Method for producing highly water-absorbent resin particles
By employing a two-step drying process with a hot air dryer followed by a heat conduction dryer, the method addresses drying uniformity issues in superabsorbent resin production, enhancing absorption properties and reducing fine powder content.
Patent Information
- Application Number
- JP2024507930
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-09-26
- Filing Date
- 2023-06-01
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-06-01
AI Technical Summary
Existing methods for producing superabsorbent resin particles face issues with drying uniformity, leading to over-drying, deterioration of physical properties, and increased fine powder generation during the crushing step.
A method involving primary drying with a hot air dryer followed by secondary drying with a heat conduction dryer to maintain pore structure and improve drying uniformity, reducing fine powder content and enhancing the physical properties of the final resin particles.
The method ensures high drying uniformity and reduces fine powder generation, thereby improving the absorption properties and physical characteristics of the superabsorbent resin particles.
Smart Images

Figure 2024537962000001_ABST
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0121702 filed on September 26, 2022, and all contents disclosed in the documents of said Korean patent application are incorporated by reference as part of this specification.
[0002] The present invention relates to a method for producing highly absorbent resin particles, and more particularly to a method for producing highly absorbent resin particles having improved drying uniformity and physical properties by using two types of dryers. [Background technology]
[0003] Super absorbent polymer (SAP) is a synthetic polymeric substance that has the ability to absorb about 500 to 1,000 times its own weight in water, and different developers give it different names, such as SAM (Super Absorbency Material) and AGM (Absorbent Gel Material). Such super absorbent polymers have started to be put to practical use as sanitary products, and are currently widely used as soil water retention agents for horticulture, water stoppers for civil engineering and construction, seedling sheets, freshness maintaining agents in the food distribution field, and materials for steaming, and are mainly used in the field of sanitary materials such as diapers and sanitary napkins.
[0004] Meanwhile, superabsorbent resin particles can generally be manufactured through steps of polymerization, drying, pulverization, and surface cross-linking. However, when the drying uniformity is reduced in the drying step, excessive drying is performed, which deteriorates the physical properties, and a large amount of fine powder is generated in the pulverization step.
[0005] Therefore, there is a need for a drying method that can achieve high drying uniformity in the drying step, improve the physical properties of the final superabsorbent resin particles, and reduce the content of fine powder. Summary of the Invention [Problem to be solved by the invention]
[0006] The problem to be solved by the present invention is to provide a method for producing superabsorbent resin particles, which can perform a drying step with high drying uniformity, reduce the amount of fine powder generated in the grinding step, and ensure the physical properties of the final product, that is, superabsorbent resin particles, in order to solve the problems mentioned in the background of the invention above. [Means for solving the problem]
[0007] According to one embodiment of the present invention for solving the above problems, the present invention provides a method for producing superabsorbent resin particles, the method including the steps of: supplying a composition containing a water-soluble ethylenically unsaturated monomer having at least a partially neutralized acidic group, an internal crosslinking agent, and a polymerization initiator to a polymerization reactor and polymerizing the composition to obtain a hydrogel polymer; primarily drying the hydrogel polymer in a hot air dryer to obtain a primary dried body; secondarily drying the primary dried body in a heat conduction dryer to obtain a secondary dried body; and pulverizing the secondary dried body to obtain superabsorbent resin particles. Effect of the Invention
[0008] According to the method for producing superabsorbent resin particles of the present invention, the drying step can be performed in primary drying and secondary drying. By performing the primary drying in a hot air dryer, the pores of the dried body can be maintained, and by performing the secondary drying in a heat conduction dryer, the drying uniformity can be improved. This can solve the problem of the undried body being introduced into the next pulverization step, and the amount of fine powder generated due to pulverization can be reduced. In addition, the physical properties of the final superabsorbent resin particles can be improved. [Brief description of the drawings]
[0009] [Figure 1] 1 is a flow chart illustrating a method for producing a superabsorbent polymer according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The terms and words used in the description of the present invention and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.
[0011] In order to facilitate understanding of the present invention, the present invention will now be described in more detail with reference to FIG.
[0012] A method for producing superabsorbent resin particles according to one embodiment of the present invention includes the steps of: supplying a composition containing a water-soluble ethylenically unsaturated monomer having at least a partially neutralized acidic group, an internal crosslinking agent, and a polymerization initiator to a polymerization reactor and polymerizing the composition to obtain a hydrous gel polymer; primarily drying the hydrous gel polymer in a hot air dryer to obtain a primary dried body; secondarily drying the primary dried body in a heat conduction dryer to obtain a secondary dried body; and pulverizing the secondary dried body to obtain superabsorbent resin particles.
