Methods for optimizing the roughness of lamination cylinders by high velocity thermal spraying.

The method optimizes the roughness and coating thickness of working mill rolls through high velocity thermal spraying with controlled particle distribution and spray parameters, enhancing the service life and reducing defects in metal sheets or coils during rolling processes.

JP2024535933AInactive Publication Date: 2024-10-02MECANIZACION IND ASTILLERO SA +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024520527
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-04
Filing Date
2022-10-03
Publication Date
2024-10-02
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing high speed thermal spray technologies fail to effectively control the roughness and coating thickness of working mill rolls, leading to issues such as increased friction, wear, and defects in metal sheets or coils during rolling processes, which affect the service life and quality of the products.

Method used

A method involving high velocity thermal spraying with controlled particle size distribution and spray parameters to achieve isotropic roughness (Ra) and uniform coating thickness, using HVOF or HVAF spraying with fine hard particles and a binder, optimizing the rotational and translational speeds to ensure uniform coating application.

Benefits of technology

The method enhances the service life of working mill rolls by maintaining consistent roughness and reducing friction, thereby improving the quality and reducing defects in metal sheets or coils, extending the rolling process duration by up to 1.5-2 times compared to chrome-plated rolls.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024535933000001_ABST
    Figure 2024535933000001_ABST
Patent Text Reader

Abstract

The present invention relates to a method for coating a cylinder by thermal spraying of powder using a spray column to form an isotropic roughness (Ra) on the surface of the cylinder, the cylinder rotates around its longitudinal axis at a speed (Vr) and the spray column translates at a speed (Vt) to deposit material in a spiral manner. After setting the particle size distribution (G) of the powder to be sprayed, the target roughness (Ra) of the coating, and the target thickness (t), the corresponding powder feed flow rate (Fr) is determined according to a predefined formula in an empirical table showing the target roughness (Ra) based on the feed flow rate (Fr) and the particle size distribution (G), and then the rotation speed (Vr) and translation speed (Vt) are defined from the equation for the target coating thickness (t) as a function of the defined feed flow rate (Fr), translation speed (Vt), and rotation speed (Vr).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a specifically designed method for producing and optimizing the roughness of coated working rolls using high velocity thermal spray technology.

[0002] These working rolls can be used in hot or cold rolling mills to produce metal sheet or coils. [Background technology]

[0003] Improving the service life of working rolls in hot and cold rolling mills is one of the primary ways to reduce a steel manufacturer's operating costs.

[0004] In order to increase the service life of working mill rolls compared to traditional solutions such as chrome plating, the hardness of the coating needs to be increased, which can be achieved by coatings containing carbide particles in a metal matrix.

[0005] These coatings are deposited on the surface of the working rolls by high velocity thermal spraying. The type of hard particles sprayed and the thickness of the coating significantly affect the service life of the working rolls.

[0006] According to standard working rolls, due to process limitations and to avoid strip defects, the roughness of the roll needs to be uniform along the length of the roll and needs to meet requirements in terms of average roughness and standard deviation.

[0007] Due to the fact that high velocity thermal spray technology has not been developed to control roughness, challenges arise in ensuring that both: - the thickness of the coating, which ensures the service life of the working rolls; ·Target roughness.

[0008] Regarding the importance of the roughness on the surface of the rolling rolls, it is worth emphasizing the following: The roughness of the rolling rolls decreases during rolling due to wear caused by friction between the strip and the rolling rolls. As the roughness increases, the coefficient of friction increases, and for the same roughness, the number of peaks increases, so does the coefficient of friction [1]. If the coefficient of friction is too low, the strip may slip / skid on the rolling rolls, which may cause defects or limit thickness reduction during rolling [2], whereas if the coefficient of friction is too high, the wear of the rolling rolls on the strip increases and the contamination of the strip with iron fines increases [1]. This is the case for cracks on the strip edges, which are usually found in reversing rolling mills. In this case, it is well known that edge cracks are sensitive to the coefficient of friction. With increasing friction, the defects increase [3]. The roughness of the strip affects the properties, quality and performance of the strip itself. To ensure good behavior during pressing, as in the case of skin-pass mills, the roughness of the strip needs to be high enough to avoid cracks in the material. The roughness of the strip is transferred from the roughness of the working rolls. The higher the roughness of the working rolls, the higher the roughness of the laminated strip. The rolling force and the strip tension affect the behavior of the roughness transfer. Therefore, knowing the roughness required for the strip, the roughness of the working rolls is defined. Depending on the rolling process conditions and the target roughness of the strip, the steel manufacturer defines the roughness of the rolling rolls.

