Hydrogenation-acid catalyst bifunctional catalyst, its preparation method and its use

A dual-functional hydrogenation-acid catalyst using silica-alumina molecular sieves with supported metals and hydrocarbyl modification addresses the inefficiencies of existing catalysts, achieving high benzene conversion and selectivity for cyclohexylbenzene production with minimized by-products.

JP2024538254AActive Publication Date: 2024-10-18CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024525085
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-06-28
Filing Date
2022-10-25
Publication Date
2024-10-18
Estimated Expiration
2042-10-25

AI Technical Summary

Technical Problem

Existing catalysts for the hydroalkylation of benzene to produce cyclohexylbenzene suffer from low catalytic efficiency, low selectivity, and high by-product formation, particularly cyclohexane, limiting their practical application in industry.

Method used

A dual-functional hydrogenation-acid catalyst comprising silica-alumina molecular sieves with supported hydrogenation-active metals like ruthenium, platinum, or palladium, and hydrocarbyl modification, optimized to minimize excess hydrogenation by-products and enhance selectivity of cyclohexylbenzene production.

Benefits of technology

The catalyst achieves high benzene conversion rates and selectivity for cyclohexylbenzene with reduced cyclohexane formation, demonstrating improved catalytic performance under mild reaction conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024538254000001_ABST
    Figure 2024538254000001_ABST
Patent Text Reader

Abstract

The catalyst comprises, based on the mass of the catalyst, 80 to 99.8% of a silicon-aluminum molecular sieve component, 0.2 to 2% of a metal component having hydrogenation activity supported on the molecular sieve, and 0 to 20% of a hydrocarbyl modifying component, the metal having hydrogenation activity being selected from ruthenium, platinum, palladium, copper, nickel, or a combination thereof, and the hydrocarbyl modifying component being C 1-20 A hydrogenation-acid catalyst bifunctional catalyst having hydrocarbyl groups. The catalyst has two functions as a hydrogenation catalyst and an acid catalyst, and is suitable for the hydroalkylation reaction of benzene and the hydroisomerization reaction of alkanes. Furthermore, when the catalyst is used in the hydroalkylation reaction of benzene to produce cyclohexylbenzene, the catalyst has the characteristics of high benzene conversion, good product selectivity, and low production of the by-product cyclohexane.
Need to check novelty before this filing date? Find Prior Art

Description

Detailed Description of the Invention

[0001] [Technical field] The present application relates to the field of catalysis, and in particular to hydrogenation-acid catalyst bifunctional catalysts, as well as methods for their preparation and their use.

[0002] [Background technology] Cyclohexylbenzene is an important chemical product and has important applications in the fields of liquid crystal and secondary batteries. Among them, cyclohexylbenzene liquid crystal has extremely high chemical stability, photochemical stability, and physical properties, making it one of the ideal materials for liquid crystal displays. Cyclohexylbenzene can also be used as an additive component in the electrolyte of lithium-ion batteries. Cyclohexylbenzene has the function of preventing overcharging, so it can effectively improve the safety of batteries. In addition, cyclohexylbenzene can be used as an intermediate to further carry out peroxidation and decomposition reactions to obtain phenol and cyclohexanone, which are important chemical products that can be used in the production of phenolic resin, caprolactam, and nylon. Therefore, the preparation and production of cyclohexylbenzene has attracted widespread attention. The basic information of cyclohexylbenzene is as follows: colorless liquid, CAS number: 827-52-1, density 0.95g / cm 3 , boiling point 238~240℃, melting point 5℃, flash point 98℃.

[0003] The main preparation methods of cyclohexylbenzene, which depend on the raw material, include the hexene alkylbenzene cyclization method and the benzene hydroalkylation method. Among these, the basic principle of the benzene hydroalkylation method is as follows: benzene and hydrogen are used as raw materials, and a part of the benzene is hydrogenated at the metal active center to obtain a six-membered cyclic olefin structure (such as cyclohexene), which is then alkylated with benzene at the position of the acidic active center to obtain the cyclohexylbenzene product. Therefore, in the production process of cyclohexylbenzene, a dual-function catalyst with both hydrogenation and alkylation active centers can be used.

[0004] Research on the hydroalkylation of benzene to prepare cyclohexylbenzene first began in the 1980s. Currently developed catalysts mainly use metals supported on molecular sieves, most of which suffer from low catalytic efficiency and low selectivity. For example, catalysts based on MCM-22 series molecular sieves (US2011 / 0015457A1, CN104105679A) suffer from slow catalytic rate and high selectivity to the by-product cyclohexane. Other catalysts, such as catalysts using HY molecular sieves treated with Ni-rare earth as a support (US4219689), suffer from low benzene conversion and low yield of cyclohexylbenzene product. It has been subsequently reported that molecular sieves loaded with Pd / HY are used as catalysts to catalyze the hydroalkylation of benzene and prepare cyclohexylbenzene in one step (Molecular Catalysis 2017, 442, 27-38). The initial conversion of benzene was 42.2%, the selectivity of cyclohexylbenzene remained at about 75%, and the selectivity of cyclohexane, a by-product of overhydrogenation, was high at about 20%. From this point of view, the existing technology poses great problems for practical application in industry, mainly due to the low product selectivity and the high amount of cyclohexane as a by-product.

[0005] Similarly, other hydrogenation-solid acid bifunctional catalytic reactions also face the problem of a large number of by-products and reduced selectivity of the target product. For example, patent CN112934251A discloses a scheme using hydrogenation metal-mordenite for n-heptane hydroisomerization reaction, in which the selectivity of isoheptane is about 60%-70%. Conventional US5643440, US5302279, US6190532, etc. disclose a scheme using a precious metal-low acidity molecular sieve as a heavy oil isomerization catalyst. However, there is a total lack of position control of the central sites of the hydrogenation catalyst and the acid catalyst, and the optimal matching effect of the dual active center has not been shown.

[0006] DISCLOSURE OF THEINVENTION The purpose of this application is to provide a hydrogenation-acid catalyst bifunctional catalyst, its preparation method and its application. This catalyst has two functions of hydrogenation and acid catalyst, and is suitable for benzene hydroalkylation and alkane hydroisomerization. When used in benzene hydroalkylation to produce cyclohexylbenzene, this catalyst has the characteristics of high benzene conversion, good product selectivity, and low by-product cyclohexane.

[0007] In order to achieve the above object, in one embodiment, the present application provides a catalyst comprising, based on the mass of the catalyst, 80 to 99.8% of a silica-alumina molecular sieve component, 0.2 to 2% of a metal component having hydrogenation activity supported on the molecular sieve, and 0 to 20% of a hydrocarbyl modifying component, wherein the hydrogenation active metal is selected from ruthenium, platinum, palladium, copper, nickel, or a combination thereof, and the hydrocarbyl modifying component is selected from C 1-20 It is a hydrocarbyl.

[0008] In another embodiment, there is provided a method for preparing the present catalyst comprising the steps of: (1) providing an H-type silica-alumina molecular sieve; and (2) Supporting a hydrogenation active metal on an H-type silica-alumina molecular sieve and optionally subjecting the resulting product to a hydrocarbylation treatment and / or reduction to obtain a catalyst.

[0009] In another embodiment, there is provided a use of the catalyst of the present application in a hydrocarbon hydrogenation reaction comprising contacting and reacting a hydrocarbon feedstock with the catalyst in the presence of hydrogen.

[0010] In another embodiment, the present application provides a one-step process for producing cyclohexylbenzene by hydrogenating benzene, the process comprising contacting and reacting benzene with the catalyst of the present application in the presence of hydrogen to obtain cyclohexylbenzene.

[0011] In another embodiment, the present application provides a process for alkane hydroisomerization comprising contacting and reacting a linear alkane with a catalyst of the present application in the presence of hydrogen to obtain an isomerization product, wherein the linear alkane is a C8 or higher linear alkane.

[0012] The advantageous effects of the catalyst of the present application compared to the prior art include: 1. The catalyst of the present application has the dual functions of hydrogenation and acid catalysis, and can realize the hydroalkylation reaction of benzene under mild reaction conditions to produce cyclohexylbenzene. The conversion rate of benzene and the selectivity of the main product, cyclohexylbenzene, are both very high, and the stability of the reaction system is good. In particular, when using the silica-alumina molecular sieve with ATS structure as the molecular sieve component, the catalyst of the present application has a special pore structure and acidic properties. The catalyst of the present application has a remarkable effect of reducing the generation of the by-products, cyclohexane and dicyclohexylbenzene, in the hydroalkylation reaction of benzene.

[0013] 2. The catalyst of the present application has a specific composition, in particular, its active metal components are mainly concentrated in the flow passages of the molecular sieve, and the outer surface has a low metal content, which ensures that the content of excess hydrogenation by-products (such as cyclohexane) is low; and the outer surface of the catalyst has high hydrophobicity, which has good affinity with various kinds of alkanes, aromatics and other non-polar substances, which ensures that the benzene conversion rate maintains a high level.

[0014] 3. When the catalyst of the present invention is used in the isomerization reaction of linear alkanes, the metal is mainly dispersed in the flow channels of the molecular sieve, and the spatial distance from the strong acid sites is short, and the amount of acid on the outer surface is small. This has the advantages of high substrate conversion and good selectivity for hydroisomerized products in the hydroisomerization reaction of alkane.

[0015] Other features and advantages of the present invention will be explained in the detailed description that follows.

[0016] BRIEF DESCRIPTION OF THE DRAWINGS The following figures are used to provide further understanding of the present application and constitute a part of this specification. They are used to explain the present application together with the following specific embodiments. However, they are not intended to limit the present application. Herein, FIG. 1 is the XRD spectrum of the catalyst prepared in Preparation Example I-1; FIG. 2 is a TEM image of the catalyst prepared in Preparation Example I-1; FIG. 3 is an SEM image of the catalyst prepared in Preparation Example I-1; FIG. 4 is the XRD spectrum of the catalyst prepared in Preparation Example II-1; FIG. 5 is an infrared absorption spectrum of the catalyst prepared in Preparation Example II-1; FIG. 6 is the XRD spectrum of the catalyst prepared in Preparation Example II-3; FIG. 7 is an XRD spectrum of the catalyst prepared in Production Example III-1.

[0017] Detailed Description of the Invention Hereinafter, specific embodiments of the present application will be described in detail with reference to the drawings. It should be understood that the specific embodiments described herein are merely used to illustrate and explain the present application, and are not intended to limit the present application in any way.

[0018] Any specific numerical value disclosed herein (including the endpoints of a numerical range) should not be construed as being limited to the exact value, but should be construed as including any possible value close to the exact value, for example, within ±5% of the exact value. In addition, for any numerical range disclosed, one or more new numerical ranges can be obtained by combining the endpoints of the range, combining the endpoints with specific numerical values ​​within the range, or combining specific numerical values ​​in any combination. Such new numerical ranges should also be considered to be specifically disclosed herein.

[0019] As used herein, the so-called "silicon-aluminum ratio" or "silicon-aluminum molar ratio" refers to the molar ratio of silicon, calculated as SiO2, to aluminum, calculated as Al2O3, in the molecular sieve.

[0020] In the present specification, w, m, s, vs, wm, ms and s-vs in the XRD data of the molecular sieve represent the relative intensity I / I0 of the diffraction peak at the corresponding 2θ angle relative to the most intense diffraction peak (i.e., the diffraction peak with the maximum intensity) calculated based on the intensity of the diffraction peaks, where I represents the peak intensity of the corresponding diffraction peak, I0 represents the peak intensity of the most intense diffraction peak, w means weak, m means medium, m and s mean strong, vs means very strong, wm means weak to medium, ms means medium to strong, and s-vs means strong to very strong. Such expressions are known to those skilled in the art. In general, w represents less than 20, m represents 20 to 40, s represents 40 to 70, vs represents more than 70, wm represents less than 40, ms represents 20 to 70, and s-vs represents more than 40.

[0021] According to the present application, the interplanar spacing of each diffraction peak in the XRD diffraction spectrum of a molecular sieve can be calculated based on the 2θ value of the diffraction peak using the following Bragg equation: λ=2dsinθ, where λ is the wavelength of the incident wave, λ=1.54 Å, d is the interplanar spacing, and θ is the angle between the incident light and the scattering plane.

[0022] In this specification, the so-called "pore volume" refers to the volume of pores per unit mass of catalyst. The so-called "total pore volume" refers to the volume of all pores per unit mass of catalyst. The so-called "micropore volume" refers to the volume of all micropores (generally meaning pores with a pore diameter of less than 2 nanometers) per unit mass of catalyst.

[0023] In this specification, the so-called "specific surface area" refers to the total area including the internal surface area and the external surface area per unit mass of the sample. Non-porous samples such as Portland cement and some clay mineral powders have only an external surface area. Porous samples such as asbestos fibers, diatomaceous earth, and molecular sieves have an external surface area and an internal surface area. In a porous sample, the surface area inside the micropores with a pore diameter of less than 2 nanometers is the internal surface area. The external surface area is the surface area minus the internal surface area. The external surface area per unit mass of the sample is the external specific surface area. Therefore, in this specification, the "external surface of the catalyst" refers to the surface of the catalyst excluding the internal surfaces of the micropores with a pore diameter of less than 2 nanometers.

[0024] As used herein, "H-type silica-alumina molecular sieve" has the meaning commonly understood in the art and specifically refers to a silica-alumina molecular sieve having activated acid sites, which can usually be prepared directly using an acidic system or by ammonium ion exchange and calcination of an alkali metal type silica-alumina molecular sieve, such as a Na-type silica-alumina molecular sieve.

[0025] In this application, unless otherwise specified, the amount and content of the metal component having hydrogenation activity is based on the metal.

[0026] Unless otherwise specified, terms used herein have the same meaning as commonly understood by one of ordinary skill in the art, and where a term is defined herein and that definition differs from the normal understanding in the art, the definition provided herein shall control.

[0027] In this application, unless expressly described, the matter not described shall be regarded as the same as that known in the art without any modification. Moreover, any of the embodiments described herein can be freely combined with one or more other embodiments described herein. Any technical solution or technical idea obtained in this way shall be regarded as part of the original disclosure or original description of this application, and shall not be regarded as a new matter not disclosed or anticipated in this specification, unless it is obvious to a person skilled in the art that such a combination is obviously unreasonable.

[0028] All patent and non-patent literature, including but not limited to textbooks and journal articles, referred to herein is hereby incorporated by reference in its entirety.

[0029] As described above, in a first aspect, the present application provides a hydrogenation-acid catalyst bifunctional catalyst comprising, based on the mass of the catalyst, 80-99.8% of a silica-alumina molecular sieve component, 0.2-2% of a metal component having hydrogenation activity supported on the molecular sieve, and 0-20% of a hydrocarbyl-modified component.

[0030] In the catalyst of the present application, the hydrocarbyl modifying component is attached to the surface of the molecular sieve through a covalent bond, such as a hydrocarbyl-Si-O-molecular sieve covalent bond. In certain embodiments, a silanizing reagent can be used as a starting material, and the hydrocarbyl modifying component can be attached to the surface of the molecular sieve through the reaction of the silicon-oxygen bond linked to the silicon with the active hydroxyl groups on the surface of the molecular sieve.

[0031] In preferred embodiments, the hydrogenation active metal is selected from ruthenium, platinum, palladium, copper, nickel, or a combination thereof, more preferably ruthenium, palladium, or a combination thereof.

[0032] In a preferred embodiment, the hydrocarbyl modifying component is1-20 Hydrocarbyl, preferably C 1-10 It is hydrocarbyl, more preferably selected from methyl, ethyl, propyl, isopropyl, butyl, phenyl, benzyl, phenethyl, or combinations thereof.

[0033] In a preferred embodiment, the mass content of the silica-alumina molecular sieve in the catalyst is 90-99.8%, for example, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, 99.5%, etc., based on the mass of the catalyst. More preferably, the mass content of the silica-alumina molecular sieve is 90-98%.

