or bake steps, improves lithographic performance. This can include wet development or dry development, and combinations thereof. The use of a first wet development step before a second (or subsequent) dry development step removes resist in low dose areas where most of the residue forms, but does not fully resolve the critical features. This avoids pattern distortion or collapse and prevents other defects. At the same time, the dose vs. size required to print the desired features can be reduced through process modifications at each step. Subsequent dry development process steps further resolve the critical features while mitigating pattern collapse through the lack of capillary forces. The dry development process can be repeated until the desired (target) critical dimension (CD) is achieved. The hybrid multi-step development method disclosed herein provides a path to reduce the probability of pattern collapse and reduce scum generation / residue, while simultaneously providing control of CD stability.

[0080] In the above description, specific details have been described, such as the specific shape of the processing system and a description of various components and processes used therein. However, it will be understood that the technology herein may be practiced in other embodiments that deviate from these specific details, and such details are for illustrative purposes and are not limiting. The embodiments disclosed herein have been described with reference to the accompanying drawings. Similarly, for illustrative purposes, specific numbers, materials, and configurations have been described to provide a thorough understanding. However, the embodiments can be practiced without such specific details. Components having substantially the same functional structure are labeled with similar reference numerals, and therefore any redundant description may be omitted.

[0081] To facilitate understanding of various embodiments, various techniques have been described as multiple discrete operations. In additional embodiments, various additional operations may be performed and / or described operations may be omitted.

[0082] Exemplary embodiments of the present invention are summarized below: Other embodiments can be seen throughout the specification and claims filed herewith.

[0083] Example 1. A method of microfabrication includes depositing a photoresist film on a working surface of a semiconductor wafer, the photoresist film being sensitive to extreme ultraviolet light, exposing the photoresist film to a pattern of extreme ultraviolet light, and performing hybrid development of the photoresist film. The hybrid development includes performing a first development process to remove a first portion of the photoresist film, stopping development of the photoresist film after the first development process, where after stopping, the photoresist film includes a structure having a first critical dimension that is greater than a target critical dimension, and after stopping development, performing a second development process to remove a second portion of the photoresist film and reduce the critical dimension of the structure from the first critical dimension to a second critical dimension that is less than the first critical dimension.

[0084] Example 2. The method of example 1, wherein the second development process further comprises performing a dry development process to remove increasing amounts of the photoresist until the critical dimension of the structure is reduced to the target critical dimension.

[0085] Example 3. The method according to any one of Examples 1 or 2, wherein the first development process is a wet development process using a developer comprising propylene glycol monomethyl ether acetate, acetic acid, methyl isobutyl carbinol, 2-heptanone, or n-butyl acetate.

[0086] Example 4. The method of any one of Examples 1-3, wherein the developer comprises propylene glycol monomethyl ether acetate and acetic acid.

[0087] Example 5. The method of any one of Examples 1-4, further comprising: measuring a critical dimension value of the structure following the first development process; and performing a corrective treatment process during the second development process in response to identifying the measured critical dimension value being greater than a predetermined range.

[0088] Example 6. The method according to any one of Examples 1 to 5, further comprising: performing a first heat treatment after exposing the photoresist to a pattern of EUV; and performing a second heat treatment after the first development process and before the second development process.

[0089] Example 7. The method according to any one of Examples 1-6, wherein the bake time and bake temperature of the first heat treatment are different from the bake time and bake temperature of the second heat treatment.

[0090] Example 8. The method of any one of Examples 1-7, wherein the second development process comprises a chemical vapor etch development using a gas comprising hydrogen chloride, hydrogen bromide, argon, or helium.

[0091] Example 9. The method of any one of Examples 1-6, 8, wherein the second development process comprises a plasma etch development process using a gas comprising hydrogen chloride, hydrogen bromide, argon, or helium.

[0092] Example 10. The method of example 1, wherein the first development process is a first dry development process having a first dry development rate of the photoresist, and the second development process is a second dry development process having a second dry development rate, the first dry development rate being slower than the second dry development rate.

[0093] Example 11. The method of example 1, wherein the first developing process is a wet developing process and the second developing process is one or more dry developing processes.

[0094] Example 12. The method of any one of Examples 1-11, further comprising: determining a first dose of EUV radiation to form the target critical dimension using a single development process; and determining a second dose of EUV radiation to form the target critical dimension using hybrid development, the second dose being less than the first dose; and exposing the photoresist includes exposing the photoresist to the second dose.

