Bainitic steel and method for producing same
The bainitic steel with controlled chemical composition and manufacturing process forms a gradient structure, addressing the inefficiencies of conventional methods by achieving high mechanical properties suitable for automotive applications.
Patent Information
- Application Number
- JP2024519384
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-09-30
- Filing Date
- 2022-09-29
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2042-09-29
AI Technical Summary
Conventional methods for producing structurally gradient steel plates are costly and inefficient, unable to achieve more than a three-layer composite structure, and result in materials with imbalanced mechanical properties, limiting their application in areas requiring high surface hardness and core plasticity.
A bainitic steel composition with controlled chemical elements (C, Si, Mn, B, Cr, Mo, Al, Ti, Nb) and a specific manufacturing process involving controlled cooling stages to form a gradient structure, resulting in a two-layer surface and single-layer core structure with optimized mechanical properties.
The bainitic steel achieves yield strength ≥800 MPa, tensile strength ≥1000 MPa, elongation at break ≥12%, and hole expansion rate ≥40%, ensuring good overall formability and ductility, suitable for automotive components.
Smart Images

Figure 2024535926000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to the metallurgical field, in particular to bainitic steel and a method for making the same. [Background technology]
[0002] With the development concept of "Green & Safety" for the new generation of automobiles, the strength of steels used in automobile structural parts is becoming higher and higher, and materials with different properties in the thickness direction are gradually required. For example, the surface layer of a material is required to have high hardness and abrasion resistance, or to have a high uniformity of structure for flange forming, while the core part must have a high degree of plasticity so that necking and fracture do not occur during tensile elongation forming as a whole steel material. Or, if a layered structure with low hardness is required for the surface layer so that the material has a certain degree of bending property, the next surface layer must have a uniform hard phase structure to maintain flange forming and strength, and the core part has a softer structure to ensure plasticity, toughness, etc. As a result, the material has high strength and at the same time has good overall formability such as bending, flange forming, and tensile elongation.
[0003] In the automotive industry, the requirements for different structures and performance of steels through the thickness are increasing, while the traditional method uses slabs with different components or structures through welding, combination rolling and other methods to obtain a structure with gradient through the thickness of the steel. For example, CN201210368300.6 and CN201310724615.4 use metal combination rolling to obtain a laminated composite through the thickness. However, this method is complicated, slow and very costly.
[0004] There are also patents that use the method of surface layer decarburization to obtain steel sheets or strips with different microstructures in the surface layer and core. For example, by using strip surface decarburization to form a decarburized layer of several microns to several tens of microns, the upper and lower surface layers have a pure ferrite or ferrite >50% structure, while the core has another single-phase or multi-phase structure, such as martensite, tempered martensite or bainite structure. This method spontaneously forms a microstructure gradient in the thickness direction and can obtain a high-strength steel sheet with a three-layer composite structure, but the difference in strength or hardness between the surface layer and the core is too large, and the strength or hardness of the surface layer is too low, which greatly limits the application range of this type of product (for example, automobile seat rails, drive shafts, etc., fields where high hardness is required in the surface layer, or fields where fatigue resistance is required). As a result, the material has good bending properties, but the elongation and hole expansion ratio are not high, i.e., the plasticity and flangeability are poor. Meanwhile, this method can only form a three-layer composite structure, and it is not possible to obtain a structure with more layers. Summary of the Invention [Means for solving the problem]
[0005] In response to the problems of the high cost of steel plates with structure gradients in the prior art and the inability to obtain a composite structure with more than three layers, the present invention provides a bainite steel that can obtain mechanical properties of yield strength ≧800MPa, tensile strength ≧1000MPa, fracture elongation ≧12%, and hole expansion ratio ≧40%. In addition, since a structure with a gradient is formed in the thickness direction of the steel plate or strip, the material has good comprehensive formability, good tensile ductility and hole expansion flange formability, and high fracture elongation and hole expansion ratio, with (fracture elongation * 10 + hole expansion ratio) ≧ 170% in all embodiments.
[0006] The bainite steel of the present invention contains the following chemical components in mass percent: C: 0.10-0.19%, Si: 0.05-0.45%, Mn: 1.5-2.2%, B: 0.001-0.0035%, Al: 0.01-0.05%, Cr; 0.05-0.40%, Mo: 0.05-0.40%, Fe≧90%.
[0007] However, the design objectives of each element are as follows: C: In the bainite steel of the present invention, the element C mainly controls the structure phase transition, carbide size and bainite partial structure morphology of carbon steel, and affects the mechanical properties of the material. If the C element content in the steel is less than 0.10%, the strength of the steel does not meet the target requirements; if the C element content in the steel is more than 0.19%, martensite structure and coarse cementite are likely to be generated, and the performance of the steel plate is deteriorated. In addition, in the present invention, C further affects the bainite partial structure morphology, and the higher the C content, the more likely acicular bainite is to be generated. Therefore, in the present invention, the mass percentage of C is controlled to 0.10-0.19%. Preferably, the mass percentage of C is 0.13-0.17%.
[0008] Si: In the bainite steel of the present invention, Si has a certain solid solution strengthening effect and also affects the surface quality of the steel sheet. If the Si content in the steel is less than 0.05%, it is difficult to obtain a sufficient strengthening effect; if the Si content in the steel exceeds 0.45%, oxide scale or tiger pattern color difference is likely to be formed, which is disadvantageous to the surface quality of the steel sheet for automobiles. In addition, in the present invention, Si affects the bainite partial structure morphology, and the higher the Si content, the easier it is to form polygonal bainite, so in the present invention, the mass percentage of Si is 0.05 to 0.45%. Preferably, the mass percentage of Si is 0.05 to 0.35%. More preferably, the mass percentage of Si is 0.15 to 0.3%.
[0009] Mn: In the bainite steel of the present invention, Mn is one of the elements controlling the phase transition of the steel, and also affects the bainite substructure morphology, and the higher the Mn content, the easier it is to form polygonal bainite. However, it should be noted that the Mn content of the steel should not be too high, and when the Mn content of the steel is too high, the corrosion resistance and weldability will be deteriorated. Therefore, in the present invention, the mass percentage of Mn is controlled to 1.5-2.2%. Preferably, the mass percentage of Mn is 1.7-2.1%.
[0010] B: In the bainite steel of the present invention, B not only contributes to the formation of bainite in the steel, but also affects the strength and formability of the steel sheet, and at the same time affects the bainite substructure morphology. The higher the B content, the easier it is to obtain acicular bainite, the higher the steel sheet strength, and the easier it is to obtain brittle borides, which affects the hole expansion ratio of the steel sheet. Therefore, in the present invention, the mass percentage of B is controlled to 0.001-0.0035%.
