Steam Nozzle for PVD

The steam jet coater with a converging and diverging section geometry addresses adhesion and thickness limitations in JVD by reducing vacancy concentrations to less than 1%, achieving improved coating uniformity and mechanical resistance on steel substrates.

JP2024537358AInactive Publication Date: 2024-10-10ARCELORMITTAL SA
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024522268
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-14
Filing Date
2022-09-05
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional coating methods, such as hot-dip coating and electrocoating, fail to provide satisfactory coatings on steel grades containing high levels of oxidizable elements like Si, Mn, Al, P, Cr, or B, leading to adhesion issues and limited coating thickness due to vacancy concentrations of approximately 2% in vacuum deposition techniques like JVD.

Method used

A steam jet coater with a specific geometry comprising a converging and diverging section in the steam outlet orifice, along with a distribution chamber and reheating means, is used to uniformly distribute and accelerate metal vapor to supersonic speeds, reducing jet expansion and vacancy concentrations in the coating.

Benefits of technology

The solution significantly reduces vacancy concentrations in the coating to less than 1%, enhancing coating adhesion and mechanical resistance, resulting in more uniform and thicker coatings on substrates like steel strips.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024537358000001_ABST
    Figure 2024537358000001_ABST
Patent Text Reader

Abstract

The present invention relates to a vapour jet coater for depositing a coating made of a metal or metal alloy on a moving substrate, said vapour jet coater comprising, in succession, a distribution chamber configured to be connectable to an evaporation tube, and a vapour outlet orifice connected to said distribution chamber and capable of injecting metal alloy vapour along a main injection plan and direction, said vapour outlet orifice comprising, in succession, i. a converging section and ii. a diverging section.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a vapour jet coater and vacuum deposition equipment for the continuous deposition of metallic coatings. The present invention also relates to a method for depositing such coatings.

[0002] The present invention is particularly, but not exclusively, contemplated to deposit a zinc or zinc-magnesium based coating onto a running steel strip, which can then be cut and shaped, for example by stamping, bending or forming, to form parts which can then be painted. [Background technology]

[0003] Several coating methods exist, such as hot dip coating and electrocoating. However, these conventional methods do not provide satisfactory coatings for steel grades that contain high levels of easily oxidized elements such as Si, Mn, Al, P, Cr or B. As a result, new methods have been developed, such as vacuum deposition techniques such as JVD (Jet Vapor Deposition).

[0004] In JVD, a metal vapor spray propelled at supersonically speed contacts a substrate. WO 97 / 47782 and WO 2009 / 047333 describe such processes.

[0005] WO 2015 / 015237 discloses a process aimed at improving the temporary protection against corrosion of steel coated by JVD (Jet Vapor Deposition), which is achieved by applying a pressure ratio of 2×10 -3 From 5.5 × 10 -2 The method is carried out by coating a steel substrate in a vacuum deposition facility.

[0006] WO 2019 / 239314 discloses a steam jet coating that prevents particulate defects. As shown in FIG. 1, the steam jet coater 101 is formed of a distribution chamber 102 and a steam outlet orifice 103 with a convergent portion 104.

[0007] Nevertheless, it has been observed that prior art devices result in a vacancy concentration of about 2%, which limits the mechanical resistance of the coating and causes coating adhesion problems that limit the coating thickness. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] International Publication No. 97 / 47782 [Patent Document 2] International Publication No. 2009 / 047333 [Patent Document 3] International Publication No. 2015 / 015237 [Patent Document 4] International Publication No. 2019 / 239314 Summary of the Invention [Problem to be solved by the invention]

[0009] It is an object of the present invention to ameliorate the shortcomings of prior art equipment and processes. [Means for solving the problem]

[0010] Other features and advantages will become apparent from the following detailed description of the invention.

