Chitosan-based swollen gel

A chitosan-based composition with chelating copolysaccharides forms threads or textiles that efficiently trap and diffuse metals, addressing the limitations of existing medical devices by enhancing metal capture and diffusion for conditions like endometriosis and neurodegenerative diseases.

JP2024537858AInactive Publication Date: 2024-10-16メクスブレン +4
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024520753
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-04
Filing Date
2022-10-03
Publication Date
2024-10-16
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing medical devices for chelating metals suffer from limited efficacy and side effects, and there is a need for minimally invasive, biocompatible materials that can locally restore metal homeostasis by capturing metal cations.

Method used

A composition comprising chitosan and a statistical copolysaccharide with chelating groups, which can be formed into threads or textiles, capable of efficiently trapping metals and swelling upon contact with biological fluids, allowing for effective metal capture and diffusion.

Benefits of technology

The composition demonstrates enhanced metal trapping and diffusion capabilities, suitable for medical applications such as dressings, implants, and dermal fillers, effectively addressing metal accumulation in conditions like endometriosis, fungal infections, and neurodegenerative diseases.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024537858000032
    Figure 2024537858000032
  • Figure 2024537858000033
    Figure 2024537858000033
  • Figure 2024537858000034
    Figure 2024537858000034
Patent Text Reader

Abstract

The present invention relates to the field of compositions comprising polymers carrying chelating groups capable of chelating one or more metals, and to various uses thereof. In particular, the present invention relates to a composition carrying a copolysaccharide having chelating groups, which may be in the form of a gel, as well as to threads obtained from this gel.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of compositions comprising polymers carrying chelating groups capable of chelating one or more metals, and to their various uses. In particular, the present invention relates to compositions, which may be in the form of gels, comprising polysaccharides carrying chelating groups, and to threads obtained from these gels. [Background technology]

[0002] Polysaccharides are polymers derived from plant, fungal, animal or bacterial biomass. These polymers have very diverse physicochemical properties and are often resorbable, biocompatible and even bioactive, allowing them to be used in a wide range of biomedical applications. Chemical modification of polysaccharides allows their physicochemical properties to be adapted, in particular their solubility in aqueous media at near-neutral pH. Functionalization of polysaccharides with highly specific chelating agents also allows specific applications in the biomedical field. For example, after grafting these units onto the polysaccharide structure, the polymers can be used in the composition of detoxifying biomedical devices to remove pathogenic metals from the living body, for example in terms of maintaining homeostasis.

[0003] Maintaining the homeostasis of the body's internal environment, i.e. all the biological fluids or fluids of the body, is necessary for the body to function properly. Systemic or local dysregulation in metal homeostasis has been demonstrated in many diseases. Chelation therapy, aimed at reducing the concentration of metal ions, has already been used for many years in cases of acute poisoning. Thus, a certain number of chelating agents has already been accepted in humans, each of which is associated with a specific group of metals (G. Crisponi et al., Coordination Chemistry Reviews, 2015).

[0004] A growing number of scientific studies highlight the important role that metals, especially iron, but also copper, zinc, manganese, and also aluminum and lead, play in many neurological disorders (EJ McAllum et al., J. Mol. Neurosci., 2016).

[0005] Thus, medical devices that can be used to capture metals already exist. Nevertheless, it would still be beneficial to improve the results obtained so far, and in particular to reduce the side effects of these treatments.

[0006] Furthermore, it would be desirable to have a variety of shapes for medical devices, for example single or multiple threads that can be woven or knitted in the form of a textile, resulting in a medical device of dressing or parietal implant type. Single threads may also be advantageous when implantation needs to be combined with a minimally invasive strategy. It would therefore be particularly interesting to provide threads that allow for the capture of metal cations in order to restore metal homeostasis locally in cases of metal accumulation in the body.

[0007] Thus, one object of the present invention is to propose a composition capable of chelating one or more metals. Another object of the present invention is to provide a thread capable of chelating one or more metals. Another object of the present invention is to provide a thread that has good mechanical properties and can therefore be woven or knitted in the form of a textile. [Prior art documents] [Non-patent literature]

[0008] [Non-Patent Document 1] G. Crisponi et al., Coordination Chemistry Reviews, 2015 [Non-Patent Document 2] EJ McAllum et al., J. Mol. Neurosci., 2016 [Non-Patent Document 3] Mike Robitzer, Laurent David, Cyrille Rochas, Francesco Di Renzo, and Francoise Quignard, Nanostructure of calcium alginate aerogels obtained from multistep solvent exchange route, Langmuir 2008, 24, 12547 - 12552 [Non - Patent Document 4] Mike Robitzer, Laurent David, Cyrille Rochas, Francesco Di Renzo, and Francoise Quignard, Supercritically - dried alginate aerogels retain the fibrillar structure of the hydrogels, Macromol. Symp. 2008, 273, 80 - 84 [Non - Patent Document 5] "Physico - chemical studies of the gelation of chitosan in a hydroalcoholic medium", A. MONTEMBAULT, C. VITON, A. DOMARD, Biomaterials, 26(8), 933 - 943, 2005 [Non - Patent Document 6] A. HIRAI, HODANI, A. NAKAJIMA, Polymer Bulletin, 26(1), 87 - 94, 1991 [Non - Patent Document 7] Alexander, L. E., "X - ray Diffraction Methods in Polymer Science", Wiley - Interscience, New York, 1969, 137 [Non - Patent Document 8] Alexander, L. E., "X - ray Diffraction Methods in Polymer Science", Wiley - Interscience, New York, 1969, 137 [Non-Patent Document 9] Asako Hirai et al., Determination of degree of deacetylation of chitosan by 1H NMR spectroscopy, Polymer Bulletin, 1991, 26, pp. 87-94 [Non-Patent Document 10] TE Robinson et al., Filling the Gap: A Correlation between Objective and Subjective Measures of Injectability, Adv. Healthc. Mater., vol. 9, no. 5, pp. 1901521, 2020 Summary of the Invention [Means for solving the problem]

[0009] First, the present invention provides a. at least one chitosan A, and b. at least one statistical copolysaccharide B of formula I having a mass average molecular weight between 100 kDa and 1000 kDa:

[0010] [ka]

[0011] (In the formula, each Rc independently represents a group that comprises a chelator; - each Z independently represents a linker, which may be a single bond or a hydrocarbon-based chain containing between 1 and 12 carbon atoms, said chain being linear or branched, containing one or more unsaturations, and which may contain one or more heteroatoms, preferably selected from the group consisting of nitrogen, oxygen, sulfur and halogen atoms; - x is between 0.01 and 0.5, - y is between 0.05 and 0.5, the ratio y / x is greater than 0.2 and preferably greater than 1; - the sum of x+y is greater than 0.1, and including chelators of type Rc in which less than 10% of the groups are chelated by cations of transition elements selected from block d or f elements; and c. optionally water.

[0012] The presence of chelating groups of type Rc in the copolysaccharide B allows this composition to efficiently capture one or more metals, and in particular to capture metal cations. Furthermore, the use of chitosan A and polysaccharide B produced from chitosan makes it possible to obtain a composition with beneficial properties. In fact, this composition may be biodegradable, biocompatible and bioresorbable. The use of such a composition, which allows to chelate metals, therefore has many possible medical applications.

[0013] In addition, it is possible to form threads from this composition, particularly by extrusion of the composition, which have good mechanical properties and can be shaped, for example, the threads can be braided to form textile materials (knitted or woven) capable of capturing metals.

[0014] Moreover, the inventors have surprisingly demonstrated that this composition is capable of swelling to a significant extent upon contact with biological fluids, which makes it possible to facilitate the diffusion and entrapment of the metal species to be captured, thus improving the effectiveness of the material.

[0015] The present invention also relates to a thread comprising a gel or a lyophilisate of the composition according to the invention.

[0016] The present invention also relates to a textile material comprising the yarn according to the invention.

[0017] The present invention also relates to a medical device comprising a composition according to the present invention, which is preferably a dressing, an implant, or a dermal filling product.

[0018] The present invention relates to a composition for use in sequestering at least one metal, preferably for use in the treatment or prevention of endometriosis, fungal infections, bacterial infections, chronic wounds, neurodegenerative injuries, nervous system lesions, hemochromatosis, Wilson's disease, or lead poisoning.

[0019] The present invention also relates to a method for preparing a composition according to the invention, comprising the following steps: 1) dispersing chitosan A and statistical polysaccharide B having a mass average molecular weight between 100 kDa and 1000 kDa of formula I in water; 2) adding an acid, preferably acetic acid; 3) mixing and then centrifuging the resulting solution to recover a solution containing the composition of the present invention; 4) Optionally, treating the solution obtained in step 3 in a basic water bath to obtain a composition in the form of a gel; and 5) Optionally, washing, drying and / or sterilizing the gel obtained in step 4, preferably by autoclaving.

[0020] Other features, details and advantages will become apparent upon reading the following detailed description and upon examination of the accompanying drawings, in which: [Brief description of the drawings]

[0021] [Figure 1] Photographs of disc-shaped hydrogels according to Example 4 are shown; top left: composition 9 according to the invention (HG-5-5); bottom left: composition 12 according to the invention (HG-8-8); bottom right: composition 10 according to the invention (HG-5-10); top right: composition 11 according to the invention (HG-5-15). [Diagram 2] 1 shows a photograph of a cylindrical hydrogel obtained according to Example 4, which is Comparative Composition 2 (Ref-HG-8-0). [Diagram 3]1 shows a photograph of a cylindrical hydrogel obtained in Example 4. This is composition 10 (HG-5-10) according to the present invention. [Figure 4] 1 shows an optical microscope photograph of a knotted yarn according to Example 5. [Diagram 5] 1 shows an optical microscope photograph of two braided yarns according to Example 5. [Figure 6] 4 shows a photograph of the dried gel according to Example 6. [Figure 7] 4 shows a photograph of a swollen gel according to Example 6. [Figure 8] 1 shows an optical microscope photograph of yarn half immersed in water according to Example 6. [Figure 9] 1 shows an optical microscope photograph of a yarn having a water droplet attached only to a portion thereof according to Example 6. [Figure 10] 1 shows a photograph of the formation of a gel according to Example 12 after injection of composition 23 according to the invention (IS-1,7-3,3) in 10 mM PBS. [Figure 11] MRI images (7.1 T) of gels formed immediately after injection (day 0), 15 days later, and 30 days later according to Example 14. [Figure 12] 1 shows an MRI image (7.1 T) of the gel formed immediately after injection according to Example 14. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] definition In this disclosure, all percentages and ppm are given by weight unless otherwise stated.