[0011] Al: In the bainite steel according to the present invention, Al is added to the steel only as a deoxidizing element, which can remove the O element in the steel and ensure the performance and quality of the steel. Therefore, in the bainite steel according to the present invention, the mass percentage of Al is 0.01-0.05%. In the prior art, Al is added to the steel in large amounts (≧0.1%) as a ferrite forming element and a carbide precipitation inhibiting element for the purpose of solid solution strengthening effect, or the addition of Al changes the phase transition of the steel by changing the phase transition temperature (e.g. A1, A3), the bainite formation kinetics and the carbide precipitation kinetics, forming retained austenite or carbon-free bainite, and finally increasing the strength of the steel. However, by controlling the components and adjusting the process in the present invention, a bainite steel with good overall formability can be obtained. The formation of carbon-free bainite by adding a large amount of Al would destroy the gradient of the bainite structure formed in the thickness direction, leading to increased costs and difficulty in continuous casting production. Therefore, in the present invention, the mass percentage of Al is controlled to be between 0.01 and 0.05%, thereby avoiding increased costs and difficulty in continuous casting production and forming a gradient of the bainite structure in the thickness direction.
[0012] Cr and Mo: In the bainite steel of the present invention, Cr and Mo can form fine dispersed carbide precipitation phase with C, which can further increase the strength of the steel plate, and also affect the appearance period of pearlite and ferrite in the CCT curve, improve the hardenability of the steel plate, and can be designed together with the cooling rate of the steel plate in the annealing process to form a structure gradient in the thickness direction and control different thickness proportions. Therefore, the mass percentages of Cr and Mo in the present invention are as follows: 0.05%≦Cr≦0.40%, 0.05%≦Mo≦0.40%.
[0013] In the present invention, by rationally controlling the contents of elements such as C, Si, Mn, B, Al, Cr, and Mo in the steel, a phase with a structural gradient is spontaneously formed in the steel during the manufacturing process, and at the same time, the hardenability of the steel is improved, thereby improving the strength and formability of the bainite steel.
[0014] Furthermore, the bainitic steel further contains at least one of Ti and Nb, with the proviso that the mass percentages of Ti and Nb satisfy the following: Nb≦0.1%, Ti≦0.15%.
[0015] Ti and Nb: In the bainite steel of the present invention, Ti and Nb are optional alloying elements, which are added to the steel to form finely dispersed carbide precipitation phases, refine the grain structure, and further increase the strength and formability of the steel sheet. Therefore, in the bainite steel of the present invention, the mass percentages of Nb and Ti are as follows: Nb≦0.1%, Ti≦0.15%. Since the addition of the above alloying elements increases the cost of the material, in consideration of the performance and cost management, the technical solution of the present invention is preferable, and at least one of Nb and Ti may be added to the steel. In one embodiment, the bainite steel of the present invention contains Nb and Ti in a mass percentage content of 0.001-0.1% for Nb and 0.001-0.15% for Ti.
[0016] In one embodiment, the bainite steel of the present invention contains the following chemical compositions in mass percent: C: 0.10-0.19%, Si: 0.05-0.45%, Mn: 1.5-2.2%, B: 0.001-0.0035%, Al: 0.01-0.05%, Cr; 0.05-0.40%, Mo: 0.05-0.40%, and the balance being Fe and unavoidable impurities.
[0017] Furthermore, the above unavoidable impurities are P≦0.015% and S≦0.004%. Both P and S are impurity elements in steel, and as far as technically possible, the content of impurity elements in steel should be reduced as much as possible to obtain tempered steel with better performance and better quality.
[0018] Furthermore, in the bainitic steel of the present invention, the mass percentages of the chemical elements satisfy the following relationship: R=(Mn+Si) / (12*C+160*B), where 0.9≦R≦1.2, where each chemical element in the formula is substituted with the numerical value before the percent sign of the mass percentage content of that chemical element.
[0019] In the present invention, R=(Mn+Si) / (12*C+160*B) is defined. According to the experiment, when calculating with this formula, in order to obtain a bainite steel sheet / strip structure with an ideal texture gradient, the R value needs to be limited to a certain range, 0.9≦R≦1.2. However, the more C and B, the easier it is to form acicular bainite, and the more Mn and Si, the easier it is to form blocky bainite. Therefore, by rationally designing the contents of C and B, Mn and Si, the steel sheet and strip can be in a critical state that is favorable for the formation of both acicular bainite and blocky bainite from the viewpoint of component design, that is, in the state of 0.9≦R≦1.2 in the formula. Combined with an optimized annealing process, a texture gradient can finally be formed in the thickness direction of the steel sheet. In addition, although the C and B contents are low, they have a stronger effect on the formation and morphology of bainite, so a large coefficient is used in the formula to balance with the high contents of Mn and Si. This is because the effect of Mn and Si on the formation of bainite and its morphology is significantly weaker than that of C and B. In this design, the level of 0.9≦R≦1.2 is the most suitable critical level for the formation of gradient structure, and if R is too high, the thickness of the lumpy layer in the gradient structure is too large and the thickness of the acicular layer is too small, and in some cases, there is no acicular layer, so there is no gradient in the thickness direction of the structure, and if R is too low, the thickness of the acicular layer in the gradient structure is too large and the thickness of the lumpy layer is too small, and in some cases, there is no lumpy layer, so there is no gradient in the thickness direction of the structure. Therefore, in the present invention, R is set to 0.9≦R≦1.2 to ensure the structure gradient and mechanical properties in the thickness direction of the steel.
[0020] Furthermore, in the bainitic steel of the present invention, the mass percentages of the chemical elements must satisfy the following relationship: Q=(C+Cr+Mo+Mn / 2) / R, where 1.15≦Q≦1.5, and the numerical values before the percent sign of the mass percentages of the elements are applied in the calculation.
[0021] In the present invention, Q=(C+Cr+Mo+Mn / 2) / R is defined, which further guides the composition design of steel. Experiments have shown that when 1.15≦Q≦1.5, the steel has suitable hardenability and ability to form microstructure gradient. Since the microstructure gradient or its layer structure is distributed in the thickness direction of steel plate and strip, the hardenability of steel plate and strip is also the most important influencing factor of the gradient microstructure formation in the thickness direction. In the present application, C, Cr, Mo, and Mn all affect the hardenability of steel plate and strip, and the higher the content of these elements, the stronger the hardenability. However, the Mn content is one order of magnitude higher than other elements, and its effect on hardenability is relatively weak, so in this formula, the design of Mn has a coefficient of 1 / 2. The formation temperatures of acicular bainite and massive bainite in the annealing process are slightly different, with the formation temperature of acicular bainite being lower and that of massive bainite being higher, so the higher the hardenability of the steel plate, the more favorable the formation of acicular bainite and the less favorable the formation of massive bainite, and vice versa. Therefore, in order to ensure that the ratio of acicular bainite and massive bainite in the thickness direction in steel plate and strip steel can be formed into an appropriate sandwich, when the composition design of the steel plate is favorable for the formation of massive bainite, that is, when the R value is high, it is necessary to add higher hardenability to promote the formation of acicular bainite, and when the composition design of the steel plate is favorable for the formation of acicular bainite, that is, when the R value is low, it is necessary to add low hardenability to promote the formation of massive bainite. Therefore, the numerator of the Q value is the alloy content, which means the hardenability of the strip steel, and the higher it is, the stronger the hardenability. The denominator is the R value, which indicates the ability of blocky bainite and acicular bainite to form in the structure, and the ratio of the numerator and denominator, that is, the Q value, directly affects the ability of blocky and acicular layers to form during the annealing process and the final proportion. If the Q value is too small, the ability of blocky bainite to form is too strong, making it difficult for acicular bainite to form in the final structure and difficult for gradient structure to form. If the Q value is too large, the ability of acicular bainite to form is too strong, making it difficult for blocky bainite to form in the final structure and difficult for gradient structure to form.