[0034] In a preferred embodiment, the mass content of the hydrogenation active metal in the catalyst is 0.2 to 1.5%, preferably 0.2 to 1.2%, more preferably 0.3 to 1.0%, for example, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, etc., based on the mass of the catalyst.

[0035] In a preferred embodiment, the silica-alumina molecular sieve in the catalyst is selected from molecular sieves having MWW structure, FAU structure, MOR structure, BEA structure or ATS structure, or a combination thereof, and is preferably a molecular sieve having ATS structure. Specific examples of molecular sieves having MWW structure include SCM-1 molecular sieve, MCM-22 molecular sieve, etc. Specific examples of molecular sieves having FAU structure include X molecular sieve and Y molecular sieve. Specific examples of molecular sieves having MOR structure include LZ-211 molecular sieve. Specific examples of molecular sieves having BEA structure include β molecular sieve. In a particular embodiment, the silica-alumina molecular sieve is an H-type silica-alumina molecular sieve.

[0036] In a preferred embodiment, the silicon-aluminum ratio of the molecular sieve in the silica-alumina catalyst is 2-50, preferably 2-40, and more preferably 2-20.

[0037] In certain preferred embodiments, the molecular sieve in the catalyst is a silica-alumina molecular sieve having the ATS structure, and the X-ray diffraction spectrum of the catalyst exhibits relative intensities of diffraction peaks characteristic of the following table:

[0038] [Table 1]

[0039] In a further preferred embodiment, the X-ray diffraction spectrum of the catalyst exhibits relative intensities of diffraction peaks characteristic of any row of the following table:

[0040] [Table 2]

[0041] In a further preferred embodiment, in the catalyst, the crystals have a strip-like or rod-like morphology, the length of the crystals is 0.3-3 μm, and the aspect ratio is 2-20, preferably 5-20.

[0042] In the present application, the catalyst can be optionally subjected to one or both of hydrocarbylation and reduction treatment. Here, the hydrocarbylation and reduction treatments can be carried out during the preparation of the catalyst after the hydrogenation active metal is supported, or before the use of the catalyst. And when both the hydrocarbylation and reduction treatments are carried out, the reduction treatment can be carried out before or after the hydrocarbylation treatment, and is preferably carried out after the hydrocarbylation treatment. In a preferred embodiment, the catalyst is subjected to reduction treatment. Furthermore, when the silica-alumina molecular sieve is a molecular sieve having MWW, FAU, MOR or BEA structure, the catalyst is preferably subjected to hydrocarbylation treatment.

[0043] In the present application, the hydrogenation active metal in the catalyst may be present in various forms, such as a form selected from a metal element, an oxide, a chloride, a nitrate, or a combination thereof. In a preferred embodiment, the hydrogenation active metal is present mainly in the form of a metal element, for example, when the catalyst is subjected to a reduction treatment. Preferably, in the catalyst, the particle size of the hydrogenation active metal particles is 0.5-10 nm, preferably 1-5 nm.

[0044] In a particular preferred embodiment, the silica-alumina molecular sieve in the catalyst is a molecular sieve having an ATS structure, in particular an ATS molecular sieve having the above-mentioned XRD spectrum characteristics, and based on the mass of the catalyst, the mass content of the silicon-aluminum molecular sieve is 80-99.8%, preferably 90-99.8%, the mass content of the hydrogenation active metal is 0.2-2%, preferably 0.2-1.5%, and the catalyst does not contain a hydrocarbyl modifying component.

[0045] In another preferred embodiment, particularly when the silica-alumina molecular sieve is a molecular sieve having an MWW, FAU, MOR or BEA structure, the mass content of the silica-alumina molecular sieve in the catalyst is 80-98%, preferably 90-98%, the mass content of the hydrogenation active metal is 0.2-1.5%, preferably 0.2-1.2%, more preferably 0.3-1.0%, and the mass content of the hydrocarbyl modifying component is 1-20%, preferably 1-10%, more preferably 2-10%, for example, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, etc., based on the mass of the catalyst.

[0046] In a further preferred embodiment, the mass content of the hydrogenation active metal on the outer surface of the catalyst relative to the elements on the outer surface, as measured by X-ray photoelectron spectroscopy (XPS), is 0.5% or less, preferably 0.4% or less, more preferably 0.01 to 0.35%, for example 0.01 to 0.2%.

[0047] In a more preferred embodiment, the distribution coefficient of the hydrogenation active metal on the outer surface of the catalyst is from 1 to 20%, preferably from 1.5 to 18%, more preferably from 1.5 to 12%, for example from 1.5 to 10%.

[0048] In the present application, the distribution coefficient of the hydrogenation active metal on the outer surface of the catalyst is calculated by the following formula: distribution coefficient of the hydrogenation active metal on the outer surface=(mass content of the hydrogenation active metal on the outer surface relative to the elements on the outer surface of the catalyst*specific surface area of ​​the outer surface of the catalyst) / (total mass content of the hydrogenation active metal contained in the catalyst*specific surface area of ​​the catalyst)*100%, Here, the mass content of the hydrogenation active metals on the outer surface of the catalyst relative to the elements on the outer surface of the catalyst can be measured by X-ray photoelectron spectroscopy (XPS), and the total mass content of the hydrogenation active metals contained in the catalyst can be measured by inductively coupled plasma optical emission spectroscopy (ICP).

[0049] According to the present invention, the distribution coefficient of the hydrogenation active metal on the outer surface of the catalyst can be used to characterize the ratio of the content of the hydrogenation active metal on the outer surface of the catalyst to the total amount of the hydrogenation active metal. Specifically, when the hydrogenation active metal in the catalyst is supported on the inner and outer surfaces of a molecular sieve by a simple impregnation method, the ratio of the hydrogenation active metal content on the outer surface to the total content of the hydrogenation active metal is not only proportional to the relative distribution of the hydrogenation active metal on the outer surface, but also proportional to the ratio of the outer surface area of ​​the catalyst.

[0050] In a preferred embodiment, the specific surface area of ​​the catalyst is 200 to 800 m 2 / g, preferably 250 to 700m 2 / g, for example 300m 2 / g, 380m 2 / g, 385m 2 / g, 410m 2 / g, 490m 2 / g or 500m 2 / g.

[0051] In a preferred embodiment, the total pore volume of the catalyst is 0.15 cm 3 / g or more, preferably 0.18 to 1.0 cm 3 / g, more preferably 0.2 to 1.0 cm 3 / g, for example, 0.2 to 0.9 cm 3 / g.

[0052] In a preferred embodiment, the catalyst has a micropore volume of 0.05 to 0.30 cm 3 / g, preferably 0.10 to 0.25 cm 3 / g.

[0053] In a preferred embodiment, the total acid content of the catalyst is 400 to 1500 μmol g -1 and preferably 600 to 1500 μmol g -1 For example, 800 μmol g -1 and 1250 μmol g -1 and 1300 μmol g -1 or 1500 μmol g -1 It is.

[0054] In some preferred embodiments, for example when the catalyst is subjected to a hydrocarbylation treatment (i.e. when the content of the hydrocarbyl modifying component in the catalyst is in the range of 1-20%, preferably 1-10%), the relative acid equivalent of the outer surface of the catalyst is 15-50%, preferably 15-40%, e.g. 20%, 30% or 35%.

[0055] In certain preferred embodiments, for example when the catalyst is subjected to a hydrocarbylation process, the acid content ratio of B acid / L acid of the catalyst is from 0.2 to 8.0, preferably from 0.4 to 6.0, more preferably from 3.0 to 6.0, such as 5.0 or 5.5.

[0056] In another preferred embodiment, for example when the catalyst is based on ATS molecular sieve and has not been subjected to a hydrocarbylation treatment, the acid content ratio B acid / L acid of the catalyst is 3-10, preferably 5-7.

[0057] In a preferred embodiment, when the hydrocarbylation treatment is carried out but the reduction treatment is not carried out, the metal H2-TPR test reduction temperature of the catalyst is 470-500°C, preferably 480-500°C.

[0058] In a second aspect, there is provided a method for preparing the catalyst of the present application, comprising the steps of: (1) providing an H-type silica-alumina molecular sieve; and (2) Supporting a hydrogenation active metal on an H-type silica-alumina molecular sieve and optionally subjecting the resulting product to a hydrocarbylation treatment and / or reduction to obtain a catalyst.

[0059] In a preferred embodiment, the H-type silica-alumina molecule is selected from molecular sieves having the MWW, FAU, MOR, BEA or ATS structure, or combinations thereof, preferably a molecular sieve having the ATS structure.

[0060] In some preferred embodiments, step (1) comprises subjecting a raw material of silica-alumina molecular sieve to ammonium ion exchange and calcination to obtain an H-type silica-alumina molecular sieve.

[0061] In a more preferred embodiment, the silica-alumina molecular sieve raw material is selected from silica-alumina molecular sieves having the MWW, FAU, MOR or BEA structure, or combinations thereof.

[0062] In certain specific embodiments, the ammonium ion exchange in step (1) is carried out by removing Na from the alkali metal molecular sieve. + and K. +Alkali metal or alkaline earth metal cations such as NH 4+ The ammonium ion exchange is carried out once or multiple times at 20-60°C for 0.5-4 hours. The ammonium salt in the ammonium ion exchange is selected from one or more of ammonia, ammonium chloride, ammonium nitrate, and ammonium carbonate. The concentration of the ammonium salt is 0.1-1.0 mol / L. After the ammonium ion exchange, the molecular sieve is dried at 60-120°C for 4-24 hours and calcined. The calcination temperature is 400-650°C, the calcination time is 1-12 hours, and the calcination atmosphere is oxygen or air, and an H-type silica-alumina molecular sieve is obtained.

[0063] In another preferred embodiment, step (1) includes mixing a silicon source, an aluminum source, a fluorine source, an organic structure directing agent and water, and heating to pretreat, followed by crystallization and calcination to obtain an H-type ATS silica-alumina molecular sieve.

[0064] In a further preferred embodiment, in step (1), an added silicon source calculated as SiO, an aluminum source calculated as AlO, F - The molar ratio of the fluorine source, the organic structure directing agent and the water calculated as above is 1:(0.02-0.2):(0.5-2):(0.25-1.5):(3-15), and preferably 1:(0.05-0.15):(0.5-1):(0.5-1):(5-10).

[0065] In another preferred embodiment, in step (1), the silicon source is selected from silicic acid, silica gel, silica sol, tetraethyl silicate, sodium silicate, or a combination thereof, the aluminum source is selected from pseudoboehmite, aluminum isopropoxide, or a combination thereof, the fluorine source is hydrofluoric acid, and the organic structure directing agent is 4-pyrrolidinylpyridine. In this embodiment, 4-pyrrolidinylpyridine is used as the organic structure directing agent. There is no need to add a base during the reaction, and the obtained molecular sieve can be used as a catalyst without ammonium ion exchange.

[0066] In a further preferred embodiment, the method of pretreatment by heating in step (1) is rotary evaporation to remove moisture or open heating to remove moisture, and the treatment conditions for open heating are heating and stirring at 50 to 100°C, preferably 70 to 90°C.

[0067] In a further preferred embodiment, in step (1), after the raw material mixture is heated and pretreated, the molar ratio of the silicon source (calculated as SiO2) to water during crystallization is 1:(1-10), preferably 1:(1.5-6.5).

[0068] In a further preferred embodiment, in step (1), the crystallization conditions include a crystallization temperature of 120 to 200°C, preferably 150 to 200°C, and a crystallization time of 7 to 21 days, preferably 7 to 15 days.

[0069] In a further preferred embodiment, in step (1), the crystallization can be carried out by any method conventionally known in the art, such as by mixing a silicon source, an aluminum source, a fluorine source, an organic structure directing agent and water in a predetermined ratio, and heating the resulting mixture under crystallization conditions to cause crystallization.

[0070] In a further preferred embodiment, after the crystallization step is completed in step (1), a product can be obtained from the obtained mixture by any conventionally known separation method and calcination treatment. Examples of the separation method include a method of filtering, washing, and drying the obtained mixture. Here, the filtering, washing, and drying can be performed by any conventionally known method in the art. For example, the filtering may simply be performed by suction filtering the obtained product mixture. The washing includes, for example, washing with deionized water and / or ethanol. The drying temperature includes, for example, 40 to 250°C, preferably 60 to 150°C, and the drying time includes, for example, 8 to 30 hours, preferably 10 to 20 hours. This drying may be performed under normal pressure or under reduced pressure.

[0071] In a further preferred embodiment, in step (1), the calcination can be carried out by any method conventionally known in the art. For example, the calcination temperature is generally 300 to 800°C, preferably 400 to 650°C, and the calcination time is generally 1 to 12 hours, preferably 2 to 6 hours. Furthermore, the calcination is generally carried out in an oxygen-containing atmosphere, such as air or an oxygen atmosphere.

[0072] According to the present invention, in step (2), the hydrogenation active metal can be supported on the H-type silica-alumina molecular sieve by conventional means (such as impregnation). In a preferred embodiment, in step (2), the hydrogenation active metal is supported on the H-type silica-alumina molecular sieve by adding a solution of the hydrogenation active metal source to the H-type silica-alumina molecular sieve and then drying.

[0073] In a further preferred embodiment, in step (2), the hydrogenation active metal source is selected from a soluble compound of a metal, preferably selected from a chloride, a nitrate, or a combination thereof. Taking ruthenium as an example, the solution of the hydrogenation active metal source can be a ruthenium-containing solution prepared from ruthenium nitrate or ruthenium chloride.

[0074] In a further preferred embodiment, in the step (2), the concentration of the solution of the hydrogenation active metal source is 1.5 to 50 g / L, preferably 2 to 45 g / L, based on the mass of the hydrogenation active metal.

[0075] In a more preferred embodiment, in step (2), the solution of the hydrogenation active metal source is added dropwise to the H-type silica-alumina molecular sieve in step (1). The present application does not particularly limit the conditions for the dropwise addition. For example, after the dropwise addition at room temperature, mixing can be performed for 1 to 10 hours.

[0076] In a more preferred embodiment, in step (2), the mass ratio of the hydrogenation active metal in the solution of the hydrogenation active metal source to the H-type silica-alumina molecular sieve in step (1) is 0.002-0.015:1, for example, 0.005-0.02:1.

[0077] In a more preferred embodiment, in step (2), drying can be performed by a conventional method such as oven drying, etc. The drying conditions preferably include a drying temperature of 40 to 90° C. and a drying time of 4 to 12 hours.

[0078] According to the present application, in step (2), after the hydrogenation active metal is supported on the H-type silica-alumina molecular sieve, the resulting product can be optionally subjected to one or both of a hydrocarbylation treatment and a reduction treatment. When both the hydrocarbylation treatment and the reduction treatment are performed, the reduction treatment can be performed before or after the hydrocarbylation treatment, and is preferably performed after the hydrocarbylation treatment.

[0079] In a preferred embodiment, step (2) includes reducing the product after the hydrogenation active metal is supported. More preferably, the reduction can be carried out using a reducing gas, preferably hydrogen reduction, and the reduction conditions are preferably a reduction temperature of 300 to 550°C, a reduction time of 3 to 6 hours, and a volumetric space velocity of the reducing gas of 40 to 200 h. -1 This includes being.

[0080] In a preferred embodiment, particularly when the H-type silica-alumina molecular sieve is a molecular sieve having MWW, FAU, MOR or BEA structure, step (2) comprises subjecting the product after the hydrogenation active metal is supported to a hydrocarbylation treatment. Preferably, the product after the hydrogenation active metal is supported is first subjected to a reduction treatment and then subjected to a hydrocarbylation treatment.