[0023] Unless otherwise indicated, all viscosities referred to in this disclosure correspond to "Newtonian" kinematic viscosities at 25°C, i.e. kinematic viscosities measured in a manner known per se using a rheometer with a shear rate gradient so low that the viscosity is measured independent of the rate gradient.

[0024] For the purposes of this disclosure, "chitosan" refers to a natural copolysaccharide type polymer consisting of a random (statistical copolymer) or non-random (block or sequence copolymer) distribution of D-glucosamine (GlcN) and N-acetyl-D-glucosamine (GlcNAc) linked by glycosidic bonds of the β(1->4) type, or even consisting exclusively of D-glucosamine. Chitosan does not occur naturally in particular in biomass, but is obtained primarily by chemical modification of chitin, of which chitosan is a derivative. Chitin has a structural role; it is found mainly in some fungi (Basidiomycetes, e.g., Agariscus campestris, Agariscus bisporus, Ascomycetes, Zygomycetes, and Deuteromycetes) where it forms the cell walls, but also in arthropods (crustaceans and insects), especially the exoskeleton of shrimp and crabs, and the endoskeleton of cephalopods such as the squid or cuttlefish. Chitin can be converted to chitosan by deacetylation, i.e. alkaline hydrolysis of the acetyl groups to generate primary amine groups. Chitosan is a biodegradable and biocompatible polymer with bacteriostatic and fungistatic properties.

[0025] "Gel" means a non-fluid polymer network swollen by a solvent. The polymer network is a network consisting of cross-linked polymer chains. The interactions involved in the cross-linking of the polymers can be physical or chemical. Advantageously, in the context of the present invention, the gel consists only of chitosan A, copolysaccharide B, and optionally water and / or an active pharmaceutical ingredient.

[0026] "Hydrogel" means a viscoelastic material containing at least 60% by weight, preferably at least 80% by weight, of water. The hydrogel according to the invention generally contains 0.1% to 40% by weight, preferably 0.5% to 20% by weight, of a mixture of chitosan A and copolysaccharide B.

[0027] In the context of the present invention, hydrogels are said to be physical because the interactions involved in the inter-chain crosslinking that give them cohesive strength are physical, in particular hydrogen bonds and / or hydrophobic interactions, in contrast to "chemical" hydrogels (also called cross-linked hydrogels), in which the inter-chain interactions are of the covalent type. In a pure physical hydrogel, no chemical crosslinkers are present. Advantageously, in the context of the present invention, physical hydrogels consist only of water, chitosan A, copolysaccharide B and optionally a pharmaceutical active ingredient, preferably containing more than 80% (w / w) of water. In particular, such hydrogels do not contain collagen, polycaprolactone or toxic chemical crosslinkers (glutaraldehyde, formaldehyde, epichlorohydrin type, etc.). While chemical hydrogels are poorly resorbable due to the stability of the covalent bonds, physical hydrogels of chitosan A and copolysaccharide B according to the present invention have the advantage that they are resorbable in physiological media, in particular under weakly acidic conditions.

[0028] "Xerogel" means a material obtained by drying, in particular by drying a hydrogel, containing less than 60% by weight of water, preferably less than 50% by weight, more preferably less than 20% by weight. The xerogel according to the invention generally contains at least 40% by weight of a mixture of chitosan A and copolysaccharide B, preferably between 40 and 100% of the mixture, preferentially between 50 and 99.9% and more preferentially between 80 and 99.5% of the mixture.

[0029] "Aerogel" refers to a material that is structurally similar to a hydrogel, but in which the water has been replaced by a gas using a process that prevents the effect of the capillary forces of the solvent on the material (Mike Robitzer, Laurent David, Cyrille Rochas, Francesco Di Renzo and Francoise Quignard, Nanostructure of calcium alginate aerogels obtained from multistep solvent exchange route, Langmuir 2008, 24, 12547-12552 and Mike Robitzer, Laurent David, Cyrille Rochas, Francesco Di Renzo and Francoise Quignard, Supercritically-dried alginate aerogels retain the fibrillar structure of the hydrogels, Macromol. Symp. 2008, 273, 80-84).

[0030] In the context of the present invention, the weight-average molar masses Mw of chitosan A and copolysaccharide B were determined by size-exclusion chromatography, the experimental conditions of which are described in the publication "Physico-chemical studies of the gelation of chitosan in a hydroalcoholic medium", A. MONTEMBAULT, C. VITON, A. DOMARD, Biomaterials, 26(8), pp. 933-943, 2005.

[0031] The degree of acetylation (DA) of chitosan A and copolysaccharide B is determined using proton NMR techniques according to the methodology of HIRAI (A. HIRAI, H ODANI, A. NAKAJIMA, Polymer Bulletin, 26(1), pp. 87-94, 1991).

[0032] In the context of the present invention, crystallinity expresses the proportion of material in a crystalline state. In the case of polysaccharides, the crystallinity is often determined by X-ray diffraction, since many polysaccharides decompose below the melting point of the crystalline phase, which makes differential scanning calorimetry unusable (Alexander, LE, "X-ray Diffraction Methods in Polymer Science", Wiley-Interscience, New York, 1969, p. 137). It is this method that is therefore considered in the context of the present invention. Other spectroscopic methods are possible but must be adapted in each case (Fourier transform infrared spectroscopy, Raman spectroscopy). In principle, density measurements in gradient columns would allow the degree of crystallinity to be calculated if the densities of the amorphous and crystalline phases of the polymer are known, but many polysaccharides can swell and absorb the solvents used in density gradient columns, thus further limiting the use of this method.

[0033] In the context of the present invention, the size of the crystallites can be determined by examining the width of the diffraction peaks obtained by powder methods using the Scherrer equation (Alexander, LE, "X-ray Diffraction Methods in Polymer Science", Wiley-Interscience, New York, 1969, p. 137).

[0034] Description of the embodiments First, the present invention provides a. at least one chitosan A, and b. at least one statistical copolysaccharide B of formula I having a mass average molecular weight between 100 kDa and 1000 kDa:

[0035] [ka]

[0036] (In the formula, each Rc independently represents a group that comprises a chelator; - each Z independently represents a linker, which may be a single bond or a hydrocarbon-based chain containing between 1 and 12 carbon atoms, said chain being linear or branched, containing one or more unsaturations, and which may contain one or more heteroatoms, preferably selected from the group consisting of nitrogen, oxygen, sulfur and halogen atoms; - x is between 0.01 and 0.5, - y is between 0.05 and 0.5, the ratio y / x is greater than 0.2 and preferably greater than 1; - the sum of x+y is greater than 0.1, and including chelators of type Rc in which less than 10% of the groups are chelated by cations of transition elements selected from block d and f elements; and c. Optionally, water.

[0037] According to one embodiment, the mass ratio between A and B (A:B) is between 2:1 and 1:10, preferably between 1:1 and 1:5.

[0038] The composition may further comprise at least one active pharmaceutical ingredient, preferably selected from anti-cancer agents, antibacterial agents, antifungal agents, anti-inflammatory agents, messenger RNA, proteins and antigens.

[0039] By active pharmaceutical ingredient is meant any compound that has a therapeutic or preventive effect. The fact that this composition has good swelling properties allows it to effectively capture and release the active pharmaceutical ingredient. In fact, the composition can be brought into contact with the pharmaceutical active ingredient, for example with a solution that contains the pharmaceutical active ingredient, and then the composition can capture this ingredient. This ingredient can then be released, for example, by immersing the composition in another medium. This is advantageously done when the composition is in the form of a gel.

[0040] The composition may be in multiple forms, such as an aqueous solution, a lyophilisate or a gel.

[0041] According to one embodiment, the composition is an aqueous solution, preferably comprising at least 10 g / l, preferably at least 50 g / l, of the mixture of chitosan A and copolysaccharide B. When the composition is in the form of an aqueous solution, the composition may be injectable. The concentration of the mixture of chitosan A and copolysaccharide B may be between 10 g / l and 500 g / l, preferably between 40 g / l and 160 g / l.

[0042] The aqueous solution may have a Newtonian viscosity between 0.1 and 50000 Pa·s, preferably between 50 and 25000 Pa·s, and more preferably between 100 and 10000 Pa·s.

[0043] The aqueous solution is a gellable solution. This aqueous solution may gel when it comes into contact with a coagulation bath at basic pH. Gelation occurs when the initially protonated (NH 3 + ), an amine (NH 2 ) occurs at basic pH after neutralization. The chain entanglement due to the high initial viscosity is fixed by the formation of interchain interaction sites (crystallites, hydrophobic interactions, hydrogen bonding interactions), resulting in a stable physical hydrogel with suitable mechanical properties for handling or stretching. The resulting hydrogel is reversible by treatment in acid solution and differs from chemical hydrogels, where gelation is brought about by the formation of irreversible covalent chemical bonds. It can be reversibly dried and rehydrated. The solution can also be freeze-dried.

[0044] The composition may also be in the form of a lyophilisate or a gel, preferably in the form of a hydrogel, xerogel or aerogel.

[0045] The hydrogel according to the invention may contain a mixture of chitosan A and copolysaccharide B in an amount of 0.1% to 40% by weight, preferably 0.5% to 20% by weight.

[0046] The xerogel according to the invention may contain at least 40% by weight of a mixture of chitosan A and copolysaccharide B, preferably between 40 and 100% of the mixture, preferentially between 50 and 99.9% and more preferentially between 80 and 99.5% of the mixture. When the composition is in the form of a xerogel, the xerogel may result from at least partial drying of a hydrogel.

[0047] Upon contact with an aqueous medium or biological tissue for at least 1 hour, the xerogel swells to form a hydrogel, said hydrogel having a volume at least twice, preferably at least five times, the volume of the reference xerogel before contact with the aqueous medium or biological tissue. Swelling can be quantified by measuring the mass of the initial xerogel and the mass of the resulting hydrogel.

[0048] Living tissues are a set of differentiated or undifferentiated cells organized in characteristic structures, in combination with a network of natural polymers or extracellular matrix (ECM), all contributing to the performance of the same functions. Cellular tissues are naturally hydrated and xerogels swell.

[0049] The hydrogel obtained by rehydration of the xerogel can then be dried again to reform the xerogel. Multiple drying-swelling cycles can be carried out on this composition.

[0050] The gels according to the invention have good mechanical properties. It is therefore possible to produce threads from these gels, for example by extruding the composition according to the invention through a die in a coagulation bath. These threads can then be used to produce fiber materials. The diameter of the threads can be between 50 μm and 700 μm, preferably between 80 μm and 500 μm.

[0051] The compositions according to the invention, in particular the threads and / or textile materials, can be used in medical devices due to their good properties of swelling and trapping metals. Advantageously, the threads and / or textile materials can be degraded in the body or explanted to remove the chelated metals.