[0022] Furthermore, the bainitic steel has two surface layer structures and one core structure, the core structure being between the two surface layer structures.
[0023] Furthermore, in bainite steel, the volume of the core structure occupies 20% to 50% of the volume of the bainite steel, and the remainder is the surface layer structure.
[0024] Furthermore, the surface layer structure includes acicular bainite and granular carbide precipitate phases, and the core structure includes blocky bainite and granular carbide precipitate phases.
[0025] Furthermore, the acicular bainite and granular carbide precipitate phases occupy 99% or more of the surface layer structure volume, and the blocky bainite and granular carbide precipitate phases occupy 99% or more of the core structure volume.
[0026] Specifically, in the bainite steel according to one embodiment of the present invention, as shown in FIG. 1, there are three layers in the thickness direction of the steel plate or strip, and the structures from one surface to the other surface are as follows: Surface layer structure 2: A structure mainly composed of an acicular layer, that is, acicular bainite and dispersedly precipitated nanometer-, submicrometer- or micrometer-sized granular carbide precipitate phases, the total amount of which accounts for ≧99% of the phase in the region. The proportion in the thickness direction is 25% to 40%.
[0027] Core structure 1: A structure mainly composed of massive layer, that is, massive bainite and dispersedly precipitated nanometer-, submicrometer- or micrometer-sized granular carbide precipitate phases, the total amount of which accounts for ≧99% of the phase in the region. The proportion in the thickness direction is 20% to 50%.
[0028] Surface layer structure 2: A structure mainly composed of an acicular layer, that is, acicular bainite and dispersedly precipitated nanometer-, submicrometer- or micrometer-sized granular carbide precipitate phases, the total amount of which accounts for ≧99% of the phase in the region. The proportion in the thickness direction is 25% to 40%.
[0029] The proportion of the three-layer region in the thickness direction of the bainite steel is 100% in all cases. Furthermore, the bainitic steel has two multi-phase layers, and the two surface layer structures and one core structure form an intermediate layer, which is located between the two multi-phase layers.
[0030] Furthermore, in bainite steel, the volume of the multi-phase layer occupies 2% to 10% of the volume of the bainite steel, and the remainder is the intermediate layer.
[0031] Furthermore, the multi-phase layer includes polygonal ferrite, acicular bainite and granular carbide precipitate phases, the polygonal ferrite occupies 50% or less of the volume of the multi-phase layer, and the polygonal ferrite, acicular bainite and granular carbide precipitate phases occupy 99% or more of the volume of the multi-phase layer.
[0032] Specifically, in one embodiment of the bainite steel of the present invention, as shown in FIG. 2, there are five layers in the thickness direction of the steel plate or strip, and the structures from one surface to the other surface are as follows: Multiphase layer 3: A structure mainly composed of polygonal ferrite, acicular bainite, and dispersedly precipitated nanometer-, submicrometer-, or micrometer-sized granular carbide precipitate phases (however, polygonal ferrite structure <50%), and the proportion of the total amount of polygonal ferrite, acicular bainite, and dispersedly precipitated nanometer-, submicrometer-, or micrometer-sized granular carbide precipitate phases in the relevant region phase is ≥99%. The proportion in the thickness direction is 1% to 5%.
[0033] Surface layer structure 2: A structure mainly composed of an acicular layer, that is, acicular bainite and dispersedly precipitated nanometer-, submicrometer- or micrometer-sized granular carbide precipitate phases, the total amount of which accounts for ≧99% of the entire phase in the region. The proportion in the thickness direction is 25% to 40%.
[0034] Core structure 1: A structure mainly composed of massive layer, that is, massive bainite and dispersedly precipitated nanometer-, submicrometer- or micrometer-sized granular carbide precipitate phases, the total amount of which accounts for ≧99% of the phase in the region. The proportion in the thickness direction is 25% to 40%.
[0035] Surface layer structure 2: A structure mainly composed of an acicular layer, that is, acicular bainite and dispersedly precipitated nanometer-, submicrometer- or micrometer-sized granular carbide precipitate phases, the total amount of which accounts for ≧99% of the phase in the region. The proportion in the thickness direction is 25% to 40%.
[0036] Multiphase layer 3: A structure mainly composed of polygonal ferrite, acicular bainite, and dispersedly precipitated nanometer-, submicrometer-, or micrometer-sized granular carbide precipitate phases (however, polygonal ferrite structure <50%), and the proportion of the total amount of polygonal ferrite, acicular bainite, and dispersedly precipitated nanometer-, submicrometer-, or micrometer-sized granular carbide precipitate phases in the relevant region phase is ≥99%. The proportion in the thickness direction is 1% to 5%.
[0037] The ratio of the five-layer region is 100% in total. However, the hardness of the acicular layer is the highest and that of the multi-phase layer is the lowest.
[0038] In the bainite steel of the present invention, the diameter of the granular carbide precipitate phase is ≦5 μm. The carbide precipitate phase is limited to avoid the deterioration of the hole expansion ratio. When the carbide precipitate phase size is >5 μm, cracks are likely to occur at the bonding site between the carbide and the substrate when the steel sheet is subjected to hole expansion flange deformation or when the hole expansion ratio is measured, which leads to a decrease in the hole expansion ratio of the steel sheet and a deterioration in the hole expansion flange forming performance.
[0039] Furthermore, in the bainite steel of the present invention, the bainite steel has a tensile strength of ≧1000 MPa, a yield strength of ≧800 MPa, a hole expansion ratio of ≧40%, and a fracture elongation of ≧12%.
[0040] Furthermore, the bainite steel of the present invention has excellent tensile ductility and hole expansion flangeability, and the fracture elongation*10+hole expansion ratio≧170%.
[0041] The present invention further provides a method for producing the above bainitic steel, comprising the steps of: Smelting and foundry; Hot rolling; Post-rolling cooling and coiling; Pickling and cold rolling; Annealing.
[0042] Since a bainite steel having a structure gradient is not produced by the conventional method of decarbonizing the surface layer, the bainite steel of the present invention does not have the problem that the strength and hardness of the surface layer are lower than those of the core portion.
[0043] Furthermore, the parameters of the above-mentioned manufacturing method satisfy any one of the following: In the hot rolling process, the heating temperature is 1100-1230°C, the finish rolling start temperature is 1050-1180°C, and the finish rolling end temperature is 870-930°C; In the post-rolling cooling and coiling process, the cooling rate is 30-150°C / s and the coiling temperature is 540-620°C; In the cold rolling process, the cold rolling reduction is ≧30%.
