Adsorbent-based storage and delivery vessels with high purity delivery of gases and related methods - Patents.com

The high-pressure storage system with nanoporous pyrolytic carbon adsorbent particles addresses the limitations of current systems by enabling large volume, high flow rate delivery of reagent gases with low impurity levels, ensuring safety and purity through controlled impurity exposure and preparation techniques.

JP2024536192AActive Publication Date: 2024-10-04ENTEGRIS INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024519438
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-29
Filing Date
2022-09-26
Publication Date
2024-10-04
Estimated Expiration
2042-09-26

AI Technical Summary

Technical Problem

Current sorbent-based storage systems for high-purity reagent gases face limitations in delivering large volumes at high flow rates with low impurity levels, particularly due to the use of small, low-pressure containers and monolithic adsorbents that are not suitable for high-pressure applications, leading to safety and purity concerns.

Method used

A high-pressure storage system using nanoporous pyrolytic carbon adsorbent particles in a seamless container with polished inner surfaces and controlled impurity exposure during preparation, allowing for large volume and high flow rate delivery of reagent gases with impurity levels below 150 ppmv.

Benefits of technology

The system enables safe, high-capacity storage and delivery of reagent gases with low impurity levels, suitable for hazardous gases, by minimizing exposure to atmospheric impurities and maintaining high purity throughout the storage and delivery process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536192000001
    Figure 2024536192000001
  • Figure 2024536192000002
    Figure 2024536192000002
  • Figure 2024536192000003
    Figure 2024536192000003
Patent Text Reader

Abstract

A storage and dispensing system and associated method are described for storing and selectively dispensing high purity reagent gas from a storage vessel in which the reagent gas is held in adsorptive relationship with pyrolytic carbon adsorbent particles.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The following description relates to a storage and dispensing system, and associated method, for storing and selectively dispensing a high purity reagent gas from a storage vessel in which the reagent gas is held in adsorptive relationship to a solid sorbent medium. [Background technology]

[0002] Source gases (sometimes called "reagent gases") are used in a variety of industries and industrial applications. Some examples of industrial applications include those used in the processing of semiconductor materials or microelectronic devices, such as ion implantation, epitaxial growth, plasma etching, reactive ion etching, metallization, physical vapor deposition, chemical vapor deposition, atomic layer deposition, plasma deposition, photolithography, cleaning, and doping, among others, in the manufacturing processes of semiconductor, microelectronic, photovoltaic, and flat panel display devices and products.

[0003] There is a continuing need for reliable sources of high purity reagent gases in the manufacture of semiconductor materials and devices and in various other industrial processes and applications. Examples of reagent gases include silane, germane (GeH4), ammonia, phosphine (PH3), arsine (AsH3), diborane, stibine, hydrogen sulfide, hydrogen selenide, hydrogen telluride, and halide (chlorine, bromine, iodine, fluorine) compounds, among others. Many of these gases must be stored, transported, handled, and used with a high level of care and numerous safety precautions due to the toxicity of the reagent gases, due to the inherent instability of the reagent gases, or both.

[0004] One useful technique for enhancing safe storage of reagent gas is to store the reagent gas in an adsorbed state on a solid sorbent material. Some storage systems (referred to herein as "sorbent-based" storage systems) include a storage vessel that contains the reagent gas that is adsorbed on a solid sorbent material in the storage vessel. The adsorbed reagent gas may be contained within the vessel in equilibrium with the amount of reagent gas that is also present in the container in condensed or gaseous form. Advantageously, the vessel may contain the reagent gas in a highly concentrated form, i.e., the vessel may contain 100% of the reagent gas without other types of stabilizing or diluting gases that may be included with the stored reagent gas. Specifically, in sorbent-free high pressure storage systems that store reagent gas in a high pressure container, the stored reagent gas is often or typically combined with an inert gas, such as hydrogen, helium, or nitrogen, to dilute the reagent gas. The diluted gas is more stable, less prone to explosion or fire, and less toxic.

[0005] Another advantage of sorbent-type storage systems is the ability to store usefully large quantities of reagent gas in a container at low pressure, e.g., subatmospheric pressure, so that the reagent gas does not tend to escape from the container interior if the container is damaged.

[0006] For commercial use, the feed gas must be delivered in a highly pure form and must be available in a packaged form that provides a reliable supply of gas for efficient use in the manufacturing system. Various processing steps and techniques have been described to generally reduce the amount of impurities contained within the adsorbent-based storage system when preparing the system for use. See WO 2017 / 079550.

[0007] Current commercially available sorbent-based storage systems are used to store, transport, handle, and deliver many types of high purity reagent gases for selective delivery from a container. These storage systems are capable of delivering reagent gases that contain relatively low levels of impurities, such as atmospheric impurities (nitrogen (N2), carbon monoxide (CO), carbon dioxide (CO2), methane (CH4), and water vapor (H2O)) in amounts less than 10,000 ppmv (parts per million by volume), measured as the total of nitrogen (N2), carbon monoxide (CO), carbon dioxide (CO2), methane (CH4), and water vapor (H2O). For some reagent gases, the total amount of these atmospheric impurities may be as low as 5,000 ppmv, and for other reagent gases, the amount may be as low as 500 ppmv. However, there remains a need for improved sorbent-based storage systems that deliver reagent gases containing increasingly low levels of impurities.

[0008] Based on current and previous commercially available methods of preparing sorbent-based storage and delivery systems, suppliers of these products have not developed methods and technologies to process and assemble commercially available storage systems that achieve significantly lower levels of air impurities, including levels of total air impurities well below 500 ppmv ("total air impurities" measured as the total (combined) amounts of nitrogen (N2), carbon monoxide (CO), carbon dioxide (CO2), methane (CH4), and water vapor (H2O). Furthermore, commercially available products do not include large volume (e.g., greater than 10 or 20 liters) sorbent-based storage systems for delivering certain types of reagent gases (e.g., germane, phosphine, arsine) stored in bulk in concentrated form (undiluted, at delivery concentrations greater than 90 or 99% by volume) to commercial processes that use large volumes (by volume) of reagent gas, or higher flow rates of reagent gas. Summary of the Invention

[0009] Currently, many important reagent gases are commercially available in sorbent-type storage systems that contain the reagent gas at subatmospheric pressure, but in small volume containers. Exemplary products include low-pressure vessels containing sorbents in monolithic (non-particle) block form, which have a relatively small total internal volume. "Low-pressure" vessels are not designed to be used to contain gases in pressurized form, require welded cylinder construction, and must be used only with special Department of Transportation (DOT) permits. The vessel interior has a volume of less than 10 liters, e.g., less than 8 liters. These products have a small volume format and are not well suited for applications that require a larger supply of reagent gas (larger storage capacity) due to a need for a higher duty cycle or higher flow rate of the delivered reagent gas.

[0010] There is a need for an adsorbed reagent gas storage and delivery system that has increased volume, is capable of delivering larger quantities of reagent gas at relatively high flow rates and in a non-diluted, highly concentrated form (e.g., not combined with an inert diluent gas), and that also has high purity and safety characteristics that enable commercial storage, transportation and use of the reagent gas.

[0011] In one aspect, the invention relates to a storage system for storing an adsorbed reagent gas, the system including a high pressure storage vessel including an interior containing nanoporous pyrolytic carbon adsorbent particles, and a reagent gas adsorbed on the adsorbent particles, the pressure of the interior being less than 1500 Torr.

[0012] In another aspect, the invention relates to a storage system for storing adsorbed reagent gas, the system including a high pressure storage vessel with polished sidewall surfaces having a roughness (Ra) of less than 1 nanometer, unwelded sidewalls and bottom, and a volume of at least 10 liters, and nanoporous pyrolytic carbon adsorbent particles contained in the vessel.

