Electrode, joint and method of manufacturing same

By stacking electrode layers with conductive porous substrates, the active material loading is increased, enhancing energy and power densities while preventing structural collapse and electrolyte dissolution in battery electrodes.

JP2024537162AInactive Publication Date: 2024-10-10NATIONAL UNIVERSITY OF SINGAPORE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024520813
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-08
Filing Date
2022-10-07
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing battery technologies face challenges in increasing energy density and reducing cost due to limitations in active material loading, Li ion diffusion, and cell polarization in thick electrodes, leading to underutilization and structural issues.

Method used

Stacking multiple electrode layers with conductive porous substrates in between, forming a single electrode structure that increases active material loading per area, enhances electronic conductivity, and prevents material loss through porosity and electrolyte retention.

Benefits of technology

This configuration improves areal capacity, reduces cell polarization, and maintains capacity retention by addressing structural collapse and electrolyte dissolution, resulting in higher energy and power densities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The present disclosure relates to an electrode including a plurality of porous conductive substrates and at least one layer of an electrode composite, the at least one layer of the electrode composite being sandwiched between the plurality of porous conductive substrates, and the at least one layer of the electrode composite being in electrical communication with the plurality of porous conductive substrates. The electrode composite is at least partially impregnated into the plurality of porous conductive substrates. The present disclosure also relates to a joint, and a method of manufacturing the electrode and the joint.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates generally to electrodes, joints and methods for their manufacture. [Background technology]

[0002] The cell architecture is the core part of batteries, such as lithium-ion (Li-ion) and lithium-sulfur (Li-S) batteries. Electrode composite materials (ECMs) typically include active materials, additives, and binders coated onto an electronically conductive substrate (current collector, e.g., metal foil) to form an electrode. Several approaches, such as developing new active materials, optimizing cell engineering, optimizing material processing, and improving quality control, have been used to increase the energy density and / or reduce the cost of Li-ion batteries. The approximately three-fold incremental improvement in energy density over the past two decades is mainly due to cell engineering, and has been achieved since the early Li-ion cells (200 Wh L -1 ) to around 20% for today's state-of-the-art cells (550-600Wh L -1 ) to about 45% by volume of active material.

[0003] Thicker battery cell electrodes by increasing the active material loading while thinning the current collectors and separators is one approach to obtain higher energy density and lower cost batteries. The physics-based factors limiting the energy and power density of thick electrodes were found to be increased cell polarization and underutilization of the active material. The latter is affected by Li-ion diffusion in the active material and Li-ion depletion in the electrolyte phase. Summary of the Invention [Problem to be solved by the invention]

[0004] It would be desirable to overcome or ameliorate at least one of the above problems. [Means for solving the problem]

[0005] The inventors have found that the active material loading on an electrode can be increased by stacking two or more electrode layers together with at least one connecting component between the electrode layers. The connecting component can be a conductive porous substrate with similar or dissimilar mass loadings to form a single electrode, resulting in a high active material loading per area on the electrode, thereby increasing the areal capacity and improving the energy density of the battery.

[0006] The present invention relates to a) a plurality of porous conductive substrates; b) at least one layer of an electrode composite sandwiched between and in electrical communication with a plurality of porous conductive substrates; Equipped with An electrode is provided in which the electrode composite at least partially impregnates a plurality of porous conductive substrates.

[0007] This configuration contains the electrode composite between and within the porous conductive substrate such that the electrode composite does not form the external / outer surface of the electrode.

[0008] In some embodiments, multiple porous conductive substrates and at least one layer of electrode composite material are laminated together.

[0009] In some embodiments, the at least one layer of an electrode composite is at least two layers of an electrode composite.

[0010] In some embodiments, the porous conductive substrate and the layer of electrode composite have substantially the same planar area.

[0011] In some embodiments, the porous conductive substrate is characterized by a planar area that is between about 1% and about 50% greater than the planar area of ​​the layer of electrode composite.

[0012] In some embodiments, the electrode further comprises a binder in contact with a side of the electrode to electronically connect the side of the electrode composite to the porous conductive substrate.

[0013] In some embodiments, the binder is an aqueous binder, a non-aqueous binder, or a combination thereof.

[0014] In some embodiments, the porous conductive substrate is surface functionalized.

[0015] In some embodiments, the porous conductive substrate is functionalized with a transition metal sulfide, a transition metal selenide, a halide, a metal ion, a nanoparticle, a metal oxide, or a combination thereof.

[0016] In some embodiments, each layer of the porous conductive substrate is independently characterized by a thickness of from about 10 μm to about 1000 μm.

[0017] In some embodiments, the porous conductive substrate is selected from carbon paper, carbon cloth, carbon foam, carbon fiber, porous metal structures, grids and foams, porous conductive polymers, conductive polymer gels and aerogels, thin films, or combinations thereof.

[0018] In some embodiments, each layer of the electrode composite is independently characterized by a thickness of from about 0.1 μm to about 1000 μm.

[0019] In some embodiments, the electrode composite comprises a carbon-based material, a metal-based material, a metal oxide-based material, an electrochemically active material, a polymeric material, or a combination thereof.

[0020] In some embodiments, the electrode composite is characterized by the absence of conductive materials, binders, fillers, or combinations thereof.

[0021] In some embodiments, the electrode composite comprises conductive nanoparticles.

[0022] In some embodiments, the conductive nanoparticles include graphene, carbon black, acetylene black, carbon nanotubes, metal nanoparticles, carbon dots, or combinations thereof.

[0023] In some embodiments, the conductive nanoparticles are surface functionalized with different oxidation states of halides, chalcogenides, metals, or combinations thereof.

[0024] In some embodiments, the weight ratio of the conductive nanoparticles to the electrode composite is about 3% to about 50% by weight.

[0025] In some embodiments, the weight ratio of the conductive nanoparticles to the electrode composite is about 10% by weight.

[0026] In some embodiments, the electrode composite further comprises a conductive filler.

[0027] In some embodiments, the conductive filler is a conductive carbon-based material, a metal, or a combination thereof.

[0028] In some embodiments, the weight ratio of the conductive filler to the electrode composite is from about 1% to about 30% by weight.

[0029] In some embodiments, the weight ratio of the conductive filler to the electrode composite is about 10% by weight.

[0030] In some embodiments, the electrode composite further comprises a binder.

[0031] In some embodiments, the binder is polyvinylidene fluoride, gum arabic, cellulose gum, polyvinyl alcohol, carboxymethyl cellulose, styrene-butadiene rubber, or a combination thereof.

[0032] In some embodiments, the weight ratio of binder to electrode composite is from about 1% to about 20% by weight.

[0033] In some embodiments, the weight ratio of binder to electrode composite is about 10% by weight.

[0034] In some embodiments, the electrode is characterized by the absence of a separator between the electrode composites.

[0035] In some embodiments, the electrode has a capacity of about 50 mAh g 活物質 -1 ~About 4000mAh g 活物質 -1 It is characterized by the discharge capacity.

[0036] In some embodiments, the electrodes have a capacitance of about 2 mAh cm per layer of the stack. -2 ~about 100mAh cm -2 It is characterized by an areal capacity of

[0037] In some embodiments, the electrodes have a capacitance of about 1.5 S cm -1 ~about 100S cm -1 It is characterized by an electronic conductivity of

[0038] In some embodiments, the electrode is characterized by a capacity loss of about 5% to about 50% relative to the initial capacity of the electrode.

[0039] In some embodiments, the electrodes are characterized by a coulombic efficiency of about 70% to about 100%.

[0040] In some embodiments, the electrodes are characterized by a cycle life of greater than 40 cycles.

[0041] In some embodiments, the electrode further comprises a junction adapted to penetrate the electrode.

[0042] In some embodiments, the joint is adapted to pass through a through hole that can be formed in the electrode.

[0043] In some embodiments, the junction comprises a body adapted to pass substantially through the electrode.

[0044] In some embodiments, the body is characterized by a cross-sectional shape selected from a circle, an oval, or a polygon.

[0045] In some embodiments, the body is hollow.

[0046] In some embodiments, the body is characterized by a polygonal cross-sectional shape and, when hollow, the body includes legs extending from edges of the polygon.

[0047] In some embodiments, the joint further comprises a head at the first end of the body.

[0048] In some embodiments, the body is deformable to form the head.

[0049] In some embodiments, the joint comprises a conductive material.

[0050] In some embodiments, the conductive material is selected from a metal, an alloy, or a composite.

[0051] In some embodiments, the conductive material is selected from stainless steel, Al, Ti, Ni, or Cu.

[0052] In some embodiments, when the electrode is a cathode, the conductive material is selected from stainless steel, Al, Ti, or Ni.

[0053] In some embodiments, when the electrode is an anode, the conductive material is selected from stainless steel, Ni, or Cu.