[0044] In the above-mentioned manufacturing method, the pre-annealing process is mainly for obtaining a steel sheet or strip having uniform components and original structure, so that the subsequent annealing process can satisfy uniform and stable structure and properties, but it is the annealing process that plays an important role in the properties of the steel sheet.
[0045] Before introducing the annealing process, it is necessary to introduce the following concepts: Since the present invention is aimed at the design of the gradient structure in the thickness direction of the steel plate / strip, it is inevitable or intentional that the steel plate or strip has different temperature ranges in the thickness direction, but due to the limitation of the continuous production mode of the steel plate or strip, the temperature detection and control can only be directed to the upper and lower surface temperatures, and cannot detect the temperature at other positions in the thickness direction. The temperatures of the upper and lower surfaces are not additionally distinguished, and are called the surface temperature according to the same process. The temperature and cooling rate described below all refer to the surface temperature and the cooling rate calculated from the surface temperature. It should be noted that the temperature distribution in the thickness direction of the steel plate or strip is controlled by the surface temperature, cooling rate, the injection gas pressure during cooling (indicating the cooling capacity) and the hardenability of the steel plate during cooling.
[0046] Furthermore, the annealing process includes a heating stage, a slow cooling stage, a rapid cooling stage, a controlled cooling stage and an air cooling stage in order, and the controlled cooling rate in the three stages of the slow cooling stage, the rapid cooling stage and the controlled cooling stage satisfies the following: controlled cooling stage<slow cooling stage<rapid cooling stage.
[0047] Furthermore, in the heating stage, the material is heated to a soaking temperature of 840 to 950° C. at a heating rate of ≦50° C. / s, and then kept at that temperature for a period of 60 to 180 seconds.
[0048] In the heating stage, the bainitic steel is heated to a soaking temperature of 840-950°C at a heating rate of ≦50°C / s and then held at that temperature for 60-180s. However, if the heating rate in the heating stage is >50°C / s or the holding time is <60s, the uniformity of the strip steel structure is deteriorated, which affects the subsequent formation of a gradient structure in the thickness direction. Also, if the temperature is below the lower limit of the soaking temperature, the strip steel does not obtain a sufficient bainite structure (whether acicular bainite or blocky bainite). Furthermore, the heating rate is preferably 5-50°C / s. If the holding time is >180s or, further, the soaking temperature exceeds 950°C, the grains of the strip steel are coarsened, which deteriorates the formability of the steel.
[0049] In the present invention, in order to form a bainite steel having a three-layer structure gradient in the thickness direction, in the slow cooling stage, the slow cooling rate is Q to 10*Q°C / s to a slow cooling temperature of 720 to 800°C, and the mass percentages of the chemical elements satisfy Q=(C+Cr+Mo+Mn / 2) / R, 1.15≦Q≦1.5, R=(Mn+Si) / (12*C+160*B), 0.9≦R≦1.2, and the numerical value before the percent sign of the mass percentage content of the chemical element is substituted for each chemical element in the formula. In one embodiment, the slow cooling rate is 5Q to 10Q°C / s. In one embodiment, the slow cooling rate is 7Q to 10Q°C / s.
[0050] Specifically, in the embodiment of the present invention, the annealing is performed by injecting a cooling gas onto the surface of the bainite steel. For example, during cooling, the annealing is performed by injecting a cooling gas onto the surface of the bainite steel, the cooling gas injection pressure is 0.2*Q~QkPa, and the cooling gas injection holding time is 5~20 seconds. Of course, in other possible embodiments, the purpose of annealing may be achieved by methods such as liquid cooling, and it is sufficient to cool to an annealing temperature of 720~800°C at an annealing rate of Q~10*Q°C / s. The main purpose of this stage is to make the temperature of the steel plate or strip uniform in the width direction and non-uniform in the thickness direction, and to prevent the structure transformation at each position.
[0051] The slow cooling rate is controlled in this process to achieve a uniform temperature in the width direction of the steel plate or strip, and to prevent phase transition at each position of the strip. If the temperature is too low, austenite may decompose due to phase transition and form ferrite or pearlite, and if the temperature is too high, it is disadvantageous to the high precision control of the next cooling stage and to the achievement of a gradient structure in the thickness direction. The control of the cooling gas injection pressure onto the steel plate or strip surface and the control of the holding time are both for the purpose of controlling the cooling unevenness in the thickness direction of the strip. If the cooling gas injection pressure onto the steel plate or strip surface is less than 0.2*QkPa or the holding time is less than 5 seconds, the cooling capacity will be insufficient, and although the strip surface can be cooled to the set temperature, most of the area below the surface layer will be at a high temperature, which is unfavorable for forming a gradient structure in the thickness direction in the next process, or the acicular bainite area in the gradient structure formed in the next stage will be too small. If it exceeds QkPa or the holding time exceeds 20 seconds, the cooling capacity will be too large, and the temperature of the core part of the strip will approach or reach the surface temperature, which is unfavorable for forming a gradient structure in the thickness direction in the next process, or the blocky bainite area formed in the next stage will be too small.
[0052] In the present invention, in order to form a bainite steel having a five-layer structure gradient in the thickness direction, in the slow cooling stage, the slow cooling rate is Q to 10*Q°C / s to a slow cooling temperature of 620 to 700°C, and the mass percentages of the chemical elements satisfy Q=(C+Cr+Mo+Mn / 2) / R, 1.15≦Q≦1.5, R=(Mn+Si) / (12*C+160*B), 0.9≦R≦1.2, and each chemical element in the formula is substituted with the numerical value before the percent sign of the mass percentage content of the chemical element. In one embodiment, the slow cooling rate is 5Q to 10Q°C / s. In one embodiment, the slow cooling rate is 7Q to 10Q°C / s.
[0053] Specifically, in the embodiment of the present invention, the annealing is performed by injecting a cooling gas onto the surface of the bainite steel. For example, during cooling, the annealing is performed by injecting a cooling gas onto the surface of the bainite steel, the cooling gas injection pressure is 0.05*Q~0.15*QkPa, and the cooling gas injection holding time is 5~15 seconds. Of course, in other possible embodiments, the purpose of annealing can be achieved by methods such as liquid cooling, and any technical solution that can cool the bainite steel to an annealing temperature of 620~700°C at an annealing rate of Q~10*Q°C / s is within the scope of the present application.
[0054] In this process, the cooling to 620-700°C is to bring the surface of the steel sheet or strip into the ferrite transition temperature range, and by keeping the temperature for a certain time, a certain amount of ferrite is formed in the surface region of the steel sheet or strip, preparing the final multi-phase layer of the surface layer. If the temperature is below or above this temperature, the formation of a certain amount of ferrite on the surface of the strip is not guaranteed. Similarly, if the holding time is too short or the cooling rate is too fast, the formation of ferrite on the surface of the strip is not in time, and the final multi-phase layer of the surface layer cannot be formed. Conversely, if the holding time is too long or the cooling rate is too slow, the content of ferrite formed on the surface of the strip is too high, and the thickness is too thick, which is not only unfavorable to the formation of the multi-phase layer of the surface layer, but also insufficient acicular bainite is formed in the shallow surface layer during the quenching stage, which affects the subsequent formation of the acicular layer.