[0011] For purposes of illustrating the present invention, various embodiments will now be described with particular reference to the following figures. [Brief description of the drawings]

[0012] [Figure 1]FIG. 1 is a diagram of one embodiment of a prior art steam jet coater. [Diagram 2] FIG. 1 is a diagram of one embodiment of a steam jet coater according to the present invention. [Diagram 3] FIG. 2 is a diagram of a first embodiment of a steam outlet orifice according to the present invention; [Figure 4] FIG. 4 is a diagram of a second embodiment of a steam outlet orifice according to the present invention. [Diagram 5] FIG. 1 is a diagram of one embodiment of a vacuum deposition facility according to the present invention. [Figure 6] FIG. 2 is an SEM image of a coating achieved with a steam jet coater according to the prior art. [Figure 7] FIG. 2 is an SEM image of a coating achieved with a vapour jet coater according to the invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The invention relates to a vapour jet coater 1 for depositing a coating made of a metal or metal alloy on a moving substrate (S), as shown in figures 2 and 3, said vapour jet coater comprising: A distribution chamber 2 configured to be connectable to an evaporation tube; a steam outlet orifice 3 connected to said distribution chamber 2 and capable of injecting metal alloy steam along a main injection plan (P) and a main injection direction (D), i. a converging section 4 comprising a wall defining two converging surfaces (5, 6), one on each side of said injection plan (P), said surfaces (5, 6) being spaced apart by a distance C on the inlet side; ENTRY Distance from and to the exit side C EXIT is spaced apart from the EE (C ENTRY / C EXIT ) is 1.2 to 10, a convergence section 4; ii. A diverging section 7 comprising a wall defining two converging surfaces (8, 9), one on each side of said injection plan (P), said two surfaces (8, 9) being spaced apart by a distance D on the inlet side. ENTRY Distance D from and to the exit side EXITspaced from and ratio D EE (D ENTRY / D EXIT ) is 0.1 to 0.8, a diverging portion 7, and a vapor outlet orifice 3 that continuously includes and continuously provides.

[0014] Hereinafter, the main injection direction (D) is represented with respect to the movement of the injected metal alloy vapor.

[0015] Preferably, the substrate is a strip.

[0016] Preferably, the moving substrate is a metal substrate. Even more preferably, the moving substrate is a steel substrate.

[0017] Preferably, the moving substrate has a composition containing, by weight percentage, 0.15 < Si < 0.4, 0.5 < Mn < 2.5, 0.1 < C < 0.4, P ≤ 0.03, S ≤ 0.02, 0.01 < Al ≤ 0.1, Cu ≤ 0.2, Ti + Nb ≤ 0.20, Cr + Mo ≤ 1, and the balance consists of Fe and unavoidable impurities.

[0018] Preferably, the moving substrate has a composition containing, by weight percentage, 0.15 < Si < 0.6, 0.17 < Mn < 2.3, 0.1 < C < 0.4, P ≤ 0.05, S ≤ 0.01, 0.015 < Al ≤ 1.0, Cu ≤ 0.2, B ≤ 0.005, Ti + Nb ≤ 0.15, Cr + Mo ≤ 1.4, and the balance consists of Fe and unavoidable impurities.

[0019] The vapor jet coater 1 is an acoustic vapor jet coater, that is, a coater capable of generating a sonic vapor jet. This type of coater is usually also called a JVD (jet vapor deposition) apparatus.

[0020] The function of the distribution chamber 2 is to distribute the metal vapor evenly along the vapor exit orifice and thus along the substrate width. As shown in Figures 2 and 5, the distribution chamber 2 is configured to be connectable to an evaporation tube 10, which means that the metal vapor can flow from the evaporation tube 10 to the distribution chamber 2.

[0021] Preferably, the distribution chamber 2 comprises reheating means 11, for example a heating cartridge. Such reheating means make it possible to reheat the metal vapour coming from the evaporation tube after its expansion as it enters the vapour outlet orifice 3, preventing condensation at the vapour outlet orifice.

[0022] Preferably, the reheating means extend along the length of the distribution chamber, even more preferably along the entire length. The number and location of the reheating means can be adjusted to optimise the reheating of the steam.

[0023] The vapor outlet orifice 3 is connected to said distribution chamber 2, which means that metal vapor can flow from the distribution chamber 2 to the vapor outlet orifice 3. This connection is preferably made via an opening cut into the wall of the distribution chamber.