[0013] First, the method for producing superabsorbent resin particles according to one embodiment of the present invention can include a step of supplying a composition containing a water-soluble ethylenically unsaturated monomer having at least a partially neutralized acidic group, an internal crosslinking agent, and a polymerization initiator to a polymerization reactor and polymerizing the composition to obtain a hydrogel polymer. As described above, the composition can contain the water-soluble ethylenically unsaturated monomer, the internal crosslinking agent, and the polymerization initiator, and can further contain additives such as a thickener, a plasticizer, a storage stabilizer, and an antioxidant, as necessary.
[0014] Here, the water-soluble ethylenically unsaturated monomer may be (meth)acrylic acid or a salt thereof. For example, when acrylic acid in which at least a part of acrylic acid is neutralized and an alkali metal salt thereof, which is a sodium salt thereof, are used as the water-soluble ethylenically unsaturated monomer, a highly water-absorbent resin having improved water absorption properties can be obtained.
[0015] In addition, the water-soluble ethylenically unsaturated monomer may be an anionic monomer such as maleic anhydride, fumaric acid, crotonic acid, itaconic acid, 2-acryloylethanesulfonic acid, 2-methacryloylethanesulfonic acid, 2-(meth)acryloylpropanesulfonic acid, or 2-(meth)acrylamido-2-methylpropanesulfonic acid, or a salt thereof; a nonionic hydrophilic monomer such as (meth)acrylamide, N-substituted (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, or polyethylene glycol (meth)acrylate; and an amino group-containing unsaturated monomer such as (N,N)-dimethylaminoethyl (meth)acrylate, or (N,N)-dimethylaminopropyl (meth)acrylamide, or a quaternary product thereof. The salt of the anionic monomer may be a metal salt, a divalent metal salt, an ammonium salt, or an organic amine salt.
[0016] The water-soluble ethylenically unsaturated monomer may include at least a partially neutralized acidic group. The water-soluble ethylenically unsaturated monomer including at least a partially neutralized acidic group may be prepared by neutralizing the acidic group of the water-soluble ethylenically unsaturated monomer using a neutralizing agent. Here, the neutralizing agent may be a basic substance such as sodium hydroxide (or caustic soda), potassium hydroxide, or ammonium hydroxide that can neutralize the acidic group.
[0017] Meanwhile, the internal crosslinking agent can crosslink and polymerize the unsaturated bonds of the water-soluble ethylenically unsaturated monomer.
[0018] The internal crosslinking agent may be a (meth)acrylate-based compound that undergoes a crosslinking reaction by a free-radical polymerization (FRP) reaction. Specifically, the internal crosslinking agent may be one or more compounds selected from the group consisting of ethylene glycol di(meth)acrylate, polyethylene glycol (meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol (meth)acrylate, butanediol di(meth)acrylate, butylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, hexanediol di(meth)acrylate, triethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, and tetraethylene glycol di(meth)acrylate. More specifically, the internal crosslinking agent may be polyethylene glycol di(meth)acrylate.
[0019] Meanwhile, in the composition, the polymerization initiator may be a thermal polymerization initiator or a photopolymerization initiator by UV irradiation depending on the polymerization method. However, even in the photopolymerization method, a certain amount of heat is generated by UV irradiation, and a certain amount of heat is generated as the polymerization reaction, which is an exothermic reaction, proceeds, so a thermal polymerization initiator may also be included.
[0020] The photopolymerization initiator may be a compound capable of forming a radical by light such as ultraviolet light. The photopolymerization initiator may be at least one selected from the group consisting of benzoin ether, dialkyl acetophenone, hydroxyl alkyl ketone, phenyl glyoxylate, benzyl dimethyl ketal, acyl phosphine, and α-aminoketone. Specific examples of acyl phosphine include diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, and ethyl(2,4,6-trimethylbenzoyl)phenylphosphinate.
[0021] The thermal polymerization initiator may be one or more selected from the group consisting of persulfate initiators, azo initiators, hydrogen peroxide, and ascorbic acid.Specific examples of persulfate initiators include sodium persulfate (Na2S2O8), potassium persulfate (K2S2O8), and ammonium persulfate ((NH4)2S2O8).
[0022] Specifically, polymerization methods are broadly classified into thermal polymerization and photopolymerization depending on the polymerization energy source. Thermal polymerization can be carried out in a reactor having a stirring shaft such as a kneader, and photopolymerization can be carried out in a reactor equipped with a movable conveyor belt.
[0023] The hydrogel polymer of the present invention can be prepared by a polymerization reaction carried out by supplying a composition containing a water-soluble ethylenically unsaturated monomer, an internal crosslinking agent, and a polymerization initiator to a polymerization reactor, and in the composition, the internal crosslinking agent can be 0.01 to 5 parts by weight relative to 100 parts by weight of the water-soluble ethylenically unsaturated monomer. For example, the internal crosslinking agent can be 0.01 parts by weight or more, 0.05 parts by weight or more, 0.1 parts by weight or more, or 0.2 parts by weight or more, and 5 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, 1 part by weight or less, or 0.5 parts by weight or less relative to 100 parts by weight of the water-soluble ethylenically unsaturated monomer. If the content of the internal crosslinking agent is too low, crosslinking may not be sufficient, making it difficult to achieve strength above an appropriate level, and if the content of the upper internal crosslinking agent is too high, the internal crosslinking density may be high, making it difficult to achieve the desired water retention ability.