[0055] The injection pressure of the cooling gas on the surface of the steel plate or strip is set to 0.05*Q~0.15*QkPa in order to control the thickness of polygonal ferrite formed on the surface of the strip. When the pressure is within the range and the holding time is within the set range, the steel plate or strip actually only cools to 620~700℃ in the surface layer region and enters the ferrite phase region, while the temperature of other regions is still higher than 700℃, and ferrite transformation does not occur (the formation of ferrite also releases the transformation latent heat). However, if the pressure of the injected cooling gas is too high, the temperature of the shallow surface layer of the steel plate or strip and even the core part will decrease, which is unfavorable for the formation of the subsequent acicular layer and lumpy layer. If the pressure of the injected cooling gas is too low, a certain amount of polygonal ferrite cannot be stably formed in the surface layer, and as a result, a multi-phase layer cannot be stably formed in the surface layer.
[0056] After the slow cooling is completed, in the quenching stage, in order to form bainite steel with a gradient structure of either three or five layers in the thickness direction, it is necessary to cool the steel to a quenching temperature of 400 to 540°C at a quenching rate of 10*Q to 20*Q°C / s.
[0057] Specifically, in the embodiment of the present invention, the quenching is performed by injecting cooling gas onto the surface of the bainite steel. In this stage, the cooling gas needs to be injected onto the surface of the bainite steel twice during cooling, the first injection pressure of the cooling gas is 0.3*Q~1.5*QkPa, the first holding time of the cooling gas is 1~7 seconds, the second injection pressure of the cooling gas is 0.08*Q~0.2*QkPa, and the second holding time of the cooling gas is 5~10 seconds. Similarly, in other possible embodiments, the purpose of slow cooling can be achieved by methods such as liquid cooling, and any technical solution that can cool the bainite steel to a quenching temperature of 400~540 at a quenching rate of 10*Q~20*Q℃ / s in this stage is within the scope of the present application.
[0058] Furthermore, the cooling gas used in the annealing step is a mixture of a reducing gas and an inert gas. Preferably, in the mixture, the volume fraction of the reducing gas is 1% to 8%. In one embodiment, the reducing gas in the mixture is hydrogen gas, and the volume fraction thereof is 1% to 8%. The temperature of the cooling gas may be controlled to 5 to 50°C.
[0059] In one embodiment of the present invention, the cooling of the steel plate or strip is carried out by injecting a cooling gas (i.e. a mixture of reducing gas and inert gas) toward its surface, and the reducing gas can be hydrogen gas. In the present invention, the inert gas is a gas that does not chemically react with the bainite steel to affect the structure of the steel under experimental conditions. Specifically, in order to save costs, the inert gas can be all nitrogen gas. The content and temperature of the hydrogen gas in the cooling gas can be further controlled, as shown in Table 2. During the cooling process of the bainite steel, the cooling capacity or cooling intensity can be controlled by controlling the pressure of the injected gas, the content of the hydrogen gas in the cooling gas, and the temperature of the cooling gas, and the specific values are determined according to the hardenability of the steel plate or strip. In the same embodiment, the hydrogen gas content in the cooling gas and the cooling gas temperature are generally not changed throughout the annealing process, and the cooling strength, cooling rate and the injection gas pressure are positively correlated. For example, in the slow cooling stage, in the embodiment 1, the cooling gas injection pressure is 0.6 kPa, the slow cooling stage cooling rate is 12.5 ° C / s, and in the rapid cooling stage, the first injection pressure of the cooling gas is 1 kPa, and the cooling rate is 19.2 ° C / s. In different embodiments, the cooling capacity and cooling rate are related to the cooling gas injection pressure, the hydrogen gas content in the cooling gas, and the cooling gas temperature. The higher the hydrogen gas content in the cooling gas, the lower the cooling gas temperature, and the higher the cooling gas injection pressure, the stronger the cooling capacity and the faster the cooling rate. For example, in the embodiment 7 and the embodiment 9, the cooling gas temperature is the same, but the hydrogen gas content in the cooling gas of the embodiment 9 is higher and the cooling gas injection pressure is higher, so the cooling capacity and cooling rate are also higher.
[0060] Specifically, the quenching temperature and quenching rate of the reaction in this stage are both controlled to make the steel plate or strip enter the bainite phase region in this stage. If the temperature is too high or too low, sufficient bainite cannot be formed in the steel plate or strip. The quenching rate is controlled to 10*Q~20*Q℃ / s in order to make the quenching rate as close as possible to the nose region of the CCT curve of the bainite phase region, so that the bainite transformation is more complete and faster. From the initial smelting stage to the long production process, it is inevitable that the steel plate or strip will have non-uniform composition and structure in some regions, and in some regions the carbon equivalent will be too low or the austenite will be undercooled to a small extent, and in some regions the carbon equivalent will be too high or the austenite will be undercooled to a large extent. If the cooling rate is below the set range, the cooling rate is too slow in regions with low carbon equivalent or low austenite undercooling, resulting in the transition to the pearlite phase, or the bainite transition rate is too slow, resulting in insufficient transition. Similarly, if the cooling rate is higher than the set range, regions with low carbon equivalent or high austenite undercooling will avoid the bainite phase and transition to the martensite phase, or the bainite transition rate will be too slow, resulting in insufficient transition. All of these factors lead to failure to form a gradient structure through the thickness.
[0061] Among all the factors that affect the progress of the quenching stage, the injection pressure of the cooling gas onto the steel plate or strip surface is the most important. First, the pressure is controlled to 0.3*Q~1.5*QkPa and held for 1~7 seconds to form an acicular bainite layer in the thickness direction of the steel plate or strip other than the core region, and these regions release the transformation latent heat during the bainite phase transformation, and the temperature of the core region in the thickness direction of the strip is higher than that of the surface layer and the sub-surface layer, which prepares the core region for the formation of blocky bainite. At this time, if the cooling gas injection pressure or holding time is lower than the set range, it is unfavorable to the formation of acicular bainite in the surface layer and the sub-surface layer, and if the injection pressure or holding time is higher than the set range, the cooling capacity is too strong, and acicular bainite is also formed in the core region in the thickness direction of the strip, making it impossible to form a gradient structure in the thickness direction. After that, the injection pressure is further reduced to 0.08*Q~0.2*QkPa and maintained for 5~10 seconds, so that the surface and subsurface layers can still be effectively cooled, and acicular bainite can be continuously formed, and due to the reduction in the cooling gas pressure and the release of the transformation latent heat of the surface and subsurface layers, the temperature of the core region in the thickness direction of the steel strip does not decrease further or increases slightly, and blocky bainite is formed in the core of the steel strip. Finally, a steel plate or strip with a structure gradient in the thickness direction is formed.