[0024] The steam exit orifice 3 and diverging geometry are configured to prevent any flow disturbances at the diverging section.

[0025] As shown in FIG. 2, the steam outlet orifice comprises a converging section 4 and a diverging section 7 .

[0026] The converging section 4 comprises two surfaces (5, 6) converging towards each other, one on each side of the injection plan (P).

[0027] The two faces define an inlet side and an outlet side. Through the inlet side the metal vapour enters the convergence from the restoration chamber 2. Through the outlet side the metal vapour leaves the convergence.

[0028] In the plan perpendicular to the main injection plan, the convergence plane is at a distance C EXIT Distance C from the inlet ENTRY Furthermore,

number

[0029] By "converging towards each other" it is meant that the width on the inlet side of the steam outlet orifice is smaller than the width on the outlet side. This does not limit the shape of the sides in any way.

[0030] Such a convergence makes it possible to accelerate the jet, i.e. the metal vapour jet, to reach supersonic speeds at the exit of the convergence.

[0031] The divergent portion 7 comprises two faces (8, 9), one on each side of the injection plan (P), the two faces (8, 9) diverging from each other.

[0032] The two faces define an inlet side and an outlet side. Through the inlet side, the metal vapor enters the emitting section. Through the outlet side, the metal vapor exits the emitting section.

[0033] In the plan perpendicular to the main injection plan, the diverging surface is at a distance D ENTRY and the distance D from the exit EXIT Furthermore,

number

[0034] By "converging to each other" is meant that the width of the steam outlet orifice on the inlet side is greater than the width on the outlet side. This does not limit the shape of the sides in any way.

[0035] Such a divergence makes it possible to accelerate the jet, ie the metal vapour jet, and to reduce its pressure, so long as the jet velocity is supersonic on the inlet side of this point.

[0036] It has been found by the inventors that having such a converging section followed by such a diverging section can reduce the jet expansion (for the same vapor flow) upon entering the vacuum chamber due to a reduction in the jet pressure.

[0037] The reduction in jet expansion makes it possible to reduce the porosity of the coating, both at the steel-coating interface and at the top surface of the coating.

[0038] Preferably, in the convergent portion, the ratio C EE is 3 to 5.

[0039] Preferably, in the convergence, the two faces are essentially symmetrical with respect to the main injection plan (P). Such an arrangement improves the coating uniformity.

[0040] Preferably, said convergent portion has a cross section along a plan perpendicular to its length that is trapezoidal, even more preferably, said convergent portion has a cross section along a plan perpendicular to its length that is an isosceles trapezoid.

[0041] Preferably, in said converging portion, the base angle of the isosceles trapezoid has a value greater than 60°.

[0042] Preferably, the length of the convergent portion L CONV The length is along the main injection direction D.

[0043] Preferably, the distance C ENTRY More preferably, the distance C is 30 mm to 180 mm. ENTRY is 50mm~150mm.

[0044] Preferably, the distance C EXIT More preferably, the distance C EXIT is 35mm~55mm.

[0045] Preferably, the angle between the main injection plan (P) and any of the two walls defining the convergent plane (5, 6) is between 5° and 45°, preferably between 15° and 35°.

[0046] Preferably, the beginning of the entrance of the convergent section 4 has a radius of curvature ρ according to the following condition: ENTRY That is, 0.5 × C ENTRY <ρ ENTRY <2×C ENTRY It is.

[0047] Preferably, the diverging portion, the ratio D EE is 0.3 to 0.6.

[0048] Preferably, in the diverging section, the two planes are symmetrical with respect to the main injection plan (P).

[0049] Preferably, said diverging portion has a cross section along a plan perpendicular to its length that is trapezoidal. Even more preferably, said diverging portion has a cross section along a plan perpendicular to its length that is an isosceles trapezoid.

[0050] Preferably, in the diverging portion, the base angle of the isosceles trapezoid has a value greater than 60°.

[0051] Preferably, the length of the diverging portion is in the range of 30 mm to 280 mm.

[0052] Preferably, the distance D ENTRY More preferably, the distance D ENTRY is 30mm~50mm.

[0053] Preferably, the distance D EXIT More preferably, the distance D EXIT is 60mm~200mm.