[0081] In a further preferred embodiment, the hydrocarbylation treatment in step (2) comprises mixing and reacting the hydrogenation active metal-supported product, preferably after reduction, with a hydrocarbylation reagent in a solvent.

[0082] In a further preferred embodiment, the hydrocarbylating agent is methyltrimethoxysilane, dimethyldimethoxysilane, ethyltrimethoxysilane, diethyldimethoxysilane, propyltrimethoxysilane, isopropyltrimethoxysilane, phenyltrimethoxysilane, tolyltrimethoxysilane, phenylsilanetriol, tolylsilanetriol, diphenylsilanediol, or a combination thereof, preferably selected from dimethyldimethoxysilane, diethyldimethoxysilane, isopropyltrimethoxysilane, phenyltrimethoxysilane, tolyltrimethoxysilane, phenylsilanetriol, tolylsilanetriol, or a combination thereof.More preferably, the solvent used in the hydrocarbylating process is selected from ethanol, toluene, or a combination thereof.

[0083] In a further preferred embodiment, the mass ratio of the product carrying a hydrogenation active metal, the hydrocarbylation reagent, and the solvent in the hydrocarbylation treatment is 1:(0.05-0.45):(5-55), preferably 1:(0.06-0.40):(6-50), for example, 1:(0.10-0.33):(8-50), or 1:(0.12-0.35):(7.5-52).

[0084] In a further preferred embodiment, in the hydrocarbylation process, the reaction conditions include a reaction temperature of 40-110° C., preferably 70-110° C., and a reaction time of 6-48 hours, preferably 8-24 hours.

[0085] In a particular more preferred embodiment, after the hydrocarbylation treatment, the resulting reaction product is separated (e.g., filtered), washed, and dried. According to the present invention, the separation, washing, and drying can be carried out by any method conventionally known in the art. For example, the filtration may simply involve suction filtering of the resulting product mixture. Examples of washing include washing with deionized water and / or ethanol. An example of the drying temperature is 40 to 250°C, preferably 60 to 150°C. An example of the drying time is 8 to 30 hours, preferably 10 to 20 hours. The drying may be carried out under normal pressure or under reduced pressure.

[0086] In a third aspect, there is provided a hydrogenation-acid catalyst bifunctional catalyst prepared by the method of the present application.

[0087] In specific embodiments, the various features of the hydrogenation-acid catalyst bifunctional catalyst obtained by the process of the present application are as described in the first aspect of the present application and will not be described again here.

[0088] In a fourth aspect, there is provided a use of the catalyst of the present application in a hydrocarbon hydroconversion reaction comprising contacting and reacting a hydrocarbon feedstock with the catalyst in the presence of hydrogen.

[0089] In a preferred embodiment, the hydrocarbon hydroconversion reaction is selected from a benzene hydroalkylation reaction and an alkane hydroisomerization reaction.

[0090] In a fifth aspect, the present application provides a one-step process for hydrogenating benzene to produce cyclohexylbenzene, the process comprising contacting and reacting benzene with a catalyst as described herein in the presence of hydrogen to obtain cyclohexylbenzene.

[0091] In a preferred embodiment, the reaction conditions include a mass ratio of benzene to catalyst of 8 to 40, preferably 10 to 40; a reaction temperature of 100 to 220°C, preferably 120 to 200°C; a reaction time of 2 to 8 hours, preferably 2.5 to 6 hours; and a hydrogen pressure of 0.8 to 2.5 MPa, preferably 1.0 to 2.5 MPa.

[0092] In a sixth aspect, the present application provides a method for hydroisomerizing an alkane, the method comprising contacting and reacting a linear alkane with the present catalyst in the presence of hydrogen to obtain an isomerization product, the linear alkane being a C8 or higher linear alkane, e.g., n-heptane, n-decane, etc., preferably a C8-C20 linear alkane, more preferably a C8-C12 linear alkane.

[0093] In a preferred embodiment, the reaction conditions include: a mass ratio of linear alkane to catalyst is 10-100, preferably 10-50; a reaction temperature is 250-400°C, preferably 300-400°C; a reaction time is 3-10 hours, preferably 4-10 hours; and a hydrogen pressure is 2.5-5.0 MPa, preferably 3.0-4.0 MPa.

[0094] In certain preferred embodiments, the following technical solutions are provided: A1. A catalyst for producing cyclohexylbenzene, having an approximate chemical composition represented by the formula "xM·ySiO2·zAl2O3"; wherein M is a metallic element selected from one or more of ruthenium, platinum, palladium, copper and nickel metals; In the chemical composition in the formula, 0.001≦x / y≦0.02 and 8≦y / z≦80.

[0095] A2. The catalyst according to item A1, characterized in that the mass content of the metal M is 0.2% to 2% based on the mass of the catalyst.

[0096] A3. The catalyst according to item A1, characterized in that it has an X-ray diffraction pattern as shown in the table below:

[0097] [Table 3]

[0098] A4. The catalyst according to paragraph A1 or A3, further comprising the X-ray diffraction pattern shown in the table below.

[0099] [Table 4]

[0100] A5. Total acid content is 500-1500 μmol g -1 and preferably 800 to 1500 μmol g -1 and the acid content ratio of B acid / L acid is 3-10, preferably 5-7.

[0101] A6. The catalyst according to item A1, wherein the crystal has a strip-like or rod-like morphology, the length of the crystal is 0.3 to 3 μm, and the aspect ratio is 2 to 20.

[0102] A7. The specific surface area of ​​the catalyst is 200 to 600 m 2 / g, preferably 250 to 500m 2 / g; the catalyst has a micropore volume of 0.05 to 0.30 cm 3 / g, preferably 0.10 to 0.25 cm 3 / g of the catalyst according to item A1.

[0103] A8. A method for preparing a catalyst for producing cyclohexylbenzene according to any one of items A1 to A7, comprising the following steps: (1) Mix a silicon source, an aluminum source, a fluorine source, an organic structure directing agent and water, heat to pretreat, and then crystallize and calcinate to obtain sample B; (2) A solution containing metal M is added to sample B from step (1), followed by drying and reduction to prepare a catalyst.

[0104] A9. In step (1), an added silicon source calculated as SiO2, an aluminum source calculated as Al2O3, and F - The preparation method according to item A8, characterized in that the molar ratio of the fluorine source, calculated as: fluorine, organic structure directing agent and water is 1:(0.02-0.2):(0.5-2):(0.25-1.5):(3-15), preferably 1:(0.05-0.15):(0.5-1):(0.5-1):(5-10).

[0105] A10. The preparation method according to item A8 or A9, characterized in that in step (1), the silicon source is selected from at least one of silicic acid, silica gel, silica sol, tetraethyl silicate, and sodium silicate; the aluminum source is selected from at least one of pseudoboehmite and aluminum isopropoxide; in step (1), the fluorine source is hydrofluoric acid; and the organic structure directing agent is 4-pyrrolidinylpyridine.

[0106] A11. The preparation method according to item A8 or A9, characterized in that in step (1), the molar ratio of the silicon source, calculated as SiO2, in the raw material mixture after pretreatment by heating to water during crystallization is 1:(1-10), preferably 1:(1.5-6.5).

[0107] A12. The method according to item A8 or A9, wherein in step (1), the crystallization conditions include a temperature of 120-200°C and a time of 7-21 days, preferably a temperature of 150-200°C and a time of 7-15 days.

[0108] A13. The preparation method according to item A8 or A9, wherein in step (2), the concentration of the solution containing the metal M is 2 to 50 g / L.

[0109] A14. A one-step process for producing cyclohexylbenzene by hydrogenating benzene using the catalyst according to any one of items A1 to A7.

[0110] A15. The method according to item A14, characterized in that hydrogen is used as a hydrogen source for producing cyclohexylbenzene, and the method comprises contacting raw material benzene with a catalyst; where the mass ratio of raw material benzene to catalyst is 8-40; the reaction temperature is 100-220°C; the reaction time is 2-8 hours; and the hydrogen pressure is 0.8-2.5MPa.

[0111] B1. A catalyst for producing cyclohexylbenzene, comprising a molecular sieve, an active metal M, and a hydrocarbyl modifying group; wherein the active metal M is selected from one or more of ruthenium, platinum, palladium, copper and nickel; wherein the hydrocarbyl modifying group is selected from at least one of C1 to C4 alkyl groups; Here, based on the mass of the catalyst, the mass content of the active metal M is 0.2% to 1.5%, the mass content of the metal M on the outer surface of the catalyst relative to the elements on the outer surface is 0.4% or less, and the distribution coefficient of the metal M on the outer surface is 1.2% to 20%.

[0112] B2. The catalyst according to item B1, characterized in that the mass content of the metal M is 0.2% to 1.2% based on the mass of the catalyst.

[0113] B3. The catalyst according to item B1, characterized in that the mass content of the hydrocarbyl modifying group is 1% to 10% based on the mass of the catalyst.

[0114] B4. The catalyst according to item B1, characterized in that the molecular sieve in the catalyst is selected from at least one of MWW, FAU, MOR, BEA, and ATS molecular sieves; the molecular sieve in the catalyst accounts for 90%-98% of the catalyst mass; and the silicon / aluminum ratio is 2-50, preferably 4-40.

[0115] B5. The specific surface area of ​​the catalyst is 380 to 800 m 2 / g, preferably 400 to 700m 2 / g; the total pore volume of the catalyst is 0.15 cm 3 / g or more, preferably 0.2 to 0.9 cm 3 / g of the catalyst according to item B1.

[0116] B6. A method for preparing a catalyst for producing cyclohexylbenzene according to any one of items B1 to B5, comprising the steps of: (i) calcining the ammonium ion-exchanged molecular sieve raw material to obtain an H-type molecular sieve; (ii) adding a solution containing metal M to the H-type molecular sieve of step (1), followed by drying and reducing to obtain a catalyst precursor; (iii) Mixing and reacting the catalyst precursor, the alkylating reagent and the solvent, followed by filtering, washing and drying to prepare the catalyst.

[0117] B7. The preparation method according to item B6, wherein in step (i), the concentration of the solution containing the metal M is 2 to 50 g / L.

[0118] B8. The preparation method according to item B6, characterized in that in step (ii), the alkylating agent is selected from one or more of methyltrimethoxysilane, dimethyldimethoxysilane, ethyltrimethoxysilane, diethyldimethoxysilane, propyltrimethoxysilane, isopropyltrimethoxysilane, preferably one or more of dimethyldimethoxysilane, diethyldimethoxysilane and isopropyltrimethoxysilane; the solvent is at least one of ethanol or toluene.

[0119] B9. The preparation method according to item B6, characterized in that in step (iii), the mass ratio of the catalyst precursor, the alkylating reagent and the solvent added is 1:(0.05-0.40):(5-50).

[0120] B10. A one-step process for producing cyclohexylbenzene by hydrogenating benzene using a catalyst according to any one of items B1 to B5.

[0121] C1. The method comprises contacting raw benzene with a catalyst to produce cyclohexylbenzene using hydrogen as a hydrogen source; the catalyst comprises a molecular sieve, an active metal M and a hydrocarbyl modifying group; wherein the active metal M is selected from one or more of ruthenium, platinum, palladium, copper and nickel; wherein said hydrocarbyl modifying group is selected from at least one of phenyl, benzyl, and phenethyl; Here, the total acid content of the catalyst is 400–1500 μmol g -1 and the relative acid equivalent of the outer surface of the catalyst is 15-35%.

[0122] C2. The method according to item C1, characterized in that the metal M is preferably a ruthenium and / or palladium metal element.

[0123] C3. The method according to item C1, wherein the mass content of the hydrocarbyl modifying group is 2% to 20%, based on the mass of the catalyst.

[0124] C4. The method according to item C1, characterized in that the molecular sieve in the catalyst is selected from at least one of MWW, FAU, MOR, BEA, and ATS molecular sieves; the molecular sieve in the catalyst accounts for 80%-95% of the catalyst mass; and the molar ratio of silicon to aluminum is 2-50, preferably 4-40.

[0125] C5. The specific surface area of ​​the catalyst is 385 to 500 m 2 / g, preferably 410 to 490m 2 / g; the total pore volume of the catalyst is 0.18 cm 3 / g or more, preferably 0.18 to 1.0 cm 3 The method according to item C1, characterized in that:

[0126] C6. The method according to item C1, characterized in that the method for preparing the catalyst comprises the following steps: (A) mixing a solution containing metal M with H-type molecular sieves, followed by drying and reduction to prepare a catalyst precursor; (B) A process for preparing a catalyst by mixing and reacting a catalyst precursor, an arylating reagent and a solvent, followed by filtering, washing and drying.

[0127] C7. The method according to item C6, wherein in step (A), the concentration of the solution containing the metal M is 1.5 to 45 g / L.

[0128] C8. The method according to item C6, wherein in step (B), the arylating reagent is selected from one or more of phenyltrimethoxysilane, tolyltrimethoxysilane, phenylsilanetriol, tolylsilanetriol and diphenylsilanediol; the solvent is at least one of ethanol or toluene.

[0129] C9. The method according to item C6, characterized in that in step (B), the mass ratio of the catalyst precursor, the arylating reagent and the solvent added is 1:(0.06-0.45):(6-55).

[0130] C10. The method according to item C1, characterized in that in the reaction, the mass ratio of the raw material benzene to the catalyst is 8 to 40, the reaction temperature is 100 to 220°C, the reaction time is 2 to 8 hours, and the hydrogen pressure is 0.8 to 2.5 MPa.

[0131] [Example] The technical solutions of the present invention are further illustrated in detail by the following examples, but the protection scope of the present invention is not limited to these examples.

[0132] In the following Examples and Comparative Examples, unless otherwise specified, all reagents and raw materials used are commercially available products and have analytical grade purity.

[0133] In the following examples and comparative examples, the experimental methods without specific conditions should be selected according to conventional methods and conditions or product instructions.

[0134] In the present invention, including the following examples and comparative examples, the structure of the sample is determined by X-ray diffraction spectrum (XRD), and the XRD spectrum is determined by an X-ray powder diffractometer. The type of X-ray powder diffractometer used is a Panalytical X PERPRO X-ray powder diffractometer. To analyze the physical phase of the sample, the following conditions were used: CuKα source (λ=1.54 Å), nickel filter, 2θ scan range 2-50°, operating voltage 40 kV, current 40 mA, scan speed 10° / min.

[0135] In this application, including the following examples and comparative examples, the scanning electron microscope (SEM) used was an S-4800II field emission scanning electron microscope. The crystal grain size of the sample was measured as follows: an observation field was randomly selected, and the molecular sieve was observed at a magnification of 10,000 times using a scanning electron microscope. The average value of the sum of the grain sizes of all the crystals in the observation field was calculated, and this operation was repeated a total of 10 times. The average value of the sum of the 10 average values ​​was taken as the crystal grain size.

[0136] In this application, including the following examples and comparative examples, the size of the sample was measured as follows: using a transmission electron microscope (G2F30 transmission electron microscope, manufactured by FEI, Netherlands, operating voltage 300 kV), an observation field was randomly selected, and the molecular sieve was observed at a magnification of 100,000 times, and the average value of the sum of the sizes of all particles within the observation field was calculated. This operation was repeated a total of 10 times, and the average value of the sum of the 10 average values ​​was used as the particle size.