[0062] After the quenching step is completed, a controlled cooling step needs to be further carried out to obtain a bainite steel having a three- or five-layer structure gradient in the thickness direction. In the controlled cooling step, the controlled cooling rate is ≦Q°C / s, the controlled cooling time is 100-200 seconds, and the controlled cooling temperature of the bainite steel is ≧350°C when the controlled cooling step is completed. In one embodiment, the temperature of the bainite steel is 350-410°C when the controlled cooling step is completed.
[0063] By controlling the cooling of the steel plate or strip for a long time, the phase transformation of each bainite is sufficiently completed, and the structure is formed slowly and stably under the set temperature, and a steel plate or strip having a structure gradient in the thickness direction is formed. At this stage, if the controlled cooling rate exceeds the set value or the controlled cooling temperature of the final steel plate or strip is lower than the set value, martensite will be formed in the structure, which will deteriorate the forming performance of the steel plate or strip.
[0064] After the controlled cooling phase is over, the bainitic steel is air-cooled to room temperature. A steel plate or strip with a structure gradient through the thickness is obtained. The air-cooling phase does not affect the structure of the bainitic steel.
[0065] As described above, in one embodiment of the present invention, in order to obtain a bainite steel having a five-layer structure gradient, by changing the cooling parameters in the controlled slow cooling stage, a multi-phase layer is formed in the surface layer on top of the conventional three-layer gradient structure, and a steel plate or strip having a five-layer structure gradient in the thickness direction can be obtained. After that, through further quenching and controlled cooling stages, acicular bainite or blocky bainite is similarly generated in other regions of the bainite steel at different positions in the thickness direction. Finally, a multi-phase layer containing ferrite is formed in the surface layer, an acicular layer in the shallow surface layer, and a blocky layer in the core, resulting in a five-layer structure steel plate or strip having a structure gradient.
[0066] The beneficial effects of the present invention are as follows: 1. The present invention provides a rational elemental composition design for bainite steel, in particular by rationally controlling the contents of C, Si, Mn, and B in the steel, and rationally controlling the contents of C, Cr, Mo, and Mn in the steel, thereby optimizing the hardenability of the steel, and the steel spontaneously forms a phase with a structural gradient during the manufacturing process, thereby improving the strength and formability of the bainite steel.
[0067] 2. The present invention discloses a method for producing bainite steel, and by designing a detailed annealing process, especially by controlling the cooling gas pressure and temperature during the cooling stage, the steel plate / strip with suitable chemical composition will spontaneously form a three-layer or five-layer structure gradient under the annealing conditions of the present invention. The bainite steel obtained by the technical solution of the present invention has a tensile strength of ≥ 1000 MPa, a yield strength of ≥ 800 MPa, a hole expansion ratio of ≥ 40%, and a fracture elongation of ≥ 12%. [Brief description of the drawings]
[0068] [Figure 1] FIG. 1 is a schematic diagram of a steel strip having a three-layer structure in the thickness direction in an embodiment of the present invention. [Diagram 2]FIG. 2 is a schematic diagram of a steel strip having a five-layer structure in the thickness direction in an embodiment of the present invention. [Diagram 3] FIG. 3 is a metallographic photograph of the transition between the acicular layer (top) and the multi-phase layer (bottom) in Example 7 of the present invention. [Figure 4] FIG. 4 is a metallographic photograph of the transition between the acicular layer (upper part) and the lumpy layer (lower part) in Example 1 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0069] Hereinafter, the embodiments of the present invention will be described with reference to certain specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed herein. The present invention will be described in conjunction with a preferred embodiment, but this does not mean that the features of the present invention are limited to this embodiment only. On the contrary, the purpose of describing the present invention in conjunction with the embodiment is to cover other options and modifications that may be extended based on the claims of the present invention. Indeed, the purpose of introducing the invention in conjunction with the embodiment is to cover other options and modifications that may be obtained based on the claims of the present invention. In order to provide a deeper insight into the present invention, the following description includes numerous specific details. The present invention can be practiced without these details. In addition, some specific details are omitted from the description to avoid obscuring the focus of the present invention. Unless inconsistent, the embodiments of the present invention and the features in the embodiments can be combined with each other.
[0070] Examples 1 to 14 and Comparative Examples 1 to 6 In the present invention, the bainite steels of Examples 1 to 14 were produced by the following process: Process 1, smelting and casting; Step 2, hot rolling: the heating temperature is 1100-1230°C, the finish rolling start temperature is 1050-1180°C, and the finish rolling end temperature is 870-930°C; Step 3, cooling after rolling and coiling: the cooling rate is 30-150°C / s, and the coiling temperature is 540-620°C; Step 4: Remove oxide scale by pickling; Step 5, cold rolling: cold rolling reduction rate is ≧30% to achieve the required target thickness. Specifically, in the embodiment of the present invention, the thickness of the steel sheet or strip after cold rolling is ≦2.2 mm; Step 6: Annealing.
[0071] The bainite steels of Comparative Examples 1 to 6 were also produced by the processes of smelting, continuous casting, hot rolling, cooling and coiling after rolling, pickling, cold rolling, and annealing, and the chemical components of the steels and the parameters of the production process are shown in Tables 1 and 2.
[0072] Table 1 shows the mass percentages of each chemical element in the bainitic steels of Examples 1-14 and Comparative Examples 1-3.
[0073] Table 2 shows specific parameters of the bainite steels of Examples 1-14 and the comparative steels of Comparative Examples 1-6.
[0074] [Table 1]
[0075] [Table 2-1]
[0076] [Table 2-2]
[0077] In Examples 1 to 5, 8, 10 to 11, a structure having three layers in the thickness direction was obtained, and the upper and lower surface layers were both acicular layers, and the core part was a lumpy layer. In Examples 6 to 7, 9, 12 to 14, a structure having five layers in the thickness direction was obtained, and the upper and lower surface layers were both multi-phase layers, the upper surface layer and the lower surface layer were acicular layers, and the core part was a lumpy layer. In the structure of the bainite steel of the present application, the hardness of the acicular layer was the highest, the hardness of the multi-phase layer was the lowest, and the hardness of the lumpy layer was between the acicular layer and the multi-phase layer. Therefore, in the three-layer composite material, the acicular layers of the upper and lower surface layers give the material high surface hardness and surface yield strength, and the central lumpy layer also gives the material high toughness and plasticity, so that it is suitable for automotive parts that require surface hardness or fatigue limit and at the same time toughness and plasticity of the entire material, such as automotive seat rails, drive shafts, and other structural components. In addition, in the five-layer composite material, the upper and lower surface layers have relatively soft multi-phase layers that give the surface layers good local formability, and the adjacent hard acicular layer and core block layer also give the material high strength and good toughness, making it suitable for manufacturing parts that require strength and overall formability, such as control arms and triangular arms of automobile chassis.