[0013] In yet another aspect, the invention relates to a method of preparing carbon adsorbent particles in a high pressure vessel, the method comprising forming synthetic polymeric carbon precursor resin particles, pyrolyzing the precursor resin particles in an inert atmosphere to produce nanoporous pyrolytic carbon adsorbent particles, placing the pyrolytic carbon adsorbent particles in a high pressure storage vessel while containing the particles and the vessel in an inert gas atmosphere, exposing the pyrolytic carbon adsorbent particles in the vessel to elevated temperatures and reduced pressures, and charging the vessel with a reagent gas. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The present disclosure relates to a storage system for storing a reagent gas on nanoporous pyrolytic carbon sorbent particles contained within a high pressure vessel for selectively dispensing the reagent gas from the vessel. In use, the high pressure vessel contains the sorbent, the sorbed reagent gas, and low levels of impurities at a relatively low pressure. The vessel has a relatively large volume to accommodate large volumes of the stored reagent gas even at the relatively low pressure. The large volume vessel is capable of dispensing large volumes and large volume flows of the reagent gas in an undiluted form to a process or device that uses the reagent gas.

[0015] Advantageously, the high pressure, large capacity storage vessel used with the nanoporous pyrolytic carbon sorbent particles to store and deliver the adsorbed reagent gas allows for high storage and delivery volumes even though the reagent gas is not stored at high pressure in the storage vessel. Based on the exemplary system described, by using high purity nanoporous pyrolytic carbon sorbent particles prepared by pyrolysis of a high purity carbon source (e.g., high purity synthetic hydrocarbon resin), and by using methods of treating the sorbent particles, vessel and reagent gas during preparation and assembly that control or minimize exposure to impurities and control or minimize surface chemical activity of the carbon sorbent with the adsorbed reagent gas, the stored reagent gas can be delivered from the vessel after storage at high purity levels.

[0016] The system is useful as a storage and dispensing system that allows any of a variety of reagent gases to be stored on a sorbent in a container, selectively desorbed from the sorbent, and dispensed (delivered) from the container under fluid dispensing conditions. An exemplary system is prepared from materials and processing steps that reduce or avoid contact of the sorbent, reagent gas, and container with impurities, such as atmospheric impurities, or steps that remove such impurities from the system. In a preferred system, the level of impurities that can be present in the reagent gas when dispensed is very low. A preferred system can individually dispense reagent gas from a container with the delivered reagent gas containing relatively small amounts of atmospheric impurities, for example, small amounts of one or more of nitrogen (N2), carbon monoxide (CO), carbon dioxide (CO2), methane (CH4), and water vapor (H2O) individually, and low total amounts (sum) of these impurities measured together.

[0017] Useful storage vessels may be vessels designed to contain reagent gases at high pressure. Generally, vessels referred to herein as "high pressure vessels" or "high pressure containers" or "high pressure cylinders" are storage vessels designed and rated to store and transport gaseous contents, or combinations of liquid and gaseous contents, at high pressure, e.g., pressures greater than 500 pounds per square inch (psi). The reason for using "high pressure vessels" in the systems or methods as described is to increase the level of safety when storing and transporting large quantities of reagent gas in large (large volume) storage vessels. Although the vessels are designed for use to contain gases at high pressure, such as at least 500 psi, the systems and methods may be used to store reagent gases at pressures that are not considered to be high pressure and may be as low as atmospheric or subatmospheric pressure.

[0018] Examples of high pressure vessels include vessels defined as high pressure vessels and regulated for use in transportation by the U.S. Department of Transportation (DOT), the Occupational Safety and Health Association (OSHA), the Compressed Gas Association (CGA), or two or more of these. See, for example, DOT specifications 3E, 3AA, and 3AAX. High pressure vessels useful according to the present specification may desirably meet the requirements of DOT 3E, DOT 3AA, or DOT 3AAX having a "service capacity" of at least 150 psi (gauge) or 500 psi (gauge) (see 49 C.FR section 178.37 "Specification 3AA and 3AAX seamless steel cylinders"). However, vessels for use according to the present specification need not necessarily meet all of those requirements for the vessel to be useful as described, and high pressure vessels that do not meet all DOT requirements may still be useful for use according to the present specification.

[0019] A high pressure vessel is typically a metal cylinder, including a cylindrical sidewall, a bottom that may be flat or domed, and an upper curved shoulder of gradually decreasing diameter that connects the top of the sidewall to a collar that includes an upper opening of the cylinder adapted to receive a valve to enclose an interior space within the cylinder. A typical high pressure cylinder is a seamless metal cylinder, which means a metal cylinder including a sidewall and bottom made of a single continuous ("seamless") piece of metal, and is manufactured by a step that does not include connecting two separately prepared pieces of metal with a seam or lap (e.g., by welding, brazing, or other methods).

[0020] An exemplary high pressure vessel is prepared by known methods, some exemplary methods being referred to as the "plate drawing method," the "blow bottle method," and the "hot billet pierce method," each of which forms a high strength metal cylinder having a seamless cylindrical structure, particularly a cylinder that does not include a seam (e.g., a weld) at the location of the cylinder sidewall that connects to the cylinder bottom. Because the finished vessel does not include a seam formed by contact between two edges of separately prepared parts, the method of preparing the vessel does not require joining two parts to each other along the edges of the two parts by welding or brazing the two parts at their edges.

[0021] For the uses described herein, the storage vessels of the described systems can have internal volumes sized larger than those of typical low pressure sorbent-based storage systems, preferably to provide high storage volumes (high storage capacity of reagent gas) and high flow rates of reagent gas dispensed from the vessel at very high purity compared to other sorbent-based storage systems.

[0022] Many sorbent-based storage systems use non-high pressure (or "low pressure") storage vessels having a volume of less than 8 liters, e.g., less than 5 liters. Examples of such low pressure (small volume) sorbent-based storage system vessels contain the sorbent in monolithic form, e.g., the vessel contains one or a few monolithic blocks of sorbent. These systems store reagent gases adsorbed on the monolithic sorbent at low pressure (usually below atmospheric pressure) in "low pressure" metal containers prepared by welding the vessel parts together to form welded seams in the vessel structure. Welded vessels are compatible with the use of monolithic sorbents because the monolithic sorbent cannot pass through the top opening of a conventional non-welded vessel.

[0023] In contrast, the exemplary high pressure vessels described herein do not include a welded structure (do not include a seam formed by welding or joining two pieces of metal) and can have an internal volume of at least 2 liters, at least 5 liters, or at least 10 liters, e.g., 20, 30, 40, or 50 liters or more.

[0024] As also preferred as a method for reducing the presence of impurities in vessels housing sorbents and reagent gases as described above, high pressure vessels (e.g., seamless steel vessels) can have polished interior surfaces which have a smaller surface area and are less likely to retain adsorbed impurities compared to unpolished interior surfaces. Useful or preferred interiors of vessels as described can have a surface roughness (Ra) of less than 1 micron over most, preferably all, or substantially all, of the interior surface of the vessel's interior surface area.

[0025] High pressure vessels are typically constructed from high strength metals such as steel or aluminum; examples include high strength chromium-molybdenum steels and high strength carbon steels.

[0026] High pressure vessels are typically made with side walls and bottoms having a greater thickness than vessels rated for non-high pressure use ("low pressure containers"). An example side wall thickness for a high pressure vessel may be at least 5 millimeters.

[0027] Thus, the preferred system described includes a high pressure vessel housing a sorbent for storing and transporting the reagent gas. The sorbent is a pelletized form of high purity pyrolytic carbon formed by pelletizing and pyrolyzing (by any useful steps, in any order) a carbon source to produce a pelletized carbon sorbent. The carbon source may be a synthetic hydrocarbon resin such as polyacrylonitrile (PAN), sulfonated polystyrene-divinylbenzene (PS-DVB), polyvinylidene chloride (PVDC), polyetheretherketone (PEEK), polyetherimide (PEI), phenol, polyfurfuryl alcohol (PFA), or a naturally occurring hydrocarbon source such as starch, coal tar pitch, microcrystalline cellulose, or maltodextrin. This type of sorbent may be referred to herein as "pyrolytic carbon sorbent particles," "pelletized carbon sorbent," or sometimes simply "sorbent" for short. The preferred carbon source may be a synthetic hydrocarbon resin with a low amount of chlorine (Cl2) contamination. Useful or preferred synthetic hydrocarbon resins (e.g., PVDC) may contain chlorine as an impurity at residual chlorine levels of less than 50 ppm (by mass), such as levels of less than 120 ppm (by mass) by XRF (X-ray fluorescence) or PIXE (proton induced X-ray emission).