[0054] In some embodiments, the junction is adapted to electrically connect two or more electrodes.

[0055] In some embodiments, the junction is adapted to electrically connect at least one electrode to at least one contact tab.

[0056] In some embodiments, the junction is adapted to electrically connect the at least one electrode to the at least one lead.

[0057] In some embodiments, the junction is adapted to electrically connect the at least one contact tab to at least one lead on the electrode.

[0058] The present invention relates to a) forming at least one electrode layer, the at least one electrode layer being formed by coating a layer of an electrode composite material on at least a surface of a porous conductive substrate; b) laminating at least one electrode layer with another porous conductive substrate such that a layer of electrode composite is sandwiched between the porous conductive substrates, the at least one electrode layer being in electrical communication with the porous conductive substrate; Including, A method of making an electrode is provided in which the electrode composite is at least partially impregnated into a porous conductive substrate.

[0059] In some embodiments, the method further comprises laminating another electrode layer onto the porous conductive substrate of step a) or b).

[0060] In some embodiments, the electrode composite is provided as a slurry, dough, paste, or powder.

[0061] In some embodiments, the electrode composite has a density of about 1 mg cm -2 ~about 100mg cm -2is characterized by a mass loading on the surface of the porous conductive substrate of

[0062] In some embodiments, the laminating step includes applying a compressive force to the electrode layer and the separate porous conductive substrate.

[0063] In some embodiments, the compression force is provided by a hydraulic press, a pneumatic press, a weight press, or a roller press.

[0064] In some embodiments, the method further comprises connecting the junction to an electrode.

[0065] In some embodiments, the joint is connected to the electrode via punching or via a through hole formed in the electrode.

[0066] In some embodiments, the joint comprises a body, the body being deformable to form a head.

[0067] In some embodiments, the body is deformed by bending an end of the body so that the head is substantially parallel to the surface of the electrode.

[0068] In some embodiments, the body is bent in a direction away from the longitudinal axis of the body.

[0069] The present invention also provides a method of connecting a junction to an electrode, comprising the steps of: a) passing the body of the junction through an electrode; b) deforming the body of the joint to form a head for connecting the joint to an electrode; The present invention provides a method comprising:

[0070] Embodiments of the invention will now be described, by way of non-limiting example, with reference to the drawings, in which: [Brief description of the drawings]

[0071] [Figure 1]FIG. 1 shows examples of stacking configurations: (A) uses a single porous conductive substrate (or current collector (CC)) surface fully coated with an electrode composite (ECM); (B) uses double CC surfaces fully coated with ECM; (C) uses four electrodes consisting of two single CC surfaces and two double surfaces fully coated with ECM before compression; (D) uses four final electrodes stacked with partially exposed ECM; (E) uses a single CC surface partially coated with ECM; (F) uses double CC surfaces partially coated with ECM; (G) uses four electrodes consisting of two single CC surfaces and two double surfaces partially coated with ECM before compression; and (H) uses four final electrodes stacked with ECM encapsulated between the CCs. [Diagram 2] (A) shows an example of a method for continuous lamination of two single CC surfaces coated with ECM and one double CC surface coated with ECM by roller press, and (B)-(C) show examples of a method for batch lamination of two single CC surfaces coated with ECM and two double CC surfaces coated with ECM by pneumatic / hydraulic press to form a laminated electrode (SE). [Diagram 3] FIG. 1 shows the first specific discharge capacity at 0.05 C rate of a cell made with two individual electrodes stacked together. [Figure 4] FIG. 1 shows the specific discharge capacity at 0.25 C rate of a cell made with two individual electrodes stacked together. [Diagram 5] 1 shows examples of joint shapes and formats: (A) cylindrical joints with and without pre-fitted heads, cylindrical heads with cubic legs, and joints with bifurcated fastener shapes connected by heads; (B) optimized joint leg shapes and flange / hole legs to reduce weight in joints with cubic shaped holes; (C) different hole shapes and joint leg shapes (independent of head shape). [Figure 6] Schematic examples of joints in the form of a bifurcated fastener connected by a head that joins the electrode and the tab / lead, and examples of joining methods: (A) the joint is pressed into the electrode and the tab / lead pierces them, (B) the legs of the joint are bent inwards or outwards to join the electrode and the tab / lead, and (C) the final electrode with the tab / lead joined. [Figure 7] 1A-1C show examples of methods for joining electrodes, tabs, and / or leads, where (A) is an electrode, tab, and / or lead, (B) is pre-forming of a hole (which can optionally be done by, for example, puncturing or drilling), (C) is the pre-formed hole viewed from above, (D) is insertion of the joint with or without a pre-formed head, in (E) the legs of the joint (and head in the case of joints without a pre-formed head) are flared / collared / bent outward to join the electrode, tab, and / or lead, and (F) is the final joined electrode, tab, and / or lead. [Figure 8] FIG. 1 shows a schematic example of a joint consisting of three parts (two heads and one leg) and how to assemble them. [Figure 9] 1 is an image to illustrate the use of an aluminum joint connecting an aluminum tab to a cathode electrode that uses carbon paper as a current collector. A front view of the electrode is shown on the left and a back view of the electrode is shown on the right. [Figure 10] Figure 1 shows the specific discharge capacity at 0.6C rate after cycling of a cell made with a dry electrode composite (in powder form, 3 mg cm-2) laminated between two porous current collectors. No binder or extra conductive carbon was used in the electrode composition. [Figure 11] Figure 1 shows the specific charge / discharge capacity profiles at 0.1 C rate of a cell fabricated with a dry electrode composite (in powder form, 3 mg cm-2) laminated between two porous current collectors. No binder or extra conductive carbon was used in the electrode composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0072] Typically, Li-ion and Li-S batteries have capacities of 25–30 mg cm, respectively. -2 and 1–5 mg cm -2 Increasing the active material loading on the electrodes of alkaline-sulfur batteries comes at the cost of reduced conductivity throughout the electrode bulk, worse electrode wetting, poor active material utilization, and increased cell polarization.

[0073] To allow electrons to pass in and out of a battery electrode, it is useful for the electrode active material to be in electronic communication with a current collector, which in turn is in electronic communication with an external load. During battery cycling, stresses can develop in the electrode that can disrupt the contact between the active material and its current collector, causing battery degradation or failure.

[0074] The inventors have found that the active material loading on the electrode can be increased by stacking two or more electrode layers with an intervening connecting component. These layers can then be stacked. The connecting component serves to separate two or more electrode layers, which may be conductive porous substrates with similar or dissimilar mass loadings, to form a single electrode, resulting in a high active material loading per area on the electrode, thereby increasing the areal capacity and improving the energy density of the battery.

[0075] For example, electrode materials can be directly laminated with porous and electronically conductive substrates to improve areal capacity. This improves volumetric and gravimetric energy density and facilitates scalable and sustainable manufacturing. Direct contact of the conductive substrates acting as current collectors reduces cell polarization and improves electronic conductivity. This provides higher rate power capability. Confining the electrode composite between the porous substrates helps retain electrolyte soluble electroactive species that prevent irreversible capacity loss. This improves cycle life and coulombic efficiency. Additionally, multiple laminated electrode configurations provide room for volume expansion into the pores of the conductive substrate, preventing material loss due to structural collapse caused by volume change. In this way, higher active material utilization, capacity and capacity retention can be achieved. Additionally, it allows for the use of high capacity materials such as silicon and sulfur with higher volume expansion issues.

[0076] Thus, the present invention provides a) a plurality of porous conductive substrates; b) at least one layer of an electrode composite sandwiched between and in electrical communication with a plurality of porous conductive substrates; Equipped with An electrode is provided in which the electrode composite at least partially impregnates a plurality of porous conductive substrates.

[0077] In some embodiments, the present invention provides a method for the preparation of a a) a plurality of porous conductive substrates; b) at least two layers of an electrode composite, each layer of the electrode composite being sandwiched between a porous conductive substrate, and the at least two layers of the electrode composite being in electrical communication with the porous conductive substrate; and Equipped with An electrode is provided in which the electrode composite at least partially impregnates a plurality of porous conductive substrates.

[0078] At least one layer or layers of the electrode composite can be laminated and compressed to form a single indivisible electrode in which all layers are physically separated but electronically connected without the use of additional tabs. The exterior surface of the electrode is coated by a porous conductive substrate, thus electrically protecting the electrode composite internally. The porous conductive substrate not only acts as a current collector, but also as an active filter or trap for the electroactive material and electrolyte-soluble active material due to its porosity. This function helps to address the problems associated with electrolyte-soluble active materials losing electrical contact, including structural collapse of the coating due to eventual volume changes that cannot be performed by the separator. Additionally, the porosity present within the porous conductive substrate aids in the uniform wetting of the electrode composite. This also allows the electrolyte to uniformly penetrate the electrode so that the electrode composite deep within the electrode can be in contact with the electrolyte.

