Catalyst for fuel cell as well as preparation method and application of catalyst
By introducing nitrogen-containing organic small molecules and carbon coating technology in the preparation process of the fuel cell catalyst, the stability and durability problems of the platinum alloy catalyst are solved, the stability and activity of the catalyst are improved, the service life of the fuel cell is extended and Reduced costs.
Patent Information
- Application Number
- CN202410799854.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-01
AI Technical Summary
Existing fuel cell catalysts have stability problems, especially the precipitation of cobalt ions and the growth of metal particles in platinum alloy catalysts, which lead to performance degradation and poor durability, affecting the service life and cost efficiency of fuel cells.
By introducing nitrogen-containing organic small molecules during the preparation of precious metal-transition metal alloy catalysts by the impregnation method, the dispersion of metal ions and the anchoring effect of alloy particles are improved, and slow cooling and carbon coating technologies are used to form nitrogen-doped carbon The shell enhances the stability and order of alloy particles.
It significantly improves the stability and electrochemical active area of the catalyst, slows down the migration and dissolution of metal nanoparticles, extends the service life of the fuel cell and reduces the cost.
Smart Images

Figure CN118738424A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fuel cell catalysts, and in particular to a fuel cell catalyst and a preparation method and application thereof. Background Art
[0002] In recent years, the development of highly active fuel cell cathode catalysts has become the most urgent need for breakthroughs and promotion of fuel cell technology, which is of great significance for improving energy utilization, increasing power density and reducing the use of precious metals.
[0003] In recent years, precious metal alloy catalysts (such as platinum alloy catalysts) have shown significantly higher mass specific activity than platinum-carbon catalysts, and are a new generation of high-performance fuel cell cathode catalysts with great potential. By alloying precious metals (such as platinum) with non-precious transition metal elements, not only can cheap non-precious metals be introduced to reduce the amount of platinum, but alloying can also adjust the d-band center of platinum and introduce stress-strain effects, significantly improving the electrochemical oxygen reduction activity, which is of great significance to the breakthrough of fuel cell technology cost efficiency.
[0004] However, fuel cell catalysts currently face serious stability issues. For example, platinum alloy catalysts have high mass specific activity, but platinum and cobalt precipitation is still serious. In particular, the precipitation of cobalt ions will coordinate with the sulfonate ions of the proton exchange membrane, which will significantly reduce its proton conductivity and reduce the performance and life of the fuel cell. In addition, the maturation and migration of platinum-cobalt nanoparticles during the catalytic process will also lead to significant particle growth and reduce its active area. The dissolution of active metal ions and the growth of metal particles are often the main reasons for the attenuation of catalyst performance, and are also one of the main reasons for the poor durability of fuel cells.
[0005] Therefore, the research and development of high-performance and high-durability fuel cell cathode catalysts is of great significance for reducing the cost of fuel cells, increasing their service life, and promoting the mature commercialization of fuel cells. Summary of the invention
[0006] In view of the above problems existing in the prior art, the object of the present invention is to provide a catalyst for fuel cells and a preparation method and application thereof.
[0007] To achieve the above object, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a method for preparing a fuel cell catalyst, the preparation method comprising the following steps:
[0009] The carbon carrier, the noble metal source, the transition metal source and the nitrogen-containing organic small molecule are uniformly mixed in a solvent, dried, and then calcined to obtain the fuel cell catalyst.
[0010] At present, common commercial platinum-carbon catalysts often face the problem of weak adhesion of metal active particles on the carrier. This is mainly because the metal particles have weak interaction with the carbon carrier, which leads to the peeling of active particles during the actual long-term operation of the catalyst.
[0011] The method of the present invention introduces nitrogen-containing organic small molecules during the process of preparing the noble metal-transition metal alloy catalyst by the impregnation method, and the nitrogen-containing organic small molecules can interact with the metal ions in a coordinated manner, thereby improving the dispersibility of the metal ions and preventing agglomeration during the drying process. During the high-temperature calcination process, the alloy particles can have good dispersibility, and the nitrogen-containing organic molecules decompose to form nitrogen doping on the carbon carrier. The doped nitrogen atoms can interact well with the alloy particles, thereby improving the anchoring effect of the alloy particles, improving the stability, preventing the alloy particles from growing too large and agglomerating during the calcination process, and maintaining a small particle size.