[0028] Exemplary methods of forming pyrolytic carbon from a carbon source are described in U.S. Pat. No. 6,132,492 and PCT Patent Publication WO2017 / 079550, each of which is incorporated by reference herein in its entirety.

[0029] The sorbents used in the systems or methods herein are non-monolithic (i.e., pelletized, or "pellets" or "particles") pyrolytic carbon sorbents. The sorbents are referred to as "pyrolytic" carbon sorbents because they are prepared by pyrolyzing a carbon source.

[0030] The sorbents are non-monolithic, meaning that the sorbent is in the form of "particles" (aka "pellets"), terms known and used in the art of sorbent materials. Consistent with this, "monolithic" sorbents refer to sorbent material in the form of one to a few relatively large sized block-type pieces contained within a storage vessel, as opposed to a very large number ("multiple") of small (e.g., centimeter or millimeter scale) particles or pellets conglomerates contained within a vessel. Monolithic sorbents may be in the form of blocks, bricks, three-dimensional disks ("packs"), which may be stacked within vessels, boules, and the like, generally having centimeter or larger scale dimensions and features that, due to size and shape, are too large to pass through the top opening of a typical high pressure seamless non-welded storage vessel.

[0031] In comparison, a pelletized sorbent is understood to be in the form of a multitude of individual, separate pieces of sorbent having shapes referred to as beads, particles, granules, pellets, etc., with typical dimensions (e.g., particle size at average diameter) on the scale of less than one centimeter, e.g., less than half a centimeter.

[0032] In a container containing a large number of sorbent particles, the space inside the container includes the particles and "void space," which refers to the portion of the interior (volume) located between the particles and not occupied by the volume of the particles (void space does not include the container's "headspace," which refers to the amount of head space in the container above the particles contained therein). The void space in a container is the space that exists between the particles contained therein and that forms a network of interconnected pathways between the surfaces of the particles, within which gas may reside or flow. The amount of void space in a container containing sorbent particles varies depending on the size, shape, and packing density of the sorbent particles.

[0033] Non-monolithic sorbent particles in the form of an aggregate of multiple particles or pellets may be particularly effective for use in high pressure vessels because the particles can easily pass through the top opening of the high pressure vessel (before a valve is secured to the top opening), whereas monolithic sorbents will not pass through the top opening of the high pressure vessel. The aggregate of particles may be effectively fluid, such that the particles can be poured, blown, flowed, forced into a conduit (pipe or straw), or otherwise passed through a top opening of a high pressure storage vessel having an opening size (diameter) substantially larger than the dimensions of the individual particles of sorbent.

[0034] Pyrolytic carbon sorbent particles can be formed, handled, and processed to exhibit properties that provide useful or advantageous performance for use as a sorbent for storing and delivering (adsorbing and selectively desorbing) reagent gases. Generally, these properties include high purity (very low levels of impurities) and physical properties that have the combined effect of allowing the sorbent to be easily added to the interior of a high pressure vessel through a top opening of the vessel, to be contained within the vessel at a relatively high density (e.g., bulk density) with acceptably small void spaces between the particles (void volume), and to adsorb large amounts of reagent gas (even at low pressures, such as subatmospheric pressures within a storage vessel) that can be desorbed for delivery from the vessel by selective desorption.

[0035] In the described systems and methods, a large volume pressure vessel is used to accommodate large quantities (by volume) of reagent gas, with an additional degree of safety provided by the high pressure rating of the pressure vessel. Using a relatively large volume pressure vessel in combination with a high purity pelletized pyrolytic carbon sorbent, the described methods and systems are capable of storing and transporting large quantities of reagent gas (i.e., exhibiting high storage capacity) and are capable of delivering large volumes of very high purity (as delivered) reagent gas at high flow rates.

[0036] One useful physical property of pyrolytic carbon sorbent particles is that the sorbent has a size that easily passes through the top opening of a storage container and can be formed within the container at a high density (high packing density, measured to include voids between particles), e.g., as particles with desirably little void space between particles.

[0037] Useful particles of the adsorbent can have an average size within the range of 0.5 to 20 millimeters, e.g., 1 to 15 or 1 to 10 millimeters (mm). The average particle size of a collection of adsorbent particles can be measured by standard techniques, including randomly selecting particles from the collection of particles and measuring the size (e.g., diameter) with the use of a micrometer.

[0038] Useful or preferred particles can also have a shape that, in combination with the average size, produces a relatively high packing density and a relatively low void space. Exemplary shapes are rounded shapes, including substantially rounded, substantially spherical, or cylindrical particles, or other densely packed or "space-filling" forms or shapes, such as space-filling polyhedra. An example of a preferred amount of void space between sorbent particles (not including head space within the vessel) when the particles are contained within a high-pressure container can be less than 50%, for example less than 40, 30, or 25%.

[0039] Useful or preferred pyrolytic carbon sorbent particles, when contained within a storage container, can have a bulk density of at least 0.55 or 0.60 grams / cubic centimeter, e.g., at least 0.65 grams / cubic centimeter, e.g., in the range of 0.60-0.75 grams / cubic centimeter, 0.6-0.85 grams / cubic centimeter, 0.65-0.95 grams / cubic centimeter, or 0.60-0.95 grams / cubic centimeter ("bulk density" or "packed density" is density measured to include the density (mass per volume) of a sample volume of particles within a confined volume, where the volume includes the void space between the particles). To achieve this density, the particles can be allowed to settle together or lightly compressed or compacted against the bottom of a container, for example by applying pressure to the particles from above so that they are "tapped down," or by causing the particles to decelerate against the bottom of the vessel by dropping or hitting the container onto a solid surface, or by another technique such that the weight (force) of the decelerating particles compresses the particles toward the bottom of the vessel.

[0040] Pyrolytic carbon sorbent particles can also be formed as particles having a relatively high particle density, which means the density of a single particle and does not include the void space between the particles (as in bulk density measurements). Exemplary sorbent particles can have a particle density of at least 0.8 grams per cubic centimeter, preferably at least 1.0 grams per cubic centimeter or at least 1.1 grams per cubic centimeter, for example, in the range of 0.85 to 1.15 grams per cubic centimeter or 1.05 to 1.15 grams per cubic centimeter.

[0041] The pyrolytic carbon sorbent particles can be formed as porous particles that include an interconnected network of pores extending between the solid pyrolytic carbon of the particle. The pores have any useful pore size, by which is meant any pore size that allows for the desired performance of the sorbent in terms of the storage capacity of the vessel that contains the sorbent particles and the purity of the reagent gas that is stored in an adsorbed state on the pyrolytic carbon sorbent and then desorbed and delivered as a reagent gas.

[0042] Pore ​​sizes of carbon adsorbent materials are classified into general ranges based on the average pore size of the particle. Particles with an average pore size greater than 50 nanometers (nm) are typically referred to as macroporous. Particles with an average pore size in the range of 2 to 50 nanometers (nm) are typically referred to as mesoporous particles. Particles with an average pore size less than 2 nanometers are typically referred to as microporous. These terms are defined by IUPAC terminology.

[0043] The term "nanoporous" does not have a standard meaning in the art of adsorbent materials. Herein, the term "nanoporous" is used to describe particles having an average pore size of less than 5 nanometers (50 angstroms). Useful or preferred carbon adsorbent particles can be "nanoporous", meaning that the particles have an average pore size of less than 50 angstroms, or less than 40, less than 30, less than 20 angstroms, or less than 10 angstroms. Particularly preferred adsorbent particles can have an average pore size of less than 10 or 20 angstroms, for example, in the range of 3-9 angstroms, 3-15 angstroms, 5-8 angstroms, or 5-12 angstroms. Pore size can be measured by known techniques, such as probe molecular porosimetry, and the optimal pore size can be a function of the reagent gas to be adsorbed and the desired desorption rate during delivery.

[0044] Another characteristic of an adsorbent particle is porosity or "pore volume," which is the amount of a single adsorbent pellet that is occupied by pores relative to the total volume of the pellet (percentage or volume units per mass of adsorbent). Exemplary adsorbent particles can have a porosity of at least 0.35 cubic centimeters per gram, preferably at least 0.40 cubic centimeters per gram, and most preferably greater than 0.50 cubic centimeters per gram.