[0052] The medical device is preferably a dressing, an implant or a dermal filler product. According to one embodiment, the medical device comprises the thread and / or textile material according to the invention.

[0053] In the case of a dermal filler product, said product may be in the form of a thread, said thread preferably being in the form of a xerogel that can swell on contact with an aqueous medium or biological tissue to form a hydrogel. The dermal filler product may also be a solution according to the invention, which can thus be injected.

[0054] Due to the good metal scavenging properties of this composition, it can be used to scavenging at least one metal in the treatment or prevention of endometriosis, fungal infections, bacterial infections, chronic wounds (pressure ulcers, diabetic wounds), neurodegenerative disorders (Parkinson's disease, Alzheimer's disease), hemochromatosis, Wilson's disease, or lead poisoning. The metal is preferably a metal cation. According to one embodiment, the metal belongs to the group consisting of copper, iron, lead, zinc, aluminum, gadolinium, and manganese, more preferably belongs to the group consisting of copper, iron, and lead.

[0055] The present invention also relates to the use of a composition according to the invention for sequestering at least one metal, optionally for treating or preventing a disease.

[0056] The present invention also relates to a method for treating or preventing endometriosis, fungal infections, bacterial infections, chronic wounds (pressure ulcers, diabetic wounds), neurodegenerative disorders (Parkinson's disease, Alzheimer's disease), hemochromatosis, Wilson's disease or lead poisoning, comprising the use of a composition according to the present invention to scavenge at least one metal.

[0057] Methods for preparing compositions The present invention also relates to a method for preparing a composition according to the invention, comprising the following steps: 1) dispersing chitosan A and a statistical copolysaccharide B of formula I having a mass average molecular weight between 100 kDa and 1000 kDa in water; 2) adding an acid, preferably acetic acid; 3) mixing and then centrifuging the resulting solution to recover a solution containing the composition; 4) Optionally, treating the solution obtained in step 3 in a basic water bath to obtain a composition in the form of a gel; and 5) Optionally, washing, drying and / or sterilizing the gel obtained in step 4, preferably by autoclaving.

[0058] Preferably, the acid is added in a stoichiometric ratio to the non-functionalized functional groups of primary amine type of chitosan A and copolysaccharide B. The acid is preferably an organic acid.

[0059] The solution containing the composition preferably has a viscosity between 0.1 and 50,000 Pa.s.

[0060] The basic water bath of step 4 is a coagulation bath that allows the solution to gel. This coagulation bath is preferably an alkaline solution, such as sodium hydroxide, aqueous ammonia or potassium hydroxide, with a concentration between 0.5 and 10 M, preferably between 1 and 5 M. The coagulation bath may also be a coagulation chamber in which alkaline vapors, such as ammonia vapor, are used.

[0061] To obtain threads, during step 4, the composition according to the invention can be extruded through a die (or extrusion cone). The extrudate is then introduced into a coagulation bath. It is also possible to extrude the composition directly into the coagulation bath.

[0062] Step 5 may include one or more washing steps, which may be performed using water or a buffer.

[0063] Step 5 can also include one or more solvent exchange steps, for example to replace water with ethanol.

[0064] Step 5 can include one or more drying steps. Drying in step 5 can be carried out outdoors, at room temperature, or under hot air at a temperature between 30 and 250° C., for example, between 100 and 200° C. According to one embodiment, drying is carried out by exchanging water for ethanol using successive baths of increasing alcohol concentration, followed by the ethanol being cooled in a pressurized chamber with liquid CO. 2 Then, supercritical CO 2 This is carried out after expansion in a medium, which allows the formation of an aerogel.

[0065] Any sterilization technique known to those skilled in the art may be used, in particular steam sterilization by autoclaving, or gamma or beta radiation.

[0066] Chitosan A The composition according to the invention comprises chitosan A.

[0067] The composition may comprise: - a crystallinity with respect to chitosan A of at least 10% relative to the total dry weight of the composition, and - Chitosan A crystallite size less than 20 nm.

[0068] The degree of crystallinity for chitosan A can be between 10 and 25%. Chitosan A crystallites act as physical crosslinking nodes essential for the formation of a gel. The size of the crystallites can be, for example, between 1 and 20 nm.

[0069] Advantageously, the chitosan A has an average molecular weight Mw between 100 kg / mol and 1000 kg / mol, preferably between 200 kg / mol and 700 kg / mol.

[0070] According to a preferred embodiment, chitosan A has a degree of acetylation x of less than 40%, preferably less than 10%, for example between 0% and 10%.

[0071] Copolysaccharide B The composition comprises a statistical copolysaccharide B of formula I having a mass average molecular weight between 100 kDa and 1000 kDa.

[0072] In the above formula I, it is understood that there may be multiple Rc groups in the polysaccharide. These Rc groups may be the same or different from each other. They are all independently selected from groups that carry chelating agents. The same is true for the linker Z: there may be multiple linkers Z, and the multiple linkers may be the same or different from each other.

[0073] Copolysaccharide B has the formula II:

[0074] [ka]

[0075] It may be of the following type. (In the formula, - Rc 1 and Rc 2 are different and are groups that contain a chelating agent, -Z 1 and Z 2 are the same or different and may be single bonds or hydrocarbon-based chains containing between 1 and 12 carbon atoms, said chains being linear or branched and containing one or more unsaturations and one or more heteroatoms, preferably selected from the nitrogen, oxygen, sulfur and halogen family of atoms; - x is between 0.01 and 0.5, preferably between 0.01 and 0.1 and preferentially between 0.05 and 0.1, - y is between 0.01 and 0.5, preferably between 0.05 and 0.2, - z is between 0 and 0.2; and (including chelators of type Rc1 and Rc2, in which less than 10% of the groups are chelated by cations of transition elements selected from the block d and f elements)

[0076] Groups of the type Rc include the Rc groups in the polysaccharides of formula I as well as the Rc groups in the polysaccharides of formula II. 2 When the group Rc is present, 1 and Rc 2 means.

[0077] According to one embodiment, less than 10%, preferably less than 5%, of the groups of type Rc are chelated by cations, in particular metal cations. The groups of type Rc are in free form and therefore have good metal capture. Copolysaccharide B is also highly hydrophilic, resulting in good swelling properties.

[0078] According to the invention, the groups Rc, Rc 1 and Rc 2 is a chelating agent. In other words, the groups Rc, Rc 1 and Rc 2 is capable of chelating one or more metals by forming a complex.

[0079] Rc, Rc 1 and Rc 2 Each of the groups may contain one or more coordination sites. The coordination sites are preferably nitrogen or oxygen atoms. Advantageously, Rc, Rc 1 and Rc 2 Each of the groups contains between 4 and 8 coordination sites, more preferably between 6 and 8 coordination sites, and even more preferably, R, R 1 and Rc 2 Each of the groups contains eight coordination sites.

[0080] Coordination site means a single functional group capable of binding to a metal. For example, an amine functional group represents a coordination site by forming a coordinate bond between the nitrogen atom and the metal, and a hydroxamic acid functional group also represents a coordination site by forming a coordinate bond with the oxygen of a carbonyl unit, which in turn forms a five-membered ring through a covalent bond with the oxygen of an N-oxide unit.

[0081] In one embodiment of the invention, for the polysaccharide of formula I, each Rc group is selected from the group consisting of DOTA (N,N',N'',N'''-(1,4,7,10-tetraazacyclododecane)tetraacetic acid), NOTA (1,4,7-triazacyclononane-1,4,7-triacetic acid), NODAGA (1,4,7-triazacyclononane-1-glutaric acid-4,7-diacetic acid), DOTAGA (2-(4,7,10-tris(carboxymethyl)-1,4,7,10-tetraazacyclododecane-1-yl)pentanedioic acid), DOTAM (1,4,7,10-tetrakis(carbamoylmethyl)-1,4,7,10-tetraazacyclododecane), NOTAM (1,4,7-tetrakis(carbamoylmethyl)-1,4,7-triazacyclononane), DOT Rc is independently selected from the group consisting of P(1,4,7,10-tetraazacyclododecane-1,4,7,10-tetrakis(methylene phosphonate), NOTP(1,4,7-tetrakis(methylene phosphonate)-1,4,7-triazacyclononane), TETA(1,4,8,11-tetraazacyclotetradecane-N,N',N'',N''''-tetraacetic acid), TETAM(1,4,8,11-tetraazacyclotetradecane-N,N',N'',N''''-tetrakis(carbamoylmethyl), DTPA(diethylenetriaminepentaacetic acid) and DFO(deferoxamine), preferably from the group consisting of DOTAGA, DFO, DOTAM, and DTPA. The Rc group is more preferably DOTAGA.

[0082] In one embodiment of the present invention, for the polysaccharide of formula II, Rc 1 and Rc 2are independently selected from the group consisting of DOTA, NOTA, NODAGA, DOTAGA, DOTAM, NOTAM, DOTP, NOTP, TETA, TETAM, DTPA and DFO, preferably from the group consisting of DOTAGA, DFO, DOTAM and DTPA.

[0083] According to one embodiment, for the polysaccharide of formula II, Rc 1 The group is DOTAGA, preferably where z=0.

[0084] According to one embodiment, for the polysaccharide of formula II, Rc 1 The group is DOTAGA, and Rc 2 The base is DFO.

[0085] The Z-type linker is a linker Z in a polysaccharide of formula I, and a linker Z in a polysaccharide of formula II. 2 If present, linker Z 1 and linker Z 2 means.

[0086] The linkers Z, Z in formula I and II 1 and Z 2 The choice is Rc, Rc 1 and Rc 2 This depends essentially on the group, as well as the metal to be chelated. This is especially true for steric reasons, where Rc, Rc 1 and Rc 2 This is because the group may be closer to or farther from the nitrogen of the six-membered ring of the glucosamine unit.

[0087] Preferably, in formula I, each Z is independently a single bond or a hydrocarbon-based chain containing between 1 and 12 carbon atoms, said chain being linear or branched, containing one or more unsaturations, and capable of containing one or more heteroatoms, preferably selected from the nitrogen, oxygen, sulfur and halogen group of atoms.