[0009] This patent presents a solution and methodology to achieve uniform roughness in response to customer demands.

[0010] In this sense, the terminology used in the present invention is introduced.

[0011] Ra is defined as the arithmetic mean deviation of the roughness profile. The calculation is done according to ISO standard 4287, with a cut-off of 0.8 mm.

[0012] RPC is defined as the number of peaks per unit of length in centimeters. Calculations are done according to ISO standard 4287, with a strip width of 1 micrometer.

[0013] With respect to the rolls used in the cold rolling process, it should be noted that the working rolls used in the cold rolling mill provide different types of surface finishes.

[0014] Standard values ​​for the texture of working rolls are given in Table 1.

[0015] [Table 1]

[0016] Regarding the progression of the roughness during rolling, it is worth emphasizing the following: During the rolling motion, the roughness of the working rolls decreases due to wear caused by friction between the strip and the rolls. The use of coatings such as chrome retards this phenomenon. See Figure 2. The reduction in roughness also depends on the type of texture used in the mill rolls, see Figure 3. Because the initial roughness of the rolling rolls is slightly higher than the roughness at the end of the rolling motion, steelmakers regularly monitor the roughness of the rolling rolls to prevent it from deviating from the range required to ensure quality on the surface of the strip. When the roughness is too low, the rolling rolls are changed.

[0017] Furthermore, with regard to texturing techniques, the following is worth emphasizing:

[0018] Currently, several texturing techniques exist that produce roughness on the surface of working rolls. i.Shot Blasting (SBT): Steel or cast iron shot has a specific particle size distribution and is sprayed onto the surface of the working mill roll. The kinetic energy of the particles is sufficient to produce a plastic deformation of the surface. The resulting roughness is a function of the mass and size of the shot, the speed of the shot, the hardness of the substrate of the mill roll, the number of passes along the mill roll, and the rotational speed of the mill roll. ii. Electric Discharge Texturing (EDT): A voltage applied between a rolling roll (cathode) and a copper electrode (anode), separated by a dielectric medium, generates an electrical discharge capable of producing craters on the surface of the rolling roll. The roughness is a function of the frequency, the voltage applied to the electrodes of the electronics, and the level of capacitance. This technique is rarely used in cold rolling, where the reduction index is high, since it is very sensitive to the wear of the rolling roll. Today, this texture is the standard for skin pass mills and temper mills. iii. Laser Texturing (LT): The laser light strikes the surface of the rolling roll, melting the material and releasing gas (O 2 , CO 2 The material is expelled out of the craters produced by the aid of a laser (Ar, or Ar). The final texture of the rolling roll corresponds to a uniform distribution of craters along a helical pitch over the circumference of the working roll. The axial distance of the craters is controlled by the speed of the longitudinal movement of the rolling roll. In the tangential direction, the distance of the craters is determined by both the speed of the rolling roll and the speed of the mechanical shutter. The depth of the craters is determined by the power of the laser. This technique is not very commonly used today. iv. Electron Beam Texturing (EBT) This technique involves impinging an electron beam on the surface of a rolling roll. During a single shot, a lens focuses the beam to preheat the material of the rolling roll, which then impinges the surface with a first flame, creating a crater, and then heating the rim around the crater. This cycle can be done two or three times at the same location to create a deeper crater. During the firing cycle, the beam is deflected to compensate for the continuous motion (displacement and rotation) of the surface of the rolling roll. This technique is only occasionally used for skin pass mills, and is now less commonly used.

[0019] These different techniques are illustrated in FIG.

[0020] With regard to coatings using high velocity thermal spraying, it is worth emphasizing the following: Thermal spraying is a coating process in which a molten material is sprayed onto a surface. A mixture of gases is burned in a combustion chamber, heating and accelerating the powder and depositing it onto the substrate. When the combustion gas is oxygen, thermal spraying is called HVOF. When the combustion gas is air, thermal spraying is called HVAF. To increase the service life, rolling mill rolls are coated with a tungsten carbide alloy, usually a single layer, with a thickness of 0.003mm-0.020mm, affecting 100% of the workpiece surface. The alloy is preferably selected from WC-CoCr, WC-NiCr, WC-Co, WC-Ni or WC-CrC-Ni. Preferably, the permeability of the coating ranges from 0% to 0.1%. The coating layer has a final hardness comprised between 1000Hv and 1600Hv. WO 2021148690 describes the use of tungsten carbide coatings for cold rolling mill rolls for HVAF technology. [Prior art documents] [Patent documents]

[0021]

Patent Document 1

Patent Document 2

Non-Patent Document

[0022]

Non-Patent Document 1

Non-Patent Document 2

Non-Patent Document 3

Non-Patent Document 4

[0023] The method proposed in the present invention solves the above mentioned problems quite satisfactorily.