[0045] Certain physical characteristics of pyrolytic carbon sorbent particles, such as the average pore size, pore volume ("porosity"), and pore size distribution, can be influenced or controlled by characteristics of the process or materials used to prepare the particles in the pyrolysis step. These characteristics include the carbon source used to prepare the particles, the presence of solvents or fugitive pore formers, and the conditions used during the step of pyrolyzing the carbon to form the pyrolytic carbon particles, or the use of post-pyrolysis modification techniques such as physical oxidative activation with steam or CO2.

[0046] Useful pyrolysis methods can be carried out at temperatures above 600°C in an oxygen-free atmosphere for several hours. Pyrolysis is a process that causes the decomposition of a polymeric carbon source at high temperatures under inert conditions. Inert conditions can include vacuum or inert gas blanketing with noble gases such as argon or nitrogen, or a combination of inert and reducing gases to minimize the risk of oxidative combustion. The inert gas blanket can be delivered as a pressurization of the furnace or a continuous purge flow of the furnace. Several hours at high temperatures may be required to completely decompose the polymeric source material into high purity carbon. In order to control the decomposition of the feedstock polymer to result in the desired pore size distribution in the resulting carbon, it is necessary to understand when decomposition occurs and what gas species are evolved, and to control the decomposition rate and gas evolution. Those practiced in the art of preparing activated carbon from polymeric sources understand these factors involved in the pyrolysis process. Achieving the desired carbon porosity properties may be an iterative process and may be different for different furnaces or systems.

[0047] Useful or preferred carbon sorbents may be of a type and character that is substantially pure before being placed in the container as a sorbent in the system as described. As one measure, the purity of effective carbon sorbent particles may be characterized in terms of the ash content of the carbon. Useful or preferred carbon sorbents may contain 0.01 weight percent or less ash as measured by standard tests, e.g., ASTM D2866-83 or ASTM D2866.99. Carbon purity may preferably be at least 99.99% as measured by proton induced x-ray emission techniques (PIXE).

[0048] In order to prepare and assemble a storage system as described above that contains pyrolytic carbon sorbent particles having a very high level of purity, various steps or techniques are used to prevent the sorbent, container, and reagent gas from being exposed to or contaminating atmospheric gases during preparation of the storage container. Useful steps reduce the amount of impurities that are present in the container and sorbent when they are prepared, present in the reagent gas when the reagent gas is added to the container and sorbent, and ultimately present in the reagent gas when it is delivered from the storage container after the storage period.

[0049] An exemplary process includes preparing high purity pelletized nanoporous sorbent particles (sometimes referred to as "pellets") made from pyrolytic carbon, placing the pyrolytic carbon sorbent particles inside a high pressure storage vessel by passing the sorbent particles through an opening in the vessel, and exposing the sorbent inside the vessel to elevated temperatures and reduced pressures to desorb and remove trace amounts of atmospheric impurities that may have been adsorbed on or within the porous sorbent particles during preparation, handling, and placement within the vessel.

[0050] Various other optional treatments of the pyrolytic carbon sorbent particles may be performed in situ (inside the vessel) prior to adding the reagent gas to the sorbent-filled container to reduce the amount of atmospheric impurities present in the vessel and in the reagent when the reagent gas is vented from the vessel after storage.

[0051] For example, a useful optional step may be to chemically passivate the pyrolytic carbon sorbent particles of active surface sites that may react with the particular reagent gas being stored. The details of such treatment will depend on the particular sorbent used and the particular type of reagent gas being adsorbed, stored, transported, and dispensed from the vessel and sorbent. Such treatment may involve physical or chemical means to neutralize Lewis acid or base sites.

[0052] More generally, after exposing the sorbent inside the vessel to elevated temperatures and reduced pressures, or after any additional or alternative in situ treatment of the sorbent-containing vessel, a reagent gas can be added inside the vessel to adsorb the reagent gas onto the sorbent and to be contained or available within the vessel for storage and selective delivery (exhaust) from the vessel. The reagent gas may be added and contained within the vessel at any pressure, such as superatmospheric or subatmospheric. For added safety, the reagent gas can be contained at pressures of up to 5, 3, or 2 atmospheres, or below 1 atmosphere.

[0053] The reagent gas can be stored in a container for a useful period of time and selectively dispensed (evacuated and delivered) from the container for use, where the dispensed reagent gas contains less than 150 ppm (by volume) total amounts of impurities selected from, for example, CO, CO2, N2, CH4, hydrogen (H2), and HO and combinations thereof, e.g., the dispensed reagent gas can contain less than 50, 25, 15, or 10 ppmv total amounts of these impurities.

[0054] Alternatively, or in addition, the dispensed reagent gas may contain small amounts of each of one or more of the individual impurities selected from CO, CO2, N2, CH4, hydrogen (H2), and H2O, and combinations thereof. For example, the dispensed reagent gas may contain less than 25, 20, 15, 10, or 5 ppmv of any of these impurities. Alternatively or additionally, the dispensed reagent gas may contain less than 25, 20, 15, 10, or 5 ppmv of two or more different components, each individually measured, such as less than 25, 20, 15, 10, or 5 ppmv of two or more of CO, CO2, N2, CH4, hydrogen (H2), and H2O, individually measured. Additionally or alternatively, a useful or preferred dispensed reagent gas may contain less than 120 ppm chlorine (Cl2), preferably less than 50 ppm chlorine.

[0055] A specific example of the described system is the increased level of stability of germane (GeH4) stored in the described system, where the carbon sorbent is derived from a high purity synthetic polymer resin such as polyvinylidene chloride (PVDC). The sorbent particles derived from this type of carbon source are able to physically adsorb gaseous germane molecules and store unreacted germane on the sorbent in an adsorbed state, with low levels of decomposition of germane during storage. Germane is inherently unstable. When stored in a pressurized metal cylinder, pure unstabilized germane will decompose to some extent to produce impurities and increase the cylinder pressure as germane decomposes into germanium metal and hydrogen gas. This decomposition reaction can be autocatalytic, possibly dangerously so. When adsorbed within the pores of a suitable sorbent (i.e., carbon) without chemical interaction, the germane molecules are stabilized and can prevent catastrophic decomposition, deflagration, or detonation. With other lower purity or highly reactive adsorbents, the adsorbed germane in contact with the adsorbent contained within the storage vessel may denature to form hydrogen gas within the storage container, which may collect in the vessel headspace and increase gas pressure within the storage vessel.

[0056] In an exemplary system, when germane is stored on a carbon sorbent derived from a high purity synthetic hydrocarbon resin such as polyvinyl chloride (PVDC) at room temperature (e.g., 20-25 °C) and elevated temperatures (e.g., 65 °C), the amount of hydrogen produced within the vessel is well controlled. In a specific example, when germane is stored on a high purity PVDC-derived carbon sorbent in a 2.2 liter vessel at 65 °C for 6 hours, the amount of hydrogen in the vessel headspace may increase by 3% or less, or even 2% or less.

[0057] Traditionally, the purity of the reagent gas contained in a sorbent-based storage system has been measured, monitored, and described in terms of the purity of the reagent gas that is initially added to the container for storage, i.e., before the reagent gas is loaded into the storage container for storage within the container. However, depending on the type of storage container, sorbent, and their preparation and assembly, this measure of purity may not be representative of the purity of the reagent gas that is ultimately delivered from the container after transportation, handling, and storage.

[0058] The methods of preparation and handling of pyrolytic carbon sorbent particles are effective to control the amount of impurities (particularly, but not exclusively, atmospheric impurities) present in sorbent-based storage systems containing pyrolytic carbon sorbent particles in systems and equipment used to supply reagent gases to the sorbent-based storage systems, and ultimately to reduce impurities in the reagent gases stored in and delivered from the sorbent-based storage systems. According to the methods described, the purity of the reagent gas stored in the sorbent-containing vessel is improved as measured as the reagent gas is delivered (dispensed, evacuated) from the vessel.