[0024] The composition of the present invention may be prepared in the form of a solution dissolved in a solvent. Here, the solvent that can dissolve the above-mentioned raw materials may be used. For example, the solvent may be water, ethanol, ethylene glycol, diethylene glycol, triethylene glycol, 1,4-butanediol, propylene glycol, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, methyl ethyl ketone, acetone, methyl amyl ketone, cyclohexanone, cyclopentanone, diethylene glycol monomethyl ether, diethylene glycol ethyl ether, toluene, xylene, butyrolactone, carbitol, methyl cellosolve acetate, N,N-dimethylacetamide, or a mixture thereof.
[0025] Next, the hydrogel polymer obtained by the polymerization reaction may be dried and pulverized to obtain superabsorbent resin particles. Here, in order to increase efficiency when drying the hydrogel polymer, a chopping (coarse pulverization) step may be further performed. The "chopping" is distinct from the pulverization performed in the pulverization step described below, and may refer to the coarse pulverization of the hydrogel polymer before the drying step.
[0026] The pulverizer used in the chopping step may be any one selected from the group of pulverizing devices consisting of a vertical pulverizer, a turbo cutter, a turbo grinder, a rotary cutter mill, a cutter mill, a disc mill, a shred crusher, a crusher, a chopper, and a disc cutter.
[0027] Then, the chopped hydrogel polymer may be subjected to a drying step, which may include primary drying and secondary drying.
[0028] According to one embodiment of the present invention, the hydrous gel polymer can be primarily dried in a hot air dryer to obtain a primary dried material. The hot air dryer can be a device that applies heat through high-temperature air (hot air) to directly evaporate and discharge the moisture of the material to be dried until the moisture content reaches a target moisture content. In this specification, the hot air dryer can directly dry the material to be dried with hot air while stirring the material with a rotary drum or the like. Here, the hot air dryer can be a kiln dryer, a tube bundle dryer, a rotary dryer, or the like, and in the present invention, a rotary dryer can be used.
[0029] The rotary dryer may have a central tube in a rotating drum, and one or more hot air supply pipes may be attached to the central tube. The hydrogel polymer introduced into the rotary dryer may be agitated by the rotation of the rotating drum and heated by hot air supplied from one or more hot air supply pipes. The hot air directly contacts the hydrogel polymer introduced into the rotary dryer, so that drying can be efficiently performed and the drying time can be shortened.
[0030] Here, the temperature of the hot air from the hot air supply pipe in the rotary dryer can be 100°C or more, 110°C or more, or 120°C or more, and 200°C or less, 190°C or less, or 180°C or less.
[0031] The hot air velocity can be 20 m / s or more, 22 m / s or more, or 24 m / s or more, and 30 m / s or less, 29 m / s or less, or 27 m / s or less. By operating the rotary dryer with the temperature and velocity of the hot air within the above ranges to perform primary drying, the desired moisture content of the primary dried product can be obtained in the present invention.
[0032] According to one embodiment of the present invention, the moisture content of the primary dried body may be 20 wt% or more, 23 wt% or more, or 25 wt% or more, and 35 wt% or less, 32 wt% or less, or 30 wt% or less. By drying the primary dried body to a moisture content within the above range, the primary dried body can be introduced into a heat conduction dryer described below and secondary dried in a state where it is not over-dried in a hot air dryer.
[0033] When the moisture content of the primary dried body is less than 20 wt%, the content of fine powder of the primary dried body may increase excessively. When the moisture content of the primary dried body is more than 35 wt%, the adhesiveness of the primary dried body may increase excessively, which may make it difficult to recover the primary dried body using a hot air dryer. Here, the moisture content can be measured by a moisture meter (AND MX_50).
[0034] According to an embodiment of the present invention, the primary dried material is secondarily dried in a heat conduction dryer to obtain a secondary dried material.
[0035] The heat conduction dryer may be a dryer having a jacket structure in which a heat medium (heat transfer oil or steam) flows, and indirectly heating and drying the material to be dried by receiving heat energy from the outside of the jacket through conduction. In this specification, the heat conduction dryer may perform indirect drying while stirring the material to be dried by a paddle or screw of the jacket structure. Here, as the heat conduction dryer, a disk type dryer, a screw type dryer, a paddle type dryer, a drum type dryer, a stirring type dryer, a thin film type dryer, etc. may be used depending on the structure and type of heat transfer, and in the present invention, a paddle dryer may be used.