[0079] In some embodiments, the layers of the porous conductive substrate and electrode composite are laminated together. In some embodiments, at least two layers of the porous conductive substrate and electrode composite are laminated together. As used herein, a "laminate" refers to two or more layers of material rolled or compressed together such that the interfaces of the layers are fused together. A laminate is a permanently assembled object created using heat, pressure, welding, or adhesives. A variety of coating machines, mechanical presses, and calendering devices can be used. In this context, a layer of material may be a layer of porous conductive substrate interfaced with a layer of electrode composite.

[0080] In some embodiments, the electrode composite is at least partially impregnated into the porous conductive substrate. In this way, the layers of the electrode composite are physically separated from each other. In other embodiments, the electrode composite is completely impregnated into the porous conductive substrate. This is done without impairing the extrusion of the porous conductive substrate, i.e., without impairing the passage of the electrode composite from one surface of the porous conductive substrate to the opposite surface of the porous conductive substrate. The impregnation enhances the conductivity of the electrode and prevents dissolution of the material into the electrolyte by sandwiching. This type of electrode is particularly useful for the construction of cathodes for Li-S batteries, where polysulfide dissolution is a challenge, and LiMn2O4 cathodes, where manganese dissolution is a challenge. It also provides room for volume expansion, preventing starvation of the active material, making it very useful for silicon-based anodes.

[0081] In some embodiments, the electrode composite is at least about 10% impregnated into the porous conductive substrate. In this regard, 10% of the thickness (or volume) of the porous conductive substrate comprises the electrode composite. In other embodiments, the electrode composite is at least about 20%, about 30%, about 40%, about 50%, about 60%, about 70%, about 80%, or about 90%, or about 100% impregnated into the porous conductive substrate.

[0082] The electrode composite is arranged such that each planar side thereof is connected to a porous conductive substrate. In this regard, the electrode has a side that faces the exterior and includes the porous conductive substrate. By having the porous conductive substrate on the exterior surface, the inner electrode composite is protected from oxidation.

[0083] The electrodes can be formed from a porous conductive substrate and an electrode composite of substantially the same dimensions. In some embodiments, the layers of the porous conductive substrate and the electrode composite have substantially the same planar area. When formed in this manner, the edges (or sides) of the electrode composite are exposed, i.e., are not covered by the porous conductive substrate.

[0084] Alternatively, the electrode composite can have dimensions smaller than those of the porous conductive substrate. When the electrode composite is applied as a layer centered on the porous conductive substrate, this results in a boundary surrounding the electrode composite. The boundary can have a thickness of about 1 mm to about 10 cm, or about 1 mm to about 9 cm, about 1 mm to about 8 cm, about 1 mm to about 7 cm, about 1 mm to about 6 cm, about 1 mm to about 5 cm, about 1 mm to about 4 cm, about 1 mm to about 3 cm, about 1 mm to about 2 cm, or about 1 mm to about 1 cm.

[0085] In some embodiments, the porous conductive substrate is characterized by a planar area that is about 1% to about 50% greater than the planar area of ​​the layer of electrode composite, in other embodiments, the size difference is about 1% to about 45%, about 1% to about 40%, about 1% to about 35%, about 1% to about 30%, about 1% to about 25%, about 1% to about 20%, about 1% to about 15%, or about 1% to about 10%.

[0086] The formed electrode thus comprises a layer of electrode composite material completely enveloped by a porous conductive substrate, which minimizes the rate of oxidation of the electrode composite material, thus extending the life of the electrode.

[0087] The boundaries can be filled with a binder. In some embodiments, the electrode further comprises a binder in contact with a side of the electrode, which can electrically connect the side of the electrode composite to the porous conductive substrate.

[0088] Electronically conductive binders include conductive polymer binders such as graphene polymer binders and polyfluorene polymer binders, as well as binders with conductive particle additives.

[0089] The binder may be a non-aqueous binder, an aqueous binder, or a combination thereof. There is no particular limitation on the binder, so long as it binds the active material and the conductive material on the current collector and does not simultaneously (or concurrently) degrade electrochemically.

[0090] The non-aqueous binder can be, but is not limited to, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or combinations thereof.

[0091] The aqueous binders can be either natural, modified, or synthetic materials, including but not limited to rubber-based, polymeric resin, or polysaccharide binders. The rubber-based binders can be selected from styrene-butadiene rubber, acrylated styrene-butadiene rubber (SBR), acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber, natural rubber, and combinations thereof. The polymeric resin binders can be selected from ethylene propylene copolymers, epichlorohydrin, polyphosphazenes, polyacrylonitrile, polystyrene, ethylene propylene diene copolymers, polyvinylpyridine, chlorosulfonated polyethylene, polyester resins, acrylic resins, phenolic resins, epoxy resins, polyvinyl alcohol, and combinations thereof.

[0092] The polysaccharide binder may be selected from carboxymethylcellulose, hydroxypropylmethylcellulose, methylcellulose, or alkali metal salts thereof, tragacanth gum, gum arabic, gellan gum, xanthan gum, guar gum, karaya gum, chitosan, sodium alginate, cyclodextrin, starch, and combinations thereof. The alkali metal may be Na, K, or Li. Such cellulose-based compounds may be included in an amount of about 0.1 parts by weight to about 20 parts by weight per 100 parts by weight of the active material. Preferred binders that may be mentioned herein are sodium salts of carboxymethylcellulose, gum arabic, polyvinyl alcohol, or combinations thereof.

[0093] In some embodiments, the binder is gum arabic, polyvinyl alcohol, carboxymethyl cellulose, styrene-butadiene rubber, polyvinylidene fluoride, or a combination thereof.

[0094] An electrode composite is a material made from two or more constituent materials, one of which is a chemically active material involved in the electrochemical charge / discharge reaction. For reference, the theoretical capacity of silicon is 4200 mAh / g. Examples of high capacity materials for lithium-ion electrodes can include various silicon-containing materials, such as crystalline silicon, amorphous silicon, silicides, silicon oxides, secondary oxides, and oxynitrides. Other examples include sulfur and its complexes with carbon, metals or metal oxides, tin-containing materials (such as tin and tin oxide), transition metal sulfides and selenides, germanium-containing materials, carbon-containing materials, various metal hydrides (such as magnesium hydride), silicides, phosphides, and nitrides. Still other examples include carbon-silicon combinations, such as carbon-coated silicon, silicon-coated carbon, silicon-doped carbon, carbon-doped silicon, and alloys containing carbon and silicon. Similar combinations of carbon and germanium, and similar combinations of carbon and tin may be used. Various aluminum-containing materials may be used as well.

[0095] Other examples of active materials for lithium-ion batteries can include lithium cobalt oxide and lithium iron phosphate (e.g., for the cathode) and graphite or other forms of carbon (e.g., for the anode). Structures formed from active materials, including high capacity active materials, may have a variety of shapes and dimensions (e.g., spherical, tubular, fibrous morphology) depending on the composition, crystal structure (e.g., crystalline, amorphous), deposition process parameters, and many other factors. Shape and size may also change during cycling.

[0096] Active materials, including high capacity active materials, can generally be formed into structures whose cross-sectional dimensions are generally less than their fracture limits. In particular embodiments, the cross-sectional dimensions are about 1 nm to 10,000 nm. In some embodiments, the cross-sectional dimensions are about 5 nm to 1000 nm, more specifically 10 nm to 200 nm. These size ranges are generally applicable to silicon, including high capacity active materials, such as amorphous or crystalline silicon.

[0097] Active materials, including high capacity active materials, can be formed into various types of nanostructures having cross-sectional dimensions less than 1,000 nm, i.e., at least one nanoscale dimension. Some examples of nanostructures include nanofilms, which have nanoscale dimensions along one axis, nanowires, which have nanoscale dimensions along two axes, and nanoparticles, which have nanoscale dimensions along all three axes.

[0098] In some embodiments, each layer of the electrode composite is independently characterized by a thickness of about 0.1 μm to about 1000 μm. In other embodiments, the thickness is about 0.2 μm to about 1000 μm, about 0.3 μm to about 1000 μm, about 0.4 μm to about 1000 μm, about 0.5 μm to about 1000 μm, about 0.6 μm to about 1000 μm, about 0.7 μm to about 1000 μm, about 0.8 μm to about 1000 μm, about 0.9 μm to about 1000 μm, about 1 μm to about 1000 μm, about 10 μm to about 1000 μm, about 50 μm to about 1000 μm. m, about 100 μm to about 1000 μm, about 150 μm to about 1000 μm, about 200 μm to about 1000 μm, about 250 μm to about 1000 μm, about 300 μm to about 1000 μm, about 350 μm to about 1000 μm, about 400 μm to about 1000 μm, about 500 μm to about 1000 μm, about 600 μm to about 1000 μm, about 700 μm to about 1000 μm, or about 800 μm to about 1000 μm.