[0137] In this application, including the following examples and comparative examples, the acid content and type of the sample were measured using a pyridine adsorption infrared method (Nicolet Model 710 spectrometer). The specific operation procedures are as follows: a. Sample pretreatment. The sample (about 30 mg) was pressed into a thin disk shape with a diameter of 13 mm and placed in an infrared sample tank. Then, the sample was pretreated at 400 °C for 1 hour under vacuum cell conditions. After the sample tank was cooled to room temperature, the infrared data of the sample was scanned as the background. b. Pyridine adsorption. At room temperature and in a vacuum environment, pyridine vapor was introduced into the original position until the adsorption reached equilibrium. The adsorption time was 1 hour. c. Pyridine desorption. After the adsorption was completed, the inside pressure was evacuated at 100 °C until it did not change. The desorption time was 40 minutes, and the infrared absorption spectrum was scanned and recorded respectively. The difference spectrum before and after pyridine adsorption is the obtained pyridine adsorption infrared absorption spectrum. Based on this spectrum, the acid content of the sample was calculated:

[0138]

number

[0139] In the formula, r and w are the diameter (cm) and mass (g) of the catalyst thin plate, A is the integrated absorbance value at a given wave number peak based on the scanning pyridine adsorption infrared absorption spectrum, IMEC is the integrated molar attenuation coefficient, and IMEC L 2.22, IMEC B is 1.67. -1 The peak near the B acid is 1455 cm -1 The peak nearby is L acid.

[0140] In this application, including the following examples and comparative examples, the properties of the relative acid equivalent of the outer surface of the catalyst were measured using the pyrolysis of triisopropylbenzene, which is a "probe reaction". The specific operation is to prepare a chromatography column sample by mixing 50 mg of catalyst and 100 mg of quartz sand, and then inject 1 μL of triisopropylbenzene liquid into a gas chromatograph (GC, Agilent 7890B) at 250 °C at once. Then, the structure of the "metal molecular sieve" that has not been hydrocarbyl-treated was compared according to the yield of cyclohexene in the chromatogram, and the relative acid content and activity of the outer surface of the catalyst were evaluated. The specific calculation method is as follows: Relative acid equivalent of outer surface=(amount of propylene produced from hydrocarbyl groups / (amount of triisopropylbenzene added to hydrocarbyl groups×3)) / (amount of propylene produced from unhydrocarbyl groups / (amount of triisopropylbenzene added to unhydrocarbyl groups×3))×100%.

[0141] In this application, including the following examples and comparative examples, the total pore volume, micropore volume, total specific surface area and outer surface specific surface area of ​​a sample are measured by nitrogen physical adsorption desorption method (BET method): a physical adsorption apparatus (e.g., Micromeretic ASAP2020M physical adsorption apparatus) is used to measure the nitrogen physical adsorption / desorption isotherm of a molecular sieve, and the values ​​are calculated using the BET equation and the t-plot equation.

[0142] In the present application, including the following examples and comparative examples, the model of the inductively coupled plasma optical emission spectrometer (ICP) used is a Varian 725-ES. The analysis sample was dissolved in hydrofluoric acid, and the element content (molar) including the hydrogenation active metal (hereinafter referred to as "metal M") in the sample was detected and converted to obtain the mass content.

[0143] In this application, including the following examples and comparative examples, the mass content of metal M on the outer surface of the catalyst relative to the elements on the outer surface of the catalyst is determined by X-ray photoelectron spectroscopy (XPS), which is a test of the catalyst surface element state. The model of the X-ray photoelectron spectrometer used is ESCA LAB-250 X-ray photoelectron spectrometer manufactured by Thermo Company, using Al Ka=1486.6eV as the X-ray source, operating voltage is 12KV, operating current is 20mA, detection thickness is 3nm, and C1s=284.6eV is used as the internal standard for correcting the measured element signal.

[0144] In this application, including the following Examples and Comparative Examples, the distribution coefficient of the metal M at the outer surface of the catalyst is calculated by the following formula: Partition coefficient of metal M=(mass content of metal M on the outer surface of the catalyst relative to the elements on the outer surface of the catalyst × specific surface area of ​​the outer surface of the catalyst) / (total mass content of metal M in the catalyst × specific surface area of ​​the catalyst) × 100%.

[0145] In this application, including the following examples and comparative examples, the metal reduction temperature is determined by H2-TPR test (hydrogen temperature programmed reduction). The TPR tester is an AMI-3300 temperature programmed absorption device from Altamira Instruments. The test method is to fill the sample, purge with argon at 300°C for 1 hour, and then cool to 50°C. A 10% H2-Ar mixed gas is introduced at a total flow rate of 30 mL / min, and the temperature is increased to 900°C at 10°C / min to measure the H2 consumption curve, and the peak temperature of the curve is recorded as the reduction temperature of the sample.

[0146] In this application, including the following examples and comparative examples, thermogravimetry-mass spectrometry (TG-MS) mass loss ratios are used to measure the mass content of the hydrocarbyl modification components and to confirm the type of hydrocarbyl modification by mass spectrometry. The analyzer is a Netzsch STA449F3-QMS403 model. Thermogravimetry results of samples from 25 to 1000°C were measured at a heating rate of 10°C / min.

[0147] In the present application, including the following Examples and Comparative Examples, the infrared absorption spectrum of the catalyst was measured using a Fourier transform infrared spectrometer (FTIR). The analyzer was a Nicolet 5700 model manufactured by Thermo Fisher Scientific. The test range was wavenumber 400 to 4000 cm. -1 The absorption spectrum was taken at

[0148] In this application, including the following examples and comparative examples, the reaction product cyclohexylbenzene was characterized by gas chromatography-mass spectrometry (GC-MS), and the yield of the product cyclohexylbenzene and the conversion of the reaction substrate were analyzed by gas chromatography (GC). The GC / MS instrument was an Agilent 7890A from Agilent, USA, and the chromatography column was an HP-5 non-polar capillary column (30 m, 0.53 mm). The gas chromatograph was an Agilent 7890B, the detector was a flame ionization detector (FID), and the chromatography column was an SE-54 capillary column (30 m, 0.53 mm).

[0149] The formula for calculating the yield and selectivity of the product cyclohexylbenzene is as follows: Yield (%) of the product cyclohexylbenzene = (number of moles of cyclohexylbenzene produced by the reaction × 2) / (number of moles of benzene as the reaction substrate) × 100%.

[0150] Selectivity (%) of the product cyclohexylbenzene = (number of moles of cyclohexylbenzene produced by reaction × 2) / (number of moles of benzene reacted) × 100%.

[0151] Similarly, in this application, including the following Examples and Comparative Examples, the yields and selectivities of the isomerized products in the n-decane hydroisomerization reaction are as follows: Yield (%) of isomerization product = (number of moles of isomerization product produced by reaction) / (number of moles of n-decane, the reaction substrate) x 100%.

[0152] Selectivity of isomerized product (%) = (number of moles of isomerized product produced in the reaction) / (number of moles of n-decane reacted) × 100%.

[0153] (Preparation Example 1-1) 4 g of deionized water, 0.75 g of 4-pyrrolidinylpyridine, 0.42 g of aluminum isopropoxide, 1.5 g of silica sol, and 0.5 g of hydrofluoric acid were mixed uniformly to obtain a solution of 1SiO2:0.1Al2O3:1F - A component having a composition of :29H2O:0.5OSDA was obtained. After that, it was pretreated by heating in the open at 80°C to obtain a block mixture. After the raw material mixture was pretreated by heating, the molar ratio of silicon source (calculated as SiO2) to water during crystallization was set to 1:5, and it was crystallized in a crystallization kettle at 170°C for 15 days. After the product was taken out, it was washed three times with deionized water, dried, and then calcined at 550°C for 6 hours to obtain the desired H-type silica-alumina molecular sieve (ATS structure).

[0154] 1.2 mL of 3.2 g / L ruthenium chloride solution was added dropwise onto 1 g of H-type silica-alumina molecular sieve. After drying at 80°C for 2 hours, the catalyst was reduced in a fixed bed reactor at 350°C with a hydrogen flow rate of 10 mL / min for 3 hours to obtain the required catalyst.

[0155] The XRD spectrum data of the catalyst is shown in Table I-1. The XRD spectrum of the catalyst is shown in Figure 1. The TEM and SEM photographs of the catalyst are shown in Figure 2 and Figure 3, respectively. The composition of the catalyst was n(SiO2):n(Al2O3)=10, the mass fraction of Ru was 0.3%, and the chemical composition of the catalyst was expressed as "xM ySiO2 zAl2O3", where x / y=0.0021 and y / z=10. The properties of the obtained catalyst are shown in Table I-13.

[0156] The SEM of FIG. 3 showed that the crystals in the catalyst were long strips with crystal lengths of 0.4-1.5 μm and aspect ratios of 2-10.

[0157] [Table 5]

[0158] (Preparation example I-2) 4 g of deionized water, 0.75 g of 4-pyrrolidinylpyridine, 0.42 g of aluminum isopropoxide, 1.5 g of silica sol, and 0.5 g of hydrofluoric acid were mixed uniformly to obtain a solution of 1SiO2:0.1Al2O3:1F - A component with a composition of :29H2O:0.5OSDA was obtained. Pretreatment was performed by open heating at 80°C to obtain a block mixture. After pretreatment by heating the raw material mixture, the molar ratio of silicon source (calculated as SiO2) to water during crystallization was set to 1:5, and crystallization was performed in a crystallization kettle at 170°C for 15 days. After the product was taken out, it was washed three times with deionized water, dried, and then calcined at 550°C for 6 hours to obtain the desired H-type silica-alumina molecular sieve (ATS structure).

[0159] 2.5 mL of 3.2 g / L ruthenium chloride solution was added dropwise onto 1 g of H-type silica-alumina molecular sieve. After drying at 80°C for 2 hours, the catalyst was reduced in a fixed bed reactor at 350°C with a hydrogen flow rate of 10 mL / min for 3 hours to obtain the required catalyst.

[0160] The XRD spectrum data of the catalyst is shown in Table I-2. The XRD spectrum of the catalyst is the same as that in Figure 1. In the composition of the catalyst, n(SiO2):n(Al2O3)=10, the mass fraction of Ru was 0.6%, and the chemical composition of the catalyst was expressed as "xM·ySiO2·zAl2O3", where x / y=0.0041 and y / z=10. The properties of the obtained catalyst are shown in Table I-13.

[0161] The SEM of the catalyst is similar to that in Figure 3. In this catalyst, the crystals were long bands with crystal lengths ranging from 0.4 to 1.5 μm and aspect ratios ranging from 2 to 10.

[0162] [Table 6]

[0163] (Preparation example I-3) 4 g of deionized water, 0.75 g of 4-pyrrolidinylpyridine, 0.42 g of aluminum isopropoxide, 1.5 g of silica sol, and 0.5 g of hydrofluoric acid were mixed uniformly to obtain a solution of 1SiO2:0.1Al2O3:1F - A component having a composition of :29H2O:0.5OSDA was obtained. After that, it was pretreated by heating in the open at 80°C to obtain a block mixture. After the raw material mixture was pretreated by heating, the molar ratio of silicon source (calculated as SiO2) to water during crystallization was set to 1:5, and it was crystallized in a crystallization kettle at 170°C for 15 days. After the product was taken out, it was washed three times with deionized water, dried, and then calcined at 550°C for 6 hours to obtain the desired H-type silica-alumina molecular sieve (ATS structure).

[0164] 6 mL of 3.2 g / L ruthenium chloride solution was added dropwise onto 1 g of H-type silica-alumina molecular sieve. After drying at 80°C for 2 hours, the catalyst was reduced in a fixed bed reactor at 350°C with a hydrogen flow rate of 10 mL / min for 3 hours to obtain the required catalyst.

[0165] The XRD spectrum data of the catalyst is shown in Table I-3. The XRD spectrum of the catalyst was the same as that in Figure 1. In the composition of the catalyst, n(SiO2):n(Al2O3)=10, the mass fraction of Ru was 1.5%, and the chemical composition of the catalyst was expressed as "xM·ySiO2·zAl2O3", where x / y=0.0104 and y / z=10. The properties of the obtained catalyst are shown in Table I-13.

[0166] SEM of the catalyst was similar to that in Figure 3. In this catalyst, the crystals were long bands with crystal lengths ranging from 0.4 to 1.5 μm and aspect ratios ranging from 2 to 10.

[0167] [Table 7]

[0168] (Preparation example I-4) 4 g of deionized water, 1.1 g of 4-pyrrolidinylpyridine, 0.42 g of aluminum isopropoxide, 1.5 g of silica sol, and 0.75 g of hydrofluoric acid were mixed uniformly to obtain a solution of 1SiO2:0.1Al2O3:1.5F - A component with a composition of :29H2O:0.75OSDA was obtained. Pretreatment was performed by heating in the open at 80°C to obtain a block mixture. After pretreatment by heating the raw material mixture, the molar ratio of silicon source (calculated as SiO2) to water during crystallization was set to 1:4.5, and crystallization was performed in a crystallization kettle at 170°C for 15 days. After the product was taken out, it was washed three times with deionized water, dried, and then calcined at 550°C for 6 hours to obtain the desired H-type silica-alumina molecular sieve (ATS structure).

[0169] On top of 1 g of H-type silica-alumina molecular sieve, 1.2 mL of 3.2 g / L ruthenium chloride solution was added dropwise. After drying at 80° C. for 2 h, it was reduced in a fixed-bed reactor at 350° C. with a hydrogen flow rate of 10 mL / min for 3 h to obtain the required catalyst.

[0170] The XRD spectrum data of the catalyst is shown in Table I-4. The XRD spectrum of the catalyst was the same as that in Figure 1. In the composition of the catalyst, n(SiO2):n(Al2O3)=10, the mass fraction of Ru was 0.3%, and the chemical composition of the catalyst was expressed as "xM·ySiO2·zAl2O3", where x / y=0.0021, y / z=10. The properties of the obtained catalyst are shown in Table I-13.

[0171] SEM of the catalyst is similar to that in Figure 3. In this catalyst, the crystals were long bands with crystal lengths ranging from 0.4 to 2.0 μm and aspect ratios ranging from 2 to 15.

[0172] [Table 8]

[0173] (Preparation example I-5) 4 g of deionized water, 1.5 g of 4-pyrrolidinylpyridine, 0.42 g of aluminum isopropoxide, 1.5 g of silica sol, and 1 g of hydrofluoric acid were mixed uniformly to obtain a solution of 1SiO2:0.1Al2O3:2F - A component with a composition of :30H2O:1OSDA was obtained. Pretreatment was performed by open heating at 80°C to obtain a block mixture. After pretreatment by heating the raw material mixture, the molar ratio of silicon source (calculated as SiO2) to water during crystallization was set to 1:4.5, and crystallization was performed in a crystallization kettle at 170°C for 15 days. After the product was taken out, it was washed three times with deionized water, dried, and then calcined at 550°C for 6 hours to obtain the desired H-type silica-alumina molecular sieve (ATS structure).

[0174] On top of 1 g of H-type silica-alumina molecular sieve, 1.2 mL of 3.2 g / L ruthenium chloride solution was added dropwise. After drying at 80° C. for 2 h, it was reduced in a fixed-bed reactor at 350° C. with a hydrogen flow rate of 10 mL / min for 3 h to obtain the required catalyst.

[0175] The XRD spectrum data of the catalyst is shown in Table I-5. The XRD spectrum of the catalyst was the same as that in Figure 1. In the composition of the catalyst, n(SiO2):n(Al2O3)=10, the mass fraction of Ru was 0.3%, and the chemical composition of the catalyst was expressed as "xM·ySiO2·zAl2O3", where x / y=0.0021, y / z=10. The properties of the obtained catalyst are shown in Table I-13.

[0176] SEM of the catalyst was similar to that in Figure 3. In this catalyst, the crystals were long bands with crystal lengths ranging from 0.5 to 2.5 μm and aspect ratios ranging from 3 to 20.

[0177] [Table 9]

[0178] (Preparation example I-6) 4 g of deionized water, 0.75 g of 4-pyrrolidinylpyridine, 0.42 g of aluminum isopropoxide, 1.5 g of silica sol, and 0.5 g of hydrofluoric acid were mixed uniformly to obtain a solution of 1SiO2:0.1Al2O3:1F - A component having a composition of :29H2O:0.5OSDA was obtained. After that, it was pretreated by heating in the open at 80°C to obtain a block mixture. After the raw material mixture was pretreated by heating, the molar ratio of silicon source (calculated as SiO2) to water during crystallization was set to 1:5, and it was crystallized in a crystallization kettle at 170°C for 15 days. After the product was taken out, it was washed three times with deionized water, dried, and then calcined at 550°C for 6 hours to obtain the desired H-type silica-alumina molecular sieve (ATS structure).