[0012] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.
[0013] Preferably, the model of the carbon carrier includes at least one of EC600JD, ECP600JD, EC300J, VXC-72, VXC-72R and BP2000.
[0014] Preferably, the noble metal source includes at least one of chloroplatinic acid hexahydrate, tetraammine platinum nitrate, sodium chloroplatinate and platinum acetylacetonate.
[0015] Preferably, the transition metal source includes at least one of cobalt chloride hexahydrate, cobalt nitrate, nickel nitrate and iron nitrate.
[0016] Preferably, the nitrogen-containing organic small molecule includes at least one of dicyandiamide, dopamine hydrochloride, aniline and melamine.
[0017] Preferably, the carbon carrier, the noble metal source, the transition metal source and the nitrogen-containing organic small molecule are mixed in the following manner: the carbon carrier, the noble metal source, the transition metal source and the nitrogen-containing organic small molecule are added to a solvent, ultrasonicated and stirred, and dried.
[0018] Preferably, the solvent includes at least one of water and ethanol, wherein the water may be ultrapure water.
[0019] Preferably, the ultrasonication and stirring are carried out in the following manner: first ultrasonication for 20 min to 45 min (20 min, 25 min, 30 min, 35 min, 40 min or 45 min, etc.) and then stirring for 12 h to 24 h (for example, 12 h, 13 h, 14 h, 15 h, 16 h, 17 h, 18 h, 19 h, 20 h, 21 h, 22 h, 23 h or 24 h, etc.).
[0020] As a preferred technical solution of the method for preparing the fuel cell catalyst of the present invention, the calcination is carried out in an atmosphere containing a reducing gas.
[0021] Preferably, the atmosphere containing reducing gas is a mixed gas of protective gas and reducing gas, and the volume fraction of reducing gas in the mixed gas is 5%, 6%, 7%, 8%, 9%, 10%, 12%, 13%, 14% or 15%, etc.
[0022] Preferably, the protective gas includes at least one of argon, helium and nitrogen.
[0023] Preferably, the reducing gas is hydrogen.
[0024] Preferably, the heating rate of the calcination is 1°C / min to 5°C / min, for example, 1°C / min, 2°C / min, 3°C / min, 4°C / min or 5°C / min.
[0025] Preferably, the calcination holding temperature is 700°C to 900°C, for example, 700°C, 725°C, 750°C, 770°C, 800°C, 825°C, 850°C, 875°C or 900°C.
[0026] Preferably, the calcination holding time is 1 h to 3 h, for example, 1 h, 1.5 h, 2 h, 2.5 h or 3 h.
[0027] Preferably, during the calcination process, after the insulation is completed, the temperature is first lowered to 350°C to 450°C (for example, 350°C, 375°C, 400°C, 415°C, 430°C, 440°C or 450°C, etc.) at a rate of 1°C / min to 5°C / min (for example, 1°C / min, 2°C / min, 3°C / min, 4°C / min or 5°C / min, etc.), and then cooled to room temperature.
[0028] In the method of the present invention, alloying is performed after the temperature is raised to the calcination holding temperature. After the holding temperature is completed, the temperature is slowly lowered by 1°C / min to 5°C / min during the cooling process to prolong the orderly arrangement of the alloy atoms, significantly improve the order of the alloy, and further improve the activity and stability of the alloy. As a preferred technical solution of the preparation method of the fuel cell catalyst of the present invention, the preparation method also includes carbon coating the calcined catalyst to form a carbon shell on the surface of the catalyst.
[0029] In the prior art, the exposed metal particles are in direct contact with the reaction system and are easily corroded by the acidic and oxidative environment, resulting in metal dissolution and redeposition, leading to the loss and maturation of active metal species, which greatly reduces the activity and life of the fuel cell in practical applications.
[0030] The present invention can protect metal particles, reduce corrosion and increase the life of the catalyst by carbon coating the catalyst.
[0031] Preferably, the carbon coating method comprises: uniformly mixing the calcined catalyst with a nitrogen-containing organic liquid, and then sintering to obtain a catalyst with a carbon shell.