[0036] The paddle dryer includes an agitator arranged horizontally, and the agitator may include one or more paddles. The agitator in the paddle dryer rotates, and a heat source such as heat transfer oil or steam flows inside the paddle of a jacket structure, and the material to be dried can be indirectly dried by contact with the paddle and the inner wall surface. Therefore, the thermal efficiency of the paddle dryer can be maximized by heat conduction due to friction.
[0037] Meanwhile, the temperature of the heat transfer medium (heat transfer oil or steam) flowing inside the agitator installed in the paddle dryer and the paddle attached to the agitator may be 100° C. or more, 110° C. or more, 120° C. or more, or 130° C. or more, and 200° C. or less, 190° C. or less, 180° C. or less, or 170° C. or less. By increasing the temperature of the heat transfer medium within the above range, the temperature of the secondary drying performed in the paddle dryer can be within the above range.
[0038] The agitator in the paddle dryer may rotate at 10 rpm or more, 15 rpm or more, 20 rpm or more, or 25 rpm or more, and 50 rpm or less, 45 rpm or less, 40 rpm or less, or 35 rpm or less. Here, the rpm (rotations per minute) may indicate the unit of the number of rotations per minute of the agitator. By rotating the agitator of the paddle dryer within the above range, the secondary drying can be smoothly performed and the problem of introducing undried material into the subsequent grinding step can be prevented.
[0039] According to one embodiment of the present invention, the moisture content of the secondary dried body may be 8% by weight or more, 10% by weight or more, or 12% by weight or more, and 20% by weight or less, 18% by weight or less, or 16% by weight or less. When the moisture content of the secondary dried body is dried within the above range, it is possible to achieve a desired level of water absorption performance of the final superabsorbent resin particles.
[0040] Meanwhile, for example, when the primary drying or secondary drying is performed in a band-type dryer, the drying uniformity of the object to be dried may be low. The band-type dryer may be, for example, a conveyor belt, and such a dryer may load and move the object to be dried on a conveyer (wire mesh, perforated plate, etc.) and ventilate the object with hot air to dry it. However, since the object to be dried cannot be agitated and is dried in the form (block-like form) loaded on the conveyer, a part of the object to be dried (inside the block form) may not be dried, so over-drying may be performed. However, over-drying may reduce the absorption speed (vortex) and water absorption performance of the superabsorbent resin particles, and excessive fine powder may be generated in the pulverization step. Therefore, in order to improve this, a hot air dryer and a heat conduction dryer that agitate and dry the object to be dried according to one embodiment of the present invention may be used.
[0041] The hot air dryer is easy to improve the absorption rate of the material to be dried by maintaining the pores of the material to be dried through rotation of a rotary drum, but the filling level of the material to be dried in the rotary drum of the hot air dryer must be within 15% of the total capacity, so the drying capacity is low compared to the size of the equipment. Furthermore, the drying uniformity of the material to be dried by the hot air dryer may be relatively low.
[0042] Meanwhile, the heat conduction type dryer has a high drying capacity and can dry the material to be dried with high drying uniformity, but the high shear applied to the material can reduce the pores of the material, which can decrease the vortex of the material.
[0043] In order to compensate for the shortcomings of the hot air dryer and the heat conduction dryer, the hot air dryer and the heat conduction dryer may be connected in series in the present invention. As described above, the primary drying is performed using the hot air dryer to first maintain the pores of the hydrogel polymer, and the secondary drying is performed using the heat conduction dryer to further improve the drying uniformity of the secondary dried body. In this way, the hot air dryer and the heat conduction dryer are connected in series to perform the primary and secondary drying, so that the inflow of the undried body into the subsequent pulverization step can be prevented, and finally, the physical properties of the completed superabsorbent resin particles can be easily ensured. Here, the physical properties of the superabsorbent resin particles may mean the absorption properties that the superabsorbent resin particles are initially intended to have, and specifically, may be properties related to absorption, such as water absorption performance and absorption speed.
[0044] Next, the secondary dried product obtained through the drying steps of the primary and secondary drying may be pulverized to obtain superabsorbent resin particles. The pulverization step may be performed once, but may be performed in one or more rounds, for example. According to the present invention, a classification step may be further performed after the pulverization step. Furthermore, the classification may be performed after each pulverization.
[0045] For example, first, a primary pulverization may be performed to pulverize the secondary dried body, and the pulverizer used in this process may be, for example, a ball mill, a pin mill, a hammer mill, a screw mill, a roll mill, a disc mill, or a jog mill.