[0179] On top of 1 g of H-type silica-alumina molecular sieve, 1.2 mL of 2.7 g / L palladium chloride solution was added dropwise. After drying at 80° C. for 2 h, it was reduced in a fixed-bed reactor at 350° C. with a hydrogen flow rate of 10 mL / min for 3 h to obtain the required catalyst.

[0180] The XRD spectrum data of the catalyst is shown in Table I-6. The XRD spectrum of the catalyst was the same as that in Figure 1. In the composition of the catalyst, n(SiO2):n(Al2O3)=10, the mass fraction of Pd was 0.3%, and the chemical composition of the catalyst was expressed as "xM·ySiO2·zAl2O3", where x / y=0.0021, y / z=10. The properties of the obtained catalyst are shown in Table I-13.

[0181] SEM of the catalyst was similar to that in Figure 3. In this catalyst, the crystals were long bands with crystal lengths ranging from 0.4 to 1.5 μm and aspect ratios ranging from 2 to 10.

[0182] [Table 10]

[0183] (Preparation example I-7) 4 g of deionized water, 0.75 g of 4-pyrrolidinylpyridine, 0.21 g of aluminum isopropoxide, 1.5 g of silica sol, and 0.5 g of hydrofluoric acid were mixed uniformly to obtain a solution of 1SiO2:0.05Al2O3:1F - A component with a composition of :29H2O:0.5OSDA was obtained. Pretreatment was performed by open heating at 80°C to obtain a block mixture. After pretreatment by heating the raw material mixture, the molar ratio of silicon source (calculated as SiO2) to water during crystallization was set to 1:5, and crystallization was performed in a crystallization kettle at 170°C for 15 days. After the product was taken out, it was washed three times with deionized water, dried, and then calcined at 550°C for 6 hours to obtain the desired H-type silica-alumina molecular sieve (ATS structure).

[0184] On top of 1 g of H-type silica-alumina molecular sieve, 1.2 mL of 3.2 g / L palladium chloride solution was added dropwise. After drying at 80° C. for 2 h, it was reduced in a fixed-bed reactor at 350° C. with a hydrogen flow rate of 10 mL / min for 3 h to obtain the required catalyst.

[0185] The XRD spectrum data of the catalyst is shown in Table I-7. The XRD spectrum of the catalyst was the same as that in Figure 1. In the composition of the catalyst, n(SiO2):n(Al2O3)=20, the mass fraction of Ru was 0.3%, and the chemical composition of the catalyst was expressed as "xM·ySiO2·zAl2O3", where x / y=0.0021, y / z=20. The properties of the obtained catalyst are shown in Table I-13.

[0186] SEM of the catalyst was similar to that in Figure 3. In this catalyst, the crystals were long bands with crystal lengths ranging from 0.4 to 1.5 μm and aspect ratios ranging from 2 to 12.

[0187] [Table 11]

[0188] (Preparation example I-8) 4 g of deionized water, 0.75 g of 4-pyrrolidinylpyridine, 0.08 g of aluminum isopropoxide, 1.5 g of silica sol, and 0.5 g of hydrofluoric acid were mixed uniformly to obtain a solution of 1SiO2:0.02Al2O3:1F - A component having a composition of :29H2O:0.5OSDA was obtained. After that, it was pretreated by heating in the open at 80°C to obtain a block mixture. After the raw material mixture was pretreated by heating, the molar ratio of silicon source (calculated as SiO2) to water during crystallization was set to 1:5, and it was crystallized in a crystallization kettle at 170°C for 15 days. After the product was taken out, it was washed three times with deionized water, dried, and then calcined at 550°C for 6 hours to obtain the desired H-type silica-alumina molecular sieve (ATS structure).

[0189] On top of 1 g of H-type silica-alumina molecular sieve, 1.2 mL of 3.2 g / L ruthenium chloride solution was added dropwise. After drying at 80° C. for 2 h, it was reduced in a fixed-bed reactor at 350° C. with a hydrogen flow rate of 10 mL / min for 3 h to obtain the required catalyst.

[0190] The XRD spectrum data of the catalyst is shown in Table I-8. The XRD spectrum of the catalyst was the same as that in Figure 1. In the composition of the catalyst, n(SiO2):n(Al2O3)=50, the mass fraction of Ru was 0.3%, and the chemical composition of the catalyst was expressed as "xM·ySiO2·zAl2O3", where x / y=0.0021, y / z=50. The properties of the obtained catalyst are shown in Table I-13.

[0191] SEM of the catalyst was similar to that in Figure 3. In this catalyst, the crystals were long bands with crystal lengths ranging from 0.4 to 1.5 μm and aspect ratios ranging from 2 to 12.

[0192] [Table 12]

[0193] (Preparation example I-9) 4 g of deionized water, 0.75 g of 4-pyrrolidinylpyridine, 0.42 g of aluminum isopropoxide, 1.5 g of silica sol, and 0.5 g of hydrofluoric acid were mixed uniformly to obtain a solution of 1SiO2:0.1Al2O3:1F - A component having a composition of :29H2O:0.5OSDA was obtained. After that, it was pretreated by heating in the open at 80°C to obtain a block mixture. After the raw material mixture was pretreated by heating, the molar ratio of silicon source (calculated as SiO2) to water during crystallization was set to 1:5, and it was crystallized in a crystallization kettle at 170°C for 15 days. After the product was taken out, it was washed three times with deionized water, dried, and then calcined at 550°C for 6 hours to obtain the desired H-type silica-alumina molecular sieve (ATS structure).

[0194] On 1g of H-type silica-alumina molecular sieve, 1.2mL of 3.2g / L ruthenium chloride solution was added dropwise. After drying at 80°C for 2 hours, it was reduced in a fixed bed reactor at 450°C with a hydrogen flow rate of 10mL / min for 3 hours to obtain a catalyst precursor. 0.3g of dimethyldimethoxysilane, 1g of catalyst precursor, and 20mL of ethanol solvent were mixed and refluxed at 75°C for 24 hours, after which water was added and centrifuged. After washing, it was dried at 80°C for 12 hours to obtain a catalyst. The properties of the obtained catalyst are shown in Table I-13.

[0195] The XRD spectrum data of the catalyst is shown in Table I-9. The XRD spectrum of the catalyst was similar to that in Figure 1. The SEM of the catalyst was similar to that in Figure 3. The crystals in the catalyst were long bands, with the crystal lengths ranging from 0.4 to 1.5 μm and the aspect ratios ranging from 2 to 10.

[0196] [Table 13]

[0197] (Preparation example I-10) 4 g of deionized water, 1.5 g of 4-pyrrolidinylpyridine, 0.42 g of aluminum isopropoxide, 1.5 g of silica sol, and 1 g of hydrofluoric acid were mixed uniformly to obtain a solution of 1SiO2:0.1Al2O3:2F - A component with a composition of :30H2O:1OSDA was obtained. Pretreatment was performed by open heating at 80°C to obtain a block mixture. After pretreatment by heating the raw material mixture, the molar ratio of silicon source (calculated as SiO2) to water during crystallization was set to 1:4.5, and crystallization was performed in a crystallization kettle at 170°C for 15 days. After the product was taken out, it was washed three times with deionized water, dried, and then calcined at 550°C for 6 hours to obtain the desired H-type silica-alumina molecular sieve (ATS structure).

[0198] On 1g of H-type silica-alumina molecular sieve, 2.5mL of 3.2g / L ruthenium chloride solution was added dropwise. After drying at 80°C for 2 hours, it was reduced in a fixed bed reactor at 450°C with a hydrogen flow rate of 10mL / min for 3 hours to obtain a catalyst precursor. 0.3g of phenyltrimethoxysilane, 1g of catalyst precursor, and 20mL of ethanol solvent were mixed and refluxed at 75°C for 24 hours, then water was added and centrifuged. After washing, it was dried at 80°C for 12 hours to obtain a catalyst. The properties of the obtained catalyst are shown in Table I-13.

[0199] The XRD spectrum data of the catalyst is shown in Table I-10. The XRD spectrum of the catalyst was similar to that in Figure 1. The SEM of the catalyst was similar to that in Figure 3. The crystals in the catalyst were long bands, with the crystal lengths ranging from 0.5 to 2.5 μm and the aspect ratios ranging from 3 to 20.

[0200] [Table 14]

[0201] (Preparation example I-11) 4 g of deionized water, 0.75 g of 4-pyrrolidinylpyridine, 0.42 g of aluminum isopropoxide, 1.5 g of silica sol, and 0.5 g of hydrofluoric acid were mixed uniformly to obtain a solution of 1SiO2:0.1Al2O3:1F - A component having a composition of :29H2O:0.5OSDA was obtained. After that, it was pretreated by heating in the open at 80°C to obtain a block mixture. After the raw material mixture was pretreated by heating, the molar ratio of silicon source (calculated as SiO2) to water during crystallization was set to 1:5, and it was crystallized in a crystallization kettle at 170°C for 15 days. After the product was taken out, it was washed three times with deionized water, dried, and then calcined at 550°C for 6 hours to obtain the desired H-type silica-alumina molecular sieve (ATS structure).

[0202] On 1g of H-type silica-alumina molecular sieve, 1.2mL of 2.7g / L palladium chloride solution was added dropwise. After drying at 80°C for 2 hours, it was reduced in a fixed bed reactor at 450°C with a hydrogen flow rate of 10mL / min for 3 hours to obtain a catalyst precursor. 0.3g of phenyltrimethoxysilane, 1g of catalyst precursor, and 20mL of ethanol solvent were mixed, refluxed at 75°C for 24 hours, centrifuged with water, washed, and dried at 80°C for 12 hours to obtain a catalyst. The properties of the obtained catalyst are shown in Table I-13.

[0203] The XRD spectrum data of the catalyst is shown in Table I-11. The XRD spectrum of the catalyst was similar to that in Figure 1. The SEM of the catalyst was similar to that in Figure 3. The crystals in the catalyst were long bands, with the crystal lengths ranging from 0.4 to 1.5 μm and the aspect ratios ranging from 2 to 10.

[0204] [Table 15]

[0205] (Preparation example I-12) 4 g of deionized water, 0.75 g of 4-pyrrolidinylpyridine, 0.21 g of aluminum isopropoxide, 1.5 g of silica sol, and 0.5 g of hydrofluoric acid were mixed uniformly to obtain a solution of 1SiO2:0.05Al2O3:1F - A component having a composition of :29H2O:0.5OSDA was obtained. After that, it was pretreated by heating in the open at 80°C to obtain a block mixture. After the raw material mixture was pretreated by heating, the molar ratio of silicon source (calculated as SiO2) to water during crystallization was set to 1:5, and it was crystallized in a crystallization kettle at 170°C for 15 days. After the product was taken out, it was washed three times with deionized water, dried, and then calcined at 550°C for 6 hours to obtain the desired H-type silica-alumina molecular sieve (ATS structure).

[0206] On 1g of H-type silica-alumina molecular sieve, 1.2mL of 3.2g / L ruthenium chloride solution was added dropwise. After drying at 80°C for 2 hours, the mixture was reduced in a fixed-bed reactor at 450°C with a hydrogen flow rate of 10mL / min for 3 hours to obtain a catalyst precursor. 0.3g of phenyltrimethoxysilane, 1g of catalyst precursor, and 20mL of ethanol solvent were mixed and refluxed at 75°C for 24 hours, after which water was added and centrifuged. After washing, the mixture was dried at 80°C for 12 hours to obtain a catalyst. The properties of the obtained catalyst are shown in Table I-13.

[0207] The XRD spectrum data of the catalyst is shown in Table I-12. The XRD spectrum of the catalyst was similar to that in Figure 1. The SEM of the catalyst was similar to that in Figure 3. The crystals in the catalyst were long bands, with the crystal lengths ranging from 0.4 to 1.5 μm and the aspect ratios ranging from 2 to 12.

[0208] [Table 16]

[0209] (Example I-1) 0.25g of the catalyst synthesized in Preparation Example I-1 was added to a high-pressure reactor, then 8g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.2MPa. The temperature of the system was then raised to 150°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table I-14.

[0210] (Example I-2) 0.25g of the catalyst synthesized in Preparation Example I-1 was added to a high-pressure reactor, then 8g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.6MPa. The temperature of the system was then raised to 150°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table I-14.

[0211] (Example I-3) 0.25g of the catalyst synthesized in Preparation Example I-1 was added to a high-pressure reactor, then 8g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 2.0MPa. The temperature in the system was then raised to 150°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table I-14.

[0212] (Example I-4) 0.25g of the catalyst synthesized in Preparation Example I-1 was added to a high-pressure reactor, then 8g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.2MPa. The temperature of the system was then raised to 180°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table I-14.

[0213] (Example I-5) 0.25g of the catalyst synthesized in Preparation Example I-1 was added to a high-pressure reactor, then 8g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.2MPa. The temperature of the system was then raised to 200°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table I-14.

[0214] (Example I-6) 0.25g of the catalyst synthesized in Preparation Example I-2 was added to a high-pressure reactor, then 8g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.2MPa. The temperature of the system was then raised to 150°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table I-14.

[0215] (Example I-7) 0.25g of the catalyst synthesized in Preparation Example I-3 was added to a high-pressure reactor, then 8g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.2MPa. The temperature in the system was then raised to 150°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table I-14.

[0216] (Example I-8) 0.25g of the catalyst synthesized in Preparation Example I-4 was added to a high-pressure reactor, then 8g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.2MPa. The temperature of the system was then raised to 150°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table I-14.

[0217] (Example I-9) 0.25g of the catalyst synthesized in Preparation Example I-5 was added to a high-pressure reactor, then 8g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.2MPa. The temperature of the system was then raised to 150°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table I-14.

[0218] (Example I-10) 0.25g of the catalyst synthesized in Preparation Example I-6 was added to a high-pressure reactor, then 8g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.2MPa. The temperature of the system was then raised to 150°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table I-14.

[0219] (Example I-11) 0.25g of the catalyst synthesized in Preparation Example I-7 was added to a high-pressure reactor, then 8g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.2MPa. The temperature of the system was then raised to 150°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table I-14.

[0220] (Example I-12) 0.25g of the catalyst synthesized in Preparation Example I-9 was added to a high-pressure reactor, then 8g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.2MPa. The temperature in the system was then raised to 150°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table I-14.

[0221] (Example I-13) 0.25g of the catalyst synthesized in Preparation Example I-9 was added to a high-pressure reactor, then 8g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.6MPa. The temperature in the system was then raised to 150°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table I-14.

[0222] (Example I-14) 0.25g of the catalyst synthesized in Preparation Example I-9 was added to a high-pressure reactor, then 8g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 2.0MPa. The temperature in the system was then raised to 150°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table I-14.

[0223] (Example I-15) 0.25g of the catalyst synthesized in Preparation Example I-9 was added to a high-pressure reactor, then 8g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.2MPa. The temperature of the system was then raised to 180°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table I-14.

[0224] (Example I-16) 0.25g of the catalyst synthesized in Preparation Example I-9 was added to a high-pressure reactor, then 8g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.2MPa. The temperature in the system was then raised to 200°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table I-14.

[0225] (Example I-17) 0.25g of the catalyst synthesized in Preparation Example I-10 was added to a high-pressure reactor, then 8g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.2MPa. The temperature of the system was then raised to 150°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table I-14.

[0226] (Example I-18) 0.25g of the catalyst synthesized in Preparation Example I-11 was added to a high-pressure reactor, then 8g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.2MPa. The temperature of the system was then raised to 150°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table I-14.