[0032] The method of the present invention uses nitrogen-containing organic liquid to mix with the catalyst after the noble metal transition metal alloy is formed, so that the nitrogen-containing organic molecules can be adsorbed on the surface of the alloy particles, and a carbon shell can be formed after simple sintering, thereby avoiding the migration of alloy particles and relieving the precipitation of metal ions, which helps to overcome the problem of weak stability of platinum-cobalt alloy catalysts at this stage and improve the stability and life of fuel cell catalysts. Moreover, this stabilization strategy has the good advantages of being simple and easy to implement, and has good industrialization prospects.
[0033] Preferably, the nitrogen-containing organic liquid includes at least one of aniline and imidazole ionic liquids.
[0034] Preferably, the mass ratio of the calcined catalyst to the nitrogen-containing organic liquid is (0.1-0.5):1, such as 0.1:1, 0.2:1, 0.3:1, 0.4:1 or 0.5:1.
[0035] Preferably, the sintering atmosphere is an inert atmosphere.
[0036] Preferably, the gas in the inert atmosphere includes at least one of nitrogen, helium and argon.
[0037] Preferably, the sintering temperature is 650°C to 750°C, for example, 650°C, 660°C, 680°C, 690°C, 700°C, 715°C, 725°C, 730°C, 740°C or 750°C.
[0038] Preferably, the sintering time is 0.5 h to 2 h, for example, 0.5 h, 0.6 h, 0.8 h, 1 h, 1.2 h, 1.3 h, 1.5 h, 1.6 h, 1.8 h or 2 h.
[0039] Preferably, the calcined catalyst and the nitrogen-containing organic liquid are mixed in the following manner: the calcined catalyst and the nitrogen-containing organic liquid are mixed with an organic solvent and stirred for 12 h to 24 h (e.g., 12 h, 13 h, 14 h, 15 h, 16 h, 17 h, 18 h, 19 h, 20 h, 21 h, 22 h, 23 h or 24 h, etc.), followed by separation and collection of solid materials for sintering.
[0040] Preferably, the organic solvent comprises at least one of acetone, methanol and DMF.
[0041] In a second aspect, the present invention provides a catalyst prepared by the preparation method described in the first aspect;
[0042] Preferably, the catalyst comprises a nitrogen-doped carrier and metal nanoparticles supported on the carrier, and the surface of the metal nanoparticles is coated with a nitrogen-doped carbon shell.
[0043] Preferably, the mass proportion of the precious metal element in the catalyst is 10% to 60%, for example, it can be 10%, 12%, 14%, 15%, 17%, 18%, 20%, 23%, 26%, 30%, 32%, 35%, 40%, 45%, 50%, 55% or 60%; the mass proportion of the transition metal element is 1% to 30%, for example, it can be 1%, 3%, 5%, 8%, 10%, 12%, 15%, 18%, 20%, 22%, 24%, 26%, 28% or 30%; the mass proportion of the nitrogen element is 0.5% to 8%, for example, it can be 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5% or 8%, etc.
[0044] Preferably, the particle size of the metal nanoparticles is 3.5 nm to 7.5 nm, for example, it may be 3.5 nm, 3.8 nm, 4.0 nm, 4.5 nm, 5.0 nm, 5.5 nm, 6.0 nm, 6.5 nm, 7.0 nm or 7.5 nm.
[0045] Preferably, the thickness of the carbon shell is 0.6 nm to 2.7 nm, for example, it can be 0.6 nm, 0.8 nm, 1.0 nm, 1.2 nm, 1.3 nm, 1.5 nm, 1.7 nm, 1.8 nm, 2.0 nm, 2.2 nm, 2.4 nm, 2.5 nm, 2.6 nm or 2.7 nm.
[0046] In the catalyst prepared by the method of the present invention, the nitrogen-doped carrier carries metal nanoparticles, the surface of the metal nanoparticles is coated with a carbon shell, the metal nanoparticles include noble metal transition metal alloy particles, the metal and the nitrogen-doped carrier have a strong interaction, and at the same time, the dual effects of nitrogen doping and carbon coating are conducive to enhancing the order of the alloy and making the metal nanoparticles have a smaller particle size. Compared with commercial platinum-carbon catalysts and platinum alloy catalysts, the catalyst of the present invention can significantly slow down the migration and dissolution of metal nanoparticles, while maintaining a smaller size distribution of platinum alloy nanoparticles, significantly improving the stability and electrochemical active area of the catalyst.