[0059] In accordance with this specification, steps and techniques that can be used in the preparation, handling, and assembly of sorbent-based storage system components are performed to remove atmospheric impurities from the storage system components or to reduce or prevent exposure of the storage system components (particularly the sorbent) to atmospheric gases ("atmospheric impurities") such as nitrogen (N2), carbon monoxide (CO), carbon dioxide (CO2), methane (CH4), and water vapor (H2O). Useful techniques can reduce the amount of these atmospheric impurities present in the storage vessel (including the sorbent), the system for adding the reagent gas to the storage vessel, or both, to desirably reduce the amount of these atmospheric impurities present in the reagent gas when it is stored in and ultimately dispensed from the storage vessel.

[0060] Users of stored reagent gases continue to require ever-higher levels of reagent gas, including lower levels of atmospheric impurities that may be introduced into the storage vessel as part of a storage vessel component (e.g., sorbent or vessel) or that may be introduced during assembly, filling, or handling of the vessel or vessel components. Even more specifically, certain applications of reagent gases desire a larger volume of gas stored and transported in a single storage vessel in order to deliver a higher total volume of reagent gas, a higher flow rate of reagent gas, or both to the process. Certain uses also require that the gas be undiluted, i.e., free of added amounts of inert or diluent gases such as hydrogen, helium, nitrogen, etc., that are intentionally added and mixed with the reagent gas during storage to improve safety. Gases preferred for many current processing methods can be delivered at high purity and high concentration, preferably in the absence of any type of inert or diluent gas, i.e., as 80, 90, 95, 99, or essentially 100% reagent gas, with very low levels of impurities.

[0061] The described storage system includes a high pressure vessel having a relatively large internal volume (e.g., at least 10 liters) and containing nanoporous pyrolytic carbon sorbent particles inside the vessel. The pyrolytic carbon sorbent particles are effective to contain, store, and deliver a reagent gas to the storage vessel. The reagent gas is adsorbed onto the sorbent and exists as a gas inside the vessel, with a portion of the reagent gas adsorbed onto the sorbent and another portion in gaseous form in equilibrium with the adsorbed portion, or in condensed and gaseous form. The reagent gas can be initially charged to the vessel up to a desired (e.g., maximum) volume of reagent gas relative to the sorbent, based on a desired initial storage pressure in the vessel, which may be subatmospheric (less than 760 Torr) or superatmospheric pressure (the initial storage pressure is referred to as the "working pressure" or "target pressure" of the loading step following equilibration of the initial amount of reagent gas). The reagent gas is adsorbed onto the sorbent for storage and exists in gaseous or condensed form in equilibrium with the adsorbed reagent gas. Gas can then be selectively delivered (dispensed) from the container for use by exposing the adsorbent and adsorbed reagent gas within the container to dispensing conditions.

[0062] As used herein, "dispensing conditions" means one or more conditions effective to desorb a reagent gas held in a container having a sorbent, such that the reagent gas is separated from the sorbent to which it is adsorbed, such that the separated reagent gas is dispensed from the sorbent and container for use. Useful dispensing conditions can include conditions of temperature and pressure that cause the reagent gas to desorb and release from the sorbent, e.g., heating the sorbent (and the container containing the sorbent) to effect thermal-mediated desorption of the reagent gas, exposing the sorbent to reduced pressure to effect pressure-mediated desorption of the reagent gas, combinations of these, as well as other effective conditions.

[0063] The pressure inside the vessel (initial "use" pressure) may be subatmospheric, meaning less than about 760 Torr (absolute), or may be superatmospheric. For subatmospheric pressure storage, during storage of the vessel or during use of the vessel to store and dispense reagent gas, the pressure inside the vessel may be less than 760 Torr, e.g., less than 700, 600, 400, 200, 100, 50, 20 Torr, or even lower.

[0064] The described vessels and methods may be useful for storing, handling, and delivering any reagent gas that may be stored as described in equilibrium between adsorbed and condensed or gaseous portions. High pressure vessels as described may be particularly desirable for storing relatively large quantities of reagent gases that are hazardous (e.g., explosive or otherwise unstable), toxic, harmful, flammable, pyrophoric, or otherwise dangerous. Illustrative examples of reagent gases for which the described vessels and methods may be particularly useful include the following non-limiting examples: methane (CH4), acetylene (C2H2), ammonia (NH3), silane (SiH4), germane (GeH4), diphosphene (P2H4), phosphine (PH3), arsine (AsH3), diborane (B2H6), stibine (SbH3), hydrogen sulfide (H2S), hydrogen selenide (H2Se), hydrogen telluride (H2Te), digermane (Ge2H6), diacetylene (C4H2). For each of these compounds, all isotopes are contemplated.

[0065] In accordance with this specification, one or more various steps can be performed on the sorbent, on the container, or during assembly of the storage system (including filling the container with reagent gas) to reduce the amount of atmospheric impurities present in the container, sorbent, and reagent gas during storage and delivery of the reagent gas.

[0066] After a typical storage period of the reagent gas in the container, a reduced amount of atmospheric impurities is present in the reagent gas as it is stored in and delivered from the container. A typical storage period (ambient temperature, 25° C.) of the described system including a container containing a sorbent and reagent gas may be for a period of several weeks (e.g., 1, 2, 6, or 8 weeks) or several months (e.g., 3, 6, 9, or 12 months), during and after which a useful or preferred system can deliver a reagent gas containing relatively low levels of the described atmospheric impurities, e.g., as compared to alternative storage systems.

[0067] As one technique for reducing the presence of impurities in a storage system, particularly impurities contained in the sorbent, pyrolytic carbon sorbent particles can be prepared by a pyrolysis step that reduces the amount of impurities contained in the pyrolytic carbon sorbent particles.

[0068] The sorbent particles are formed by forming particles of a carbon source, for example a synthetic polymeric carbon precursor resin, such as a high purity synthetic PVDC copolymer or homopolymer.

[0069] The particles are treated by a pyrolysis step by exposing the particles of the carbon source to suitable pyrolysis conditions. As desired or useful, the conditions are carried out in a gradual manner, including increasing the temperature from an ambient starting temperature to a desired high temperature pyrolysis temperature, for example, in the temperature range of 600°C to 1000°C. The amount of time of the pyrolysis treatment step may be any effective time, for example, a total time in the range of 1 to 7 days, or longer, as desired. The atmosphere in which the pyrolysis step may be carried out may be an inert atmosphere free of oxygen, carbon monoxide, carbon dioxide, and moisture. Exemplary atmospheres include nitrogen, argon, and forming gas (a mixture of 5% hydrogen in nitrogen). During the pyrolysis step, the particles may be supported by or contained within a non-contaminating containment structure, such as a quartz or graphite tray or a quartz rotating tube.

[0070] Useful methods for preparing a storage system with reduced levels of atmospheric impurities after the sorbent particles are formed by pyrolysis can include steps and techniques for handling the pyrolytic carbon sorbent particles to prevent exposure of the sorbent to atmospheric gases before and when the sorbent particles are placed in a storage vessel (e.g., after pyrolysis) and a reagent gas is added to the interior of the storage vessel.

[0071] As one example for reducing or preventing exposure of the pyrolytic carbon sorbent particles to atmospheric impurities, the pyrolyzed sorbent particles may be placed in a storage vessel immediately after the pyrolysis step after formation and prior to placing the pyrolyzed sorbent in a storage vessel. The pyrolyzed sorbent may be packaged or loaded directly into a high pressure storage vessel without exposure to the ambient environment by loading directly into a dry, inert (e.g., nitrogen or argon atmosphere) purged containment system. The pyrolyzed sorbent particles may be loaded into a high pressure vessel shortly after the pyrolysis step, e.g., within 30 minutes of the end of the pyrolysis step, without exposure to the ambient atmosphere (i.e., air) while in a controlled atmosphere (e.g., dry nitrogen, optionally cooling the ambient environment to reduce the moisture content of the air). Because the adsorption capacity of the adsorbent decreases at elevated temperatures, the adsorbent medium may be transferred from the pyrolysis step to a storage vessel for a short period of time (e.g., less than 30, 20, or 10 minutes) at elevated temperatures between 40° C. and 65° C., optionally in a dry, low-oxygen (e.g., containing less than 1, 0.5, or 0.1 volume percent oxygen) environment (e.g., concentrated nitrogen).