[0054] Preferably, said converging and diverging portions are contiguous.Even more preferably, the curvature at the junction between the converging and diverging portions is less than 40°, preferably less than 30°.

[0055] Preferably, a neutral section is arranged between the converging and diverging sections, the neutral section comprising a wall with two faces, one on each side of the injection plan (P), the two spaces being spaced apart from each other by a distance that is essentially constant along the main injection direction D. Even more preferably, the curvature between the converging and neutral sections is less than 40°, preferably less than 30°. Even more preferably, the curvature between the diverging and neutral sections is less than 40°, preferably less than 30°.

[0056] Preferably, as shown in FIG. 4, the steam outlet orifice 3 has an end with two parallel faces (80, 90), one on each side of the injection plan (P), said two faces being spaced apart by a distance D. EXIT Even more preferably, said end has a length between 5% and 15% of the length of the diverging portion (7).

[0057] This end is downstream of the convergence when following the path of the metal vapor.

[0058] As shown in FIG. 5, the invention also relates to a vacuum deposition installation 12 for the continuous deposition of a coating made of a metal or metal alloy on a moving substrate (S), said installation comprising a deposition chamber 13 suitable for passing the substrate (S) along a given path, and an evaporation crucible 14 suitable for delivering metal or metal alloy vapor; An evaporation tube 10; At least one steam jet coater 1 as described above; are continuously provided.

[0059] The installation comprises means 15 for passing the substrate through the deposition chamber. The substrate may be moved by any suitable means, depending on the nature and shape of said substrate. Rotating support rollers capable of supporting a steel strip may in particular be used.

[0060] The deposition chamber is preferably 10 -8 ~10 -3 It is preferably a sealable box kept under bar pressure. The deposition chamber preferably has an inlet lock and an outlet lock (not shown) between which the substrate S, e.g. a steel strip, can travel along a given path in the travel direction.

[0061] The vapour jet coater is suitable for spraying metal alloy vapour coming from an evaporation crucible 14 onto a traveling substrate S.

[0062] The evaporation crucible 14 consists mainly of a pot and a cover. The evaporation crucible is provided with heating means that allow the metal vapor to be formed and fed to the vapor jet coater. The evaporation crucible is advantageously provided with an induction heater, which has the advantage of making the stirring and compositional homogenization of the metal alloy bath easier.

[0063] The evaporation tube 10 is connected on one side to an evaporation crucible 14 and on the other side to the vapor jet coater 1. Preferably, a valve located between the evaporator and the ejector controls the metal vapor flow.

[0064] These different parts may be made, for example, of graphite.

[0065] The invention also relates to a method for continuously depositing a coating made of at least one metal in a vacuum deposition installation as described above onto a moving substrate (S), the method being carried out at a pressure P VACUUM In the vacuum chamber having a pressure P EJECTED and a step of forming at least one metal layer by spraying the metal toward a side surface of the moving substrate; EJECTED / P VACUUM ) is 2 to 15, and the injected steam has a supersonic speed on the inlet side of the diverting portion 7.

[0066] P VACUUM is the pressure of the chamber measured by the pressure sensor.

[0067] Pressure in the distribution chamber P REP is calculated by the following equation (1): ZINC , the zinc temperature in the distribution chamber T ZINC , and the cross section A of the ejector throat THROAT can be derived from

number

[0068] Next, the pressure of the jet ejected by the steam outlet orifice, P EJECTED can be calculated using the following equation (2):

number

[0069] The traveling substrate is preferably a metal strip, even more preferably a steel strip. The width of the traveling substrate is preferably 200-2200 mm.

[0070] The traveling substrate preferably has a traveling speed of 10 to 800 m / min.

[0071] The layer of at least one metal is preferably formed by condensation of an injected vapor.

[0072] Preferably, the coating has a thickness of 0.1 to 20 μm. If the thickness is less than 0.1 μm, the coating does not provide sufficient corrosion protection.

[0073] The coating preferably contains zinc as the main element. The coating may contain the following additional elements: chromium, nickel, titanium, manganese, magnesium, silicon and aluminum, considered individually or in combination.