[0024] To achieve that object, and more specifically, the method of the present invention comprises a method for coating a roll by high velocity spraying, more specifically by spraying a powder using a spray column, to form an isotropic roughness (Ra) on the surface of said roll, the roll rotating around its longitudinal axis with a speed (Vr) and a spray cone translating parallel to the axis of the roll with a speed (Vt) to deposit material following a helical shape, in which the following operating phases (a) to (d) are set up: a) setting the particle size distribution (G) of the powder to be sprayed; b) setting the target roughness (Ra) and target thickness (t) of the coating; c) finding the corresponding powder feed flow rate (Fr) from an empirical table showing the target roughness (Ra) based on the feed flow rate (Fr) and particle size distribution (G) according to the following formula:

[0025]

number

[0026]

number

[0027] The thermal spray process can be HVOF or HVAF spray.

[0028] The spray powder then contains hard particles with dimensions less than 1 μm, and the target final roughness (Ra) is determined by the average particle size distribution (G) of the powder.

[0029] At the same time, the number of peaks (RPc) on the surface of the coating must not exceed a value related to the roughness (Ra).

[0030] To complement the description given below and to facilitate a deeper understanding of the characteristics of the present invention, a set of drawings is attached as an integral part of said description, according to a preferred practical embodiment of the invention, and is referred to below with exemplary and non-limiting characters. [Brief description of the drawings]

[0031] [Figure 1] Below is an illustration of the different texturing techniques that currently exist: (1) Shot blasting (SBT). Stochastic coating. (2-2') Electric discharge texturing (EDT). Stochastic coating. (3) Laser texturing (LT). Deterministic coating. (4) Electron beam texturing (EBT). Deterministic coating. (5) Chromium deposition texturing (TST). Nodular coating. (6) HVAF thermal spray coating. Stochastic coating. [Diagram 2] Figure 1 shows a graph of the evolution of roughness during the rolling process and how the use of a coating such as chrome plating retards the wear caused by friction between the strip and the rolls. The y-axis represents the surface roughness in microns, the x-axis is the length of the strip in kilometers, and the lower curve represents the behavior of a forged steel roll with 5% chrome (uncoated roll) whilst the upper curve represents the behavior of rolls with an electrolytic coating of chrome or silver chrome. [Diagram 3] 1 shows a graph illustrating the reduction in roughness as a function of the layup tonnage of the steel sheet depending on the type of texture used in the rolling rolls, specifically for four different textures. [Figure 4] A schematic diagram of the method of the invention is shown in which a mill roll (7) rotates at a controlled speed about its longitudinal axis (8) and a spray cone translates parallel to the axis of the mill roll to deposit material following a helical shape (10). [Diagram 5] 1 shows a graph of the progression of the arithmetic mean deviation of the roughness profile as a function of the number of peaks per unit length (in centimeters), the upper curve corresponding to the maximum peak ratio and the lower curve corresponding to the minimum peak ratio. [Figure 6] 5 shows a graph similar to that of FIG. 5, but corresponding to a comparison between a curve for a process without additional treatment and a curve corresponding to additional treatment to reduce roughness peaks below 2 microns. [Figure 6.1]Shown is a profile cut of a coating for measuring the number of peaks and, in particular, a relief made using a tool for this purpose. The y-axis shows the magnitude of the peaks in microns (both peaks and valleys are considered peaks), while the x-axis represents the length of the profile in microns. Shown is a profile without additional processing. [Figure 6.2] Shown is a profile cut of a coating to measure the number of peaks, and in particular a relief made using a tool for this purpose. The y-axis shows the peak size in microns (both peaks and valleys are considered peaks), while the x-axis represents the profile length in microns. Shown is an extreme case where all peaks above 0.25 microns of the coating thickness tracked in a particular case have been removed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0032] In accordance with the method of the present invention, the following instructions are provided for controlling roughness. - For thermal spray coatings, the thickness (t) is closely related to the powder feed rate (Fr), which in turn is closely related to the tangential velocity of the piece (Vr) and the transverse velocity of the gun (Vt) according to the following equation:

[0033]

number

[0034]

number

[0035] For your convenience, use the table explained below.