[0046] Next, the primary pulverized material after the primary pulverization can be classified based on a specific particle size using a standard mesh of ASTM standard. Here, the specific particle size can be a standard particle size of particles to be classified for the secondary pulverization described later. By such classification, the particles can be classified into particles below the specific particle size and particles above the specific particle size. As an example, the primary pulverized material can be put into a mesh (mesh) set and classified into particles above #40 (425 μm or more) and particles below #40 (less than 425 μm) based on a #40 mesh.
[0047] Then, the particles classified by the primary classification that are equal to or larger than a specific particle size may be separately pulverized to obtain a secondary pulverized product, and the secondary pulverization may be performed using the same pulverizer as that used in the primary pulverization.
[0048] After the secondary pulverization, secondary classification can be performed to control the physical properties of the superabsorbent resin particles to be manufactured into a final product. The secondary classification can use the standard mesh of the ASTM standard used in the primary classification, and the mixture of particles classified in the primary classification that fall below a specific particle size and secondary pulverized material pulverized in the secondary pulverization can be finally classified according to an appropriate particle size. Here, the appropriate particle size (D50) can be a particle size of 150 μm to 850 μm, and particles having such a particle size can be classified as normal particles. Meanwhile, particles having a particle size of less than 150 μm can be classified as fine particles. Such particle size can be measured according to the EDANA WSP 220.3 method of the European Disposables and Nonwovens Association (EDANA).
[0049] Through such a series of grinding steps, normal particles, that is, highly water-absorbent resin particles, can be produced.
[0050] Next, if necessary, the method may further include a step of surface-crosslinking the produced superabsorbent resin particles in the presence of a surface crosslinking agent to produce superabsorbent resin particles having a surface crosslinked layer formed on at least a portion thereof, where the surface crosslinked layer may be produced from a surface crosslinking agent, the surface crosslinking agent may include a polyfunctional epoxy compound, and the polyfunctional epoxy compound may be a glycidyl ether compound of a polyhydric alcohol.
[0051] Specifically, the surface cross-linking agent may include one or more polyfunctional epoxy compounds selected from the group consisting of ethylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, triethylene glycol diglycidyl ether, tetraethylene glycol diglycidyl ether, glycerin polyglycidyl ether, and sorbitol polyglycidyl ether.
[0052] The surface cross-linking agent may be mixed with the superabsorbent resin particles in a solution state, specifically, in a surface cross-linking solution state dissolved in a solvent. The surface cross-linking solution may contain water and methanol in addition to the surface cross-linking agent. In general, the surface cross-linking solution is applied to the surface of the superabsorbent resin particles. Thus, the surface cross-linking reaction is carried out on the surface of the superabsorbent resin particles, which improves the cross-linking property on the surface of the particles without substantially affecting the inside of the particles. Thus, the surface cross-linked superabsorbent resin particles have a higher degree of cross-linking near the surface than in the inside. The surface cross-linking reaction and drying can be carried out simultaneously by heating the polymer to which the surface cross-linking agent has been added.
[0053] The present invention will be described in more detail with reference to the following examples. However, the following examples are merely for the purpose of illustrating the present invention, and it is obvious to those skilled in the art that various changes and modifications are possible within the scope of the scope and technical idea of the present invention, and the scope of the present invention is not limited thereto.
[0054] Working Example Example 1 (1) Preparation of hydrogel polymer In a 3 L glass container equipped with a stirrer and a thermometer, 1000 g of acrylic acid, 1.6 g of polyethylene glycol diacrylate (PEGDA) as an internal crosslinking agent, 0.08 g of diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide as a photopolymerization initiator, 1.2 g of sodium persulfate as a thermal polymerization initiator, and 1235 g of caustic soda (NaOH) solution as a neutralizing agent were mixed at room temperature to a solid content of 45.0 wt %, to prepare a composition.
[0055] Next, the composition was supplied at a rate of 500 to 2000 mL / min onto a conveyor belt having a width of 10 cm and a length of 2 m, which was moving at a speed of 10 cm / min. 2 After the polymerization reaction was completed, the mixture was pulverized with a chopper to obtain a hydrogel polymer having a water content of 65% by weight.
[0056] (2) Manufacturing of superabsorbent resin particles Next, 1 kg of the hydrous gel polymer was fed to a rotary dryer and primary drying was carried out until the water content of the primary dried body reached 24.9% by weight. Here, the hydrous gel polymer was dried with hot air fed from a hot air feed pipe of the rotary dryer at a temperature of 100°C and a wind speed of 26 m / s to obtain a primary dried body. Here, the water content was measured with a moisture meter (AND MX_50; heating temperature: 180°C, heating time: 40 minutes).
[0057] The primary dried material was then placed in a paddle dryer and secondary drying was carried out until the moisture content of the secondary dried material reached 12.0% by weight. Here, the secondary drying temperature was also 105°C through an agitator installed in the paddle dryer and a heat medium at 105°C flowing inside a paddle attached to the agitator, and the agitator in the paddle dryer was rotated at 10 rpm.