[0227] (Example I-19) 0.25g of the catalyst synthesized in Preparation Example I-12 was added to a high-pressure reactor, then 8g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.2MPa. The temperature of the system was then raised to 150°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table I-14.

[0228] [Table 17]

[0229] [Table 18]

[0230] (Comparative example I-1) <1. Preparation of catalyst> A catalyst was prepared with reference to Preparation Example I-1, except that the H-type silica-alumina molecular sieve was changed to an H-type Y molecular sieve (FAU structure) with n(Si):n(Al)=10.

[0231] Onto 1 g of the above molecular sieve, 1.2 mL of 3.2 g / L ruthenium chloride solution was added dropwise. After drying at 80° C. for 2 hours, it was reduced in a fixed bed reactor at 350° C. with a hydrogen flow rate of 10 mL / min for 3 hours to obtain the required catalyst.

[0232] 2. Catalyst evaluation The catalyst evaluation method is as shown in Example I-1. The catalyst composition and evaluation results are shown in Table I-15.

[0233] (Comparative example I-2) 1. Catalyst Preparation A catalyst was prepared with reference to Preparation Example I-1, except that the H-type silica-alumina molecular sieve was changed to an H-type Y molecular sieve (FAU structure) with n(Si):n(Al)=20.

[0234] Onto 1 g of the above molecular sieve, 1.2 mL of 3.2 g / L ruthenium chloride solution was added dropwise. After drying at 80° C. for 2 hours, it was reduced in a fixed bed reactor at 350° C. with a hydrogen flow rate of 10 mL / min for 3 hours to obtain the required catalyst.

[0235] 2. Catalyst evaluation: The catalyst evaluation method is shown in Example I-1. The catalyst composition and evaluation results are shown in Table I-15.

[0236] (Comparative example I-3) 1. Catalyst Preparation A catalyst was prepared by referring to Preparation Example I-1, except that the H-type silica-alumina molecular sieve was changed to an H-type MCM-22 molecular sieve (MWW structure) with n(Si):n(Al)=20.

[0237] Onto 1 g of the above molecular sieve, 1.2 mL of 3.2 g / L ruthenium chloride solution was added dropwise. After drying at 80° C. for 2 hours, it was reduced in a fixed bed reactor at 350° C. with a hydrogen flow rate of 10 mL / min for 3 hours to obtain the required catalyst.

[0238] 2. Catalyst evaluation: The catalyst evaluation method is shown in Example I-1. The catalyst composition and evaluation results are shown in Table I-15.

[0239] (Comparative example I-4) 1. Catalyst Preparation A catalyst was prepared by referring to Preparation Example I-1, except that the H-type silica-alumina molecular sieve was changed to an H-type MCM-22 molecular sieve (MWW structure) with n(Si):n(Al)=30.

[0240] 1.2 mL of 3.2 g / L ruthenium chloride solution was added dropwise onto 1 g of the above molecular sieve. After drying at 80° C. for 2 hours, it was reduced in a fixed bed reactor at 350° C. with a hydrogen flow rate of 10 mL / min for 3 hours to obtain the required catalyst.

[0241] 2. Catalyst evaluation: The catalyst evaluation method is shown in Example I-1. The catalyst composition and evaluation results are shown in Table I-15.

[0242] [Table 19]

[0243] (Example I-20) The catalyst prepared in Preparation Example I-1 was washed and dried six times in total, and then used in the next reaction. The reaction conditions in Example I-1 were used for the evaluation of the catalyst. That is, 8 g of benzene was added to the high-pressure reactor, and hydrogen was added to adjust the pressure in the system to 1.2 MPa. The temperature of the system was then raised to 150°C, and the reaction was terminated after 4 hours. The evaluation results of the catalyst are shown in Table I-16.

[0244] [Table 20]

[0245] (Example I-21) The catalyst prepared in Preparation Example I-9 was washed and dried six times in total, and then used in the next reaction. The reaction conditions in Example I-12 were used for the evaluation of the catalyst. That is, 8 g of benzene was added to the high-pressure reactor, and hydrogen was added to adjust the pressure in the system to 1.2 MPa. The temperature of the system was then raised to 150°C, and the reaction was terminated after 4 hours. The catalyst evaluation results are shown in Table I-17.

[0246] [Table 21]

[0247] (Preparation Example II-1) A Na-type MCM-22 molecular sieve (MWW structure) with a silicon to aluminum molar ratio of 25:1 was subjected to ammonium ion exchange with a 0.2 mol / L NH4NO3 solution (mass ratio 1:20) at 45°C for 2 hours, followed by centrifugation and washing. The ammonium ion exchange was repeated twice, and the obtained sample was dried at 100°C overnight and calcined in air at 550°C for 6 hours to obtain an H-type silica-alumina molecular sieve.

[0248] 1.5mL of 3.2g / L ruthenium chloride solution (solution concentration is based on ruthenium element, same below) was added dropwise onto 1g of H-type silica-alumina molecular sieve. After that, it was dried at 80℃ for 2 hours to obtain ruthenium-supported molecular sieve. When H2-TPR test was performed on this ruthenium-supported molecular sieve, the reduction temperature was 451℃.

[0249] 0.2g of methyltrimethoxysilane, the ruthenium-supported molecular sieve, and 10mL of toluene solvent were mixed and refluxed at 110°C for 24 hours, followed by addition of water, centrifugation, washing, and drying at 80°C for 12 hours to obtain a hydrocarbyl molecular sieve. When the obtained hydrocarbyl molecular sieve was subjected to an H2-TPR test, the reduction temperature was 476°C. This result indicates that the active metal M supported on the hydrocarbyl molecular sieve is mainly distributed in the channels of the molecular sieve.

[0250] The hydrocarbyl molecular sieve was then subjected to a fixed-bed reactor at 450°C and a hydrogen volumetric space velocity of 50 h -1 The catalyst was then reduced at 40° C. for 3 hours to obtain the desired catalyst.

[0251] The XRD spectrum of the obtained catalyst is shown in Figure 4. XRD shows that the catalyst as a whole retains the MWW molecular sieve structure. The infrared absorption spectrum of the obtained catalyst is shown in Figure 5. Wave number 2950 cm -1It can be seen that a Si-C absorption peak appears near the peak. The hydrocarbyl was determined to be methyl by the TG-MS test, and its content is shown in Table II-1. The specific surface area, pore volume, acid properties (including total acid content and outer surface acid equivalent), metal M content, and metal M content on the outer surface of the catalyst are shown in Table II-1.

[0252] (Preparation Example II-2) A Na-type MCM-22 molecular sieve (MWW structure) with a silicon to aluminum molar ratio of 25:1 was subjected to ammonium ion exchange with a 0.2 mol / L NH4NO3 solution (mass ratio 1:20) at 45°C for 2 hours, then centrifuged and washed. The sample obtained by repeating the ammonium ion exchange twice was dried at 100°C overnight and calcined in air at 550°C for 6 hours to obtain an H-type silica-alumina molecular sieve.

[0253] 1.5 mL of 3.2 g / L ruthenium chloride solution was added dropwise onto 1 g of H-type silica-alumina molecular sieve. It was then dried at 80 °C for 2 h and then cooled to 450 °C in a fixed-bed reactor at a hydrogen volumetric space velocity of 50 h -1 The catalyst precursor was obtained by reducing the catalyst at 100°C for 3 hours. 0.3 g of dimethyldimethoxysilane, 1 g of catalyst precursor, and 15 mL of toluene solvent were mixed and refluxed at 110°C for 24 hours, after which water was added and centrifuged. After washing, the catalyst was obtained by drying at 80°C for 12 hours.

[0254] The XRD spectrum of the obtained catalyst is the same as that in Figure 1. The specific surface area, pore volume, acid properties (including total acid content and outer surface acid content), metal M content and metal M content on the outer surface of the catalyst are as shown in II-1.

[0255] (Preparation Example II-3) A Na-type Y molecular sieve (FAU structure) with a silicon to aluminum molar ratio of 10:1 was subjected to ammonium ion exchange with a 0.2 mol / L NH4NO3 solution (mass ratio 1:20) at 45°C for 2 hours, then centrifuged and washed. The sample obtained by repeating the ammonium ion exchange twice was dried at 100°C overnight and calcined in air at 550°C for 6 hours to obtain an H-type silica alumina molecular sieve.

[0256] 2.5 mL of 3.2 g / L ruthenium chloride solution was added dropwise onto 1 g of H-type silica-alumina molecular sieve. After drying at 80 °C for 2 h, it was then subjected to a fixed-bed reactor at 450 °C and a hydrogen volumetric space velocity of 100 h -1 The catalyst precursor was obtained by reducing the catalyst at 100°C for 3 hours. 0.3 g of ethyltrimethoxysilane, 1 g of the catalyst precursor, and 15 mL of toluene solvent were mixed and refluxed at 110°C for 24 hours, after which water was added and centrifuged. After washing, the catalyst was obtained by drying at 80°C for 12 hours.

[0257] The XRD spectrum of the obtained catalyst is shown in Figure 6. The catalyst as a whole retains the FAU molecular sieve structure. The specific surface area, pore volume, acid properties (including total acid content and outer surface acid equivalent), metal M content and metal M content on the outer surface of the catalyst are as shown in Table II-1.

[0258] (Preparation Example II-4) A Na-type Y molecular sieve (FAU structure) with a silicon to aluminum molar ratio of 5:1 was subjected to ammonium ion exchange with a 0.2 mol / L NH4NO3 solution (mass ratio 1:20) at 45°C for 2 hours, then centrifuged and washed. The sample obtained by repeating the ammonium ion exchange twice was dried at 100°C overnight and calcined in air at 550°C for 6 hours to obtain an H-type silica-alumina molecular sieve.

[0259] 1.5 mL of 2.6 g / L palladium chloride solution (solution concentration is based on palladium element, same below) was added dropwise onto 1 g of H-type silica-alumina molecular sieve. After drying at 80 °C for 2 hours, it was stirred in a fixed bed reactor at 450 °C and hydrogen volumetric space velocity of 100 h -1The catalyst precursor was obtained by reducing the catalyst at 100°C for 3 hours. 0.2 g of isopropyltrimethoxysilane, 1 g of the catalyst precursor, and 10 mL of toluene solvent were mixed and refluxed at 110°C for 24 hours, followed by addition of water, centrifuging, washing, and drying at 80°C for 12 hours to obtain the catalyst.

[0260] X-ray diffraction shows that the catalyst as a whole retains the FAU molecular sieve structure. The specific surface area, pore volume, acid properties (including total acid content and outer surface acid equivalent), metal M content and metal M content on the outer surface of the catalyst are as shown in Table II-1.

[0261] (Preparation Example II-5) A Na-type Y molecular sieve (FAU structure) with a silicon to aluminum molar ratio of 5:1 was subjected to ammonium ion exchange with a 0.2 mol / L NH4NO3 solution (mass ratio 1:20) at 45°C for 2 hours, then centrifuged and washed. The ammonium ion exchange was repeated twice, and the obtained sample was dried at 100°C overnight and calcined in air at 550°C for 6 hours to obtain an H-type silica-alumina molecular sieve.

[0262] 1.5 mL of nickel nitrate (6.0 g / L)-copper nitrate (3.0 g / L) mixed solution (solution concentration depends on metal element, same below) was added dropwise onto 1 g of H-type silica-alumina molecular sieve. After drying at 80 °C for 2 hours, it was heated at 450 °C in a fixed bed reactor with a hydrogen volumetric space velocity of 100 h -1 The catalyst precursor was obtained by reducing the catalyst at 100°C for 3 hours. 0.2 g of isopropyltrimethoxysilane, 1 g of the catalyst precursor, and 10 mL of toluene solvent were mixed and refluxed at 110°C for 24 hours, followed by addition of water, centrifuging, washing, and drying at 80°C for 12 hours to obtain the catalyst.

[0263] X-ray diffraction shows that the catalyst as a whole retains the FAU molecular sieve structure. The specific surface area, pore volume, acidic properties (including total acid content and outer surface acid equivalent), metal M content and metal M content on the outer surface of the catalyst are as shown in Table II-1.

[0264] (Preparation Example II-6) 4 g of deionized water, 0.75 g of 4-pyrrolidinylpyridine, 0.42 g of aluminum isopropoxide, 1.5 g of silica sol, and 0.5 g of hydrofluoric acid were mixed uniformly to obtain a solution of 1SiO2:0.1Al2O3:1F - After obtaining the components with the composition of :29H2O:0.5OSDA, they were pretreated by heating in the open at 80°C to obtain a block mixture. After the raw material mixture was pretreated by heating, the molar ratio of silicon source (calculated as SiO2) to water during crystallization was set to 1:5, and crystallization was carried out in a crystallization kettle at 170°C for 15 days. After taking out the product, it was washed three times with deionized water, dried, and calcined at 550°C for 6 hours to obtain H-type silica-alumina molecular sieve (ATS structure).

[0265] 1.5 mL of 3.2 g / L ruthenium chloride solution was added dropwise onto 1 g of H-type ATS molecular sieve. After drying at 80 °C for 2 h, the mixture was heated at 450 °C in a fixed bed reactor at a hydrogen volumetric space velocity of 50 h -1 The catalyst precursor was obtained by reducing the catalyst at 100°C for 3 hours. 0.2 g of isopropyltrimethoxysilane, 1 g of the catalyst precursor, and 10 mL of toluene solvent were mixed and refluxed at 110°C for 24 hours, after which water was added and centrifuged. After washing, the catalyst was obtained by drying at 80°C for 12 hours.

[0266] X-ray diffraction shows that the catalyst as a whole retains the ATS molecular sieve structure. The specific surface area, pore volume, acid properties (including total acid content and outer surface acid equivalent), metal M content and metal M content on the outer surface of the catalyst are shown in Table II-1.

[0267] (Preparation Example II-7) The catalyst was prepared by referring to Preparation Example II-1, except that the raw material was changed to Na-type MCM-22 molecular sieve with a silicon-aluminum molar ratio of 50:1, and the remaining steps were not changed. The catalyst properties are shown in Table II-1.

[0268] The XRD spectrum of the obtained catalyst is the same as that in Figure 1. The specific surface area, pore volume, acid properties (including the total acid content and the acid content on the outer surface), metal M content and metal M content on the outer surface of the catalyst are shown in Table II-1.

[0269] (Examples II-1 to II-4) 0.25g of the catalyst synthesized in Preparation Example II-1 was added to a high-pressure reactor, then 8g of benzene was added to the reactor, and hydrogen was added. The reaction was terminated after 4 hours. The specific evaluation conditions and evaluation data are shown in Table II-2.

[0270] (Example II-5) 0.25g of the catalyst synthesized in Preparation Example II-2 was added to a high-pressure reactor, then 8g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.2MPa. The temperature of the system was then raised to 150°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table 2.

[0271] (Example II-6) 0.25g of the catalyst synthesized in Preparation Example II-3 was added to a high-pressure reactor, then 8g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.2MPa. The temperature of the system was then raised to 150°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table II-2.

[0272] (Example II-7) 0.25g of the catalyst synthesized in Preparation Example II-4 was added to a high-pressure reactor, then 8g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.2MPa. The temperature of the system was then raised to 150°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table II-2.

[0273] (Example II-8) 0.25g of the catalyst synthesized in Preparation Example II-5 was added to a high-pressure reactor, then 8g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.2MPa. The temperature of the system was then raised to 150°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table II-2.

[0274] (Example II-9) 0.25g of the catalyst synthesized in Preparation Example II-6 was added to a high-pressure reactor, then 8g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.2MPa. The temperature of the system was then raised to 150°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table II-2.

[0275] (Example II-10) 0.25g of the catalyst synthesized in Preparation Example II-7 was added to a high-pressure reactor, then 8g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.2MPa. The temperature of the system was then raised to 150°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table II-2.