[0047] In a third aspect, the present invention provides a fuel cell, wherein the cathode of the fuel cell comprises the catalyst prepared by the preparation method described in the first aspect or the catalyst described in the second aspect.
[0048] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0049] Compared with the prior art, the present invention has the following beneficial effects:
[0050] (1) The method of the present invention introduces nitrogen-containing organic small molecules during the process of preparing the precious metal-transition metal alloy catalyst by the impregnation method. The nitrogen-containing organic small molecules can interact with the metal ions to improve the dispersion of the metal ions and prevent agglomeration during the drying process. During the high-temperature calcination process, the alloy particles can have good dispersion. The nitrogen-containing organic molecules decompose to form nitrogen doping on the carbon carrier. The doped nitrogen atoms can interact well with the alloy particles, thereby improving the anchoring effect of the alloy particles, improving the stability, preventing the alloy particles from growing too large and agglomerating during the calcination process, and maintaining a small particle size.
[0051] (2) The method of the present invention can prolong the process of orderly arrangement of alloy atoms by adopting a slow cooling method, which can significantly improve the orderliness of the alloy and is beneficial to further improve the activity and stability of the alloy.
[0052] (3) After the noble metal transition metal alloy is formed, the method of the present invention uses a nitrogen-containing organic liquid to mix with the catalyst, so that the nitrogen-containing organic molecules can be adsorbed on the surface of the alloy particles, and a carbon shell can be formed after simple sintering, thereby avoiding the migration of alloy particles and relieving the precipitation of metal ions, which helps to overcome the problem of weak stability of platinum-cobalt alloy catalysts at this stage and improve the stability and life of fuel cell catalysts. Moreover, this stabilization strategy has the good advantages of being simple and easy to implement, and has good industrialization prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] Figure 1 This is the X-ray diffraction pattern of the carbon shell-coated platinum-cobalt alloy catalyst prepared in Example 1. DETAILED DESCRIPTION
[0054] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.
[0055] The specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0056] Example 1
[0057] This embodiment provides a method for preparing a fuel cell catalyst, comprising the following steps:
[0058] (1) 700 mg of carbon support (EC600JD), 609 mg of chloroplatinic acid hexahydrate, 363 mg of cobalt chloride hexahydrate, and 2.86 mmol of nitrogen-containing organic small molecule (dicyandiamide) were dissolved in 50 ml of deionized water, ultrasonicated for 30 minutes, stirred for 24 hours to mix thoroughly, then evaporated to dryness and collected the sample.
[0059] (2) The collected samples were heated to 800°C at a rate of 2°C per minute in a hydrogen-argon mixture (the volume fraction of hydrogen is 10%), maintained for 2 hours, then cooled to 400°C at a rate of 1°C per minute, and then naturally cooled to room temperature. Finally, a highly uniformly dispersed nitrogen-doped carbon carrier-supported platinum-cobalt alloy catalyst was obtained.
[0060] (3) Take 200 mg of the catalyst prepared in step (2), mix it with 1 g of nitrogen-containing organic liquid (aniline), add 100 mL of acetone, stir for 24 hours to mix evenly, then filter and separate, maintain the collected material at 700° C. in a nitrogen atmosphere for 1 hour, and obtain a carbon shell-coated platinum-cobalt alloy catalyst.
[0061] Figure 1 This is the X-ray diffraction pattern of the carbon shell-coated platinum-cobalt alloy catalyst prepared in this embodiment. It can be seen from the figure that the prepared catalyst alloy particles show an obvious ordered phase, and the calculated alloy particles have a smaller size (the average particle size is 4.8nm), indicating that the dual effects of nitrogen doping and carbon coating are beneficial to enhancing the order of the alloy while maintaining its particle size at a smaller level.
[0062] The catalyst prepared in this embodiment includes a nitrogen-doped carrier and metal nanoparticles loaded on the carrier, and the surface of the metal nanoparticles is coated with a carbon shell (thickness of 0.835 nm). The mass proportion of the precious metal element Pt in the catalyst is 21.8%, the mass proportion of the transition metal element Co is 8.2%, and the mass proportion of the nitrogen element N is 4.2%.