[0058] Next, the secondary dried body was subjected to primary pulverization with a roll mill to obtain a primary pulverized material. The primary pulverized material was put into a mesh set (a mesh set consisting of ASTM meshes #6, #10, #20, #25, #30, #40, #50, #70 and #100), and then subjected to primary classification to classify the particles into #40 or more (425 μm or more) and particles less than #40 (less than 425 μm). The particles classified in the primary classification of #40 or more (425 μm or more) were subjected to secondary pulverization with the roll mill to obtain a secondary pulverized material. Finally, a mixture of the particles classified in the primary classification of less than #40 (less than 425 μm) and the secondary pulverized material was subjected to secondary classification to obtain superabsorbent resin particles having a particle size of 150 μm to 850 μm. Here, the secondary classification was performed using the same mesh set as the primary classification.
[0059] Example 2 The superabsorbent resin particles were produced using the same method as in Example 1, except that primary drying was performed until the moisture content of the primary dried material reached 25.5% by weight, and secondary drying (agitator rotation speed: 30 rpm) was performed until the moisture content of the secondary dried material reached 12.9% by weight.
[0060] Example 3 The superabsorbent resin particles were produced in the same manner as in Example 1, except that primary drying was performed until the moisture content of the primary dried material reached 21.9% by weight, and secondary drying (agitator rotation speed: 50 rpm) was performed until the moisture content of the secondary dried material reached 10.8% by weight.
[0061] Example 4 The superabsorbent resin particles were produced in the same manner as in Example 1, except that the primary drying was performed until the moisture content of the primary dried material reached 33.6% by weight, and the secondary drying was performed until the moisture content of the secondary dried material reached 11.4% by weight.
[0062] Example 5 The superabsorbent resin particles were produced in the same manner as in Example 1, except that primary drying was performed until the moisture content of the primary dried material reached 29.1% by weight, and secondary drying (temperature: 200°C) was performed until the moisture content of the secondary dried material reached 11.8% by weight.
[0063] Example 6 The superabsorbent resin particles were produced using the same method as in Example 1, except that primary drying was performed until the moisture content of the primary dried material reached 29.3% by weight, and secondary drying (temperature: 200°C, agitator rotation speed: 50 rpm) was performed until the moisture content of the secondary dried material reached 7.5% by weight.
[0064] Example 7 The superabsorbent resin particles were produced in the same manner as in Example 1, except that the primary drying was performed until the moisture content of the primary dried material reached 31.4% by weight, and the secondary drying was performed until the moisture content of the secondary dried material reached 21.3% by weight.
[0065] Example 8 The superabsorbent resin particles were produced in the same manner as in Example 1, except that the primary drying was performed until the moisture content of the primary dried material reached 16.5% by weight, and the secondary drying was performed until the moisture content of the secondary dried material reached 10.3% by weight.
[0066] Example 9 The superabsorbent resin particles were produced in the same manner as in Example 1, except that the primary drying was performed until the moisture content of the primary dried material reached 37.5% by weight, and the secondary drying was performed until the moisture content of the secondary dried material reached 12.9% by weight.
[0067] Comparative Example Comparative Example 1 In Example 1, the primary drying was performed in a rotary dryer (hot air temperature: 100°C, air speed: 26 m / s) until the moisture content of the primary dried material reached 10.2% by weight, and the secondary drying was not performed. Except for this, the same method as in Example 1 was used to produce superabsorbent resin particles.
[0068] Comparative Example 2 In Example 1, the primary drying was performed in a rotary dryer (hot air temperature: 250°C, air speed: 8 m / s) until the moisture content of the primary dried material reached 11.0% by weight, and the secondary drying was not performed. Except for this, the same method as in Example 1 was used to produce superabsorbent resin particles.
[0069] Comparative Example 3 The superabsorbent resin particles were produced in the same manner as in Example 1, except that primary drying was performed in a paddle dryer (temperature: 105°C, agitator rotation speed: 10 rpm) until the moisture content of the primary dried material reached 12.6% by weight, and secondary drying was not performed.
[0070] Comparative Example 4 The superabsorbent resin particles were produced in the same manner as in Example 1, except that primary drying was performed in a paddle dryer (temperature: 200°C, agitator rotation speed: 50 rpm) until the moisture content of the primary dried body reached 11.0% by weight, and secondary drying was not performed.
[0071] Comparative Example 5 The superabsorbent resin particles were produced in the same manner as in Example 1, except that the primary drying was performed using a paddle dryer (temperature: 105°C, agitator rotation speed: 10 rpm) until the moisture content of the primary dried material reached 31.1% by weight, and the secondary drying was performed using a rotary dryer (temperature: 100°C, wind speed: 26 m / s) until the moisture content of the secondary dried material reached 12.6% by weight.