[0088] According to one embodiment, in formula I, each Z is independently selected from the group consisting of a bond, a linear or branched alkyl chain containing between 1 and 12 carbon atoms, and a linear or branched alkenyl chain containing between 2 and 12 carbon atoms; The alkyl and alkenyl chains may be one or more C 6 ~C 10 may be interrupted by aryl groups and / or one or more heteroatoms or groups selected from the group consisting of -O-, -S-, -C(O)-, -NR'-, -C(O)NR'-, -NR'-C(O)-, -NR'-C(O)-NR'-, -NR'-C(O)-O-, -OC(O)NR', ​​-C(S)NR'-, -NR'-C(S)-, -NR'-C(S)-NR'; The alkyl and alkenyl chains may be selected from the group consisting of halogen, -OR', -COOR', -SR', -NR' 2 and optionally substituted with one or more groups selected from the group consisting of Each R' is independently H or C 1 ~C 6 It is an alkyl.

[0089] Advantageously, in formula I, each Z is independently selected from the group consisting of a bond and a linear or branched alkyl chain containing from 1 to 12 carbon atoms; The alkyl chain may be one or more C 6 ~C 10 may be interrupted by aryl groups and / or one or more heteroatoms or groups selected from the group consisting of -O-, -S-, -C(O)-, -NR'-, -C(O)NR'-, -NR'-C(O)-, -C(S)NR'-, -NR'-C(S)-, -NR'-C(S)-NR'; Each R' is independently H or C 1 ~C 6 It is an alkyl.

[0090] In certain embodiments, each Z is an alkyl chain containing 1 to 12 carbon atoms.

[0091] In another particular embodiment, each Z is a polyethylene glycol (PEG) segment.

[0092] Preferably, in formula II, Z 1 and Z 2 are independently a single bond or a hydrocarbon-based chain containing between 1 and 12 carbon atoms, said chain being straight or branched, containing one or more unsaturations, and capable of containing one or more heteroatoms, preferably selected from the group consisting of nitrogen, oxygen, sulfur and atoms of the halogen family.

[0093] According to one embodiment, in formula II, Z 1 and Z 2 are independently selected from the group consisting of a bond, a straight or branched alkyl chain containing between 1 and 12 carbon atoms, and a straight or branched alkenyl chain containing between 2 and 12 carbon atoms; The alkyl and alkenyl chains may be one or more C 6 ~C 10 may be interrupted by aryl groups and / or one or more heteroatoms or groups selected from the group consisting of -O-, -S-, -C(O)-, -NR'-, -C(O)NR'-, -NR'-C(O)-, -NR'-C(O)-NR'-, -NR'-C(O)-O-, -OC(O)NR', ​​-C(S)NR'-, -NR'-C(S)-, -NR'-C(S)-NR'; The alkyl and alkenyl chains may be selected from the group consisting of halogen, -OR', -COOR', -SR', -NR' 2 and optionally substituted with one or more groups selected from the group consisting of Each R' is independently H or C 1 ~C 6 It is an alkyl.

[0094] Advantageously, in formula II, Z 1 and Z 2 is independently selected from the group consisting of a bond and a straight or branched alkyl chain containing 1 to 12 carbon atoms; The alkyl chain may be one or more C 6 ~C 10 may be interrupted by aryl groups and / or one or more heteroatoms or groups selected from the group consisting of -O-, -S-, -C(O)-, -NR'-, -C(O)NR'-, -NR'-C(O)-, -C(S)NR'-, -NR'-C(S)-, -NR'-C(S)-NR'; Each R' is independently H or C 1 ~C 6 It is an alkyl.

[0095] In certain embodiments, Z 1 and / or Z 2 is an alkyl chain containing 1 to 12 carbon atoms.

[0096] In another particular embodiment, Z 1 and / or Z 2 is polyethylene glycol (PEG).

[0097] According to the present invention, z is between 0 and 0.2. In other words, the type C units are exclusively composed of Z as a linker. 1 and Rc as a group carrying a chelating agent. 1 The unit may include.

[0098] The polysaccharides according to the invention have a mass average molecular weight between 100 kDa and 1000 kDa, preferably the mass average molecular weight of the polysaccharides according to the invention is between 200 kDa and 750 kDa, more preferably between 250 kDa and 500 kDa, and even more preferably between 300 kDa and 400 kDa.

[0099] According to one embodiment, the copolysaccharide B is the following polysaccharide: - a copolysaccharide of formula II, in which y=0.15, Rc 1 is DOTAGA, and Z 1 is a bond; - a copolysaccharide of formula II, in which 0.05≦z<0.06 and Rc 1is DOTAGA, and Z 1 is a bond and Rc 2 is DFO, and Z 2 is selected from the group consisting of a bond, and a straight or branched alkyl chain containing between 1 and 12 carbon atoms; The alkyl chain may be one or more C 6 ~C 10 may be interrupted by aryl groups and / or one or more heteroatoms or groups selected from the group consisting of -O-, -S-, -C(O)-, -NR'-, -C(O)NR'-, -NR'-C(O)-, -C(S)NR'-, -NR'-C(S)-, -NR'-C(S)-NR'; Each R' is independently H or C 1 ~C 6 It is an alkyl.

[0100] Copolysaccharide B can be obtained according to a method comprising three successive steps: Step 1: Dissolving chitosan in an acidic solution with a pH between 4 and 5; Step 2: Partial acetylation of the amine functional groups of the chitosan dissolved in step 1 (formation of acetylated units); Step 3: Functionalization of at least a portion of the amine functions still present at the end of step 2 (formation of units containing an Rc group).

[0101] Step 3 can be subdivided into several steps, particularly when the linker Z is a hydrocarbon-based chain as defined above.

[0102] In the embodiment in which the linker Z is a hydrocarbon-based chain as defined above, step 3 can comprise a substep 3-1 consisting of grafting said hydrocarbon-based chain onto at least a portion of the amine functional groups still present at the end of step 2, followed by a substep 3-2 consisting of grafting an Rc group onto said hydrocarbon-based chain. Alternatively, step 3 does not comprise any substeps. In this alternative, said hydrocarbon-based chain is coupled with an Rc group prior to step 3; thus, said step 3 is carried out with a molecule comprising an Rc group and said hydrocarbon-based chain.

[0103] Alternatively, copolysaccharide B can be obtained from chitosan having the desired degree of acetylation; therefore, in this embodiment, the acetylated units are already present and do not need to be formed. In this embodiment, the method for obtaining copolysaccharide B comprises at least the following two successive steps: Step 1b: dissolving the partially acetylated chitosan in an acidic solution of pH 4-5; Step 2b: Functionalization of at least a portion of the amine functional groups of said partially acetylated chitosan dissolved in step 1b (forming units containing Rc groups).

[0104] As with step 3 above, particularly when the linker Z is a hydrocarbon-based chain as defined above, step 2b above can be subdivided into several steps.

[0105] In the embodiment where the linker Z is a hydrocarbon-based chain as defined above, step 2b can comprise substep 2b-1 consisting of attaching said hydrocarbon-based chain to at least a portion of the amine functional groups, followed by substep 2b-2 consisting of grafting an Rc group to said hydrocarbon-based chain. Alternatively, step 2b does not comprise any substeps. In this alternative, said hydrocarbon-based chain is attached to an Rc group prior to step 2b; thus, said step 2b is carried out with a molecule comprising an Rc group and said hydrocarbon-based chain. EXAMPLES

[0106] Materials and Methods Compositions according to the invention were prepared using several chitosans A and copolysaccharides B. Table 1 summarizes the compounds used. The synthesis of compounds B1 and B2 is presented in Examples 1 and 2, respectively.

[0107] [Table 1]

[0108] The degree of acetylation (DA) of compounds B1 and B2 is obtained as follows: 1H NMR spectra of the products to be analyzed are obtained using a Bruker Avance III HD 400 MHz NanoBay spectrometer. The phase is manually corrected using the water peak at 4.7 ppm. The peaks are manually integrated, integrating the set of peaks between 4.1 and 2.9 ppm, and integrating between 2.02 and 1.90 ppm to bring the peak to 2.00 ppm. The DA as a percentage is obtained directly by normalizing the integrals of the set of peaks to 200.

[0109] The degree of substitution (DS) with DOTAGA is obtained as follows: various samples of the product to be analyzed are obtained by redispersing the lyophilized product in acetate buffer (0.1 M acetic acid and 0.1 M ammonium acetate) to obtain a final polymer concentration of 0.1% by weight. Different amounts of copper nitrate solution are added so that the copper concentration in each sample ranges from 0 to 1 mM, and each sample is then stirred. The absorbance of the resulting solution is then measured using a Varian Cary® 50 UV-visible spectrophotometer. The DS is determined by plotting the absorbance at 295 nm (maximum absorption of DOTAGA) as a function of the copper concentration, with the discontinuous area corresponding to the amount of DOTAGA per gram of product.

[0110] The purity of compounds B1 and B2 is verified as follows: HPLC-SEC-UV chromatograms of the products to be analyzed are recorded on samples at a concentration of 1% by weight of polymer using a Shimadzu Prominence HPLC system. The SEC column used is a PolySep-GFC-P4000 column, with acetate buffer as eluent (0.1M acetic acid and 0.1M ammonium acetate). The operating temperature is 30°C and the absorption wavelength is 295 nm. The flow rate of the eluent is 0.8 ml / min. The purity of the products is verified by the integration of the peak of free DOTAGA relative to the integration of the peak of chitosan to which DOTAGA is grafted.

[0111] Example 1 Synthesis of MEX-CD2(B1) The chitosan precursor of polysaccharide MEX-CD2 (B1) is of medical grade and of animal origin. The mass-average and number-average molar masses (Mw = 2.583x10, respectively) are: 5 g / mol, Mn=1.323x10 5 The acetylation degree of such chitosan (proportion of N-acetyl-D-glucosamine units) was determined using the Hirai method. 1 It is estimated to be 6±0.5% as determined by H NMR spectroscopy (Asako Hirai et al., Determination of degree of deacetylation of chitosan by 1H NMR spectroscopy, Polymer Bulletin, 1991, 26, 87-94).

[0112] 60 g of chitosan are introduced into a 10 l reactor together with 4 l of ultrapure water and 50 ml of acetic acid, then the mixture is placed under mechanical stirring at 500 rpm. After the chitosan has completely dissolved (3 h), 4 l of 1,2-propanediol are added to the medium and the mixture is kept under stirring until homogenization (2 h). 120 g of DOTAGA anhydride are then introduced and the mixture is kept under stirring overnight until complete dissolution. The synthesis product is then filtered through a Sartocon® Slice PESU cassette (polyethersulfone membrane; cut-off threshold: 100 kDa, filtration surface area: 0.1 m 2 The product is purified by tangential flow filtration using a Sartoflow® Advanced device equipped with a diafiltration concentration model against 200 l of 0.1 M acetic acid solution, then 200 l of 5 mM acetic acid solution. The purification is monitored by size exclusion chromatography coupled to a UV detector until less than 5% free DOTAGA is obtained. The product is then lyophilized and the degree of acetylation (DA) and the degree of substitution (DS) are determined, respectively. 1 Determined by 1 H NMR and copper chelation method as above. Purity is verified by HPLC as above.