[0063] Example 2
[0064] This embodiment provides a method for preparing a fuel cell catalyst, comprising the following steps:
[0065] (1) 700 mg of carbon support (EC600JD), 609 mg of chloroplatinic acid hexahydrate, 363 mg of cobalt chloride hexahydrate, and 2.86 mmol of nitrogen-containing organic small molecule (dopamine hydrochloride) were dissolved in 50 ml of deionized water, ultrasonicated for 20 minutes, stirred for 18 hours to mix thoroughly, then evaporated to dryness and collected the sample.
[0066] (2) The collected samples were heated to 900°C at a rate of 3°C per minute in a hydrogen-argon mixture (the volume fraction of hydrogen is 8%), maintained for 1.5 hours, then cooled to 450°C at a rate of 1.5°C per minute, and then naturally cooled to room temperature. Finally, a highly uniformly dispersed nitrogen-doped carbon carrier-supported platinum-cobalt alloy catalyst was obtained.
[0067] (3) Take 300 mg of the catalyst prepared in step (2), mix it with 1 g of nitrogen-containing organic liquid (1,3-dimethylimidazole hexafluorophosphate), add 100 mL of acetone, stir for 15 h to mix evenly, then filter and separate, maintain the collected material at 720° C. in a nitrogen atmosphere for 0.7 h, and obtain a carbon shell-coated platinum-cobalt alloy catalyst.
[0068] The catalyst prepared in this embodiment includes a nitrogen-doped carrier and metal nanoparticles loaded on the carrier, and the surface of the metal nanoparticles is coated with a carbon shell (thickness of 0.727 nm). The mass proportion of the precious metal element Pt in the catalyst is 22.3%, the mass proportion of the transition metal element Co is 7.8%, and the mass proportion of the nitrogen element N is 3.9%.
[0069] Example 3
[0070] This embodiment provides a method for preparing a fuel cell catalyst, comprising the following steps:
[0071] (1) 700 mg of carbon support (EC600JD), 609 mg of chloroplatinic acid hexahydrate, 363 mg of cobalt chloride hexahydrate, and 2.8 mmol of nitrogen-containing organic small molecule (melamine) were dissolved in 50 ml of deionized water, ultrasonicated for 35 minutes, stirred for 12 hours to mix thoroughly, then evaporated to dryness and collected the sample.
[0072] (2) The collected samples were heated to 700°C at a rate of 2°C per minute in a hydrogen-argon mixture (the volume fraction of hydrogen is 10%), maintained for 3 hours, then cooled to 350°C at a rate of 2.5°C per minute, and then naturally cooled to room temperature. Finally, a highly uniformly dispersed nitrogen-doped carbon carrier-supported platinum-cobalt alloy catalyst was obtained.
[0073] (3) Take 500 mg of the catalyst prepared in step (2), mix it with 1 g of nitrogen-containing organic liquid (aniline), add 100 mL of acetone, stir for 20 h to mix evenly, then filter and separate, maintain the collected material at 670° C. in a nitrogen atmosphere for 2 h, and obtain a carbon shell-coated platinum-cobalt alloy catalyst.
[0074] The catalyst prepared in this embodiment includes a nitrogen-doped carrier and metal nanoparticles loaded on the carrier, and the surface of the metal nanoparticles is coated with a carbon shell (thickness of 0.643 nm). The mass proportion of the precious metal element Pt in the catalyst is 20.6%, the mass proportion of the transition metal element Co is 7.2%, and the mass proportion of the nitrogen element N is 2.8%.
[0075] Example 4
[0076] This embodiment provides a method for preparing a fuel cell catalyst. The difference from Embodiment 1 is that the amount of nitrogen-containing organic small molecules in step (1) is changed so that the mass proportion of nitrogen in the catalyst is 0.4%.
[0077] Example 5
[0078] This embodiment provides a method for preparing a fuel cell catalyst. The difference from Embodiment 1 is that the amount of nitrogen-containing organic small molecules in step (1) is changed so that the mass proportion of nitrogen in the catalyst is 8.5%.
[0079] Example 6
[0080] This embodiment provides a method for preparing a catalyst for a fuel cell. The difference from Embodiment 1 is that in step (2), the cooling rate is adjusted from 1° C. per minute to 10° C. per minute.