[0099] In some embodiments, the electrode composite comprises a carbon-based material, a metal-based material, a metal oxide-based material, an electrochemically active material, a polymeric material, or a combination thereof.

[0100] In some embodiments, the carbon-based material is selected from natural graphite, synthetic graphite, carbon black, acetylene black, ketjen black, carbon fiber, graphene, or a combination thereof. In some embodiments, the electrode composite comprises conductive nanoparticles. In some embodiments, the conductive nanoparticles comprise graphene, carbon black, acetylene black, carbon nanotubes, metal nanoparticles such as silver nanoparticles, carbon dots, or a combination thereof.

[0101] In some embodiments, the conductive nanoparticles are surface functionalized with different oxidation states of halides, chalcogenides, metals, or combinations thereof. In some embodiments, the graphene nanoplatelets are surface functionalized with sulfur to form an electrochemically active material. The sulfur acts as a redox active material and undergoes redox reactions via a conversion process. This can be used as a cathode against a low voltage anode such as Li metal in Li-S batteries, or as an anode against a high voltage cathode.

[0102] In some embodiments, the electrode composite includes a metal-based material. The metal-based material can be a bulk metal, a metal powder, a metal fiber, and / or a metal-based material. For example, metals such as copper, nickel, aluminum, silver, niobium, etc. can be used.

[0103] The electrode composite may be impregnated into the porous conductive substrate in dry powder form (solid state). In this regard, no other components such as polymer binders, solvents, or additional conductive materials (optionally in slurry form) are added. This simplifies the manufacturing process and further improves its areal capacity, volumetric energy density and / or gravimetric energy density. Alternatively, the electrode composite may be added as a slurry (wet form). In these cases, other components such as polymer binders, solvents, or conductive materials may be added to improve its flow and dispersion properties.

[0104] In some embodiments, the electrode composite is characterized by the absence of a conductive polymer. In some embodiments, the electrode composite includes a conductive polymer. The conductive polymer may be polyphenylene and its derivatives.

[0105] In some embodiments, the electrode composite is characterized by the absence of conductive nanoparticles. In some embodiments, the weight ratio of the conductive nanoparticles to the electrode composite is about 1% to about 50% by weight, about 3% to about 50% by weight. In other embodiments, the weight ratio is about 5% to about 40% by weight, about 6% to about 30% by weight, about 70% to about 20% by weight, about 8% to about 15% by weight, about 9% to about 10% by weight. In some embodiments, the weight ratio is about 50% by weight, about 40% by weight, about 30% by weight, about 20% by weight, about 10% by weight, about 5% by weight, or less than about 1% by weight. In some embodiments, the weight ratio of the conductive nanoparticles to the electrode composite is about 10% by weight.

[0106] In some embodiments, the electrode composite is characterized by the absence of additives. The electrode composite may include other additives. In some embodiments, the electrode composite further includes a conductive filler. The conductive filler helps to improve electrical contact between the active materials in the electrode, thereby reducing the overall electrode impedance.

[0107] In some embodiments, the conductive filler is a carbon nano object such as conductive carbon, graphene nanoplatelets, silver nanoparticles, carbon nanotubes, carbon fibers, etc. Any conductive material can be used as the conductive material as long as it does not cause a chemical change, examples of which may be natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, carbon fibers, graphene and / or similar carbon-based materials, copper, nickel, aluminum, silver, niobium and / or similar metal powders or metal fibers and / or similar metal-based materials, polyphenylene derivatives and / or similar conductive polymers, and / or mixtures thereof.

[0108] In some embodiments, the electrode composite is characterized by the absence of conductive filler. In some embodiments, the weight ratio of the conductive filler to the electrode composite is about 1% to about 30% by weight. In some embodiments, the weight ratio of the conductive filler to the electrode composite is about 1% to about 20% by weight. In some embodiments, the weight ratio is about 30%, about 25%, about 20%, about 15%, about 10%, about 5%, or less than about 1% by weight. In some embodiments, the weight ratio of the conductive filler to the electrode composite is about 10% by weight.

[0109] In some embodiments, the electrode composite is characterized by the absence of a binder. The electrode composite can further include a binder for adhering the active material to the current collector substrate. In some embodiments, the electrode composite further includes a binder.

[0110] The binder may be a non-aqueous binder, an aqueous binder, or a combination thereof. There is no particular limitation on the binder, so long as it binds the active material and the conductive material on the current collector and is not electrochemically degraded (or both).

[0111] The non-aqueous binder can be, but is not limited to, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or combinations thereof.

[0112] The aqueous binders can be either natural, modified, or synthetic materials, including but not limited to rubber-based, polymeric resin, or polysaccharide binders. The rubber-based binders can be selected from styrene-butadiene rubber, acrylated styrene-butadiene rubber (SBR), acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber, natural rubber, and combinations thereof. The polymeric resin binders can be selected from ethylene propylene copolymers, epichlorohydrin, polyphosphazenes, polyacrylonitrile, polystyrene, ethylene propylene diene copolymers, polyvinylpyridine, chlorosulfonated polyethylene, polyester resins, acrylic resins, phenolic resins, epoxy resins, polyvinyl alcohol, and combinations thereof.

[0113] The polysaccharide binder may be selected from carboxymethylcellulose, hydroxypropylmethylcellulose, methylcellulose, or alkali metal salts thereof, tragacanth gum, gum arabic, gellan gum, xanthan gum, guar gum, karaya gum, chitosan, sodium alginate, cyclodextrin, starch, and combinations thereof. The alkali metal may be Na, K, or Li. Such cellulose-based compounds may be included in an amount of about 0.1 parts by weight to about 20 parts by weight per 100 parts by weight of the active material. Preferred binders that may be mentioned herein are sodium salts of carboxymethylcellulose, gum arabic, polyvinyl alcohol, or combinations thereof.

[0114] In some embodiments, the binder is gum arabic, polyvinyl alcohol, or a combination thereof. In some embodiments, the binder is polyvinylidene fluoride, gum arabic, cellulose gum, polyvinyl alcohol, carboxymethyl cellulose, styrene-butadiene rubber, or a combination thereof.

[0115] In some embodiments, the ratio of gum arabic to polyvinyl alcohol is about 1:1.

[0116] In some embodiments, the electrode composite is characterized by the absence of a binder. In some embodiments, the weight ratio of the binder to the electrode composite is about 1% to about 20% by weight. In other embodiments, the weight ratio is about 2% to about 20% by weight, about 4% to about 20% by weight, about 6% to about 20% by weight, about 8% to about 20% by weight, about 10% to about 20% by weight, about 10% to about 18% by weight, about 10% to about 16% by weight, about 10% to about 14% by weight, or about 10% to about 12% by weight. In some embodiments, the weight ratio is about 20% by weight, about 18% by weight, about 16% by weight, about 15% by weight, about 10% by weight, about 5% by weight, or less than about 1% by weight. In some embodiments, the weight ratio of the binder to the electrode composite is about 10% by weight.

[0117] The electrode may include multiple layers of electrode composite. In other embodiments, there are at least three layers. In all of these embodiments, each electrode composite layer is separated from the other by a porous conductive substrate, which forms at least the outer planar surface of the electrode. The electrode composite layers may be the same or may each include different active materials and / or additives to provide different capacities for each layer.

[0118] As used herein, a "substrate" is a surface capable of carrying out or supporting a chemical reaction. Thus, a porous conductive substrate provides a porous surface that is also conductive to an electric charge. The substrate can be a flat sheet (in a macroscopic sense) of various thicknesses.

[0119] The porous conductive substrate or porous current collector material is a material that has a higher electronic conductivity than the active material. In some embodiments, the current collector layer, if present, may have a conductivity equal to or less than that of the current collector substrate. In some embodiments, the material is such that the contact resistance per unit surface area of ​​the current collector layer is less than 10 ohms-centimeter squared.

[0120] Examples of materials include metals such as copper, nickel, chromium, tungsten, metal nitrides, metal oxides, metal carbides, carbon, conductive polymers, and combinations thereof. In some implementations, the current collector layer can be a nanomaterial network, including nanofiber, nanowire, and nanotube networks. Further examples of nanomaterial networks can include networks of spheres, cones, rods, tubes, wires, arcs, belts, saddles, flakes, ellipsoids, meshes, laminated foams, tapes, and combinations thereof. The network can be a non-uniform continuous film in some implementations. That is, the film provides one or more continuous conductive paths while allowing electrochemical species to be transported through the film. An electronically conductive binder can also be added to any of the current collectors described herein. Additionally, combinations of materials described herein can be used to form the current collector layer.