[0072] According to a single example of such steps, particles formed from a synthetic polymeric carbon precursor resin can be subjected to a pyrolysis step in a pyrolysis furnace to form pyrolytic carbon sorbent particles. The pyrolyzed sorbent particles can be discharged from the pyrolysis furnace at a discharge location and placed directly into a high pressure storage vessel at the discharge location, for example, delivered to the interior of a high pressure gas storage dispensing vessel described herein. These steps can be performed in a manufacturing facility that includes an enclosure that houses the pyrolysis furnace. The enclosure can further house (enclose) a sorbent loading station at the discharge location of the pyrolysis furnace, the sorbent loading station configured to place the pyrolytic carbon sorbent particles directly into the storage vessel. The pyrolytic carbon sorbent particles can be placed in the vessel under a concentrated inert atmosphere (e.g., containing at least 99 or 99.9% (by volume) of one or more of nitrogen, helium, argon, xenon and krypton), or under a reducing atmosphere of hydrogen, hydrogen sulfide, or other suitable gas, or a combination of an inert gas and a reducing gas.

[0073] To further reduce the presence of atmospheric impurities in the storage system, particularly those contained in the materials of the high pressure storage vessel, the vessel interior can be prepared using materials and processing steps that reduce the presence of atmospheric impurities in the vessel interior during use of the vessel. The vessel or other components of the storage system (e.g., valves) may be made of materials such as metals, metal alloys, coated metals, plastics, polymers, or combinations thereof that can be selected or treated to reduce the introduction of impurities into the interior of the storage vessel. Polished, smooth, low surface roughness surfaces, such as vessel walls, may be less reactive with the reagent gas contained inside the vessel and less likely to adsorb gas or moisture from its surroundings, and therefore may be preferred as the interior surface of the storage vessel as described above. Highly polished (low surface roughness) or coated metals or high performance plastics may help minimize interactions and impurities, particularly with halide gases as stored reagent gases.

[0074] Alternatively or additionally, to further reduce the presence of atmospheric impurities in the storage system, particularly those contained in the material of the container, the container (of any material) can be subjected to heating and an optional vacuum step prior to adding the sorbent to reduce the amount of impurities that may be contained within the material of the container, e.g., adsorbed in trace amounts within the material of the container, e.g., within the sidewalls and bottom of the container, or within other components of the storage system, such as the container or valves. The container or other components of the system may be made of materials such as metals, metal alloys, coated metals, polished metals, plastics, polymers, or combinations thereof. Any of these materials may contain very small or trace amounts of adsorbed impurities, such as moisture, another atmospheric impurity, or organic volatile materials.

[0075] The steps of cleaning, drying, passivating, purging, or heating the container before a sorbent is added and contained within the container can be performed by exposing the container or other components of the storage system to any suitable conditions while the container does not contain a sorbent that will release (degas) or otherwise remove impurities that may be contained in the material, for example, by high temperature, reduced pressure, chemical or physical mechanisms, etc. One or more of these steps may be performed prior to adding any sorbent to the interior of the container.

[0076] Even the cleanest, freshest, smoothest metal surfaces typically have a thin surface layer of metal oxide, which can act as an adsorbent to soak up atmospheric impurities and moisture that may subsequently react when a reagent gas is added to the vessel. Thus, an optional step in the preparation of the vessel can include chemical passivation of the cleaned vessel. As a single example, vessels intended for containment of reactive fluoride reagent gases, such as germanium tetrafluoride (GeF4), phosphorus pentafluoride (PF5), arsenic pentafluoride (AsF5), silicon tetrafluoride (SiF4), antimony pentafluoride (SbF5), boron trifluoride (BF3), boron tetrafluoride (B2F4), or other reactive fluoride reagent gases, can advantageously undergo passivation prior to loading of the adsorbent. For example, the vessel is pressurized with a dilute mixture of fluorine (F2) gas in a dry inert gas (i.e., nitrogen or argon) above the target fill pressure, preferentially above 1000 Torr, perhaps in the range of a mixture of 5-10% fluorine (by volume), and the pressure is held for a period such as greater than 5 hours. Such fluorine exposure and treatment can convert a thin surface layer of metal oxide on the vessel's inner walls into a dense fluoride layer that is less reactive with the stored fluoride gas and less likely to contaminate the reagent gas with adsorbed traces of atmospheric contaminants.

[0077] The step of heating the vessel at any reduced pressure to remove adsorbed impurities from the vessel or system materials can be carried out in any effective manner at useful temperatures and pressures, including temperatures at which the vessel or system materials are thermally stable. Certain materials used in the vessel or storage system are less stable than others, and the temperature used during the heating step is one at which the particular material remains stable and does not degrade. The heating step can be carried out in a gradual manner involving a temperature increase from an ambient starting temperature to a desired elevated temperature above temperatures the vessel will encounter during storage, transport, and use, at temperatures ranging from, for example, 110°C to 300°C, and the heating step can be carried out for a period of time ranging from 8 to 40 hours, as desired and effective. A preferred heating step can also be carried out in a vacuum atmosphere, for example at pressures below 650 Torr, for example below 3 Torr, or at pressures below 1×10 -4 Less than 1×10 -5 It may be carried out at a pressure below Torr.

[0078] While held at elevated temperature, the vessel may alternatively or additionally be repeatedly cycled between exhaust pressure and an atmosphere of 1000 Torr of a dry, inert purge gas such as helium, nitrogen, or argon.

[0079] As another specific technique for reducing the presence of atmospheric impurities in a storage system, particularly as contained in a sorbent, after the sorbent is placed in the storage vessel, it can be subjected to a heating and depressurization step (a "degassing step") to reduce the amount of impurities present in the sorbent. This step removes physisorbed and some chemisorbed species that can adversely affect the adsorbed reagent gas purity or sorbent capacity.

[0080] The heating step can be performed on the sorbent contained in the container by subjecting the sorbent and the container containing the sorbent to any suitable heat and pressure conditions that remove amounts of atmospheric impurities that may be present in the sorbent after the sorbent is placed in the container, without causing undue detrimental thermal effects to the sorbent or the container. The heating step is performed prior to adding the reagent gas to the sorbent and inside the container.

[0081] The step of heating the adsorbent in the vessel to remove atmospheric impurities can be carried out in any effective manner and at useful temperatures and pressures, including temperatures at which the adsorbent is thermally stable. The heating step can be carried out in a gradual manner, optionally involving a temperature increase from an ambient starting temperature to a desired elevated temperature, for example, in the temperature range of 110° C. to 300° C., and the heating step can be carried out for a range of times, from 8 to 40 hours or more, as desired and effective. A preferred heating step is in a vacuum atmosphere, for example, at a pressure of less than 5 Torr, for example, 1×10 -5 or 1×10 -6 It may be carried out at a pressure below Torr.

[0082] The described methods may also include a step of chemically passivating the adsorbent after it is placed in the container. The chemical passivation step may include exposing the surface sites of the adsorbent particles to a chemical in the form of a gas (a passivation gas) to remove residual adsorbed impurities (e.g., atmospheric impurities) or to neutralize or inactivate active surface sites on the adsorbent. The amount and type of passivation gas in the passivation step as well as the conditions and time of exposure of the passivation gas to the adsorbent may depend on the type of adsorbent and the type of reagent gas stored by adsorption on the adsorbent.

[0083] As a single example, the step of chemically passivating the pyrolytic carbon sorbent particles may be performed in a high pressure vessel containing the sorbent by exposing the sorbent to a reagent gas that is the same reagent gas that is loaded into the vessel in a subsequent filling step for storage in the vessel. That is, the reagent gas stored in the vessel is used as a passivating gas in the step of passivating the sorbent. The sorbent may be exposed to the reagent gas at any pressure and for any time that will chemically passivate the sorbent by reacting with and passivating active surface sites on the sorbent prior to loading the vessel with the same reagent gas for the purpose of storing the reagent gas in the vessel. Optionally, the sorbent may be exposed to the reagent gas as a high pressure but low concentration passivating gas in an inert, non-reactive gas, such as diluted to a concentration of 2, 5, or 10% (by volume) in a mixture with an inert gas and pressurized to 1,000, 2,000, or 5,000 Torr.