[0074] Preferably, P EJECTED / P VACUUM is between 2 and 10. Such a ratio further reduces the jet expansion in the vacuum chamber.

[0075] Preferably, the P VACCUM is 1.10 -4 mbar~3.10 -1 mbar.

[0076] Preferably, the vapour jet coater is at a distance of 20mm to 80mm from the traveling substrate.

[0077] Preferably, the metal vapor flow sprayed by the vapor jet coater is between 3 and 300 g.s. -1 It is.

[0078] The invention also relates to a steel sheet produced as described above and provided with a metal coating containing impurities possibly present in trace amounts unavoidable during production, said metal coating having a vacancy concentration of less than 1%.

[0079] The steel sheet is preferably hot rolled and then cold rolled so that it can be used to manufacture body parts for automobiles, although the invention is not necessarily limited to this field and may find application in any steel part, regardless of its final use.

[0080] The substrate steel can be, for example, one particular grade of VHS steel (very high strength, typically 450-900 MPa) or UHR (ultra high strength, typically above 900 MPa), and is free of the following elements which are highly susceptible to oxidation: Interstitial-free steel (IF - very low carbon), which may contain up to 0.1% Ti (by weight); Duplex steels such as steels up to 1200 DP 500 DP steels which may contain up to 3% Mn (by weight) in combination with up to 1% Si, Cr and / or Al (by weight); TRIP steel (induced plastic transformation), e.g. TRIP steel 780, containing about 1.6% (by weight) Mn and 1.5% Si; TRIP steel or phosphorus-containing duplex, TWIP steel (TWining induced plasticity) - steel with a high content of Mn (generally 17 to 25% by weight); Steels such as Fe-Al, e.g. low density steels which may contain up to 10% Al (by weight); Stainless steels with a high chromium content (generally 13-35% by weight) in combination with other alloying elements (Si, Mn, Al...); It is.

[0081] The vacancy concentration is estimated by comparing the contrast of the SEM images. Approximately 10 images were used to evaluate the vacancies. The estimation of the vacancy concentration is done on a square cross section, with sides the same size as the coating thickness. Darker pixels correspond to vacancies.

[0082] Preferably, said metal coating comprises at least one layer of pure zinc. The steel sheet may be optionally coated with one or more layers in addition to the zinc layer in a manner suited to the desired properties of the final product. The zinc layer is preferably the top layer of the coating.

[0083] Preferably, a layer of electrophoretically produced paint is on top of said metal coating.

[0084] Experimental Results To demonstrate the effect of the claimed vapour jet coater on the coating density, comparative tests were carried out on steel strips on which a zinc coating was formed by a jet deposition process in the same vacuum deposition installation.

[0085] The vacuum deposition equipment comprises a deposition chamber suitable for passing the substrate continuously along a given path, an evaporation crucible suitable for zinc vapor, an evaporation tube and one vapor jet coater, as shown in FIG. 5 .

[0086] To compare the results, two samples, A and B, were manufactured. Both coatings were made of martensitic steel (MS1500 from ArcelorMittal) with the same composition.

[0087] In both JVD processes, the pressure in the vacuum chamber P VACUUM is 1.2 × 10 -4 The distance between the steam jet coater and the substrate was 50 mm, and the steam flow was about 108 g.s -1 It is.

[0088] The substrate of sample A was coated with a vapour jet coater as described in WO 2019 / 129314, the vapour jet coater comprising only a converging section as shown in Figure 1. The important characteristics of the vapour jet coater are summarised in Table 1.

[0089] The substrate of sample B was coated with a vapor jet as claimed and shown in Figure 4, with a converging section, a diverging section and then an end. The important characteristics of the vapor jet coater are summarized in Table 1.

[0090] For each sample, SEM images were taken and ten SEM images were used to estimate the denseness of the zinc coating.

[0091] The vacancy concentration is significantly reduced when the claimed vapor jet coating is used. Furthermore, the zinc coating is more uniform.

[0092] This improvement in the coating is also visually noticeable when comparing SEM images of the zinc coatings of samples A (Figure 6) and B (Figure 7).