[0121] In some embodiments in which the current collector layer is nanostructured, the nanostructures may be oriented such that their longest dimension extends in a direction approximately parallel to the underlying layer or to the plane of the current collector substrate, if present.

[0122] As described above, in some embodiments, the current collector layer comprises carbon. The carbon may be, for example, carbon fibers or tubes, graphite, graphene, and / or carbon sheets. In one configuration, the carbon is in the form of linear carbon nanostructures, such as nanofibers or nanotubes. The nanostructures can form a network on the active material layer. In another configuration, the carbon is in the form of graphene sheets, including one or more layers of graphene. In another configuration, the carbon is in the form of amorphous carbon.

[0123] In some implementations, the current collector layer comprises a metal, such as copper or nickel. In one configuration, the metal is in the form of linear nanostructures, such as nanowires. The nanostructures can form a mesh on the active material layer. In another configuration, the metal is in the form of thin sheets that include one or more atomic layers of the metal. In such configurations, the thin sheets can be non-uniformly distributed.

[0124] In some embodiments, the porous conductive substrate is a non-metallic porous conductive substrate, which prevents side reactions (e.g., oxidation of Cu, Fe, Ni) or plating typically observed with metal current collectors (e.g., aluminum).

[0125] In some embodiments, the porous conductive substrate is selected from carbon paper, carbon cloth, carbon foam, carbon fiber, porous metal structures, grids and foams, porous conductive polymers, conductive polymer gels and aerogels, thin films, or combinations thereof.

[0126] Porosity is a measure of the void (i.e., "empty") space in a material, and is the ratio of void volume to total volume, ranging from 0 to 1, or as a percentage, from 0% to 100%. Porosity can be measured, for example, using confocal microscopy, profilometers, AFM, or gas absorption spectrometry (such as gas absorption porosimetry).

[0127] In some embodiments, the porous conductive substrate has a pore size of about 1 nm to about 20,000 nm. In other embodiments, the pore size is about 100 nm to about 20,000 nm, about 200 nm to about 20,000 nm, about 300 nm to about 20,000 nm, about 400 nm to about 20,000 nm, about 500 nm to about 20,000 nm, about 500 nm to about 18,000 nm, about 500 nm to about 15,000 nm, about 500 nm to about 10,000 nm, about 500 nm to about 5,000 nm, or about 500 nm to about 2,000 nm.

[0128] In some embodiments, the porous conductive substrate has a through-plane air permeability of about 10 to about 50 Gurley units. Gurley seconds or Gurley units are units that express air permeability as a function of the time required for a specified amount of air to pass through a specified area of ​​a separator under a specified pressure. Specifically, it is defined as the number of seconds required for 100 cubic centimeters (1 deciliter) of air to pass through 1.0 square inch of a given material with a pressure difference of 4.88 inches of water (0.176 psi) (ISO 5636-5:2003). In other embodiments, the through-plane air permeability is about 15 to about 50 Gurley units, about 15 to about 45 Gurley units, about 20 to about 45 Gurley units, about 25 to about 45 Gurley units, about 30 to about 45 Gurley units, or about 30 to about 40 Gurley units. In other embodiments, the through-plane air permeability is about 35 Gurley units.

[0129] In some embodiments, the porous conductive substrate has a porosity of about 30% to about 90%. In other embodiments, the porosity is about 40% to about 90%, about 50% to about 90%, about 60% to about 90%, about 70% to about 90%, or about 80% to about 90%.

[0130] In some embodiments, the porous conductive substrate has an apparent porosity of about 60% to about 90%. Apparent porosity can be defined as the amount of voids (or pores) present in a volume of a porous solid. In other embodiments, the apparent porosity is about 65% to about 90%, about 70% to about 90%, about 70% to about 85%, or about 75% to about 80%.

[0131] In some embodiments, the porous conductive substrate has a connected porosity of about 50% to about 90%. Connected porosity can be defined as void space where there is an uninterrupted pathway between the boundaries of the substrate volume or subvolumes. Connected porosity can be measured by the volume of gas or liquid that can flow into the rock, but the fluid cannot access the unconnected pores. In other embodiments, the connected porosity is about 50% to about 85%, about 50% to about 80%, about 50% to about 75%, or about 55% to about 75%.

[0132] In some embodiments, the porous conductive substrate is surface functionalized. In some embodiments, the porous conductive material is functionalized with transition metal sulfides, transition metal selenides, halides, metal ions, nanoparticles, metal oxides, or combinations thereof. In some embodiments, the porous conductive substrate is functionalized with transition metal sulfides or selenides (e.g., NbS2, MoS2, CoS2, NbSe2) or halides (e.g., F, Cl, br) or metal ions / nanoparticles (e.g., Cu, Al, Li, K, Na, Ag, Au, Ti, W, Ta, Nb) or metal oxides (e.g., Ti4O7, TiO2, SiO2, Al2O3).

[0133] In some embodiments, the porous conductive substrate between the electrode composite and the terminal is independently characterized by a thickness of about 10 μm to about 1000 μm. In other embodiments, the thickness is about 10 μm to about 900 μm, about 10 μm to about 800 μm, about 10 μm to about 700 μm, about 10 μm to about 600 μm, about 10 μm to about 500 μm, about 10 μm to about 400 μm, about 10 μm to about 300 μm, or about 10 μm to about 200 μm. For example, when carbon paper is used, the thickness of one sheet of carbon paper is about 115 μm. Multiple sheets of carbon paper can be used. Two sheets of carbon paper are stacked and compressed to obtain a thickness of about 175 μm.

[0134] In some embodiments, the electrodes are characterized by the absence of a separator between the electrode composites. The separator is a permeable membrane disposed between the electrode composites. The separator functions to keep the two electrode composites apart to prevent electrical communication while allowing the transport of ionic charge carriers necessary to close the circuit during the passage of current in the electrochemical cell. A separator may be required between the anode and cathode only during assembly of the cell, and the separator can be fabricated separately from the laminated electrodes. Typical separators are polypropylene, polyethylene, nylon, etc.

[0135] For example, two sheets of carbon paper can be used as porous conductive substrates to sandwich a layer of electrode composite. After lamination, the final thickness of the entire electrode (two sheets of carbon paper + electrode material) can be the same as one sheet of carbon paper alone. In this way, the volumetric energy density is not compromised.

[0136] In some embodiments, when the electrode includes sulfur as the active material, it has an active capacity of about 50 mAh g 活物質 -1 ~About 4000mAh g 活物質 -1 In another embodiment, the discharge capacity is about 200 mAh g S -1 ~Approx. 1,450mAh g S -1 , about 200mAh g S -1 ~Approx. 1,300mAh g S -1 , about 200mAh g S -1 ~Approx. 1,250mAh g S -1 , about 400mAh g S -1 ~Approx. 1,250mAh g S -1 , about 600mAh g S -1 ~About 1250mAh g S -1 , about 700mAh g S -1 ~About 1250mAh g S -1 , or about 800mAh g S -1 ~About 1250mAh g S -1 In some embodiments, the electrode has a capacity of about 1,240 mAh g S -1 It is characterized by the discharge capacity.

[0137] In some embodiments, when the electrode comprises NMC811 (composition: 80% nickel, 10% manganese, 10% cobalt), the capacity is about 200 mAh g 活物質 -1 It is characterized by the discharge capacity.

[0138] In some embodiments, the electrode has a capacitance of about 2 mAh cm -2 ~about 100mAh cm -2 In another embodiment, the areal capacity is about 3 mAh cm -2 ~about 50mAh cm -2 , about 4mAh cm -2 ~about 25mAh cm -2 , about 5mAh cm -2 ~about 20mAh cm -2 , about 6mAh cm -2 ~about 10mAh cm -2 , about 7mAh cm -2 ~about 10mAh cm -2 , or about 8mAh cm -2 ~about 10mAh cm -2 It is.

[0139] In some embodiments, the electrode has a capacity of about 500 Wh L -1 ~About 1000Wh L -1 In another embodiment, the volumetric energy density is about 300 Wh L -1 ~about 800Wh L -1 , about 400Wh L -1 ~about 800Wh L -1 , about 500Wh L -1 ~about 800Wh L -1 , about 600Wh L -1 ~about 800Wh L -1 , or about 700Wh L -1 ~about 800Wh L -1 It is.

[0140] In some embodiments, the electrode has a capacity of about 40 Wh kg -1 ~ approx. 600Wh kg -1In another embodiment, the gravimetric energy density is about 100 Wh kg -1 ~ approx. 600Wh kg -1 , about 150Wh kg -1 ~ approx. 600Wh kg -1 , about 200Wh kg -1 ~ approx. 600Wh kg -1 , about 250Wh kg -1 ~ approx. 600Wh kg -1 , about 300Wh kg -1 ~ approx. 600Wh kg -1 , about 350Wh kg -1 ~ approx. 600Wh kg -1 , about 400Wh kg -1 ~ approx. 600Wh kg -1 , about 450Wh kg -1 ~ approx. 600Wh kg -1 , or about 500Wh kg -1 ~ approx. 600Wh kg -1 It is.