[0113] Example 2 Synthesis of MEX-CDDFO1(B2) The chitosan precursor of polysaccharide MEX-CDDFO1 (B2) is the same as that described in Example 1 (M w =2.583×10 5 g / mol, Mn = 1.323 x 10 5 g / mol, D A = 6 ± 0.5%).

[0114] 60 g of chitosan, 4 l of ultrapure water and 45 ml of glacial acetic acid are introduced into a 10 l reactor and left under stirring at pH 4.5 ± 0.5 for 16 hours. 1.2 l of propane-1,2-diol are added to the solution and stirring is maintained for 1 hour. A solution consisting of 14 ml of acetic anhydride dissolved in 600 ml of propane-1,2-diol is then added slowly over 30 minutes and the reaction medium is kept under stirring for 4 hours. 120 g of DOTAGA anhydride are then weighed out and added to the reactor, then 2 l of propane-1,2-diol are added and stirring is maintained for 16 hours. At the end of the reaction, the solution is purified by tangential filtration using a 100 kDa membrane. The synthesis product is then purified by tangential flow filtration against 200 l of a 0.1 M acetic acid solution and then 200 l of ultrapure water in the same way as described in example 1. The purification is monitored by size exclusion chromatography coupled to a UV detector until less than 5% free DOTAGA is obtained. The product is then lyophilized at a concentration of 7 g / l and the degree of acetylation (DA) and degree of substitution (DS) are determined, respectively. 1 Determined by 1 H NMR and the copper chelation method described above.

[0115] 720 ml of purified chitosan-DOTAGA at a concentration of 7 g / l are introduced into a 2 l round-bottom flask. This solution (pH 6-6.5) is supplemented with ultrapure water to a total volume of 900 ml. In parallel, 143.1 mg of p-NCS-Bz-DFO are weighed out and dissolved in 100 ml of DMSO. This solution is then added dropwise to the chitosan-DOTAGA solution. The solution is maintained under stirring and heated overnight at a temperature of 40 °C. 500 ml of this solution are diluted to 5 l with ultrapure water and then transferred to two Sartocon® Slice PESU cassettes (polyethersulfone membrane; cut-off threshold: 100 kDa, filtration surface area: 0.02 m 2 ) to 1 L. Continue filtration at constant concentration against 4 L of ultrapure water, then reconcentrate the solution to 500 ml.

[0116] HPLC-SEC-UV analysis of the product makes it possible to verify the grafting of DFO and the removal of residual p-NCS-Bz-DFO.Comparing the HPLC-SEC-UV of chitosan DOTAGA and chitosan DOTAGA-DFO shows that the absorbance of the polymer peak (at about 7 min) increases when p-NCS-Bz-DFO is grafted.

[0117] In the case of MEX-CDDFO1(B2), the copper chelation method was applied to the product before functionalization with DFO, which made it possible to determine a DOTAGA DS of 8.6%. A method similar to the copper chelation method made it possible to determine the DFO DS. Increasing concentrations of iron(III) were added to a 0.1 g / l solution of MEX-CDDFO1(B2) in acetate buffer (0.1 M ammonium acetate and 0.1 M acetic acid) at pH 4.5. The absorbance measured at 425 nm ([Fe(η 6 It is possible to plot the λmax of the complex (MEX-CDDFO1(B2)) as a function of the iron concentration and obtain the DS at the iron concentration corresponding to the discontinuous region of the slope. This method allows the DS of MEX-CDDFO1(B2) to be estimated as 0.7%.

[0118] The intermediate product (N-DOTAGA chitosan) obtained by the above method 1 H NMR analysis allowed the determination of a DA of 26%. 1 H NMR analysis reveals the presence of a peak at 7.3 ppm, characteristic of the protons of substituted benzenes. The NMR spectrum of this product also has peaks between 1.1 and 1.7 ppm, which are identical to those of deferoxamine mesylate alone, confirming the effective grafting of DFO onto N-DOTAGA chitosan after purification.

[0119] Example 3 Synthesis of MEX-CDFO(B3) The chitosan precursor of the polysaccharide MEX-CDFO (B2) is the same as that described in Example 1 (M w =2.583×10 5g / mol, Mn = 1.323 x 10 5 g / mol, DA=6±0.5%). For 2.5 g of chitosan, 170 ml of ultrapure water and 2.25 ml of glacial acetic acid are introduced into a 1 liter reactor and left under stirring until the chitosan is completely dissolved. 50 ml of propane-1,2-diol are added to the solution. Subsequently, a solution consisting of 785 μl of acetic anhydride dissolved in 25 ml of propane-1,2-diol is slowly added and the reaction medium is kept under stirring for 4 hours. 40 ml of ultrapure water and 43 ml of a 1M solution of NaOH are added to obtain a solution with a pH between 5.5 and 6.5. 75 ml of propane-1,2-diol and 35 ml of DMSO are added. At the same time, 576 mg of p-NCS-Bz-DFO are weighed and dissolved in 57.6 ml of DMSO. This solution is added at a rate of 150 μl / min. During the addition of DFO, 3.1 ml of 1 M HCl is also added at a rate of 8 μl / min. The solution is kept under stirring and heated at a temperature of 40° C. overnight. 250 ml of this solution is diluted 5-fold with 0.1 M acetic acid and then transferred to two Sartocon® Slice PESU cassettes (polyethersulfone membrane; cut-off threshold: 100 kDa, filtration surface area: 0.02 m 2 The solution is reconcentrated to 500 ml by tangential filtration using a Sartoflow® Smart device equipped with a centrifuge. The filtration is continued at constant concentration against 5 l of acetic acid and 2.5 l of ultrapure water, then the solution is reconcentrated to 250 ml.

[0120] For MEX-CDFO(B3), the iron chelation method described above is also used to estimate the DS, which allows the DS of MEX-CDFO(B3) to be estimated as 3%.

[0121] 1 H NMR analysis makes it possible to confirm the grafting of DFO and DS by the peaks characteristic of DFO. According to the NMR spectrum, the DS is equal to 2.9%. With this same spectrum it is also possible to determine the DA. The measured DA is 41%.

[0122] Example 4 Composition according to the present invention (aqueous solution) Different compositions according to the invention were prepared. Non-functionalized chitosan A with low DA, which can be 250 kDa or 650 kDa, is mixed with copolysaccharide B in a ratio of α / β%, where α is the mass concentration of chitosan A and β is the mass concentration of copolysaccharide B in the blend (table 2). Different amounts of lyophilized forms of chitosan A (α) and copolysaccharide B (β) are introduced into a 50 ml reactor and redispersed in a suitable amount of water under gentle stirring. Acetic acid is added in a stoichiometric ratio with respect to the non-functionalized primary amine functions present in the medium. The mixture is left under stirring until the product is completely dissolved.

[0123] As an example, composition 10 (HG-5-10) according to the invention is prepared as follows: 3.0 g of B1 (MEX-CD2) and 1.5 g of chitosan A1 are dispersed in 28.93 ml of ultrapure water and 1.07 ml of ultrapure acetic acid are added to a 50 ml reactor with mechanical stirring at 100 rpm. The mixture is left under stirring for 24 hours until it is completely dissolved and the medium is homogenized.

[0124] The different compositions and their preparations are shown in table 2.

[0125] [Table 2A] TIFF2024537858000006.tif11144

[0126] [Table 2B] TIFF2024537858000008.tif16150

[0127] The resulting solutions are collected and introduced into a suitable fluid metering device, then centrifuged at 4000 rpm for 10 minutes to obtain a bubble-free solution containing the composition. The Newtonian viscosity of each solution was measured using a TA Instruments AR200 rheometer. Each resulting solution was also tested to see if it was possible to produce gels and / or threads. The results are shown below (table 3).

[0128] [Table 3]

[0129] These results show that, unlike the compositions according to the invention, it is not possible to gel the solution or to produce threads when the composition contains only copolysaccharide B. However, the addition of copolysaccharide B to chitosan A makes it possible to obtain gellable solutions and in some cases to reduce the viscosity of the resulting solutions (see Comparative Compositions 2 and 3 and 9, as well as Comparative Compositions 4 and 13), which contributes to a better manageability of the solution and thus allows good thread formation.

[0130] Example 5 Composition (gel) according to the present invention Several hydrogels were obtained by gelling the solution obtained in Example 3. The gelling of the solution occurs after immersion in a 3 mol / l sodium hydroxide bath. The hydrogels obtained according to the invention are formed by the initial protonation of the (NH 3 + ), an amine (NH 2It is characterized as a physical hydrogel in which gelation occurs at basic pH after neutralization of the hydroxyl group. The chain entanglement state due to the high initial viscosity is fixed by the formation of interchain physical interaction nodes, resulting in a stable physical hydrogel with suitable mechanical properties for handling or stretching. The resulting hydrogel is reversible by treatment in acid solution, which distinguishes it from chemical hydrogels in which gelation is brought about by the formation of irreversible covalent chemical bonds. It can be reversibly dried and rehydrated.

[0131] Obtaining disc-shaped hydrogels After centrifugation, compositions 9-12 according to the invention are introduced into a PVC mould, the dimensions of which are either Φ=1 cm and h=2 mm, or Φ=3 cm and h=2.5 mm. After the solution has spread evenly, the mould with the solution is introduced into a 3 mol / l sodium hydroxide (NaOH) bath for 1 hour and 30 minutes. The hydrogel disc thus formed is removed from the mould and introduced into a water bath for 30 minutes. The disc is then rinsed a second time in another ultrapure water bath for 30 minutes. The hydrogel is then rinsed for 24 hours in a phosphate buffer solution at pH=7.4. The hydrogel is then placed in a glass vial together with the phosphate buffer solution and sterilised in an autoclave at 121 ° C for 20 minutes. The hydrogel obtained in the form of a disc is presented in FIG. 1.

[0132] Obtaining cylindrical hydrogels After centrifugation, the comparative composition 2 and the composition 10 according to the invention are connected to a compressed air system (Nordson Ultimus™) to allow the solution to be extruded. An extrusion tube with a diameter of 5 mm is attached to the syringe of a dispenser and the solution is extruded directly into a 3 mol / l sodium hydroxide bath. The extrusion pressure is adapted to the initial viscosity of the precursor solution and is between 1 and 3 bar. The hydrogel thus formed is left immersed in the sodium hydroxide bath for 1 hour and 30 minutes. The disk is removed and introduced into a bath formulation of ultrapure water for 30 minutes. The tube is then rinsed a second time for 30 minutes in another ultrapure water bath. The hydrogel is then rinsed for 24 hours in a phosphate buffer solution with a pH of 7.4. Finally, the hydrogel is placed in a glass vial together with the phosphate buffer solution and sterilized in an autoclave at 121° C. for 20 minutes. The hydrogel obtained in cylindrical form is shown in figures 2 and 3.