[0084] For example, in a chemical passivation step, the adsorbent may be exposed to the reagent gas at a relatively low pressure, e.g., a pressure less than 760 Torr, e.g., 1, 2, 5, or 10 Torr, up to 50, 100, 200, or 500 Torr. The time for which the adsorbent is exposed to the passivation gas may be any useful time, e.g., a time in the range of 15 to 2500 minutes, e.g., 60 to 1000 minutes. The passivation step may be carried out at ambient temperature or at an elevated temperature, e.g., a temperature in the range of 60 to 300°C, e.g., 85 to 250°C. After exposing the adsorbent to the passivation gas for the desired time, the passivation gas is then passed through a vacuum, e.g., a pressure less than 3 Torr, e.g., 1×10 -5 or 1×10 -6 The sorbent is removed by exposure to a pressure of less than Torr.

[0085] After the desired steps of preparing the sorbent and disposing it inside the storage vessel, the vessel can be filled ("loaded" or "charged") with a reagent gas to a desired pressure, and the reagent gas is introduced into the interior of the vessel and adsorbed onto the sorbent, while the sorbent is treated as described above to reduce or minimize the amount of atmospheric impurities to which it is exposed or contains.

[0086] In order to reduce or control the amount of atmospheric impurities that become present in the vessel, i.e., that may be added to the vessel or reagent gas during the step of loading the vessel with the reagent gas, various steps can be performed on the vessel and sorbent during the loading step, and specific loading equipment can be used during the loading step. These generally include any one or more of the following: use of the highest purity reagent gas possible, or purification of the reagent gas prior to introduction into the storage vessel; use of loading equipment that is processed, handled, and used in a manner that reduces exposure of the equipment (especially the interior space) to the atmospheric gas or gases; steps in the loading process that may be effective to remove atmospheric impurities from the loading equipment and vessel, either during or after the addition of the reagent gas to the vessel; any of which may be useful alone or in combination of two or more of these.

[0087] In an exemplary method, reagent gas may be initially added to and retained within a receiving vessel in an amount that exceeds the working pressure (also known as the "target pressure" or "final fill pressure") of the storage vessel ("target pressure" or "final fill pressure" refers to the initial pressure of the vessel when the vessel contains an amount of reagent gas for which the vessel is used to selectively release gas from the vessel for storage, transport, and use). When initially adding reagent gas to the vessel, the reagent gas may be added to create an internal pressure within the vessel that is greater than the working pressure (the "initial fill pressure"). This initial fill pressure may be a maximum pressure that the vessel interior will encounter during storage, transport, and use of the vessel when filled with reagent gas, or a pressure that is expected to be lower and higher than the working pressure. For vessels designed to accommodate subatmospheric reagent gas, examples of internal pressures of the vessel with excess amounts of reagent gas added as described may be pressures of at least 760, 1000, or 1200 Torr. For example, with a target pressure (final fill pressure) of 650 Torr, the vessel can be initially filled to a range of 700-1000 Torr, such as above 760 Torr or above 800 Torr, and allowed to equilibrate before pumping back to the target 650 Torr.

[0088] Measured in another way, as described, an example internal fill pressure of a container (designed for subatmospheric storage of reagent gas) to which an excess amount of reagent gas has been added can be at least 10, 20, or 50% higher than the target pressure ("operating pressure"). For example, if the container contains a pressure of reagent gas of 760 Torr during use ("operating pressure" means the pressure of the container when it is filled with reagent gas for storage, transport, and selective delivery of the reagent gas), the container can be filled with excess reagent gas in this initial fill step to achieve an internal pressure of 10, 20, or 50% greater than the "operating pressure" of 760 Torr, i.e., 836 Torr, 912 Torr, or 1,140 Torr, respectively.

[0089] After adding an excess amount of reagent gas, the container is equilibrated, meaning that the amount of reagent gas adsorbed on the sorbent and the amount of gaseous reagent gas present as a gas in the headspace volume of the container are in thermodynamic equilibrium. After adding an excess amount of reagent gas, the container is held (e.g., at a constant temperature) for a sufficient time to achieve equilibrium, and the gaseous reagent gas contained as a gas in the headspace potentially contains an amount of atmospheric impurities that have migrated from the sorbent to the gaseous reagent gas in the headspace. The reagent gas in the headspace can then be released from the container along with the contained impurities to remove the impurities and bring the container to a lower reagent gas content and lower pressure, e.g., to a reagent gas content and initial pressure, e.g., a "target pressure" or "working pressure", as intended for the purpose of transporting and storing the reagent gas in the container.

[0090] The amount of time required to reach the described equilibrium after adding an excess amount of reagent gas can vary depending on factors such as the type of sorbent, the type of reagent gas, the amount of sorbent relative to the total volume of the vessel and the volume of the headspace in the vessel, the amount of reagent gas added to the vessel, and the pressure inside the vessel. Exemplary amounts of time after adding reagent gas to the described excess pressure and releasing an amount of reagent gas along with impurities can be amounts of time in the range of 30 minutes to 1000 hours, e.g., 1 hour to 500 hours, e.g., 2 hours to 100 hours.

[0091] Below is a sequence of preparation and handling steps for an exemplary method of preparing sorbent particles for use in a high pressure vessel for storing reagent gases.

[0092] High purity synthetic adsorbent particles, such as 1-PVDC copolymer or homopolymer, are pressed into particles, pellets or tablets that exhibit high particle and bulk density within a storage container.

[0093] 2- Pyrolyze the particles in an inert atmosphere furnace using uncontaminated containment such as quartz or graphite trays or quartz rotating tubes with a recipe designed to remove all non-carbon by-products under inert gas purging conditions.

[0094] 3- Removing the pyrolysis particles from the furnace in a manner that protects the highly adsorbed carbon products from atmospheric exposure or other means of contamination.

[0095] 4-Prepare a clean, highly polished or coated high pressure (HP) cylinder. Cylinder preparation may include cylinder shell washing to remove grease solvents, rust, etc.; turning or rolling the cylinder shell with metal, mechanical or mechanical-chemical polishing of the cylinder shell with ceramic shot to smooth out roughness and remove a thin layer on the inner surface; further cleaning followed by loading with carbon sorbent using water vapor, followed by drying at high temperature and purging with clean inert gas; and optional passivation just prior to loading with sorbent.

[0096] 5- Loading the cleaned, treated, and dried cylinder with high purity carbon particles in a manner that minimizes exposure to air or other sources of contamination. An exemplary technique may include connecting the cylinder inlet to an airless chamber adapted to load the carbon sorbent particles under an atmosphere containing no measurable gaseous water and / or oxygen levels greater than 10 ppm, preferably less than 1 ppm; loading the carbon sorbent particles into the container through the container inlet under low water and low oxygen conditions; and installing a valve at the container inlet while preventing the ingress of air.

[0097] The 6-HP cylinder can be valved and then leak tested, evacuated, possibly cycle purged with a dry inert purge gas, and degassed to high vacuum levels at elevated temperatures. The degassing step removes physisorbed and some chemisorbed species from the loaded carbon adsorbent particles that can adversely affect the purity of the adsorbed reagent gas (e.g., GeH4) or the carbon capacity of a reagent gas such as GeH4.

[0098] 7- Passivate the carbon in the container to maintain high purity of the adsorbed reagent gas (e.g., GeH4) during storage by adsorbing a small amount of sacrificial reagent gas (e.g., GeH4), heating for several hours to react the sacrificial reagent gas (e.g., GeH4) with sites that can decompose the reagent gas (e.g., GeH4) and inactivate them, followed by cooling and venting the gaseous products of the passivation reaction.

[0099] 8- Cycle-purging the vessel and sorbent, then using a high purity gas manifold to fill the vessel (containing the fully degassed sorbent) with reagent gas (e.g., the same reagent gas used in the passivation step). Cycle-purging refers to alternating cycles of applying high vacuum and pressure (e.g., up to 1 bar) with an inert purge gas such as helium, nitrogen, or argon for a sufficient number of cycles and at a sufficient temperature to remove adsorbed atmospheric gas species that may interact with the reagent gas that becomes adsorbed onto the sorbent.