[0095] Example 13. A method of microfabrication includes depositing a photoresist film on a working surface of a semiconductor wafer, the photoresist film being sensitive to extreme ultraviolet radiation; exposing the photoresist film to a pattern of extreme ultraviolet radiation to form an EUV photoresist pattern; performing a wet development process to remove a first portion of the EUV photoresist pattern to obtain a structure having a first critical dimension that is larger than a target critical dimension; and, after performing the wet development process, performing a dry development process to remove a second portion of the EUV photoresist pattern to obtain a structure having the target critical dimension.

[0096] Example 14. The method of example 13, further comprising: measuring a critical dimension after the wet development process and before the dry development process; and, in response to identifying a measured critical dimension value that is greater than a predetermined range, performing a corrective treatment process to bring the critical dimension value within the predetermined range.

[0097] Example 15. The method according to any one of Examples 13 or 14, further comprising performing a first bake after exposing the photoresist film to patterned EUV radiation, and performing a second bake after the wet development process and before the dry development process.

[0098] Example 16. The method according to any one of Examples 13-15, further comprising exposing the EUV photoresist pattern to UV light after the wet developing process and before the dry developing process.

[0099] Example 17. The method according to any one of Examples 13-16, wherein the solvent for the wet development process comprises 2-heptanone, n-butyl acetate, propylene glycol methyl ether acetate, or methyl isobutyl carbinol.

[0100] Example 18. The method of any one of Examples 13-17, wherein the dry development process comprises chemical vapor etching using hydrogen bromide.

[0101] Example 19. The method of any one of Examples 13-16, 18, wherein the dry development process comprises plasma etching using a gas comprising hydrogen chloride, hydrogen bromide, argon, or helium.

[0102] Example 20. A semiconductor manufacturing apparatus including a first developing chamber and a second developing chamber, the semiconductor manufacturing apparatus being configured to sequentially process a substrate in the first developing chamber and the second developing chamber.

[0103] Example 21. The apparatus of example 20, wherein the first developing chamber is a wet developing chamber for treating the substrate with a liquid phase developing chemistry and the second developing chamber is a dry developing chamber for treating the substrate with a vapor phase developing chemistry.

[0104] Example 22. The apparatus of one of Examples 20 or 21, further comprising a plasma etch chamber configured for anisotropic etching of a semiconductor wafer, wherein after exposure to the pattern of EUV radiation, a gas phase developer chemistry in a dry developer chamber removes the photoresist material.

[0105] Example 23. An apparatus according to any one of Examples 20 to 22, wherein the first developing chamber is a first dry developing chamber for treating the substrate with a first vapor phase developing chemistry, and the second developing chamber is a second developing chamber for treating the substrate with a second vapor phase developing chemistry, and the development rate of the first vapor phase developing chemistry is less than the development rate of the second vapor phase developing chemistry.

[0106] Example 24. The apparatus of any one of Examples 20-23, wherein the vapor phase development chemistry is a chemical vapor etching chemistry.

[0107] Example 25. The apparatus of any one of Examples 20-24, wherein the vapor phase development chemistry is a plasma enhanced vapor etching chemistry.

[0108] Example 26. A method of microfabrication, the method further comprising: depositing a photoresist film on a working surface of a semiconductor wafer, the photoresist film being sensitive to extreme ultraviolet light; using a first set of semiconductor wafers to determine a first dose of extreme ultraviolet light to fully develop the photoresist film using a wet development process; exposing a second set of semiconductor wafers having the photoresist film to a second dose of extreme ultraviolet light, the second dose being less than the first dose; and developing the photoresist film on each of the semiconductor wafers of the second set using a corresponding hybrid development process including a wet development process followed by a dry development process.

[0109] Example 27. The method of example 26, further comprising determining a second dose of EUV radiation, wherein determining the second dose of EUV radiation and the corresponding hybrid development process further comprises: depositing a photoresist film on a working surface of a plurality of semiconductor wafers; exposing the plurality of semiconductor wafers to a series of doses of EUV radiation that decrease from the first dose; and performing a series of hybrid developments on the plurality of semiconductor wafers using a series of wet development times and a series of dry development times, wherein the hybrid development achieves a target critical dimension; and selecting a second dose of EUV radiation and a corresponding hybrid development process for developing the further wafers, wherein the second dose of EUV radiation is lower than the first dose.

[0110] Example 28. The method of any one of examples 26 or 27, wherein the second dose of EUV radiation is lower than the first dose by an amount greater than 15%.

[0111] Although the present invention has been described with reference to exemplary embodiments, this specification is not intended to be construed in a limiting sense. Various modifications and combinations of those exemplary embodiments, as well as other embodiments of the present invention, will become apparent to those skilled in the art upon reference to this specification. Therefore, it is intended that the appended claims cover any such modifications or embodiments.