[0081] Example 7
[0082] This embodiment provides a method for preparing a catalyst for a fuel cell. The difference from Embodiment 1 is that after maintaining the temperature at 800° C. for 2 hours, the heating device is directly turned off and the catalyst is naturally cooled to room temperature.
[0083] Example 8
[0084] This embodiment provides a method for preparing a catalyst for a fuel cell. The difference from Embodiment 1 is that the aniline in step (3) is replaced by glucose, and the amount of glucose used satisfies that the mass of carbon converted from glucose is equal to the mass of carbon converted from aniline in Embodiment 1.
[0085] Comparative Example 1
[0086] This comparative example provides a method for preparing a catalyst for a fuel cell, which differs from Example 1 in that no nitrogen-containing organic small molecules are added in step (1).
[0087] Performance Test:
[0088] 3 mg of the catalyst prepared in Examples 1 to 8 and Comparative Example 1 was weighed, and the catalyst was dispersed in 3 mL of ethanol solution by ultrasonic treatment. After uniform ultrasonic dispersion, 8 μL was dripped dropwise on the surface of a gold electrode (diameter 5 mm), and dried at room temperature to form a uniform and smooth catalyst thin layer. In a nitrogen-saturated 0.1 mol / L perchloric acid solution, the catalyst was activated by scanning 100 cycles from 0V initial potential to 1.2V (relative to a reversible hydrogen electrode) using a cyclic voltammetry (CV) test method at a scanning speed of 100 mV / s, and then in an oxygen-saturated 0.1 mol / L perchloric acid solution, 0V-1.2V was forward scanned at a speed of 10 mV / s at a rotating electrode speed of 1600 rpm to obtain a linear sweep voltammetry (LSV) curve of the catalyst. The working electrode was cyclically voltammetrically scanned for 30,000 cycles in a nitrogen-saturated 0.1 mol / L perchloric acid solution, with a scanning range of 0.6V to 0.95V and a scanning speed of 100 mV / s. The linear polarization curve was also recorded for 30000 cycles. The results are shown in Table 1.
[0089] Table 1
[0090] Mass activity (A / mg) Mass activity decay rate Example 1 1.06 5% Example 2 0.81 9% Example 3 0.64 7% Example 4 0.48 27% Example 5 0.71 15% Example 6 0.85 12% Example 7 0.95 8% Example 8 0.57 10% Comparative Example 1 0.26 48%
[0091] As can be seen from Table 1, the method of the present invention can improve the dispersion uniformity of alloy particles, reduce the size, and improve the anchoring effect of alloy particles, thereby improving the activity and stability of the catalyst by introducing nitrogen-containing organic small molecules during the process of preparing the noble metal-transition metal alloy catalyst by impregnation. In Comparative Example 1, the activity and stability of the catalyst were greatly reduced due to the lack of addition of nitrogen-containing organic small molecules.
[0092] By comparing Example 1 with Examples 4-5, it can be seen that there is a preferred range for the nitrogen content in the catalyst. If the nitrogen content is too little, the anchoring effect of the nitrogen atoms is insufficient, which is not conducive to improving the dispersion uniformity of the alloy particles, thereby resulting in a decrease in the effect of improving the activity and stability of the catalyst; if the nitrogen content is too much, it may clog the carrier pores, which is not conducive to the dispersion of the alloy particles and material transfer, thereby reducing the activity and stability of the catalyst.
[0093] By comparing Example 1 with Examples 6-7, it can be seen that by regulating the cooling rate, the process of orderly arrangement of alloy atoms can be prolonged, the order of the alloy can be improved, and then the activity and stability of the alloy can be improved.
[0094] By comparing Example 1 with Example 8, it can be seen that using nitrogen-containing organic liquid as a carbon source for carbon coating is more conducive to exerting the anchoring effect of nitrogen atoms, improving particle uniformity and reducing size, thereby improving catalyst performance, compared with ordinary carbon sources (such as glucose in Example 8).
[0095] The applicant declares that the present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a fuel cell catalyst, characterized in that: The preparation method comprises the following steps: The carbon carrier, the noble metal source, the transition metal source and the nitrogen-containing organic small molecules are uniformly mixed and then calcined to obtain the fuel cell catalyst.