[0276] (Comparative Example II-1) <1. Preparation of catalyst> A catalyst was prepared by referring to Preparation Example II-1, except that the methyltrimethoxysilane treatment step was omitted. The properties of the obtained catalyst are shown in Table II-1.

[0277] 2. Catalyst evaluation The catalyst evaluation method is as shown in Example II-5. The catalyst evaluation results are shown in Table II-2.

[0278] (Comparative Example II-2) <1. Preparation of catalyst> The catalyst was prepared by referring to Preparation Example II-1, except that the amount of the ruthenium chloride solution of the same concentration was increased to 8 mL, that is, only the metal content in the catalyst was increased. The properties of the catalyst are shown in Table II-1.

[0279] 2. Catalyst evaluation The catalyst evaluation method was the same as in Example II-5, and the catalyst evaluation results are shown in Table II-2.

[0280] (Comparative Example II-3) <1. Preparation of catalyst> The catalyst was prepared according to Preparation Example II-2, except that the amount of dimethyldimethoxysilane added was increased from 0.3 g to 1.0 g. The remaining steps were not changed. The catalyst properties are shown in Table II-1.

[0281] 2. Catalyst evaluation The catalyst evaluation method was the same as in Example II-5, and the catalyst evaluation results are shown in Table II-2.

[0282] (Comparative Example II-4) The catalyst obtained in Preparation Example II-1 was evaluated according to the method of Preparation Example II-5, except that the hydrogen partial pressure of the reaction conditions was changed to 4.0 MPa, and the remaining steps were not changed. The evaluation results of the catalyst are shown in Table II-2.

[0283] [Table 22]

[0284] [Table 23]

[0285] (Example II-10) The catalyst prepared in Preparation Example II-1 was washed and dried before being put into the next reaction, and cycled a total of six times. The catalyst evaluation included adding 8g of benzene to the high-pressure reactor and charging hydrogen to make the internal pressure of the system 1.2MPa. Then, the temperature of the system was raised to 150°C, and the reaction was terminated after 4 hours. The catalyst evaluation results are shown in Table II-3.

[0286] [Table 24]

[0287] (Preparation Example III-1) (1) Preparation of H-type MWW molecular sieves MCM-22 molecular sieve (MWW structure) with a silicon to aluminum molar ratio of 20:1 was subjected to ammonium ion exchange with 0.2 mol / L NH4NO3 solution (mass ratio 1:20) at 45°C for 2 hours, and then centrifuged and washed. The sample obtained by repeating the ammonium ion exchange twice was dried at 100°C overnight and calcined in air at 550°C for 6 hours to obtain H-type silica alumina molecular sieve.

[0288] (2) Preparation of catalyst 0.5 mL of 8 g / L ruthenium chloride solution was added dropwise onto 1 g of H-type silica-alumina molecular sieve with a silicon-aluminum ratio of 20:1. After drying at 80 °C for 2 hours, the mixture was stirred in a fixed-bed reactor at 500 °C and hydrogen volumetric space velocity of 80 h -1 The catalyst precursor was obtained by reducing the catalyst at 40°C for 2 hours. 0.3 g of phenyltrimethoxysilane, 1 g of the catalyst precursor, and 20 mL of ethanol solvent were mixed and refluxed at 75°C for 24 hours, followed by addition of water, centrifuging, washing, and drying at 80°C for 12 hours to obtain the catalyst.

[0289] The XRD spectrum of the obtained catalyst is shown in Figure 7. The catalyst as a whole retains the MWW molecular sieve structure. The specific surface area, pore volume, acidity (including total acid content and outer surface acid equivalent), metal M content and metal M content on the outer surface of the catalyst are shown in Table III-1.

[0290] (Preparation Example III-2) (1) Preparation of H-type MWW molecular sieves The preparation process was the same as in Preparation Example III-1, except that Na-type MCM-22 molecular sieve with a silicon-aluminum molar ratio of 25:1 was used.

[0291] (2) Preparation of catalyst 1 mL of 8 g / L ruthenium chloride solution was added dropwise onto 1 g of H-type silica-alumina molecular sieve with a silicon-aluminum ratio of 25:1. After drying at 80 °C for 2 hours, the mixture was stirred in a fixed-bed reactor at 500 °C and hydrogen volumetric space velocity of 80 h -1The catalyst precursor was obtained by reducing the catalyst at 40°C for 3 hours. 0.2 g of tolyltrimethoxysilane, 1 g of the catalyst precursor, and 20 ml of toluene solvent were mixed and refluxed at 110°C for 24 hours, followed by addition of water, centrifuging, washing, and drying at 80°C for 12 hours to obtain the catalyst.

[0292] The XRD spectrum of the obtained catalyst is the same as that in Figure 7. The specific surface area, pore volume, acid properties (including total acid amount and outer surface acid amount), metal M content and metal M content on the outer surface of the catalyst are as shown in Table III-1.

[0293] (Preparation Example III-3) (1) Preparation of H-type MOR molecular sieves The preparation process was the same as in Preparation Example III-1, except that Na-type mordenite (MOR structure) with a silicon-aluminum molar ratio of 10:1 was used.

[0294] (2) Preparation of catalyst 0.5 mL of 8 g / L ruthenium chloride solution was added dropwise onto 1 g of H-type MOR molecular sieve with a silicon to aluminum ratio of 10:1. After drying at 80 °C for 2 h, the mixture was heated at 500 °C in a fixed bed reactor at a hydrogen volumetric space velocity of 150 h -1 The catalyst precursor was obtained by reducing the catalyst at 40°C for 3 hours. 0.3 g of phenylsilanetriol, 1 g of the catalyst precursor, and 30 mL of toluene solvent were mixed and refluxed at 110°C for 24 hours, and then water was added, centrifuged, washed, and dried at 80°C for 12 hours to obtain the catalyst.

[0295] The catalyst thus obtained retained the MOR molecular sieve structure as a whole. The specific surface area, pore volume, acidity (including total acid content and outer surface acid equivalent), metal M content and metal M content on the outer surface of the catalyst are shown in Table III-1.

[0296] (Preparation Example III-4) (1) Preparation of H-type MOR molecular sieves The preparation process was the same as in Preparation Example III-1, except that Na-type mordenite (MOR structure) with a silicon-aluminum molar ratio of 15:1 was used.

[0297] (2) Preparation of catalyst 0.5 mL of 8 g / L palladium chloride solution was added dropwise onto 1 g of H-type MOR molecular sieve with a silicon to aluminum ratio of 15:1. After drying at 80 °C for 2 h, the mixture was heated at 500 °C in a fixed-bed reactor at a hydrogen volumetric space velocity of 80 h -1 The catalyst precursor was obtained by reducing the catalyst at 40°C for 3 hours. 0.2 g of diphenylsilanediol, 1 g of catalyst precursor, and 20 mL of ethanol solvent were mixed and refluxed at 75°C for 24 hours, after which water was added and centrifuged. After washing, the catalyst was obtained by drying at 80°C for 12 hours.

[0298] The catalyst thus obtained retained the MOR molecular sieve structure as a whole. The specific surface area, pore volume, acidity (including total acid content and outer surface acid equivalent), metal M content and metal M content on the outer surface of the catalyst are shown in Table III-1.

[0299] (Preparation Example III-5) 4 g of deionized water, 0.75 g of 4-pyrrolidinylpyridine, 0.42 g of aluminum isopropoxide, 1.5 g of silica sol, and 0.5 g of hydrofluoric acid were mixed uniformly to obtain a solution of 1SiO2:0.1Al2O3:1F - The composition of the components was obtained as follows: 29H2O:0.5OSDA. The mixture was then pretreated by heating in the open at 80°C to obtain a block mixture. After the raw material mixture was heated and pretreated, the molar ratio of silicon source (calculated as SiO2) to water during crystallization was set to 1:5, and the mixture was crystallized in a crystallization kettle at 170°C for 15 days. The product was taken out, washed three times with deionized water, dried, and then calcined at 550°C for 6 hours to obtain an H-type ATS molecular sieve.

[0300] 0.5 mL of 8 g / L ruthenium chloride solution was added dropwise onto 1 g of H-type ATS molecular sieve. After drying at 80 °C for 2 h, the mixture was heated at 500 °C in a fixed-bed reactor at a hydrogen volumetric space velocity of 80 h -1The catalyst precursor was obtained by reducing the catalyst at 0.2 g for 3 hours at 100 °C. 0.2 g of phenyltrimethoxysilane, 1 g of the catalyst precursor, and 10 mL of toluene solvent were mixed and refluxed at 110 °C for 24 hours, and then water was added, centrifuged, washed, and dried at 80 °C for 12 hours to obtain the catalyst.

[0301] The catalyst thus obtained retains the ATS molecular sieve structure as a whole. The specific surface area, pore volume, acidity (including total acid content and outer surface acid equivalent), metal M content and metal M content on the outer surface of the catalyst are shown in Table III-1.

[0302] (Preparation Example III-6) A catalyst was prepared by referring to Preparation Example III-1, without changing the process except that the raw material was changed to Na-type MCM-22 molecular sieve (MWW structure) with a silicon-aluminum molar ratio of 50:1.

[0303] The XRD spectrum of the obtained catalyst was the same as that in Figure 7. The specific surface area, pore volume, acid properties (including the total acid amount and the outer surface acid equivalent), metal M content and metal M content on the outer surface of the catalyst are as shown in Table III-1.

[0304] (Examples III-1 to III-3) 0.25g of the catalyst synthesized in Preparation Example III-1 was added to a high-pressure reactor, then 10g of benzene was added to the reactor, and hydrogen was added. The reaction was terminated after 4 hours. The specific evaluation conditions and evaluation data are shown in Table III-2.

[0305] (Example III-4) 0.25g of the catalyst synthesized in Preparation Example III-2 was added to a high-pressure reactor, then 10g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.0MPa. The temperature of the system was then raised to 180°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table III-2.

[0306] (Example III-5) 0.25g of the catalyst synthesized in Preparation Example III-3 was added to a high-pressure reactor, then 10g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.0MPa. The temperature of the system was then raised to 180°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table III-2.

[0307] (Example III-6) 0.25g of the catalyst synthesized in Preparation Example III-4 was added to a high-pressure reactor, then 10g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.0MPa. The temperature of the system was then raised to 180°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table III-2.

[0308] (Example III-7) 0.25g of the catalyst synthesized in Preparation Example III-5 was added to a high-pressure reactor, then 10g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.0MPa. The temperature of the system was then raised to 180°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table III-2.

[0309] (Example III-8) 0.25g of the catalyst synthesized in Preparation Example III-6 was added to a high-pressure reactor, then 10g of benzene was added to the reactor, and hydrogen was added to make the pressure in the system 1.0MPa. The temperature of the system was then raised to 180°C, and the reaction was terminated after 4 hours. The evaluation data are summarized in Table III-2.

[0310] (Comparative Example III-1) <1. Preparation of catalyst> A catalyst was prepared with reference to Preparation Example III-1, except that the treatment with phenyltrimethoxysilane was omitted.

[0311] 2. Catalyst evaluation The catalyst evaluation method was the same as in Example III-4, and the catalyst evaluation results are shown in Table III-2.

[0312] <Comparative example III-2> (1. Preparation of Catalyst) A catalyst was prepared with reference to Preparation Example III-1, except that the amount of the ruthenium chloride solution of the same concentration added was increased to 8 mL, that is, only the metal content in the catalyst was increased.

[0313] (2. Catalyst Evaluation) The catalyst evaluation method was the same as in Example III-4, and the catalyst evaluation results are shown in Table III-2.

[0314] (Comparative Example III-3) <1. Preparation of catalyst> A catalyst was prepared with reference to Preparation Example III-1, except that in the arylation step, the addition of "0.3 g of phenyltrimethoxysilane" was changed to the addition of "0.8 g of phenyltrimethoxysilane".

[0315] (2. Catalyst Evaluation) The catalyst evaluation method was the same as in Example III-4, and the catalyst evaluation results are shown in Table III-2.

[0316] (Comparative Example III-4) The catalyst obtained in Preparation Example III-1 was evaluated according to the method of Preparation Example III-4 without changing the operation except that the hydrogen partial pressure of the reaction conditions was changed to 4.0 MPa. The evaluation results of the catalyst are shown in Table III-2.

[0317] [Table 25]

[0318] [Table 26]

[0319] (Example III-9) The catalyst prepared in Preparation Example III-1 was washed and dried six times in total, and then used in the next reaction. For catalyst evaluation, 8 g of benzene was added to a high-pressure reactor, and hydrogen was added to bring the pressure inside the system to 1.2 MPa. The temperature of the system was then raised to 150°C, and the reaction was terminated after 4 hours.

[0320] [Table 27]

[0321] (Preparation example IV-1) A Na-type Y molecular sieve (FAU structure) with a silicon to aluminum molar ratio of 10:1 was subjected to ammonium ion exchange with a 0.2 mol / L NH4NO3 solution (mass ratio 1:20) at 45°C for 2 hours, then centrifuged and washed. The sample obtained by repeating the ammonium ion exchange twice was dried at 100°C overnight and calcined in air at 550°C for 6 hours to obtain an H-type silica alumina molecular sieve.

[0322] 4.0 mL of 3.0 g / L palladium chloride solution was added dropwise onto 1 g of H-type silica-alumina molecular sieve. After drying at 80 °C for 2 h, it was heated at 450 °C in a fixed-bed reactor at a hydrogen volumetric space velocity of 100 h -1 The catalyst precursor was obtained by reducing the catalyst at 40°C for 3 hours. 0.2 g of methyltrimethoxysilane, 1 g of the catalyst precursor, and 15 mL of toluene solvent were mixed and refluxed at 110°C for 24 hours, and then water was added, centrifuged, washed, and dried at 80°C for 12 hours to obtain the catalyst.

[0323] The XRD spectrum of the obtained catalyst is the same as that in Figure 7. The specific surface area, pore volume, acid properties (including total acid amount and outer surface acid equivalent), metal M content and outer surface metal M content of the catalyst are shown in Table IV-1.

[0324] (Preparation example IV-2) A Na-type Y molecular sieve (FAU structure) with a silicon to aluminum molar ratio of 10:1 was subjected to ammonium ion exchange with a 0.2 mol / L NH4NO3 solution (mass ratio 1:20) at 45°C for 2 hours, then centrifuged and washed. The sample obtained by repeating the ammonium ion exchange twice was dried at 100°C overnight and calcined in air at 550°C for 6 hours to obtain an H-type silica alumina molecular sieve.

[0325] 4.0 mL of 3.0 g / L palladium chloride solution was added dropwise onto 1 g of H-type silica-alumina molecular sieve. The mixture was then dried at 80 °C for 2 h and then heated at 450 °C in a fixed-bed reactor with a hydrogen volumetric space velocity of 100 h -1 The catalyst precursor was obtained by reducing the catalyst at 100°C for 3 hours. 0.3 g of dimethyldimethoxysilane, 1 g of the catalyst precursor, and 15 mL of toluene solvent were mixed and refluxed at 110°C for 24 hours, followed by addition of water, centrifuging, washing, and drying at 80°C for 12 hours to obtain the catalyst.

[0326] XRD shows that the catalysts obtained retain the FAU molecular sieve structure as a whole. The specific surface area, pore volume, acid properties (including total acid content and outer surface acid equivalent), metal M content and metal M content on the outer surface of the catalysts are shown in Table IV-1.

[0327] (Preparation example IV-3) A Na-type Y molecular sieve (FAU structure) with a silicon to aluminum molar ratio of 10:1 was subjected to ammonium ion exchange with a 0.2 mol / L NH4NO3 solution (mass ratio 1:20) at 45°C for 2 hours, and then centrifuged and washed. The sample obtained by repeating the ammonium ion exchange twice was dried at 100°C overnight and calcined in air at 550°C for 6 hours to obtain an H-type silica alumina molecular sieve.