[0100] Optionally, the filled containers may be handled using controlled storage and shipping conditions to further maintain purity, with "start-up" procedures at the end-use tool designed to reduce the level of impurities in the cylinder head space. Examples of such steps may include temperature control during shipping and warehousing; cylinder stabilization to ambient conditions prior to tool installation and use; and venting the "vapor phase" of the cylinder head space prior to extracting the adsorbent reagent gas for delivery to the tool.

Claims

1. 1. A storage system for storing adsorbed reagent gas, the system comprising: a high pressure storage vessel including an interior including nanoporous pyrolytic carbon sorbent particles; a reagent gas adsorbed on the adsorbent particles; Including, A storage system wherein the pressure therein is less than 1500 Torr.

2. 10. The storage system of claim 1, wherein the sorption media comprises pyrolyzed polyvinylidene chloride particles having an average particle size within the range of 1 to 10 millimeters.

3. 3. The storage system of claim 1 or 2, wherein the adsorption media comprises pyrolyzed polyvinylidene chloride particles having an average pore size of less than 20 Angstroms.

4. The storage system of any one of claims 1 to 3, wherein the adsorbent comprises pyrolyzed polyvinylidene chloride particles having a bulk density within the range of 0.55 to 0.95 grams per cubic centimeter.

5. The storage system of any one of claims 1 to 4, wherein the sorbent comprises pyrolyzed polyvinylidene chloride particles having a particle density in the range of 0.85 to 1.15 grams per cubic centimeter.

6. The storage system is capable of dispensing the reagent gas from the reservoir, the dispensed reagent gas being H 2 , CO, CO 2 , N 2 , C.H. 4 , and H 2 6. The storage system of claim 1, comprising less than 150 ppm (by volume, ppmv) total amount of impurities selected from: O, HCl, HCl, HCl+O, and combinations thereof.

7. The storage system of any one of claims 1 to 6, wherein the storage vessel has an internal volume of at least 2 liters.

8. The adsorbed reagent gas is methane (CH 4 ), acetylene (C 2 H 2 ), ammonia (NH 3 ), silane (SiH 4 ), German (GeH 4 ), diphosphene (P 2 H 4 ), phosphine (PH 3 ), arsine (AsH 3 ), diborane (B 2 H 6 ), stibine (SbH 3 ), hydrogen sulfide (H 2 S), hydrogen selenide (H 2 Se), hydrogen telluride (H 2 Te), Digermane (Ge 2 H 6 ), diacetylene (C 4 H 2 ), germanium tetrafluoride (GeF 4 ), phosphorus pentafluoride (PF 5 ), arsenic pentafluoride (AsF 5 ), silicon tetrafluoride (SiF 4 ), antimony pentafluoride (SbF 5 ), boron trifluoride (BF 3 ), boron tetrafluoride (B 2 F 4 8. The storage system of claim 7, comprising:

9. 8. The storage system of claim 7, wherein the adsorbed reagent gas is germane.

10. A storage system according to any preceding claim, wherein the vessel contains the reagent gas in a concentration of at least 90%.

11. The storage system of any one of claims 1 to 10, wherein the storage vessel has an internal pressure of 760 Torr or less.

12. the storage vessel has an internal pressure of 760 Torr or less; A storage system according to any preceding claim, wherein the storage vessel contains the reagent gas in a concentration of at least 90%.

13. The storage container comprises: a polished sidewall surface having a roughness (Ra) of less than 1 nm; an unwelded side wall and bottom; A volume of at least 10 litres The storage system according to any one of claims 1 to 12, comprising:

14. A method of dispensing an adsorbed reagent gas from a storage system according to any one of claims 1 to 13, wherein the adsorbed reagent gas is methane (CH 4 ), acetylene (C 2 H 2 ), ammonia (NH 3 ), silane (SiH 4 ), German (GeH 4 ), diphosphene (P 2 H 4 ), phosphine (PH 3 ), arsine (AsH 3 ), diborane (B 2 H 6 ), stibine (SbH 3 ), hydrogen sulfide (H 2 S), hydrogen selenide (H 2 Se), hydrogen telluride (H 2 Te), Digermane (Ge 2 H 6 ), diacetylene (C 4 H 2 ), germanium tetrafluoride (GeF 4 ), phosphorus pentafluoride (PF 5 ), arsenic pentafluoride (AsF 5 ), silicon tetrafluoride (SiF 4 ), antimony pentafluoride (SbF 5 ), boron trifluoride (BF 3 ), boron tetrafluoride (B 2 F 4 ), and all isotopes of these reagent gases.

15. A method of dispensing an adsorbed reagent gas from a storage system according to any preceding claim, wherein the adsorbed reagent gas is germane.

16. 16. The method of claim 15, comprising dispensing said germane from said container at a concentration of at least 90%.

17. Dispensing the reagent gas from the container, wherein the dispensed reagent gas is H 2 , CO, CO 2 , N 2 , C.H. 4 , and H 2 14. A method of dispensing adsorbed reagent gas from a storage system according to any one of claims 1 to 13, comprising less than 150 ppm (by volume, ppmv) total amount of impurities selected from: O, HCl, HCl, HCl+O, and combinations thereof.

18. 1. A storage system for storing adsorbed reagent gas, the system comprising: A polished sidewall surface with a roughness (Ra) of less than 1 nm; Unwelded side walls and bottom, and Volume of at least 10 litres a high pressure storage vessel comprising: Nanoporous pyrolytic carbon adsorbent particles and Including, the system.

19. 20. The storage system of claim 18, wherein the sorption media comprises pyrolyzed polyvinylidene chloride particles having an average particle size within the range of 1 to 10 millimeters.

20. 20. The storage system of claim 18 or 19, wherein the adsorption media comprises pyrolyzed polyvinylidene chloride particles having a pore size of less than 20 angstroms.

21. 21. The storage system of any one of claims 18 to 20, wherein the sorbent comprises pyrolyzed polyvinylidene chloride particles having a bulk density in the range of 0.55 to 0.95 grams per cubic centimeter.

22. 22. The storage system of any one of claims 18 to 21, wherein the sorbent comprises pyrolyzed polyvinylidene chloride particles having a particle density in the range of 0.85 to 1.15 grams per cubic centimeter.

23. 1. A method for preparing carbon adsorbent particles, the method comprising: forming synthetic polymeric carbon precursor resin particles; pyrolyzing the precursor resin particles in an inert atmosphere to produce nanoporous pyrolytic carbon adsorbent particles; placing the pyrolytic carbon sorbent particles in a high pressure storage vessel while containing the particles and the vessel in an inert gas atmosphere; exposing the pyrolytic carbon sorbent particles in the container to elevated temperatures and reduced pressures to remove air pollutants adsorbed to the particles and the container; filling said reservoir with said reagent gas; A method comprising:

24. The container comprises: a polished sidewall surface having a roughness (Ra) of less than 1 nm; an unwelded side wall and bottom; A volume of at least 10 litres 24. The method of claim 23, wherein the high pressure storage vessel comprises:

25. 25. The method of claim 24, wherein the adsorption media comprises pyrolyzed polyvinylidene chloride particles having an average particle size within the range of 1 to 10 millimeters.

26. 26. The method of claim 24 or 25, wherein the adsorption medium comprises pyrolyzed polyvinylidene chloride particles having an average pore size of less than 20 Angstroms.

27. 27. The method of any one of claims 24 to 26, wherein the adsorbent comprises pyrolyzed polyvinylidene chloride particles having a bulk density in the range of 0.55 to 0.95 grams per cubic centimeter.

28. 28. The method of any one of claims 24 to 27, wherein the adsorbent comprises pyrolyzed polyvinylidene chloride particles having a particle density in the range of 0.85 to 1.15 grams per cubic centimeter.

Citation Information

Patent Citations

  • High purity gas filling container and manufacture thereof

    JP1995167391A

  • Gas storage, metering, and distribution system with monolithic carbon adsorbent

    JP2006509974A

  • RECOVERY OF Xe AND OTHER HIGH VALUE COMPOUNDS

    US20150027202A1

  • Cylinder preparation for high purity acetylene

    US9316355B2