2. The method for preparing a fuel cell catalyst according to claim 1, characterized in that: The model of the carbon carrier includes at least one of EC600JD, ECP600JD, EC300J, VXC-72, VXC-72R and BP2000; Preferably, the noble metal source includes at least one of chloroplatinic acid hexahydrate, tetraammine platinum nitrate, sodium chloroplatinate and platinum acetylacetonate; Preferably, the transition metal source comprises at least one of cobalt chloride hexahydrate, cobalt nitrate, nickel nitrate and iron nitrate; Preferably, the nitrogen-containing organic small molecule includes at least one of dicyandiamide, dopamine hydrochloride, aniline and melamine.
3. The method for preparing a fuel cell catalyst according to claim 1 or 2, characterized in that: The carbon carrier, the noble metal source, the transition metal source and the nitrogen-containing organic small molecule are mixed in the following manner: the carbon carrier, the noble metal source, the transition metal source and the nitrogen-containing organic small molecule are added to a solvent, ultrasonicated and stirred, and dried; Preferably, the solvent comprises at least one of water and ethanol.
4. The method for preparing a fuel cell catalyst according to claim 3, characterized in that: The ultrasonication and stirring are performed in the following manner: ultrasonication for 20 min to 45 min and then stirring for 12 h to 24 h.
5. The method for preparing a fuel cell catalyst according to any one of claims 1 to 4, characterized in that: The calcination is carried out in an atmosphere containing a reducing gas; Preferably, the atmosphere containing reducing gas is a mixed gas of protective gas and reducing gas, and the volume fraction of reducing gas in the mixed gas is 5% to 15%; Preferably, the protective gas comprises at least one of argon, helium and nitrogen; Preferably, the reducing gas comprises hydrogen; Preferably, the heating rate of the calcination is 1°C / min to 5°C / min; Preferably, the calcination holding temperature is 700°C to 900°C; Preferably, the calcination holding time is 1h to 3h; Preferably, during the calcination process, after the heat preservation is completed, the temperature is firstly lowered to 350°C to 450°C at a rate of 1°C / min to 5°C / min, and then cooled to room temperature.
6. The method for preparing a fuel cell catalyst according to any one of claims 1 to 5, characterized in that: The preparation method further comprises carbon coating the calcined catalyst to form a carbon shell on the surface of the catalyst; Preferably, the carbon coating method comprises: uniformly mixing the calcined catalyst with a nitrogen-containing organic liquid, and sintering to obtain a catalyst with a carbon shell; Preferably, the nitrogen-containing organic liquid comprises at least one of aniline and imidazole ionic liquids; Preferably, the mass ratio of the calcined catalyst to the nitrogen-containing organic liquid is (0.1-0.5):1; Preferably, the sintering atmosphere is an inert atmosphere; Preferably, the gas in the inert atmosphere includes at least one of nitrogen, helium and argon; Preferably, the sintering temperature is 650°C to 750°C; Preferably, the sintering time is 0.5 h to 2 h.
7. The method for preparing a fuel cell catalyst according to any one of claims 1 to 6, characterized in that: The calcined catalyst and the nitrogen-containing organic liquid are mixed in the following manner: the calcined catalyst and the nitrogen-containing organic liquid are mixed with an organic solvent and stirred for 12 to 24 hours, and then separated and the solid material is collected for sintering; Preferably, the organic solvent comprises at least one of acetone, methanol and DMF.
8. A catalyst prepared by the preparation method according to any one of claims 1 to 7; Preferably, the catalyst comprises a nitrogen-doped carrier and metal nanoparticles supported on the carrier, and the surface of the metal nanoparticles is coated with a nitrogen-doped carbon shell.
9. The catalyst according to claim 8, characterized in that The mass proportion of the noble metal element in the catalyst is 10% to 60%, the mass proportion of the transition metal element is 1% to 30%, and the mass proportion of the nitrogen element is 0.5% to 8%; Preferably, the particle size of the metal nanoparticles is 3.5 nm to 7.5 nm; Preferably, the thickness of the carbon shell is 0.6 nm to 2.7 nm.
10. A fuel cell, characterized in that: The cathode of the fuel cell comprises a catalyst prepared by the preparation method according to any one of claims 1 to 7 or a catalyst according to claim 8 or 9.
Citation Information
Cited By
Platinum-based catalyst with gold-doped surface as well as preparation method and application of platinum-based catalyst
CN119852433A