[0141] In some embodiments, the electrodes have a capacitance of about 1.5 S cm -1 ~about 100S cm -1 In another embodiment, the electronic conductivity is about 1.5 S cm -1 ~about 100S cm -1 , about 2S cm -1 ~about 100S cm -1 , about 5S cm -1 ~about 100S cm -1 , about 10S cm -1 ~about 100S cm -1 , about 20S cm -1 ~about 100S cm -1 , about 30S cm -1 ~about 100S cm -1 , about 40S cm -1 ~about 100S cm -1 , about 50S cm -1 ~about 100S cm -1 , about 60S cm -1 ~about 100S cm -1 , about 70S cm -1~about 100S cm -1 , or about 80S cm -1 ~about 100S cm -1 It is.

[0142] In some embodiments, the electrode is characterized by a capacity loss of about 5% to about 50% relative to the initial capacity of the electrode, in other embodiments, the capacity loss is about 5% to about 45%, about 5% to about 40%, about 5% to about 35%, about 5% to about 30%, about 5% to about 25%, about 5% to about 20%, or about 5% to about 15%.

[0143] In some embodiments, the electrodes are characterized by a coulombic efficiency of about 70% to about 100%. In other embodiments, the coulombic efficiency is about 75% to about 100%, about 80% to about 100%, about 85% to about 100%, about 90% to about 100%, or about 95% to about 100%.

[0144] In some embodiments, the electrodes are characterized by a cycle life of greater than 40 cycles.

[0145] In some embodiments, when sulfur is the active material, the electrode has a cycle life of more than 40 cycles at a current rate of about 0.25, about 900 mAh g S -1 The device is characterized by a discharge capacity of 1000 mAh and a coulombic efficiency of over 90%.

[0146] In some embodiments, the electrode further comprises a junction adapted to pass through the electrode. For example, the junction may pass through the electrode. In some embodiments, the junction is adapted to pass through a through hole that can be formed in the electrode.

[0147] The joint serves to electrically connect the electrode to other components of the battery, cell or electrical system. The inventors have further found that peculiarities regarding the properties of certain materials used as current collectors or free-standing electrodes (e.g., used in solid-state batteries) that prohibit contact tabs or leads from being attached to them (or at least limit their connectivity) are due to the welding methods commonly used in this field. Examples of such materials are carbon-based current collectors (e.g., carbon paper, carbon foam, carbon cloth, carbon fiber, etc.) and alkali and alkaline earth metal / alloy electrode foils. To this end, the inventors have found that joints can be used to overcome or at least ameliorate these problems.

[0148] For example, a joint can be used to connect / bond / join one or more electrodes to one another. A joint can also be used to connect one or more electrodes to a contact tab / lead. A joint can also be used to connect one or more leads from individual cells to a contact tab to achieve physical contact between them. By using a joint, the need for welding is avoided. A joint allows for a mechanical resistance connection between the current collector and the metal tab / lead and does not impair or change the conductivity of the entire system (tab / lead + current collector). The conductivity measured through only the current collector is the same as when measured with the joint / tab (Figure 9), so this shows that the joint does not impair the conductivity.

[0149] The use of the joint instead of the high heat that melts the parts together causing fusion during welding allows the use of non-weldable materials as current collectors for the electrodes (e.g., carbon-based current collectors and alkali and alkaline earth metal / alloy electrode foils). The joint can also be integrated into the manufacturing process as a simple and automatable method, and is therefore scalable. It consumes less energy compared to welding, saving energy and reducing costs. The joint was found to provide a more robust and durable joint compared to welding, resulting in lower battery failures and batch rejections, and suitable for flexible batteries and fragile electrodes. The joint is customizable, and therefore can be used for a variety of battery applications, configurations, and chemistries. The joint is also suitable for use in liquid electrolyte batteries and solid-state batteries. In addition, excessive energy loss and localized heating due to the uncontrolled formation of the weld are also avoided.

[0150] In some embodiments, the junction comprises a body adapted to substantially penetrate the electrode, for example, the body may comprise at least one tapered end for penetrating the electrode.

[0151] In some embodiments, the body is characterized by a cross-sectional shape selected from a circle, an ellipse, or a polygon. The polygon may be a triangle, a square, a diamond, a rectangle, a star, a pentagon, or a hexagon. Using different cross-sectional shapes can increase the surface area so that more contact points can be created.

[0152] In some embodiments, the body is hollow.

[0153] In some embodiments, the body is characterized by a polygonal cross-sectional shape, and if hollow, the body includes legs extending from edges of the polygon.

[0154] In some embodiments, the joint further comprises a head at the first end of the body, the head preventing the body from being detached from the electrode at the first end of the body.

[0155] In some embodiments, the body is deformable to form a head. In other embodiments, the body is deformable to form a head at a second end of the body, which secures the junction with the electrode, wherein the length of the body is greater than the thickness of the electrode.

[0156] In some embodiments, the joint comprises a conductive material. In some embodiments, the conductive material is selected from a metal, an alloy, or a composite. In some embodiments, the conductive material is selected from stainless steel, Al, Ti, Ni, or Cu. In some embodiments, when the electrode is a cathode, the conductive material is selected from stainless steel, Al, Ti, or Ni. In some embodiments, when the electrode is an anode, the conductive material is selected from stainless steel, Ni, or Cu.

[0157] In some embodiments, the junction is adapted to electrically connect two or more electrodes. In some embodiments, the junction is adapted to electrically connect at least one electrode to at least one contact tab. In some embodiments, the junction is adapted to electrically connect at least one electrode to at least one lead. In some embodiments, the junction is adapted to electrically connect at least one contact tab to at least one lead on the electrode. The junction can also be used to electrically connect at least one contact tab on the electrode to at least one lead. The junction can also be used to electrically connect at least one contact tab to at least one lead.

[0158] The present invention also provides an electrode and a junction passing through the electrode.

[0159] In some embodiments, the electrode includes a through hole and the joint passes through the through hole of the electrode.

[0160] The present invention also provides a joint as disclosed herein.

[0161] The present invention relates to a) forming at least one electrode layer, the at least one electrode layer being formed by coating a layer of an electrode composite material on at least a surface of a porous conductive substrate; b) laminating at least one electrode layer with another porous conductive substrate such that a layer of electrode composite is sandwiched between the porous conductive substrates, the at least one electrode layer being in electrical communication with the porous conductive substrate; Including, A method of making an electrode is provided in which the electrode composite is at least partially impregnated into a porous conductive substrate.

[0162] In some embodiments, the method further comprises the step of laminating another electrode layer on the porous conductive substrate of step a) or b). The electrode layer may be laminated on the surface of the porous conductive substrate. The surface may be an exposed surface, i.e., not coated with the electrode composite material. In this way, multiple electrode layers can be built up to form a single electrode. This step can then be repeated to increase the electrode layers of the electrode.

[0163] In some embodiments, a method of manufacturing an electrode comprises the steps of: a) forming at least two electrode layers, each electrode layer being formed by coating a layer of an electrode composite material on at least a surface of a porous conductive substrate; b) laminating the electrode layer with another porous conductive substrate such that each layer of electrode composite is sandwiched between the porous conductive substrates, at least two electrode layers being in electrical communication with the porous conductive substrate; Including, The electrode composite at least partially impregnates the porous conductive substrate.

[0164] The electrode layers may be stacked adjacent to one another such that the layer of electrode composite on the first electrode layer faces the uncoated side of the porous conductive substrate of the second electrode layer, thereby forming two electrode layers parallel to one another.

[0165] In some embodiments, the method further comprises the step of laminating another electrode layer on the porous conductive substrate of step a) or b). The electrode layer may be laminated on the surface of the porous conductive substrate. The surface may be an exposed surface, i.e., not coated with the electrode composite material. In this way, multiple electrode layers can be constructed to form a single electrode. Thus, this step can be repeated to increase the electrode layer of the electrode to three or more layers.

[0166] In some embodiments, the electrode composite is provided as a slurry, dough, paste, or powder.

[0167] In some embodiments, the step of forming the electrode layer comprises drying the electrode composite.

[0168] In some embodiments, when the electrode layer is a slurry, it is dried for about 2 hours to about 24 hours, in other embodiments, the period is about 4 hours to about 24 hours, about 6 hours to about 24 hours, about 8 hours to about 24 hours, about 10 hours to about 24 hours, about 12 hours to about 24 hours, about 12 hours to about 20 hours, about 14 hours to about 20 hours, or about 16 hours to about 20 hours.