[0133] Hydrogels obtained from chitosan A alone have an opaque white appearance and are relatively stiff when handled. The more copolysaccharide B present in the hydrogel, the more transparent it appears and the less pronounced the Tyndall effect, reflecting an increased homogeneity of the structure at the microscopic level.

[0134] Example 6 Composition (yarn) according to the present invention A thread comprising a composition according to the invention is obtained as follows: a portion of the solution obtained in Example 3 is introduced into a suitable fluid dispenser (or metering device) and then centrifuged. The fluid dispenser containing the solution is then connected to a compressed air system. The dispenser is equipped with a 254 μm, 406 μm or 584 μm extrusion cone, and the solution is extruded under a constant pressure ranging from 150 kPa to 400 kPa into a 3 mol / l concentrated sodium hydroxide bath. The resulting hydrogel is neutralized in two water baths and then dried at temperatures ranging from 100 ° C to 200 ° C using a temperature-regulated blower. The dried thread is collected and wound on a reel.

[0135] By way of example, a thread of composition 10 according to the invention is prepared as follows: 3.0 g of copolysaccharide B1 and 1.5 g of chitosan A1 are dispersed in 28.93 ml of ultrapure water and 1.07 ml of ultrapure acetic acid in a 50 ml reactor with gentle mechanical stirring at 100 rpm. The mixture is left under stirring for 24 hours until it is completely dissolved and the medium is homogenized. The solution obtained is collected and introduced into a suitable fluid dispenser and then centrifuged for 10 minutes at 4000 rpm. The fluid dispenser containing the solution is then connected to a compressed air system, the system being equipped with a 406 μm extrusion cone. A constant pressure of 200 kPa is delivered until the starting solution is completely extruded. The solution is extruded directly into a 3 mol / l sodium hydroxide bath and directly gelled to form a hydrogel. The hydrogel obtained in the form of a thin cylinder is sent to a winding circuit and gradually neutralized in two ultrapure water baths, each containing 5 liters of water. The hydrogel is then dried under hot air at 150 °C using a temperature-controlled blower. The yarn obtained after drying is wound on a reel located at the end of the yarn forming circuit. The yarn obtained is shown in Figures 4 and 5. These figures show that it is possible to make knots and to braid several yarns together.

[0136] The average diameter of the yarns was determined by measuring different parts of the yarn using an optical microscope. On average, five parts of the yarn were studied in order to establish an average diameter as representative as possible of the overall structure. The linear density of the different yarns was also determined by weighing different lengths of yarn on a precision balance. The mechanical properties of the obtained yarns were measured by tensile tests using a Shimadzu Autograph AG-X plus system. On average, five tensile tests are performed for each yarn to verify the reproducibility of each measurement. The results are shown in table 4.

[0137] [Table 4A] TIFF2024537858000011.tif21149

[0138] [Table 4B]

[0139] These results show that the yarn according to the invention has satisfactory mechanical properties comparable to those of yarns containing only chitosan A. In particular, the yarn according to the invention has mechanical properties suitable for shaping yarns by interlacing several yarns together or by weaving or knitting.

[0140] Example 7 Swelling studies of threads and gels according to the invention All of the gels and threads according to the invention described in the previous section have an inherent swelling capability in the presence of aqueous fluids. First, the drying and swelling capabilities and kinetics of the gels were determined based on the initial formulation. After neutralizing the pH of the hydrogels by successive rinsing, the gels are left outdoors for one week until they are completely dried to become xerogels. The mass of the hydrogels was measured using a precision balance before and at regular time intervals during drying. The drying kinetics of the hydrogels are shown in table 6. Chitosan A is more hydrophobic than copolysaccharide B, so the gels dry slower when they contain a higher amount of copolysaccharide B. Thus, the reference gel with chitosan A alone (comparative composition 2) reaches a stable mass after 30 hours, composition 9 according to the invention (HG-5-5) after 52 hours, composition 12 according to the invention (HG-8-8) after 72 hours, and compositions 10 and 11 according to the invention (HG-5-10 and HG-5-15) after 144 hours.

[0141] [Table 5]

[0142] The xerogels were then immersed in ultrapure water for 48 hours until the gels were completely hydrated. The mass of each gel was precisely measured before hydration and at regular time intervals during the swelling test. The swelling kinetics of the gels is shown in table 6. As with the drying process, the hydrophobicity of the reference gel based only on chitosan A limits the rehydration of the gel. Thus, the maximum swelling of the gel obtained from comparative composition 2 (Ref HG-8-0) is low, with approximately doubling of its initial volume observed after 6 hours. On the other hand, a significant increase in the swelling capacity of the gels according to the invention is observed based on the amount of copolysaccharide B present in the formulation, ranging more than 22 times the initial volume for composition 11 according to the invention (HG-5-15) after 30 hours.

[0143] The gel before and after hydration is shown in Figures 6 and 7 (composition 11 according to the invention).

[0144] [Table 6]

[0145] The swelling capacity of the yarns according to the invention was also evaluated during rehydration by immersion in a bath of ultrapure water. In the same way as for the solid hydrogels, the yarns according to the invention were cut and then immersed in ultrapure water for 15 minutes. The initial mass of each yarn and the mass of the yarn at each time point were measured using a precision balance. The swelling kinetics of the yarns are shown in table 7. Based on the initial diameter of the yarn, slight differences in swelling are observed for a given formulation. For the same formulation, the swelling values ​​obtained from the yarns are relatively similar to those obtained with the hydrogels. As in the case of the hydrogels, the reference yarn based on chitosan A (comparative composition 2, Ref HG-8-0) shows a low maximum swelling of approximately 2 times its initial volume after 15 minutes. The yarn obtained with composition 11 according to the invention (HG-5-15), which contains the highest amount of copolysaccharide B, shows a swelling capacity comparable to the hydrogel of the same formulation, ranging up to 21 times its initial volume after 15 minutes of immersion. Unlike hydrogels, the rehydration observed in the yarns is very fast, which is due to the much higher surface area to volume ratio of the yarns than in solid hydrogels. The phenomenon of yarn swelling was also observed microscopically by immersing a portion of the yarn obtained with composition 11 according to the invention (HG-5-15) in ultrapure water for 5 minutes. Similarly, the effect of a water drop on a portion of the yarn was observed. The yarns are shown in Figures 8 and 9.

[0146] These results show that the composition according to the invention has a much higher swelling capacity than threads containing chitosan A alone.

[0147] [Table 7]

[0148] Experiments were carried out on discs of hydrogel according to the invention to evaluate the effect of multiple drying-swelling cycles on the hydration and dehydration capacity of the hydrogel. A solution of composition 11 (HG-5-15) according to the invention was formulated and then gelled in a mould with dimensions Φ=3 cm and h=2.5 mm to obtain a disc-shaped hydrogel, the mass of which was precisely measured using a precision balance. The hydrogel was then rinsed as described above, then left to dry for one week and weighed. The xerogel was then rehydrated, weighed after full hydration and dried again for one week. After one week, the gel was weighed and again immersed in water for 5 days. The values ​​obtained over multiple cycles are listed in table 8.

[0149] [Table 8]

[0150] A small amount of mass loss associated with a decrease in the swelling and drying capacity of the gel appears to occur gradually over the hydration and dehydration cycles, but remains very limited.Similarly, a limited loss of 14% of swelling capacity is observed even after two complete cycles of hydration and dehydration over a total period of two weeks.

[0151] Example 8 Study of the metal extraction capacity of the yarn according to the invention The ability of certain yarns according to the invention to extract lead, copper, cadmium and iron was precisely evaluated by ICP-MS analysis after immersion of the yarns in dilute solutions of the metals. First, the three metal cations (Cu 2+ , Pb 2+ , Cd 2+The experiments were carried out with metal solutions containing 0 ppb, 10 ppb and 100 ppb of the three metals Cu, Pb and Cd, respectively. 10 ml of metal solutions composed of 0 ppb, 10 ppb and 100 ppb of the three metals, Cu, Pb and Cd, respectively, were prepared in ultrapure water from a reference solution of 500 ppb of each metal. In parallel, 1 mg of thread is accurately weighed on a precision balance and then this piece is cut into four pieces of the same length and mass (mass = 0.25 mg). The four pieces of thread are subsequently immersed in the respective metal solutions. After periods of 4 h, 1 day, 2 days and 1 week, respectively, the pieces of thread are collected and dried in an oven at 40 °C for 24 h. The dried samples after 4 h, 1 day and 2 days were subsequently prepared without prior mineralization by immersing the dried thread in 1 ml of 10% by mass nitric acid (HNO 3 ) solution and then analyzed using a Perkin-Elmer ICP-MS Nexion2000 spectrophotometer. Samples were collected after one week and then diluted with 2 ml of 69% by weight HNO 3 and 1 ml of ultrapure water are introduced into a Teflon container and digested for 30 minutes at 200° C. in an Anton Paar Multiwave5000 microwave. The mineralization products are then analyzed by ICP-MS. The results obtained for the threads obtained with composition 12 according to the invention (HG-8-8) are shown in table 9.

[0152] [Table 9]

[0153] The thread used in this experiment was obtained with composition 12 (HG-8-8) according to the invention and was therefore composed of 50% by weight of chitosan A and 50% by weight of copolysaccharide B. The thread was immersed in a metal solution equivalent to 10,000 times its own volume and was able to effectively extract copper, lead and cadmium, concentrating the metals by more than 1000 times by volume compared to the surrounding solution. This thread was also able to effectively extract the three metals from a dilute metal solution of about 10 ppb.

[0154] To evaluate the iron extraction capacity of the thread, metal extraction studies were also performed in biological media on reconstituted and highly hemolyzed porcine blood. A solution of 10 ml of hemolyzed porcine blood is prepared by redispersing 10 g / l of dried powdered blood in ultrapure water. In parallel, 1 mg of thread is accurately weighed on a precision balance and then this piece is cut into four pieces of the same length and mass (mass = 0.25 mg). The four pieces of thread are subsequently immersed in a solution of reconstituted porcine blood. After periods of 1 h, 2 h, 4 h, and 24 h, respectively, the thread pieces are collected and rinsed with 60 ml of ultrapure water for 1 min and then dried in an oven at 40 °C for 24 h. The dried thread is then collected and washed with 2 ml of 69% by mass HNO. 3 and 1 ml of ultrapure water in a Teflon vessel and digested for 30 minutes at 200° C. in an Anton Paar Multiwave 5000 microwave. The mineralization products are then analyzed by ICP-MS. The results obtained with the three threads are shown in table 10.