[0036] Ra(μm) as a function of powder feed rate and particle size distribution - HVAF process

[0037] [Table 2]

[0038] Ra(μm) as a function of powder feed rate and particle size distribution in HVOF process

[0039] [Table 3]

[0040] For clarity, the powder comprises fine hard particles (such as WC) and a binder (usually a soft metal). This means that the particle size distribution of the powder is larger than the diameter of the hard particles. The granulation of the powder may contain two or more hard particles.

[0041] Regarding steps for controlling roughness, the following a) to c) can be mentioned. a) defining the particle size distribution of the powder; b) determining the particle size distribution and target roughness of the powder, and the powder supply flow rate is defined as in Table 2 or Table 3; c) Knowing the powder feed rate and target thickness, where the values ​​of Vr and Vt are defined taking into account Equation 1 and represent d / p>1.

[0042] Table 4 describes the thermal spray according to the invention compared to the standard roughness.

[0043] Comparison of sprayed roughness with standard values ​​of probabilistic roughness

[0044] [Table 4]

[0045] Regarding the particle size distribution of the powder and the diameter of its hard particles, The steps required to control the fixed size coarseness of the spray powder are explained above. - In order to reach all the required roughness levels, the powder size must be adapted to handle the different roughness ranges according to Table 5.

[0046] Required powder particle size distribution

[0047] [Table 5] -It is known that the diameter of the hard particles can affect the final roughness of the high-speed spray coating. For example, in the specification of Patent No. 09300008, it is advised to apply a hard particle diameter of 1 to 20 μm so that a roughness of 0.3 to 3 μm is obtained. For example, if the diameter of the hard particles is 1 to 5 μm, a roughness of about 0.3 μm is obtained. - As the service life of the rolling roll increases, the duration of the rolling motion increases. If the diameter of the hard particles is too large, the roughness of the rolling roll also increases as the rolling progresses, which is due to the "wear" of the metal binder. To avoid this phenomenon, the diameter of the hard particles should be less than 1 μm.

[0048] Furthermore, with regard to managing the number of roughness peaks, it is worth emphasizing the following. - As mentioned above, for uncoated or chrome-plated rolls used in tandem or reversing mills, steel manufacturers have been using it to set the roughness to ensure strip quality (no edge contamination, no cracks, etc.), but there is no specific requirement regarding the number of peaks. -HVAF or HVOF coatings with hard particles significantly increase the service life of the rolling rolls. This means that the duration of the rolling movement is significantly increased. For standard durations of rolling movements (uncoated rolling rolls or chrome-plated rolling rolls), the control of the roughness is sufficient to avoid defects in the laminate strip. For coatings with hardnesses greater than 1000 Hv, tests show that in addition to the roughness, it is important to limit the level of the number of peaks. According to [2]%, the percentage of flat areas influences friction. One way to increase the contact surface would be to reduce the number of peaks and / or round them off. In order to make it possible to increase the service life of the rolling movement by a factor of 1.5 compared to chrome-plated rolls or by a factor of 2 compared to uncoated rolls without any quality problems occurring (cracks at the edges, contamination, etc.), the maximum number of peaks (RPc) must comply with the following formula:

[0049]

number

[0050] This surface treatment can be mechanical (shot blasting, polishing, etc.), chemical, electrochemical, or thermal (laser, etc.). These treatments reduce the roughness peaks. At the same time, the roughness and the total number of peaks are reduced (see Figure 6, Figure 6.1, and Figure 6.2). The method of reducing the peaks and roughness depends on the type of final treatment performed.

[0051] At the same time, the mill rolls must be pretreated by shot blasting for a roughness greater than 5 μm.