[0169] In some embodiments, when the electrode layer is a slurry, it is dried at about 40° C. to about 80° C. In other embodiments, the temperature is about 50° C. to about 80° C., or about 50° C. to about 70° C. In some embodiments, the electrode layer is dried at about 60° C.

[0170] In some embodiments, the electrode composite has a density of about 1 mg cm -2 ~about 100mg cm -2In another embodiment, the mass loading is about 1 mg cm. -2 ~about 90mg cm -2 , about 2mg cm -2 ~about 80mg cm -2 , about 3mg cm -2 ~about 70mg cm -2 , about 4mg cm -2 ~about 60mg cm -2 , about 5mg cm -2 ~about 50mg cm -2 , or approximately 10 mg cm -2 ~about 30mg cm -2 In some embodiments, the electrode composite has a surface area of ​​about 10 mg cm -2 is characterized by a mass loading on the surface of the porous conductive substrate of

[0171] In some embodiments, the laminating step includes applying a compressive force to the electrode layer and another porous conductive substrate. The compressive force allows the electrode composite to at least partially impregnate the porous conductive substrate. In some embodiments, the compressive force is provided by a hydraulic press, a weight press, a roller press, or a pneumatic press. In some embodiments, the laminating step includes laminating the electrode layer and another porous conductive substrate.

[0172] In some embodiments, the method further comprises connecting the junction to an electrode.

[0173] In some embodiments, the joint is connected to the electrode via punching or via a through hole formed in the electrode.

[0174] In some embodiments, the joint comprises a body, the body being deformable to form a head.

[0175] In some embodiments, the body is deformed by bending an end of the body so that the head is substantially parallel to a surface of the electrode, hi some embodiments, the body is bent in a direction away from the longitudinal axis of the body.

[0176] The present invention also provides a method of connecting a junction to an electrode, comprising the steps of: a) passing the body of the junction through an electrode; b) deforming the body of the joint to form a head for connecting the joint to an electrode; The present invention provides a method comprising:

[0177] Production of individual electrode layers An electrode composition consisting of active material, conductive material, binder, and any other additives required for optimal performance of the electrode can be coated or deposited onto a porous conductive substrate to produce an individual electrode layer (IEL) (Figure 1).

[0178] The IELs can be coated with similar or different amounts of active material on one or both sides of the porous conductive substrate. The IELs can be coated to cover the entire longitudinal surface of the substrate. Alternatively, the coating can be done so that a small portion of the substrate remains uncoated (thus forming a border surrounding the IEL) to ensure electronic contact with the side edges of the coating. Another possibility to ensure electronic contact is to glue or adhere using a conductive adhesive or paste (adhesive or paste or binder containing silver nanoparticles, copper nanoparticles, graphene or carbon nanotubes or conductive carbon materials) or clamp the substrates together using a conductive material made of Al, Cu, Ni, Ti, Pb or W.

[0179] Production of laminated electrodes (SE) The IELs are placed one above the other such that the coated surfaces with the electrode composites face each other and the outer surfaces of the IELs are the uncoated surfaces of the substrate. Depending on the number of stacks, multiple double-sided coated layers of IELs can be stacked between two single-sided coated IELs (Figure 1).

[0180] The stacked IELs are then pressed together to form the SE. No separators are placed between the IEL stacks. The lamination process can be carried out using a hydraulic / pneumatic press for batch production of SEs or a roller press for continuous production of SEs (Figure 2).

[0181] As a conductive substrate or current collector (CC), the substrate material is an electronic conductor and allows the passage of ions through its structure. For example, carbon paper, carbon cloth, carbon foam, porous metal structures (e.g., metal foams), porous conductive polymers, conductive polymer gels and aerogels, thin films (e.g., produced by deposition methods such as CVD, PVD, TVD, among others), etc. can be used as current collectors.

[0182] The final SE does not require a coating on the external surface. It was found that the substrate helps to retain electrolyte soluble and electrochemically active species, thus encapsulating the ECM between the stacks, preventing, for example, irreversible capacity loss during active material dissipation, and polysulfide shuttle in the case of Li-S batteries. The surface of the current collector can be functionalized or activated to improve its action to address this issue. Nevertheless, an electronically conductive binder can also be coated on the areas not coated by the ECM to ensure electronic contact and sealing of the ECM to the stack configuration.

[0183] Figure 3 shows the first specific discharge capacity at 0.05 current rate of a battery cell made with two individual electrodes stacked together to form a single cathode electrode. The first discharge capacity was 1,240 mAh g S-1 Figure 4 shows the specific discharge capacity over 40 cycles at a current rate of 0.25 for the same cell. The cell achieved a discharge capacity of 930 mAh g over this test. S -1 average capacity and over 90% coulombic efficiency.

[0184] Thus, the electrodes of the present invention can improve energy and / or power density, thus helping to solve the problems of active material underutilization and cell polarization associated with thicker electrodes. Furthermore, the electrodes of the present invention can also improve capacity retention, which is one of the major problems seen in the capacity degradation of battery electrodes, where the electrochemically active material loses electronic contact with the electrode due to structural collapse of the coating due to dissolution in the electrolyte or volume expansion-related stresses. These electrodes can also be used in liquid and gel-polymer electrolyte configurations. The disclosed methods are also scalable and therefore suitable for manufacturing.

[0185] Connection joint The joint may be constructed from one or more parts and may or may not have a pre-fitted head (FIG. 5A). The joint may be made from conductive materials (e.g., metals, alloys, and composites) to ensure overall electrical conductivity.

[0186] Preferably, the joints should be made from materials that are non-reactive with respect to the electrolyte and electrodes of the particular electrochemical cell they are used in. For example, in a Li-S battery, aluminum is preferably used for the cathode and copper or nickel for the anode.

[0187] Electrochemical cells have different sizes and configurations. The proposed joints are agnostic with respect to the geometric shape. For example, the joints can be made in wire shape, plate shape, hollow cylinder shape, hollow square shape, hollow triangle shape, hollow hexagon shape, etc. (examples in Figure 5B and Figure 5C). It is often desirable to reduce the weight of the non-active material on the electrochemical cell. In this respect, the shape of the legs of the joints can be optimized to reduce the weight. For example, the size can be reduced or flanges / holes can be made in the legs of the joints to remove the material content and thereby the weight (example in Figure 5B).

[0188] The proper shape and size must be selected to ensure that the contact between the components will last longer than the electrochemical cell in which they are inserted.

[0189] For example, for a typical Li-ion pouch cell with dimensions of 40 x 20 x 3.5 mm (L x W x H) with a lifespan of 1,000 cycles and tabs / leads with width of 2 mm, the joints can have the shape of a bifurcated fastener connected by a head and can be made from stainless steel, Al, Ti, or Ni for the cathode and stainless steel, Ni, or Cu for the anode. In this case, the joints should have a durability of at least 1,000 cycles (method example in Figure 6).

[0190] For example, a pouch cell with dimensions of 290 x 216 x 7.1 mm (L x W x H) can be inserted into holes (preformed or not) through which electrodes, tabs, and / or leads pass, and can use ring-shaped (cylindrical) or edge strip-shaped (e.g., cubic, hexagonal, triangular, etc.) joints that are flared / collared / bent on each side (example of method in Figure 7).

[0191] For joining mechanically fragile, thin, or delicate electrodes, tabs, and / or leads, a joint with two heads and one body can be used to promote higher mechanical stability and resistance to the joining process. This class of joint is composed of two or more parts (Figure 8 shows an example of three parts). EXAMPLES

[0192] Manufacturing of laminated electrodes (SE) for Li-S batteries The positive electrode IEL used in the Li-S battery was prepared as follows. Electrode composition: 80 wt% sulfur graphene nanoplatelets, 10 wt% conductive carbon, and 10 wt% polyvinylidene fluoride (PVDF) as binder. Substrate: Conductive carbon paper ·Mass load: 3mg cm -2 Multiple IELs were fabricated and dried overnight at 60° C. before lamination. Two IELs were laminated together using a hydraulic press. EXAMPLES

[0193] Manufacturing of laminated electrodes (SE) for Li-S batteries The positive electrode IEL used in the Li-S battery was prepared as follows. Electrode composition: 100% sulfur graphene nanoplatelets by weight Substrate: Conductive carbon paper ·Mass loading amount: 1~6mg cm -2 The dried electrode composite was laminated between porous current collectors using a hydraulic press.

[0194] The laminated electrode in this example comprises two substrates and one layer of electrode composite. Figure 10 shows the specific discharge capacity of a cell made using this electrode, which indicates the performance of the electrode under cycling.