Claims

1. 1. A method of microfabrication, the method comprising: depositing a photoresist film on a working surface of a semiconductor wafer, said photoresist film being sensitive to extreme ultraviolet light; exposing the photoresist film to a pattern of extreme ultraviolet light; performing hybrid development of the photoresist film, the hybrid development comprising: performing a first development process to remove a first portion of the photoresist film; stopping development of the photoresist film after the first development process, where after the stopping step, the photoresist film has a structure having a first critical dimension that is greater than a target critical dimension; and performing a second development process after the step of stopping the developing to remove a second portion of the photoresist film and reduce the critical dimension of the structure from the first critical dimension to a second critical dimension that is smaller than the first critical dimension; and The method comprising:

2. 2. The method of claim 1, wherein the second development process further comprises performing a dry development process to remove incremental amounts of photoresist until the critical dimension of the structure is reduced to the target critical dimension.

3. 2. The method of claim 1, wherein the first development process is a wet development process using a development solvent comprising propylene glycol monomethyl ether acetate, acetic acid, methyl isobutyl carbinol, 2-heptanone, or n-butyl acetate.

4. The method of claim 3 , wherein the developing solvent comprises propylene glycol monomethyl ether acetate and acetic acid.

5. further comprising the step of measuring a critical dimension of said structure subsequent to said first development process; performing a corrective treatment process during the second development process in response to identifying a measured critical dimension value that is greater than a predetermined range; 2. The method of claim 1, comprising:

6. moreover, performing a first thermal treatment after the step of exposing the photoresist to an EUV pattern; performing a second thermal treatment after the first development process and before the second development process; 2. The method of claim 1, comprising:

7. The method of claim 6 , wherein a bake time and a bake temperature of the first thermal treatment are different from a bake time and a bake temperature of the second thermal treatment.

8. 10. The method of claim 1, wherein the second development process comprises chemical vapor etch development using a gas comprising hydrogen chloride, hydrogen bromide, argon or helium.

9. 10. The method of claim 1, wherein the second development process comprises a plasma etch development process using a gas comprising hydrogen chloride, hydrogen bromide, argon or helium.

10. the first development process is a first dry development process having a first dry development rate of a photoresist; the second development process is a second dry development process having a second dry development rate; The method of claim 1 , wherein the first dry development rate is slower than the second dry development rate.

11. The method of claim 1 , wherein the first development process is a wet development process and the second development process is one or more dry development processes.

12. moreover, determining a first dose of EUV radiation to form a target critical dimension using a single development process; determining a second dose of EUV radiation to form the target critical dimension using the hybrid development, the second dose being less than the first dose; having 2. The method of claim 1, wherein exposing the photoresist comprises exposing the photoresist to the second dose.

13. 1. A method of microfabrication, the method comprising: depositing a photoresist film on a working surface of a semiconductor wafer, said photoresist film being sensitive to extreme ultraviolet light; exposing the photoresist film to a pattern of extreme ultraviolet light to form an EUV photoresist pattern; performing a wet development process to remove a first portion of the EUV photoresist pattern to obtain a structure having a first critical dimension that is greater than a target critical dimension; performing a dry development process after performing the wet development process to remove a second portion of the EUV photoresist pattern to obtain the structure having the target critical dimension; The method comprising:

14. moreover, measuring a critical dimension after the wet development process and before the dry development process; responsive to identifying a measured critical dimension value that is outside a predetermined range, performing a corrective process to bring the critical dimension value within the predetermined range; 14. The method of claim 13, comprising:

15. moreover, performing a first bake after exposing the photoresist film to patterned EUV radiation; performing a second bake after the wet development process and before the dry development process; 14. The method of claim 13, comprising:

16. 14. The method of claim 13, further comprising exposing the EUV photoresist pattern to UV light after the wet development process and before the dry development process.

17. The method of claim 13, wherein the solvent of the wet development process comprises 2-heptanone, n-butyl acetate, propylene glycol methyl ether acetate, or methyl isobutyl carbinol.

18. 14. The method of claim 13, wherein the dry development process comprises a chemical vapor etch using hydrogen bromide.

19. 14. The method of claim 13, wherein the dry development process comprises plasma etching with a gas comprising hydrogen chloride, hydrogen bromide, argon or helium.

20. A semiconductor manufacturing apparatus comprising: a first development chamber; a second development chamber; having A semiconductor manufacturing apparatus configured to sequentially process substrates in the first and second developing chambers.

Citation Information

Patent Citations

  • Method for forming resist pattern and method for forming metal pattern using the same

    JP2009198587A

  • Method for forming contact hole of semiconductor device

    KR1020080062037A

  • Curable composition for transfer material and urea compound containing (METH)acryloyl group

    WO2010087318A1