[0072] Experimental Example The highly water-absorbent resin particles produced in the above Examples and Comparative Examples were measured by the following methods, and the results are shown in Tables 1 and 2 below.
[0073] 1) Moisture content The moisture content was measured from the weight change that occurred when the primary dried material or the secondary dried material during the manufacturing process of the superabsorbent resin particles of the Examples or Comparative Examples was heated with a halogen lamp (400W) in a moisture meter (AND MX_50) to evaporate the moisture. Specifically, the moisture content was measured according to the following procedure.
[0074] (i) Set the measurement conditions of the moisture meter (heating temperature: 180°C, heating time: 40 minutes). (ii) With no sample present on the sample pan, the weight is stabilized to zero (0). (iii) A 5 g sample (error: 0.02%) is taken from the primary dried body or secondary dried body to be measured, and the sample is evenly loaded onto the sample pan to start the measurement. (iv) After the measurement is completed, check the moisture content.
[0075] 2) Drying uniformity The drying uniformity may refer to the uniformity of the moisture content according to the particle size of the superabsorbent resin particles. Specifically, the drying uniformity of the superabsorbent resin particles prepared according to the examples and comparative examples was measured according to Equation 1.
[0076]
number
[0077] Here, the drying uniformity was measured by sampling 200 g of the final superabsorbent resin particles. The 200 g of the secondary dried body was placed into a mesh set consisting of meshes #6, #10, #20, #25, #30, #40, #50, #70 and #100, and attached to a sieve shaker. The sieve shaker was operated for 10 minutes at an amplitude of 1.5 to classify the superabsorbent resin particles.
[0078] After separating the particles according to the particle size of each mesh, the moisture content of the separated particles was measured using a moisture meter (AND MX_50; heating temperature: 180℃, heating time: 40 minutes). The standard deviation of the moisture content of the particles according to each particle size is indicated as "Std" in Equation 1.
[0079] 3) Average particle size after drying and average particle size after grinding The method for measuring the average particle size after drying was as follows.
[0080] First, the secondary dried bodies were classified in the same manner as the method for measuring the "drying uniformity" described above. Specifically, the secondary dried bodies (200 g) after secondary drying in the examples and comparative examples were put into a mesh set consisting of meshes #6, #10, #20, #25, #30, #40, #50, #70 and #100, and then classified by attaching them to a vibrating sieve (time: 10 minutes, amplitude: 1.5). The weight fractions of the secondary dried bodies classified by mesh (#6, #10, #20, #25, #30, #40, #50, #70 and #100) were analyzed, and the particle sizes were calculated by arithmetic average based on the weight fractions of each mesh, and the results are the "average particle size after drying" in Tables 1 and 2.
[0081] Meanwhile, the "average particle size after pulverization" was measured in the same manner as the "average particle size after drying" described above. However, unlike the "average particle size after drying" which was measured on the secondary dried body, the "average particle size after pulverization" was measured by classifying the mixture that had been subjected to the additional pulverization step (particles smaller than #40 classified in the primary classification and the secondary pulverized material).
[0082] 4) Fine powder content In the methods for producing superabsorbent resin particles in the examples and comparative examples, the weight of the mixture (particles less than #40 classified in the primary classification and secondary pulverized material) was measured before secondary classification. Then, after the secondary classification, the weight of fine particles having a particle size of 150 μm or less was measured. The percentage of the weight of the fine particles relative to the weight of the mixture is referred to as the "fine powder content." In other words, the fine powder content may refer to the content of fine particles contained in the mixture.
[0083] 5) Absorption speed (Vortex) The absorption rates of the highly water-absorbent resin particles of the above Examples and Comparative Examples were measured by the following method.
[0084] 50 ml of 0.9% salt water maintained at 24°C was added to a 100 ml beaker on a magnetic stirrer using a graduated cylinder. During stirring, the magnetic stirrer was operated at such a speed that the lowest surface (central space) of the vortex generated in the 100 ml beaker was in contact with the magnetic bar. Among the superabsorbent resin particles of the examples and comparative examples, 1.99 g to 2.01 g of superabsorbent resin particles corresponding to particle sizes of #40 to #50 (300 μm to 425 μm) were added to the vortex and the time was measured. The time from when the superabsorbent resin particles were added to the salt water to when viscosity was generated and the vortex disappeared and the liquid level became horizontal was measured in seconds and defined as the "absorption speed" of the present invention.
[0085] [Table 1]
[0086] [Table 2]
[0087] Referring to Tables 1 and 2, in the case of the embodiment in which superabsorbent resin particles were prepared by performing primary drying using a rotary dryer and secondary drying using a paddle dryer in the drying step, it was confirmed that the rotary dryer maintained pores to improve the absorption rate, and the paddle dryer improved the drying uniformity and reduced the fine powder content of the superabsorbent resin particles.