[0195] FIG. 11 shows that the charge / discharge profile of the electrode formed using the dry powder method is similar to that obtained by the slurry coating method (FIG. 3). EXAMPLES

[0196] Electrochemical testing of SE in Li-S batteries As an example, the SE obtained from Example 1 was evaluated for its electrochemical performance against Li metal as counter and reference electrodes. The cell configuration was kept as standard as possible to evaluate the performance of the as-synthesized material and to compare with technical literature, which means that the cell was not optimized or configured to improve capacity, rate capability, cycle life, etc., which also depend on many factors such as cathode composition, electrolyte composition, additives, electrolyte / sulfur ratio, interlayer, etc.

[0197] Electrochemical Test Procedure for Coin Cell CR2032: Cathode: SE cathode as described in Example 1 Separator: Celgard 2325 Electrolyte composition: 1M lithium bis(trifluoromethanesulfonyl)imide in 1,2-dimethoxyethane:1,2-dioxolane (1:1 v / v) Electrolyte volume: 40uL Constant current cycler: Neware, model BTS4000, room temperature, discharge cutoff voltage 1.8V, and charge end voltage 2.37V

[0198] It will be understood that many further modifications and permutations of various aspects of the described embodiments are possible, and the described aspects are therefore intended to embrace all such alterations, modifications, and variations that fall within the spirit and scope of the appended claims.

[0199] Throughout this specification and the claims that follow, unless the context requires otherwise, the word "comprises," and variations such as "comprises" and "comprising," are understood to mean the inclusion of a stated integer or step or group of integers or steps but not to the exclusion of any other integer or step or group of integers or steps.

[0200] Throughout this specification and the claims that follow, unless the context requires otherwise, the phrase "consisting essentially of" and variations such as "consists essentially of" are understood to indicate that the recited elements are essential, i.e., required elements of the invention. This phrase allows for the presence of other unrecited elements that do not materially affect the characteristics of the invention, but excludes additional unspecified elements that would affect the basic and novel characteristics of the defined method.

[0201] Reference in this specification to any prior publication (or information derived therefrom) or any known matter is not, and should not be construed as, an acknowledgement or admission, or any form of suggestion, that the prior publication (or information derived therefrom) or known matter forms part of the common general knowledge in the field of endeavor to which this specification pertains.

Claims

1. a) a plurality of porous conductive substrates; b) at least one layer of an electrode composite material sandwiched between and in electrical communication with said plurality of porous conductive substrates; Equipped with The electrode, wherein the electrode composite material at least partially impregnates the plurality of porous conductive substrates.

2. 10. The electrode of claim 1, wherein the plurality of porous conductive substrates and at least one layer of the electrode composite are laminated together.

3. 3. The electrode of claim 1 or 2, wherein the at least one layer of electrode composite is at least two layers of electrode composite.

4. 4. The electrode of claim 1, wherein the plurality of porous conductive substrates and the layer of electrode composite have substantially the same planar area or the porous conductive substrate is characterized by a planar area that is from about 1% to about 50% greater than the planar area of ​​the layer of electrode composite.

5. 5. The electrode of claim 1, further comprising a binder in contact with a side of the electrode to electronically connect the side of the electrode composite to the porous conductive substrate.

6. 6. The electrode of claim 1, wherein the porous conductive substrate is surface functionalized with a transition metal sulfide, a transition metal selenide, a halide, a metal ion, a nanoparticle, a metal oxide, or a combination thereof.

7. 7. The electrode of any one of claims 1 to 6, wherein each layer of the porous conductive substrate is independently characterized by a thickness of from about 10 μm to about 1000 μm.

8. 8. The electrode of any one of claims 1 to 7, wherein the porous conductive substrate is selected from carbon papers, carbon cloths, carbon foams, carbon fibers, porous metal structures, grids and foams, porous conductive polymers, conductive polymer gels and aerogels, thin films, or combinations thereof.

9. 9. The electrode of any one of claims 1 to 8, wherein each layer of the electrode composite is independently characterized by a thickness of from about 0.1 μm to about 1000 μm.

10. 10. The electrode of claim 1, wherein the electrode composite is characterized by the absence of conductive materials, binders, fillers, or combinations thereof.

11. 10. The electrode of claim 1, wherein the electrode composite comprises conductive nanoparticles selected from graphene, carbon black, acetylene black, carbon nanotubes, metal nanoparticles, carbon dots, or combinations thereof.

12. 12. The electrode of claim 11, wherein the conductive nanoparticles are surface functionalized with different oxidation states of halides, chalcogenides, metals, or combinations thereof.

13. 13. The electrode according to claim 11 or 12, wherein the weight ratio of conductive nanoparticles to the electrode composite is from about 3% to about 50% by weight, or preferably about 10% by weight.

14. 14. The electrode of any one of claims 1 to 9 or 11 to 13, wherein the electrode composite further comprises a conductive filler selected from a conductive carbon-based material, a metal, or a combination thereof.

15. 15. The electrode of claim 14, wherein the weight ratio of the conductive filler to the electrode composite is from about 1% to about 30% by weight, or preferably about 10% by weight.

16. 16. The electrode of any one of claims 1 to 9 or 11 to 15, wherein the electrode composite further comprises a binder selected from polyvinylidene fluoride, gum arabic, polyvinyl alcohol, carboxymethyl cellulose, styrene butadiene rubber, or combinations thereof.

17. 17. The electrode of claim 16, wherein the weight ratio of the binder to the electrode composite is from about 1% to about 20% by weight, or preferably about 10% by weight.

18. 18. The electrode of claim 1, wherein the electrode is characterized by the absence of a separator between the electrode composites.

19. a) Approximately 50mAh g 活物質 -1 ~About 4000mAh g 活物質 -1 Discharge capacity of b) Approximately 2mAh cm -2 ~Approx. 100mAh cm -2 Area capacity of, c) Approximately 1.5S cm -1 ~Approx. 100S cm -1 electronic conductivity of d) a capacity loss of about 5% to about 50% relative to the initial capacity; e) a coulombic efficiency of about 70% to about 100%; f) Cycle life of more than 40 cycles 19. The electrode according to claim 1 , characterized by at least one of the following:

20. 20. The electrode of claim 1, further comprising a junction adapted to penetrate the electrode.

21. The electrode of claim 20 , wherein the joint is adapted to pass through a through hole formable in the electrode.

22. 22. The electrode of claim 20 or 21, wherein the junction comprises a body adapted to pass substantially through the electrode, the body being characterized by a cross-sectional shape selected from a circle, an oval, or a polygon.

23. 23. The electrode of claim 22, wherein the body is hollow.

24. 24. The electrode of claim 23, wherein the body is characterized by a polygonal cross-sectional shape and, if hollow, includes legs extending from edges of the polygon.

25. 25. The electrode of any one of claims 22 to 24, wherein the junction further comprises a head at a first end of the body.

26. 26. The electrode of any one of claims 20 to 25, wherein the joint comprises a conductive material selected from stainless steel, Al, Ti, Ni, or Cu.

27. 27. The electrode of claim 26, wherein when the electrode is a cathode, the conductive material is selected from stainless steel, Al, Ti, or Ni, and when the electrode is an anode, the conductive material is selected from stainless steel, Ni, or Cu.

28. 28. The electrode of any one of claims 20 to 27, wherein the junction is adapted to electrically connect two or more electrodes, electrically connect at least one electrode to at least one contact tab, electrically connect at least one electrode to at least one lead, or electrically connect at least one contact tab to at least one lead on the electrode.

29. a) forming at least one electrode layer, said electrode layer being formed by coating a layer of an electrode composite material on at least a surface of a porous conductive substrate; b) laminating the electrode layer with another porous conductive substrate such that the layer of the electrode composite is sandwiched between the porous conductive substrates, the at least one electrode layer being in electrical communication with the porous conductive substrate; Including, A method of making an electrode, wherein the electrode composite is at least partially impregnated into the porous conductive substrate.

30. 30. The method of claim 29, further comprising laminating another electrode layer on the porous conductive substrate of step a) or b).

31. 31. The method of claim 29 or 30, wherein the electrode composite is provided as a slurry, dough, paste, or powder.

32. The electrode composite has a thickness of about 1 mg cm -2 ~Approx. 100mg cm -2 32. The method of claim 29 or 31, characterized by a mass loading on the surface of the porous conductive substrate of.

33. 33. The method of any one of claims 29 to 32, wherein the laminating step comprises applying a compressive force to the electrode layer and the further porous conductive substrate.

34. 34. The method of claim 33, wherein the compressive force is provided by a hydraulic press, a pneumatic press, a gravity press, or a roller press.

35. 35. The method of any one of claims 29 to 34, further comprising the step of connecting a joint to the electrode via punching or via a through hole formed in the electrode.

36. 36. The method of claim 35, wherein the joint comprises a body, the body being deformable to form a head.

37. 37. The method of claim 36, wherein the body is deformed by bending an end of the body so that the head is substantially parallel to a surface of the electrode.

38. 38. The method of claim 36 or 37, wherein the body is bent away from a longitudinal axis of the body.