[0052] The references used in this application are the following [1] to [7]. [1]WORK ROLL ROUGHNESS TOPOGRAPHY AND STRIP CLEANLINESS DURING COLD ROLLING AUTOMOTIVE SHEET-Claude Gaspard,Daniel Cavalier,Stefan Wahlund-Technical contribution to the 11th International Rolling Conference,part of the ABM Week 2019,October 1st-3rd,2019,Sao Paulo,SP,Brazil. [2]RELATIONS BETWEEN FRICTION COEFFICIENT AND ROLL SURFACE PROFILES,ROLLED SHEET CHARACTERISTICS IN COLD ROLLING OF STEEL SHEETS-Hiroyasu YAMAMOTO,Mansaku SASAKI and Takahiro KITAMURA-Tetsu-to-Hagane Vol.95(2009)No.5. [3]THE RESEARCH ON EDGE CARCK OF COLD ROLLED THIN STRIP-Haibo Xie-2011-Thesis of university of Wollongong. [4]TEXTURING METHODS FOR COLD MILL WORK ROLLS-Bilal COLAK * ,Fatih BASOGLU+,Naci KURGAN-UDCS’19 Fourth International Iron and Steel Symposium,4-6 April,Karabuk. [5]EFFECT OF WORK ROLL TECHNOLOGY ON COLD MATERIALS ROLLING AND PROGRESS OF MANUFACTURING FUTURE DEVELOPMENTS IN JAPAN -Mitsuo HASHIMOTO,Taku TANAKA,Tsuyoshi INOUE,1)Masayuki YAMASHITA,2)Ryurou KURAHASHI3)and Ryozi TERAKADO4)-ISIJ International,Vol.42(2002),No.9,pp.982-989. [6]International Publication No. 2021148690 [7]Specification of Patent No. 09300008

Claims

1. 1. A method for optimizing the roughness of a rolling mill roll by high velocity spraying, more particularly by spraying of a powder using a spray column, to produce an isotropic roughness (Ra) on the surface of said rolling mill roll, said rolling mill roll rotating about its longitudinal axis with a speed (Vr) and a spray cone translating parallel to said axis of said rolling mill roll with a speed (Vt) to deposit material following a helical shape, with the following operating phases (a) to (d): a) setting the particle size distribution (G) of the powder to be sprayed; b) setting a target roughness (Ra) and a target thickness (t) of the coating; c) finding the corresponding powder feed flow rate (Fr) from an empirical table showing said target roughness (Ra) based on the feed flow rate (Fr) and particle size distribution (G) according to the following formula: [0010] η is the efficiency of the process, which depends on the type of equipment used, and A(G) and B(G) are functions of the particle size distribution (G) of the powder; d) defining a rotational speed (Vr) and a translational speed (Vt), which are defined from an equation relating a target coating thickness (t) as a function of the defined feed flow rate (Fr), the translational speed (Vt), and the rotational speed (Vr) according to the following formula: [0025] where N is the number of revolutions per minute of the rolling roll and ρ is the density of the spray powder, while the ratio of the width of the spray cone (d) to the pitch (p) per revolution of the screw is greater than 1; The method by which the

2. 2. The method for optimizing the roughness of rolling mill rolls by high velocity thermal spraying according to claim 1, characterized in that an empirical table is used to calculate the desired roughness (Ra) based on the powder particle size distribution (G) and the powder feed rate (Fr) using HVAF thermal spraying method. 【Table 1】

3. 2. The method for optimizing the roughness of rolling mill rolls by high velocity thermal spraying according to claim 1, characterized in that an empirical table is used to calculate the desired roughness (Ra) based on the powder particle size distribution (G) and the powder feed rate (Fr) using HVOF thermal spraying method. 【Table 2】

4. 2. The method for optimizing the roughness of rolling mill rolls by high velocity thermal spraying according to claim 1, characterized in that the spray powder comprises hard particles with dimensions less than 1 μm and the target final roughness (Ra) is determined by the average particle size distribution (G) of the powder according to the following rules: 【Table 3】

5. 2. A method for optimizing the roughness of rolling mill rolls by high velocity thermal spraying according to claim 1, characterized in that the number of peaks (RPc) of the coating surface does not exceed a value related to the roughness (Ra) according to the following formula: [0030]

6. 4. Method for optimizing the roughness of rolling mill rolls by high velocity thermal spraying according to claims 1 and 3, characterized in that the number of peaks (RPc) is obtained by an additional surface treatment step by reducing the height and number of peaks by mechanical, thermal, chemical or electrochemical ablation / removal for roughnesses below 2 μm.

Citation Information

Patent Citations

  • Thermal spraying coating method for metallic columnar body

    JP1997248606A

  • Roll for skin pass rolling of plate

    JP1997300008A

  • Thermal spraying device for roll and roll manufacturing method

    JP2005105339A

  • Method for obtaining rolling mill rolls with a coating of tungsten carbide alloys, and resulting roll

    WO2021148690A1