[0155] [Table 10]

[0156] After immersion for 1 hour, the three threads are able to extract iron from the medium. However, the addition of copolysaccharide B to the composition makes it possible to increase the iron chelating capacity of the threads after 1 hour, which increases significantly after 2 hours. This increase is particularly evident when the composition according to the invention contains two different chelating agents of the Rc type.

[0157] The iron extraction capacity of the present invention in the face of different iron(III) chelators (citrate, NTA, deferiprone) was precisely evaluated by ICP-MS analysis after immersion of xerogel dots in iron solutions (2 ppm iron) containing iron chelators in ratios with one iron cation per complex (citrate 11 / iron 1; NTA 1.1 / iron 1; deferiprone 4 / iron 1). For solutions containing citrate or deferiprone, the solution was buffered to pH 7.4 with 0.1 M PBS; for solutions containing NTA, the buffer used was 0.05 M Tris HCl. A known mass of xerogel dots was immersed in a volume of 20 ml of metal solution for 24 hours for the experiments with deferiprone and 90 hours for the experiments with NTA and citrate. Control dots were immersed in buffer (PBS or Tris HCl) for the time corresponding to the experiment in question. Samples were collected from the solutions at t:0 and t:final. These samples were analyzed using a Perkin-Elmer ICP-MS Nexion2000 spectrophotometer. The gel dots were collected and mineralized in an Anton Paar Multiwave5000 microwave as described above. The solutions thus obtained were analyzed by ICP-MS. The results obtained for inventions 10, 16, 17, 15, 18, with compositions HG-5-10; HG-5-9,5-0,5; HG-5-9,2-0,8; HG-5-9-1; HG-5-8-2, respectively, are shown in table 11.

[0158] [Table 11]

[0159] The different compositions are able to extract iron from solutions containing iron chelators with relatively low complexation constants, such as citrate or NTA. When the dots are faced with a strong iron complexing agent, as in the case of deferiprone, only the gels containing DFO corresponding to inventions 16, 17, 15 and 18 are able to extract iron. Invention 18 (HG-5-8-2), which has the most polymer MEX-CDFO (B3) in its composition, has the best iron extraction capacity when faced with deferiprone.

[0160] To evaluate the iron extraction capacity of the dots under realistic conditions, another metal extraction study was carried out in a biological medium of bovine plasma. For inventions 10, 16, 17, 15 and 18, the dots were weighed and introduced into 20 ml of bovine plasma for 24 hours. The plasma at t:0 is analyzed by ICP-MS. The dots are mineralized and analyzed by ICP-MS according to the method described above. The results obtained for inventions 10, 16, 17, 15 and 18 with compositions HG-5-10; HG-5-9,5-0,5; HG-5-9,2-0,8; HG-5-9-1; HG-5-8-2, respectively, are shown in table 12.

[0161] [Table 12]

[0162] After 24 hours, the three gels are able to extract some of the iron from the plasma.

[0163] Example 9 Study of the release capabilities of threads and hydrogels according to the invention The ability to load a substance of interest onto the thread and control its release in another solution or medium was demonstrated. First, fluorescent molecules were used to evaluate the possibility of loading and releasing the substance from the thread. 10 ml of 25 mg / l fluorescein solution is prepared by dissolving fluorescein in ultrapure water. 4 mg of thread is then cut and weighed using a precision balance and then immersed in the fluorescein solution for 10 minutes. The thread is then removed from the solution and dried in an oven at 40° C. for 2 hours and then at room temperature for 3 days. The thread is then immersed in 20 ml of ultrapure water and 2 ml samples of this solution are collected after 0, 1, 2, 5, 10, 15, 30, 45 minutes and 15 hours and analyzed using an Agilent Cary Eclipse fluorescence spectrometer (table 11).

[0164] [Table 13]

[0165] The ability of the three thread formulations to load and release the substance of interest was studied by analyzing the fluorescence of the solution after release using fluorescein. After immersion of the loaded dry threads in ultrapure water for one minute, the three threads release fluorescein. Comparative formulation 2 (HG-8-0), consisting only of chitosan A, releases very little fluorescein. The addition of copolysaccharide B to the thread composition can increase the release capacity of the thread; this is especially true the more copolysaccharide B is loaded into the composition.

[0166] The same experiment is carried out, this time loading the thread with miconazole, an imidazole-based antifungal molecule commonly used in various medical devices (topical sprays, creams, lotions, etc.) to combat fungal infections. 100 ml of 0.1 g / l miconazole solution is prepared by dissolving miconazole in ultrapure water. 0.9 mg (10 cm) of thread from composition 10 (HG-5-10) according to the invention is then cut and weighed using a precision balance, then immersed in the miconazole solution for 10 minutes. The thread is then removed from the solution, suspended from a glass rod and allowed to dry at room temperature for 3 hours. The thread is then directly immersed in 3 ml of ultrapure water in a plastic spectrophotometer cuvette, and the medium is analyzed at regular time intervals by fluorescence analysis using an Agilent Cary Eclipse spectrophotometer (table 12).

[0167] [Table 14]

[0168] The same experiment was carried out by loading the thread with the antibiotic penicillin. A 0.1 g / 100 ml solution of penicillin is prepared by dissolving penicillin in ultrapure water. Then, 0.9 mg (10 cm) of thread from composition 10 (HG-5-10) according to the invention is cut and weighed using a precision balance, and then immersed in the penicillin solution for 5 minutes. The thread is then removed from the solution, hung from a glass rod, and dried at room temperature for 3 hours. The thread is then immersed in 10 ml of ultrapure water and samples are collected after 1 hour, 2 hours, and 22 hours. The samples are then analyzed by UV-visible absorbance using an Agilent Varian Cary50 UV-vis spectrophotometer (table 13).

[0169] [Table 15]

[0170] These results demonstrate that the compositions according to the present invention are capable of loading active pharmaceutical ingredients and also releasing said ingredients.

[0171] Example 10 Preliminary study of the composition of gelling injectable solutions. Solutions were prepared in the same manner as described in Example 4, but this time adding an amount of acetic acid that would result in a homogenous mixture with a lack of acid relative to the non-functionalized amine functional groups. Briefly, different amounts of chitosan A1 and compound B1 were added to a reactor with Milli-Q water and acetic acid. The mixture was left under stirring at 100 rpm for at least 1 hour. The solution was then collected and introduced into a fluid dispenser, which was then centrifuged at 4000 rpm for 10 minutes to remove any remaining air bubbles. The pH and osmolality of each formulation were measured using a Mettler Toledo SevenCompact S210 pH meter and a Camlab Loser Micro MOD200 Plus osmometer, respectively. The different compositions and their preparations are shown in table 16.

[0172] [Table 16]

[0173] The pH values ​​obtained for aqueous solutions of MEX-CD2 without the addition of acid are relatively low. This is explained by the pre-existence of acetic acid in the MEX-CD2 lyophilisate to ensure solubility during the purification process. The acetic acid contained in the MEX-CD2 lyophilisate is also osmotically active and contributes to the increase in osmolality.

[0174] The viscosity of each solution was measured using a HAAKE RheoStress 600 rheometer equipped with a C35 / 2° TiL plate-cone geometry. The Newtonian viscosity values ​​are shown in table 15. Note that the viscosity is directly dependent on the total polymer concentration; the lower the concentration, the lower the viscosity. Similarly, for the same total polymer concentration, a larger mass fraction of MEX-CD2 contributes to a decrease in viscosity.

[0175] The injectability of each composition was precisely measured using a Shimadzu AG-X plus force tester. Each solution was introduced into a 1 ml BDHylok™ prefillable glass syringe equipped with a Sterican 27G needle (0.4x12mm). Injectability was determined as the force (Newtons) required to expel the solution at a constant plunger speed of 1 mm / s. The injectability of the system depends primarily on the viscosity of the solution and thus on the total polymer concentration and, to a lesser extent, on the mass fraction of MEX-CD2 in the composition. Thus, a solution is easily injectable at 3% (wt / wt), moderately injectable at 5% (wt / wt), difficult to inject at 7% (wt / wt), and not injectable at 10% (wt / wt) (TE Robinson et al., Filling the Gap: A Correlation between Objective and Subjective Measures of Injectability, Adv. Healthc. Mater., vol. 9, no 5, pp. 1901521, 2020).

[0176] [Table 17]

[0177] Example 11 Determination of the suitable mass fraction of MEX-CD2 for gelling injection solutions This example makes it possible to demonstrate the effect of the mass fraction of MEX-CD2 on the final formulation. Therefore, 5% (wt / vol) solutions containing different mass fractions of MEX-CD2 ranging from 0% to 100% of MEX-CD2 were generated. Each of these formulations was sterilized in an autoclave at 121 °C for 20 min to evaluate the effect of this method on the rheological properties of the system. The pH, osmolality, viscosity, and injectability of each of these formulations were measured and are shown in table 18.

[0178] [Table 18A]

[0179] [Table 18B]

[0180] These formulations were produced by adding acetic acid in stoichiometric proportions to the free amines of the two polymers; the residual amount of acetic acid present in the MEX-CD2 lyophilisate was not taken into account. This explains why the pH decreases practically linearly with the amount of MEX-CD2 added to the composition and therefore with the mass fraction of MEX-CD2 in the formulation. The Newtonian viscosity measured on these solutions before and after sterilization decreases linearly as a function of the mass fraction of MEX-CD2. The injectability follows the same trend, thus demonstrating that the higher the amount of MEX-CD2 in the formulation, the easier the formulation is to inject. All samples formulated at 5% (w / v) are moderately injectable at 27 G with injection forces ranging from 19 N for formulations containing 100% MEX-CD2 to 38 N for formulations containing 100% standard chitosan. The effect of sterilization on the viscosity of the formulations is highly dependent on the mass fraction of MEX-CD2. Thus, formulations containing a mass fraction of 67% or greater of MEX-CD2 have a viscosity that is not adversely affected, or is only slightly affected, during sterilization of the mixture.