[0093] Experimental results clearly show that the present invention improves coatings by reducing vacancy concentration.

[0094] [Table 1]

Claims

1. A vapour jet coater 1 for depositing a coating made of a metal or metal alloy on a moving substrate (S), said vapour jet coater comprising: A distribution chamber 2 configured to be connectable to an evaporation tube; a steam outlet orifice 3 connected to said distribution chamber 2 and capable of injecting metal alloy steam along a main injection plan (P) and a main injection direction (D), iii. A converging section 4 comprising a wall defining two converging surfaces (5, 6), one on each side of said injection plan (P), said two surfaces (5, 6) having a distance C on the inlet side. ENTRY Distance C from and to the exit side EXIT and is spaced apart from the ratio C EE (C ENTRY / C EXIT ) is 1.2 to 10, a convergence section 4; iv. A diverging section 7 comprising a wall defining two converging surfaces (8, 9), one on each side of said injection plan (P), said two surfaces (8, 9) having a distance D on the inlet side. ENTRY Distance D from and to the exit EXIT and is spaced apart from the ratio D EE (D ENTRY / D EXIT ) is 0.1 to 0.8; and a steam outlet orifice (3) having a series of A steam jet coater 1 having a continuous

2. In the convergent portion, the ratio C EE The steam jet coater according to claim 1, wherein is 3-5.

3. 3. A steam jet coater according to claim 1, wherein in the convergent section the cross section along a plan perpendicular to its length is trapezoidal.

4. In the diverging portion, the ratio D EE A steam jet coater according to any one of claims 1 to 3, wherein is between 0.25 and 0.

35.

5. A steam jet coater according to any one of claims 1 to 4, wherein in the diverging section the cross section along a plan perpendicular to its length is trapezoidal.

6. The steam outlet orifice 3 has an end with two parallel faces (80, 90), one on each side of the injection plan (P), the two faces being spaced apart by a distance D. EXIT A coated steam jet according to any one of claims 1 to 5, spaced apart from

7. 1. A vacuum deposition installation for the continuous deposition of a coating made of a metal or metal alloy on a moving substrate (S), comprising: an evaporation crucible suitable for delivering metal or metal alloy vapor; An evaporation tube; a deposition chamber adapted to pass a substrate along a given path; At least one steam jet coater according to any one of claims 1 to 6, A vacuum deposition system comprising:

8. 8. A method for continuously depositing a coating made of at least one metal on a moving substrate (S) in a vacuum deposition installation according to claim 7, characterized in that the method is carried out at a pressure P VACUUM In the vacuum chamber having a pressure P EJECTED a step of spraying the metal toward a side surface of the moving substrate at a temperature of 1000° C. to form at least one metal layer; EJECTED / P VACUUM ) is 2-15 and the injected steam has a supersonic speed at the inlet side of the diverging section 7.

9. The method of claim 8, wherein the vapour jet coater is at a distance of 20 mm to 80 mm from the traveling substrate.

10. (P EJECTED / P VACUUM 10. The method according to claim 8, wherein n is 2 to 10.

11. The P VACUUM is 1.10 -4 mbar ~ 3.10 -1 11. The method according to claim 8, wherein the pressure is 100 bar.

12. The metal vapor flow sprayed by the vapor jet coater is 3 to 300 g.s -1 The method according to any one of claims 8 to 11, wherein

13. 13. A steel sheet manufactured according to any one of claims 8 to 12, provided with a metal coating, possibly including impurities present in trace amounts, unavoidable during manufacturing, said metal coating having a vacancy concentration of less than 1%.

14. 14. The steel sheet of claim 13, wherein a layer of electrophoretically produced paint is on top of the metallic coating.

Citation Information

Patent Citations

  • Vapor deposition source of vacuum deposition apparatus

    JP2021134404A

  • Vacuum deposition equipment and method for coating substrates

    JP2021526592A

  • Method and device for continuous coating of a moving substrate by means of a metallic vapour

    WO1997047782A1

  • Industrial vapour generator for the deposition of an alloy coating onto a metal strip

    WO2009047333A1

  • Steel plate provided with a zinc coating

    WO2015015237A1