[0088] In contrast, in Comparative Example 1, the superabsorbent resin particles were dried using only a rotary dryer until the moisture content of the primary dried body, i.e., the final moisture content, reached 10.2% by weight, and not only was secondary drying not performed, but a drying step was also performed using one type of dryer. In Comparative Example 1, the primary drying was performed to a level similar to the moisture content of the secondary dried body in the Example, but it was confirmed that the rotary dryer reduced the drying uniformity and increased the fine powder content. In Comparative Example 2, like Comparative Example 1, a drying step was performed using only a rotary dryer, but the operating conditions of the rotary dryer were changed for drying. Comparative Example 2 also used only a rotary dryer, and similar results to Comparative Example 1 were confirmed.
[0089] Meanwhile, in Comparative Example 3, the superabsorbent resin particles were dried using only a paddle dryer until the moisture content of the primary dried material reached 12.6% by weight, and not only was secondary drying not performed, but the drying step was performed using only one type of dryer. It was confirmed that the absorption rate was lower than in the example in which secondary drying was performed using two types of dryers. That is, it was confirmed that the high shear applied by the paddles of the paddle dryer caused stress on the dried material, and the stress reduced the pores, resulting in a lower absorption rate. In Comparative Example 4, like Comparative Example 3, the drying step was performed using only a paddle dryer, but the operating conditions of the paddle dryer were changed. Again, by using only a paddle dryer, it was confirmed that similar results to Comparative Example 3 were obtained.
[0090] Meanwhile, in Comparative Example 5, the superabsorbent resin particles were manufactured by performing the drying step by primary drying using a paddle dryer and secondary drying using a rotary dryer, and the types of the primary and secondary dryers were changed compared to the examples. As described above, when a paddle dryer is used, the pores of the dried body may decrease, and the absorption rate may decrease. In Comparative Example 5, the paddle dryer was used first as the primary dryer, so that the primary dried body with reduced pores could be put into the rotary dryer, which is the secondary dryer. However, it was confirmed from the reduced absorption rate that the pores of the primary dried body, which had already been reduced by the paddle dryer, were maintained by the rotating drum of the rotary dryer.
Claims
1. A step of supplying a composition including a water-soluble ethylenically unsaturated monomer having at least a partially neutralized acidic group, an internal crosslinking agent, and a polymerization initiator to a polymerization reactor and carrying out a polymerization reaction to obtain a hydrogel polymer; A step of primarily drying the hydrogel polymer with a hot air dryer to obtain a primary dried body; Secondarily drying the primary dried body in a heat conduction dryer to obtain a secondary dried body; and pulverizing the secondary dried body to obtain superabsorbent resin particles.
2. Before the hydrogel polymer is primarily dried, The method for producing highly water-absorbent resin particles according to claim 1 , further comprising a step of chopping the hydrous gel polymer.
3. After the step of pulverizing the secondary dried body to obtain superabsorbent resin particles, surface crosslinking is performed in the presence of a surface crosslinking agent; The method for producing the highly water-absorbent resin particles according to claim 1 , further comprising a step of forming a surface cross-linked layer on at least a part of the surface.
4. The method for producing highly water-absorbent resin particles according to claim 1 , wherein the hot air dryer and the heat conduction dryer are connected in series.
5. The method for producing highly water-absorbent resin particles according to any one of claims 1 to 3, wherein the water content of the primary dried body is 20% by weight to 35% by weight.
6. The method for producing highly water-absorbent resin particles according to any one of claims 1 to 3, wherein the moisture content of the secondary dried body is 8% by weight to 20% by weight.
7. 2. The method for producing highly absorbent resin particles according to claim 1, wherein the hot air dryer is a rotary dryer, and the heat conduction dryer is a paddle dryer.
8. The rotary dryer includes a central tube and one or more hot air supply pipes attached to the central tube.
8. The method for producing highly water-absorbent resin particles according to claim 7, wherein the temperature of the hot air supplied from the one or more hot air supply pipes is 100° C. to 200° C., and the wind speed of the hot air is 20 m / s to 30 m / s.
9. The paddle dryer is equipped with an agitator, The method for producing highly water-absorbent resin particles according to claim 7, wherein the agitator rotates at 10 rpm to 50 rpm.
10. The method for producing highly water-absorbent resin particles according to claim 1, wherein the water-soluble ethylenically unsaturated monomer is (meth)acrylic acid or a salt thereof.
Citation Information
Patent Citations
Production of hydrophilic crosslinked polymer
JP1999240914A
Production of water-absorbing resin
JP1999292919A
How to completely dry the hydrogel
JP2002528582A
Production method of water-absorbent resin, water-absorbent resin, and usage of water-absorbent resin
JP2007077393A
Method for producing water-absorbent polymer particles
JP2009516043A