[0181] Example 12 Injectability and gelation of gelling injection solution MEX-CD2-I This example aims to precisely determine the physicochemical and rheological properties of two formulations of MEX-CD2-I (gelling injectable solution) selected from the results of the previous example. Therefore, the 5% (wt / w) formulation, with a mass fraction of MEX-CD2 equal to 67% and 100%, respectively, was studied in more detail. The formulations containing 67% MEX-CD2 were synthesized at two slightly different pHs to evaluate the effect of pH on the rheological properties of the formulations. Each of these two formulations was also prepared at 10% (wt / w) in order to simulate mixing these more concentrated precursor solutions with the molecule of interest in a 1:1 ratio. Each of these formulations was sterilized in an autoclave at 121°C for 20 minutes in order to study the effect of sterilization on its properties. The pH, osmolality and viscosity of each of these formulations were measured and are shown in table 19. For the 5% (wt / w) formulation, the injectability was also measured using different needles.

[0182] [Table 19]

[0183] The injectability of the formulations depends primarily on the Newtonian viscosity of the solution, the inner radius of the needle, and, to a lesser extent, the length of the needle used. For the 5% (wt / wt) formulations, where the mass fraction of MEX-CD2 is 67%, it has been observed that the decrease in pH significantly increases the injectability of the mixture after sterilization. This is consistent with the observations made regarding the viscosity of the system. The 5% (wt / wt) formulation with 100% MEX-CD2 is easier to inject than the formulation containing 67% MEX-CD2 / CTS, regardless of the needle used. Finally, regardless of the formulation envisaged, the system does not appear to allow manual injection through a 30G needle. The two formulations can be manually injected by the physician using a needle of 27G or smaller.

[0184] Compositions IS-1,7-3,3 and IS-0-5 can gel spontaneously by immersion in a physiological medium with a pH above 6.2 and an osmolality above 285 mOsm / l [Figure 10]. To evaluate the rheological properties of the formed gels, 2 ml of composition IS-1,7-3,3 is introduced into a disk-shaped mold with a diameter of 25 mm. The mold is immersed in 20 ml of 10 mM PBS and left for 2 hours. The storage modulus (G') and loss modulus (G'') of the formed hydrogels were recorded on a TA Instruments ARES rheometer using a 25 mm plate / plate geometry. Before the measurements, the instrument tares the empty mold. After placing the mold containing the hydrogel on the geometry, a sweep with a constant deformation of 1% and a frequency of 10 Hz was performed on the formed hydrogels. The hydrogels start to form spontaneously after immersion in PBS and a progressive gelling front can be observed. The resulting gel was subjected to high vibration frequency for 10 2The G' and G'' values ​​are greater than 10 Pa, which corresponds to a very flexible gel. Furthermore, the value of G' is larger than that of G'', meaning that the resulting material is indeed closer to a gel than a solution. G' and G'' decrease with frequency, which may indicate a pronounced relaxation phenomenon (chain flow / relaxation / mobility, viscoelastic effects) due to the weakly crosslinked gel.

[0185] Example 13 In vivo tolerance study of xerogel HG-5-10 implanted into the peritoneal cavity Dot-shaped xerogels (h=1.5 mm and Φ=10 mm) were obtained by partially drying a gel containing composition HG-5-10 prepared as described in Example 4. The xerogels were implanted into the peritoneum of 10 male C57Bl / 6 mice to evaluate the biocompatibility and resistance of the implants. Parameters evaluated in this study include lifetime observations and measurements (including morbidity / mortality, clinical signs, body weight, food intake), pre- and post-treatment hematology, and blood chemistry and organ masses after treatment and dissection. Half of the mice were sacrificed on day 7 and the other half on day 56.

[0186] Under the experimental conditions employed, Xerogel HG-5-10 administered as a medical device that can be implanted in the peritoneum did not induce any signs of toxicity in male C57Bl / 6 mice. The implants did not induce any deaths, significant changes in body weight, or blood changes in the mice on days 7 and 56 of the study. Intraperitoneal implantation of Xerogel HG-5-10 did not induce any microscopic changes in the liver, nor did it induce any changes in liver mass.

[0187] Example 14 In vivo MRI study of the degradation of gelling injectable solution IS-1,7-3,3 following subcutaneous administration Approximately 300 μl of formulation IS-1,7-3,3 loaded with 305 ppm Gd (precomplexed with MEX-CD2) was injected subcutaneously into the back of healthy BALB / c mice using a 22 G syringe. MRI images in FIG. 11 of gels implanted in mice were acquired at 7.1 T on a 300 MHz Bruker Avance Neo spectrophotometer equipped with a micro2.5 microimaging probe at room temperature (RT=21° C.) one month after implantation. Signal intensity in the liver, kidneys, and spleen was also monitored.

[0188] In Figure 12, T 2W Images were acquired using a standard RARE (Rapid Acquisition with Refocused Echoes) sequence with the following parameters: TR=4000 ms, TE=24 ms, RARE factor=16, number of averages=4, FOV=30 mm, section thickness=1 mm, matrix size 128x128. 1W Images were acquired using a standard MSME (multi spins multi echoes) sequence with the following parameters: TR=400 ms, TE=3.3 ms, number of averages=6, FOV=30 mm, section thickness=1 mm, matrix size 128x128. 1 Values ​​were measured using a Saturation Recovery Spin Echo sequence (TE = 3.8 ms, 10 TR variable, range 50-5000 ms, FOV = 30 mm, slice thickness = 1 mm, matrix size 128x128) and T 1 The saturation recovery equation was used for analysis. The size of the formed gel was measured by manually drawing ROIs on the MRI images.

[0189] As listed in Table 20, the volume occupied by the formed gel decreased to approximately 50% of the initial volume over 30 days of monitoring, while the T measured in the same area 1The T values ​​measured from day 15 to day 30 increased approximately 6-fold. From day 15 after implantation, the implants began to show increased heterogeneity due to cellular infiltration. 1 The starting implant volumes in three mice were 304, 348, and 216 mm, respectively, as demonstrated by the increased standard deviation. 3 The liver, kidneys, and spleen 1W The signal intensity did not increase during the study period.

[0190] [Table 20]

Claims

1. a. at least one chitosan A, and b. at least one statistical copolysaccharide B of formula I having a mass average molecular weight between 100 kDa and 1000 kDa: 【Chemistry 1】 (In the formula, each Rc independently represents a group that comprises a chelator; - each Z independently represents a linker, which may be a single bond or a hydrocarbon-based chain containing between 1 and 12 carbon atoms, said chain being linear or branched, containing one or more unsaturations and capable of containing one or more heteroatoms, preferably selected from the group of nitrogen, oxygen, sulfur and halogen atoms; - x is between 0.01 and 0.5, - y is between 0.05 and 0.5, - the ratio y / x is greater than 0.2, preferably greater than 1 - the sum of x+y is greater than 0.1, and including chelators of type Rc in which less than 10% of the groups are chelated by cations of transition elements selected from block d and f elements; and c. A composition comprising, optionally, water.

2. - a crystallinity with respect to chitosan A of at least 10% relative to the total dry weight of the composition, and 2. The composition according to claim 1, characterized in that it has a chitosan A crystallite size of less than 20 nm.

3. 3. Composition according to claim 1 or 2, characterized in that the mass ratio between A and B (A:B) is between 2:1 and 1:10, preferably between 1:1 and 1:

5.

4. The chitosan A has an average molecular weight M between 100 kg / mol and 1000 kg / mol, preferably between 200 kg / mol and 700 kg / mol. w 4. The composition according to claim 1 , characterized in that it has

5. 5. The composition according to claim 1, wherein the chitosan A has a degree of acetylation x of less than 40%, preferably less than 10%, for example between 0% and 10%.

6. Said statistical copolysaccharide B of formula I, having a weight average molecular weight between 100 kDa and 1000 kDa, is represented by formula II: 【Chemistry 2】 6. Composition according to any one of claims 1 to 5, characterized in that it is of the formula: (In the formula, - Rc 1 and Rc 2 are different and are groups that contain a chelating agent, -Z 1 and Z 2 are the same or different and are linkers, which may be single bonds or hydrocarbon-based chains containing between 1 and 12 carbon atoms, said chains being linear or branched and containing one or more unsaturations and which may contain one or more heteroatoms, preferably selected from the nitrogen, oxygen, sulfur and halogen family of atoms; - x is between 0.01 and 0.5, preferably between 0.01 and 0.1 and preferentially between 0.05 and 0.1, - y is between 0.01 and 0.5, preferably between 0.05 and 0.2, - z is between 0 and 0.2; and (including chelators of type Rc1 and Rc2, in which less than 10% of the groups are chelated by cations of transition elements selected from the block d and f elements)

7. 7. The composition according to any one of claims 1 to 6, characterized in that it further comprises at least one active pharmaceutical ingredient, preferably chosen from anticancer agents, antibacterial agents, antifungal agents, anti-inflammatory agents, messenger RNA, proteins and antigens.

8. 8. Composition according to any one of claims 1 to 7, characterized in that it is an aqueous solution and preferably contains at least 10 g / l of a mixture of chitosan A and copolysaccharide B.

9. Composition according to any one of claims 1 to 7, characterized in that it is in the form of a lyophilisate or a gel, preferably in the form of a hydrogel, xerogel or aerogel.

10. 10. The composition according to claim 9, in the form of a xerogel, said xerogel resulting from at least partial drying of a hydrogel.

11. 11. The composition in the form of a xerogel according to claim 10, characterized in that, upon contact with an aqueous medium or biological tissue for at least 1 hour, it swells to form a hydrogel, said hydrogel having a volume at least twice, preferably at least five times, the volume of the reference xerogel before contact with said aqueous medium or biological tissue.

12. Thread, characterized in that it comprises a gel or a lyophilisate of the composition according to claim 9.

13. A textile material, characterized in that it comprises a yarn according to claim 12.

14. 12. A medical device, characterized in that it comprises a composition according to any one of claims 1 to 11, preferably being a dressing, an implant or a dermal filling product.

15. 15. The medical device according to claim 14, characterized in that it is a dermal filler product in the form of threads, said threads preferably in the form of a xerogel capable of swelling on contact with an aqueous medium or biological tissue to form a hydrogel.

16. 12. A composition according to any one of claims 1 to 11 for use in sequestering at least one metal, preferably for use in the treatment or prevention of endometriosis, fungal infections, bacterial infections, chronic wounds, neurodegenerative injuries, nervous system lesions, hemochromatosis, Wilson's disease or lead poisoning.

17. The process is as follows: 1) dispersing chitosan A and statistical polysaccharide B of formula I having a weight average molecular weight between 100 kDa and 1000 kDa in water; 2) adding an acid, preferably acetic acid 3) mixing and then centrifuging the resulting solution to recover a solution containing the composition according to any one of claims 1 to 7; 4) Optionally, treating the solution obtained in step 3 in a basic water bath to obtain the composition in gel form; and 8. A method for preparing a composition according to any one of claims 1 to 7, comprising the step 5) optionally washing, drying and / or sterilizing the gel obtained in step 4, preferably by autoclaving.