[0078] In Comparative Examples 1 to 3, the composition design deviated from the invention, and a steel plate or strip having a structure with a gradient in the thickness direction was not obtained. In Comparative Example 1, the R value was too high, and only a pure blocky layer structure was obtained, and in Comparative Examples 2 to 3, the R value was too low, and only a pure acicular layer structure was obtained. In Comparative Examples 4 to 6, steel type A was used, and although the composition design met the conditions, the annealing process in the manufacturing process deviated from the invention, and a steel plate or strip having a structure with a gradient in the thickness direction was not obtained. However, in Comparative Example 4, the cooling gas pressure in the slow cooling stage exceeded the design value, so a large proportion of ferrite was formed in the thickness direction of the steel plate or strip, and even in the rapid cooling stage, the cooling gas pressure exceeded the design value, so acicular bainite was formed in the thickness direction of the steel plate or strip, and blocky bainite could not be formed. In addition, since a large proportion of ferrite was preferentially formed in the steel plate or strip, carbon gathered in the partially supercooled austenite, preventing bainite transformation and finally transforming into new martensite in the air-cooling stage, so that a structure with a gradient in the thickness direction of the steel plate or strip could not be formed and formability was poor. In Comparative Example 5, the cooling gas pressure in the quenching stage exceeded the design value, so only a pure acicular bainite structure was obtained, and in Comparative Example 6, the cooling gas pressure in the quenching stage did not reach the design value, so only a pure blocky layer structure was obtained.
[0079] Figure 3 shows the lower surface layer region of Example 7 of the present invention, specifically a photograph (scanning electron microscope) of the metallographic structure of the transition position between the acicular layer (upper part) and the multi-phase layer (lower part). In the upper part of the figure, i.e., the region close to the core, the structure is typical acicular bainite, which means that the acicular layer begins in that region. In the lower part of the figure, i.e., the region close to the lower surface, polygonal ferrite, acicular bainite, and dispersed precipitated nano-order, sub-micro-order, or micro-order granular carbide precipitate phases are included, which means that the surface layer begins in that region.
[0080] Figure 4 shows the region near the upper surface layer in the core of Example 1 of the present invention, specifically a photograph (scanning electron microscopy) of the metallographic structure of the transition position between the acicular layer (upper part) and the massive layer (lower part). In the upper part of the figure, i.e., the region near the upper surface, a large amount of typical acicular bainite is contained in the structure, which means that the acicular layer is formed in that region. In the lower part of the figure, i.e., the region near the core, a large amount of bainite transforms into the morphology of massive polygons, which means that a large amount of massive bainite is formed in that region, which means that the lumpy layer is formed in that region.
[0081] Table 3 shows the results of mechanical property measurement of the bainite steel of Examples 1 to 14 and Comparative Examples 1 to 6. A horizontal JIS 5# tensile test piece was taken to measure the yield strength, tensile strength, and fracture elongation of the steel material, and GB / T 228.1-2010 "Tensile test of metallic materials Part 1: Room temperature test method" was adopted as the test method. The center of the steel plate was taken to measure the hole expansion ratio of the steel. The hole expansion ratio was measured by a hole expansion test, in which a sample with a hole in the center was pressed into a female die by a male die, and the center hole of the sample was expanded until necking or through cracks appeared at the edge of the plate hole. Since the method of making the initial hole in the center of the sample and the quality of the corresponding initial hole edge have a large effect on the measurement result of the hole expansion ratio, the test and measurement method were performed by the hole expansion ratio measurement method specified in the ISO / DIS16630 standard, and the central initial hole was made by a primary punch blanking hole punching method (corresponding to the processing method with the worst quality of the initial hole edge). Therefore, if the central start hole is formed by secondary punch blanking hole punching type, or drilled or reamed hole type, the corresponding hole expansion ratio is increased by 20% based on the values shown in the table. If the central start hole is formed by wire cutting, the corresponding hole expansion ratio is increased by 50% based on the values shown in the table. If the central start hole is formed by laser blanking, the corresponding hole expansion ratio is increased by 80% based on the values shown in the table.
[0082] [Table 3]
[0083] As can be seen from Table 3, when the components and processes of the steel plate or strip meet the design, all examples have mechanical properties of yield strength ≧800MPa, tensile strength ≧1000MPa, fracture elongation ≧12%, and hole expansion ratio ≧40%. In addition, a structure with a gradient in the thickness direction of the steel plate or strip is formed, so the material has good comprehensive formability, and both the tensile ductility and hole expansion flangeability are good, and the fracture elongation and hole expansion ratio are both high, with (fracture elongation * 10 + hole expansion ratio) ≧ 170% in all examples.
[0084] When the components or process do not meet the design, ideal mechanical properties cannot be obtained. For example, in Comparative Example 1, the C and Mn contents are below the lower limit, so the strength of the material is low. In Comparative Example 2, the C content exceeds the upper limit, so the strength of the material is too high and the formability is extremely poor. In Comparative Example 3, the R value is below the lower limit of the design, so the core lumpy layer cannot be formed in the steel plate or strip, and the entire structure becomes acicular bainite, and although the hole expansion ratio is extremely high, the fracture elongation is poor. Comparative Example 5 is similar, and since the process does not meet the design (as described above), the entire structure also becomes acicular bainite, and although the hole expansion ratio is extremely high, the fracture elongation is poor. In both of these two sets of comparative examples, the formability is "biased", so the overall formability is poor (fracture elongation * 10 + hole expansion ratio) < 170%. In Comparative Examples 4 and 6, the process did not satisfy the design (as described above), so a structure with a gradient in the thickness direction could not be formed, and the formability was "biased," resulting in poor overall formability (elongation at break * 10 + hole expansion ratio) < 170%.
[0085] The combination manner of each technical feature in this application is not limited to the combination manner described in the claims or the combination manner described in the specific examples, and all technical features described in this application may be freely combined or combined in any manner as long as they are not inconsistent with each other.
[0086] Furthermore, it should be noted that the above-mentioned embodiments are merely specific embodiments of the present invention, and the present invention is not limited to the above-mentioned embodiments, and similar changes and modifications thereof can be directly obtained or easily conceived by those skilled in the art from the disclosure of the present invention, and therefore, they are within the protection scope of the present invention.
Claims
1. Bainite steel containing the following chemical components in mass percent: C: 0.10-0.19%, Si: 0.05-0.45%, Mn: 1.5-2.2%, B: 0.001-0.0035%, Al: 0.01-0.05%, Cr; 0.05-0.40%, Mo: 0.05-0.40%, Fe≧90%.
2. The bainitic steel according to claim 1, further comprising at least one of Ti and Nb, Nb≦0.1%, Ti≦0.15%.
3. Bainite steel containing the following chemical components in mass percent: C: 0.10-0.19%, Si: 0.05-0.45%, Mn: 1.5-2.2%, B: 0.001-0.0035%, Al: 0.01-0.05%, Cr; 0.05-0.40%, Mo: 0.05-0.40%, with the balance being Fe and unavoidable impurities.
4. The bainite steel according to claim 3, wherein the unavoidable impurities are P≦0.015% and S≦0.004%.
5. 4. The bainite steel according to claim 1 or 3, in which the mass percentages of the chemical elements satisfy the relationship R=(Mn+Si) / (12*C+160*B), with the proviso that 0.9≦R≦1.2, the numerical values before the percent sign of the mass percentages of the elements being applied in the calculations.
6. 6. The bainitic steel according to claim 5, in which the mass percentages of the chemical elements satisfy the relationship Q=(C+Cr+Mo+Mn / 2) / R, with the proviso that 1.15≦Q≦1.5, the numerical values before the percent sign of the mass percentages of the elements being applied in the calculations.
7. 4. The bainite steel according to claim 1 or 3, wherein the bainite steel has a two-layer surface layer structure and a single layer core structure, the core structure being between the two surface layer structures.
8. 8. The bainite steel according to claim 7, wherein in the bainite steel, the volume of the core structure occupies 20% to 50% of the volume of the bainite steel, and the remainder is the surface layer structure.
9. The bainite steel according to claim 7, wherein the surface layer structure includes acicular bainite and granular carbide precipitates, and the core structure includes blocky bainite and granular carbide precipitates.
10. The bainite steel according to claim 9, wherein the acicular bainite and granular carbide precipitate phases occupy 99% or more of the surface layer structure volume, and the blocky bainite and granular carbide precipitate phases occupy 99% or more of the core structure volume.
11. 8. The bainite steel according to claim 7, further comprising two multi-phase layers, the two surface layer structures and the one core structure forming an intermediate layer, the intermediate layer being between the two multi-phase layers.
12. The bainite steel according to claim 11, wherein in the bainite steel, the volume of the multi-phase layer occupies 2% to 10% of the volume of the bainite steel, and the remainder is the intermediate layer structure.
13. 12. The bainite steel of claim 11, wherein the multi-phase layer comprises polygonal ferrite, acicular bainite and granular carbide precipitates, the polygonal ferrite occupying 50% or less of the multi-phase layer volume, and the polygonal ferrite, acicular bainite and granular carbide precipitates collectively occupying 99% or more of the multi-phase layer volume.
14. The bainite steel according to any one of claims 1 to 13, wherein the bainite steel has a tensile strength ≧1000 MPa, a yield strength ≧800 MPa, a hole expansion ratio ≧40%, and a fracture elongation ≧12%.
15. A method for producing a bainite steel according to any one of claims 1 to 14, comprising the steps of: Smelting and foundry; Hot rolling; Post-rolling cooling and coiling; Pickling and cold rolling; Annealing.
16. The method for producing a bainite steel according to claim 15, wherein the annealing step includes a heating step, a slow cooling step, a quenching step, a controlled cooling step, and an air cooling step, in that order, and the controlled cooling rate is such that the cooling rate in the controlled cooling step is less than the cooling rate in the slow cooling step and less than the cooling rate in the quenching step.
17. 17. The method for producing a bainite steel according to claim 16, wherein in the slow cooling stage, the steel is cooled to a slow cooling temperature of 720-800°C at a slow cooling rate of Q-10*Q°C / s, and the mass percentages of the chemical elements satisfy Q=(C+Cr+Mo+Mn / 2) / R, 1.15≦Q≦1.5, R=(Mn+Si) / (12*C+160*B), 0.9≦R≦1.2, and each chemical element in the formula is assigned the numerical value before the percent sign of the mass percentage content of the chemical element.
18. The method for producing bainite steel according to claim 17, wherein cooling is performed by injecting a cooling gas onto a surface of the bainite steel, the injection pressure of the cooling gas is 0.2*Q to Q kPa, and the holding time of the cooling gas injection is 5 to 20 seconds.
19. 17. The method for producing a bainite steel according to claim 16, wherein in the slow cooling stage, the steel is cooled to a slow cooling temperature of 620-700°C at a slow cooling rate of Q-10*Q°C / s, and the mass percentages of the chemical elements satisfy Q=(C+Cr+Mo+Mn / 2) / R, 1.15≦Q≦1.5, R=(Mn+Si) / (12*C+160*B), 0.9≦R≦1.2, and each chemical element in the formula is assigned the numerical value before the percent sign of the mass percentage content of the chemical element.
20. 20. The method for producing bainite steel according to claim 19, wherein cooling is performed by injecting a cooling gas onto a surface of the bainite steel, the injection pressure of the cooling gas is 0.05*Q to 0.15*Q kPa, and the holding time of the cooling gas injection is 5 to 15 seconds.
21. The method for producing a bainite steel according to claim 17 or 19, wherein in the quenching step, the steel is cooled to a quenching temperature of 400 to 540°C at a quenching rate of 10*Q to 20*Q°C / s.
22. 22. The method for producing bainite steel according to claim 21, wherein cooling is performed by injecting cooling gas onto a surface of the bainite steel twice, a first injection pressure of the cooling gas is 0.3*Q to 1.5*Q kPa, a first holding time of the cooling gas is 1 to 7 seconds, a second injection pressure of the cooling gas is 0.08*Q to 0.2*Q kPa, and a second holding time of the cooling gas is 5 to 10 seconds.
23. 23. The method for producing a bainite steel according to claim 18, 20 or 22, wherein the cooling gas is a mixture of a reducing gas and an inert gas, the reducing gas is hydrogen gas and its volume fraction is 1% to 8%, and the temperature of the cooling gas is 5 to 50°C.
24. 17. The method for producing a bainite steel according to claim 16, wherein in the controlled cooling stage, a controlled cooling rate≦Q° C. / s and a controlled cooling time are 100 to 200 seconds, and at the end of the controlled cooling stage, a controlled cooling temperature of the bainite steel is ≧350° C.
25. The method for producing a bainite steel according to claim 16, wherein in the heating step, the steel is heated to a soaking temperature of 840-950°C at a heating rate of ≦50°C / s, and then kept at that temperature for a holding time of 60-180 seconds.
26. 16. The method for producing bainite steel according to claim 15, wherein the parameters of the method satisfy any one of the following: In the hot rolling process, the heating temperature is 1100 to 1230°C, the finish rolling start temperature is 1050 to 1180°C, and the finish rolling end temperature is 870 to 930°C; In the post-rolling cooling and coiling process, the cooling rate is 30 to 150° C. / s and the coiling temperature is 540 to 620° C.; In the cold rolling step, the cold rolling reduction is ≧30%.
Citation Information
Patent Citations
550Mpa yield-strength low-carbon bainitic steel for engineering machinery and preparation method thereof
CN102162065A
Ultrahigh-strength bainitic steel and manufacture method thereof
CN102251170A
Ultrahigh-strength steel plate steel plate with yield strength of 960MPa-level, and manufacturing method thereof
CN103233183A
Heat treatment method for tricone bit claw
CN103352111A
Mo-v type ultrahigh tensile strength resistance welded steel tube excellent in ductility
JP1993287439A