[0328] 4.0 mL of 2.5 g / L palladium chloride solution was added dropwise onto 1 g of H-type silica-alumina molecular sieve. The mixture was dried at 80°C for 2 hours and then heated in a fixed-bed reactor at 450°C and hydrogen volumetric space velocity of 100 h -1 The catalyst precursor was obtained by reducing the catalyst at 0.3 g for 3 hours at 100 °C. 0.3 g of dimethyldimethoxysilane, 1 g of the catalyst precursor, and 15 mL of toluene solvent were mixed and refluxed at 110 °C for 24 hours, and then water was added, centrifuged, washed, and dried at 80 °C for 12 hours to obtain the catalyst.

[0329] XRD shows that the catalyst as a whole retains the FAU molecular sieve structure. The specific surface area, pore volume, acid properties (including total acid content and outer surface acid equivalent), metal M content and metal M content on the outer surface of the catalyst are shown in Table IV-1.

[0330] (Preparation Example IV-4) A Na-type Y molecular sieve (FAU structure) with a silicon to aluminum molar ratio of 5:1 was subjected to ammonium ion exchange with a 0.2 mol / L NH4NO3 solution (mass ratio 1:20) at 45°C for 2 hours, and then centrifuged and washed. The ammonium ion exchange was repeated twice, and the obtained sample was dried at 100°C overnight and calcined in air at 550°C for 6 hours to obtain an H-type silica alumina molecular sieve.

[0331] 4.0 mL of 3.0 g / L palladium chloride solution was added dropwise onto 1 g of H-type silica-alumina molecular sieve. After drying at 80 °C for 2 h, it was then heated at 450 °C in a fixed-bed reactor at a hydrogen volumetric space velocity of 100 h -1 The catalyst precursor was obtained by reducing the catalyst at 0.3 g for 3 hours at 100 °C. 0.3 g of dimethyldimethoxysilane, 1 g of the catalyst precursor, and 15 mL of toluene solvent were mixed and refluxed at 110 °C for 24 hours, and then water was added, centrifuged, washed, and dried at 80 °C for 12 hours to obtain the catalyst.

[0332] XRD shows that the catalysts obtained retain the FAU molecular sieve structure as a whole. The specific surface area, pore volume, acidic properties (including total acid content and outer surface acid equivalent), metal M content and metal M content on the outer surface of the catalysts are shown in Table IV-1.

[0333] (Preparation example IV-5) A Na-type Y molecular sieve (FAU structure) with a silicon to aluminum molar ratio of 10:1 was subjected to ammonium ion exchange with a 0.2 mol / L NH4NO3 solution (mass ratio 1:20) at 45°C for 2 hours, and then centrifuged and washed. The sample obtained by repeating the ammonium ion exchange twice was dried at 100°C overnight and calcined in air at 550°C for 6 hours to obtain an H-type silica alumina molecular sieve.

[0334] 4.0 mL of 3.0 g / L palladium chloride solution was added dropwise onto 1 g of H-type silica-alumina molecular sieve. After drying at 80 °C for 2 h, it was then heated at 450 °C in a fixed-bed reactor at a hydrogen volumetric space velocity of 100 h -1 The catalyst precursor was obtained by reducing the catalyst at 0.3 g for 3 hours at 100 °C. 0.3 g of phenyltrimethoxysilane, 1 g of the catalyst precursor, and 15 mL of toluene solvent were mixed and refluxed at 110 °C for 24 hours, and then water was added, centrifuged, washed, and dried at 80 °C for 12 hours to obtain the catalyst.

[0335] XRD shows that the catalyst as a whole retains the FAU molecular sieve structure. The specific surface area, pore volume, acid properties (including total acid content and outer surface acid equivalent), metal M content and metal M content on the outer surface of the catalyst are shown in Table IV-1.

[0336] (Example IV-1) 0.25g of the catalyst synthesized in Preparation Example IV-1 was added to a high-pressure reactor, and then 10g of n-decane was added to the reactor, and hydrogen was added to make the pressure in the system 3.0MPa. The temperature of the system was then raised to 350°C, and the reaction was terminated after 3 hours. The evaluation data are summarized in Table IV-2.

[0337] (Example IV-2) 0.25g of the catalyst synthesized in Preparation Example IV-1 was added to a high-pressure reactor, and then 10g of n-decane was added to the reactor, and hydrogen was added to make the pressure in the system 3.5MPa. The temperature of the system was then raised to 350°C, and the reaction was terminated after 3 hours. The evaluation data are summarized in Table IV-2.

[0338] (Example IV-3) 0.25g of the catalyst synthesized in Preparation Example IV-1 was added to a high-pressure reactor, and then 10g of n-decane was added to the reactor, and hydrogen was added to make the pressure in the system 3.0MPa. The temperature of the system was then raised to 380°C, and the reaction was terminated after 3 hours. The evaluation data are summarized in Table IV-2.

[0339] (Example IV-4) 0.25g of the catalyst synthesized in Preparation Example IV-2 was added to a high-pressure reactor, and then 10g of n-decane was added to the reactor, and hydrogen was added to make the pressure in the system 3.0MPa. The temperature of the system was then raised to 350°C, and the reaction was terminated after 3 hours. The evaluation data are summarized in Table IV-2.

[0340] (Example IV-5) 0.25g of the catalyst synthesized in Preparation Example IV-3 was added to a high-pressure reactor, and then 10g of n-decane was added to the reactor, and hydrogen was added to make the pressure in the system 3.0MPa. The temperature of the system was then raised to 350°C, and the reaction was terminated after 3 hours. The evaluation data are summarized in Table IV-2.

[0341] (Example IV-6) 0.25g of the catalyst synthesized in Preparation Example IV-4 was added to a high-pressure reactor, and then 10g of n-decane was added to the reactor, and hydrogen was added to make the pressure in the system 3.0MPa. The temperature of the system was then raised to 350°C, and the reaction was terminated after 3 hours. The evaluation data are summarized in Table IV-2.

[0342] (Example IV-7) 0.25g of the catalyst synthesized in Preparation Example IV-5 was added to a high-pressure reactor, and then 10g of n-decane was added to the reactor, and hydrogen was added to make the pressure in the system 3.0MPa. The temperature of the system was then raised to 350°C, and the reaction was terminated after 3 hours. The evaluation data are summarized in Table IV-2.

[0343] (Comparative Example IV-1) A Na-type Y molecular sieve (FAU structure) with a silicon to aluminum molar ratio of 10:1 was subjected to ammonium ion exchange with a 0.2 mol / L NH4NO3 solution (mass ratio 1:20) at 45°C for 2 hours, and then centrifuged and washed. The sample obtained by repeating the ammonium ion exchange twice was dried at 100°C overnight and calcined in air at 550°C for 6 hours to obtain an H-type silica alumina molecular sieve.

[0344] 4.0 mL of 3.0 g / L palladium chloride solution was added dropwise onto 1 g of H-type silica-alumina molecular sieve. After drying at 80 °C for 2 h, the mixture was stirred in a fixed-bed reactor at 450 °C and hydrogen volumetric space velocity of 100 h -1 The mixture was then reduced at 40° C. for 3 hours to give the required catalyst.

[0345] The specific surface area, pore volume, acid properties (including total acid amount and outer surface acid equivalent), metal M content, and metal M content on the outer surface of the catalyst are as shown in Table IV-1.

[0346] The catalyst evaluation method is shown in Example IV-1. The catalyst composition and evaluation results are shown in Table IV-2.

[0347] (Comparative Example IV-2) A Na-type Y molecular sieve (FAU structure) with a silicon to aluminum molar ratio of 10:1 was subjected to ammonium ion exchange with a 0.2 mol / L NH4NO3 solution (mass ratio 1:20) at 45°C for 2 hours, and then centrifuged and washed. The sample obtained by repeating the ammonium ion exchange twice was dried at 100°C overnight and calcined in air at 550°C for 6 hours to obtain an H-type silica alumina molecular sieve.

[0348] 4.0 mL of 3.0 g / L palladium chloride solution was added dropwise onto 1 g of H-type silica-alumina molecular sieve. After drying at 80 °C for 2 h, the mixture was heated at 450 °C in a fixed-bed reactor at a hydrogen volumetric space velocity of 100 h -1 0.8 g of phenyltrimethoxysilane, 1 g of the catalyst precursor, and 15 mL of toluene solvent were mixed and refluxed at 110°C for 24 hours, and then water was added, centrifuged, washed, and dried at 80°C for 12 hours to obtain a catalyst.

[0349] The specific surface area, pore volume, acid properties (including total acid amount and outer surface acid equivalent), metal M content, and metal M content on the outer surface of the catalyst are as shown in Table IV-1.

[0350] The catalyst evaluation method is shown in Example IV-1. The catalyst composition and evaluation results are shown in Table IV-2.

[0351] [Table 28]

[0352] [Table 29]

[0353] The preferred embodiments of the present invention have been described in detail above. However, the present invention is not limited to the specific embodiments described above. Within the technical spirit of the present invention, many simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable aspects. These simple modifications and combinations should also be considered as the disclosure of the present invention, and all of them are included in the protection scope of the present invention.

[0354] In addition, it should be noted that each of the specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction, and in order to avoid unnecessary repetition, the present application will not further describe the various possible combinations.

[0355] Furthermore, the present invention can be arbitrarily combined among various different embodiments without departing from the spirit of the present invention, and such combinations should also be considered as part of the content of the present invention. [Brief description of the drawings]

[0356] [Figure 1] FIG. 1 is an XRD spectrum of the catalyst prepared in Production Example I-1. [Diagram 2] FIG. 2 is a TEM image of the catalyst prepared in Production Example I-1. [Diagram 3] FIG. 3 is an SEM image of the catalyst prepared in Production Example I-1. [Figure 4] FIG. 4 is an XRD spectrum of the catalyst prepared in Production Example II-1. [Diagram 5]FIG. 5 is an infrared absorption spectrum of the catalyst prepared in Production Example II-1. [Figure 6] FIG. 6 is an XRD spectrum of the catalyst prepared in Production Example II-3. [Figure 7] FIG. 7 is an XRD spectrum of the catalyst prepared in Production Example III-1.

Claims

1. A hydrogenation-acid catalyst bifunctional catalyst comprising, based on the weight of the catalyst, 80 to 99.8% of a silica-alumina molecular sieve component, 0.2 to 2% of a hydrogenation active metal component supported on the molecular sieve, and 0 to 20% of a hydrocarbyl modifying component, the hydrogenation active metal being selected from ruthenium, platinum, palladium, copper, nickel, or combinations thereof, more preferably selected from ruthenium, palladium, or combinations thereof, and the hydrocarbyl modifying component being selected from C 1-20 Hydrocarbyl, preferably C 1-10 The catalyst which is hydrocarbyl, more preferably selected from methyl, ethyl, propyl, isopropyl, butyl, phenyl, benzyl, phenethyl or combinations thereof.

2. Catalyst according to claim 1, wherein the silica-alumina molecular sieve is selected from molecular sieves having MWW, FAU, MOR, BEA or ATS structure, or a combination thereof, preferably a molecular sieve having ATS structure; Preferably, the silica-alumina molecular sieve has a silicon-aluminum ratio of 2-50, preferably 2-40, more preferably 2-20.

3. The catalyst according to claim 1 or 2, wherein the silica-alumina molecular sieve is a silica-alumina molecular sieve having an ATS structure, and the X-ray diffraction spectrum of the catalyst shows the relative intensity characteristics of the diffraction peaks shown in the following table: [Table 1]

4. The catalyst of claim 3, wherein the X-ray diffraction spectrum of the catalyst exhibits relative intensity characteristics of diffraction peaks as shown in any row of the following table: [Table 2]

5. the catalyst comprises, based on the mass of the catalyst, 80-98% of a silica-alumina molecular sieve component, 0.2-2% of a metal component having hydrogenation activity, and 1-20% of a hydrocarbyl modifying component, and the mass content of the hydrogenation active metal on the outer surface of the catalyst relative to the elements on the outer surface as measured by X-ray photoelectron spectroscopy (XPS) testing is 0.5% or less, preferably 0.4% or less; Preferably, the catalyst contains, based on the weight of the catalyst, 90 to 98% of the silica-alumina molecular sieve component, 0.2 to 1.5% of the hydrogenation active metal component, and 1 to 10% of the hydrocarbyl modifying component; More preferably, the catalyst according to any one of claims 1 to 4 has a distribution coefficient of the hydrogenation active metal on the outer surface of the catalyst of 1 to 20%, preferably 1.5 to 18%.

6. The catalyst has the following characteristics: The specific surface area of ​​the catalyst is 200 to 800 m 2 / g, preferably 250 to 700m 2 / g; The total pore volume of the catalyst is 0.15 cm 3 / g or more, preferably 0.18 to 1.0 cm 3 / g; The catalyst has a micropore volume of 0.05 to 0.30 cm 3 / g, preferably 0.10 to 0.25 cm 3 / g; The total acid content of the catalyst is 400 to 1500 μmol g -1 and preferably 600 to 1500 μmol g -1 That is; The relative acid equivalent on the outer surface of the catalyst is 15-50%, preferably 15-40%; Catalyst metal H 2 - the TPR test reduction temperature is 470-500°C, preferably 480-500°C; The ratio of the acid content of the catalyst B acid / L acid is 0.2-8.0, preferably 0.4-6.0; In the catalyst, the crystals have a strip-like or rod-like morphology, the length of said crystals is 0.3-3 μm, and the aspect ratio is 2-20, preferably 5-20; The catalyst according to any one of claims 1 to 5, wherein the catalyst has one or more of the following:

7. The following steps: (1) providing an H-type silica-alumina molecular sieve; and (2) A method for preparing the catalyst according to any one of claims 1 to 6, comprising the steps of supporting a hydrogenation active metal on the H-type silica-alumina molecular sieve, and optionally subjecting the resulting product to a hydrocarbylation treatment and / or reduction to obtain a catalyst.

8. Step (1) includes a step of subjecting a raw material of a silica-alumina molecular sieve to ammonium ion exchange and calcination to obtain an H-type silica-alumina molecular sieve; Preferably, the silica-alumina molecular sieve source is selected from silica-alumina molecular sieves having MWW, FAU, MOR or BEA structures, or combinations thereof; The method according to claim 7.

9. Step (1) includes mixing a silicon source, an aluminum source, a fluorine source, an organic structure directing agent and water, performing a heating pretreatment, followed by a crystallization treatment and a calcination to obtain an H-type ATS silica-alumina molecular sieve, wherein the silicon source is selected from silicic acid, silica gel, silica sol, tetraethyl silicate, sodium silicate, or a combination thereof, the aluminum source is selected from pseudoboehmite, aluminum isopropoxide, or a combination thereof, the fluorine source is hydrofluoric acid, and the organic structure directing agent is 4-pyrrolidinylpyridine; Preferably, step (1) has the following characteristics: SiO 2 and an added silicon source calculated as Al 2 O 3and an aluminum source calculated as F - the molar ratio of the fluorine source, the organic structure directing agent, and water calculated as: is 1:(0.02-0.2):(0.5-2):(0.25-1.5):(3-15), preferably 1:(0.05-0.15):(0.5-1):(0.5-1):(5-10); In the crystallization process, SiO 2 the molar ratio of silicon source to water, calculated as: is 1:(1-10), preferably 1:(1.5-6.5); and The crystallization conditions include a crystallization temperature of 120 to 200° C., preferably 150 to 200° C., and a crystallization time of 7 to 21 days, preferably 7 to 15 days; The method of claim 7, further comprising one or more of the following:

10. In step (2), a solution of a hydrogenation active metal source is added to an H-type silica-alumina molecular sieve and dried to support the hydrogenation active metal on the H-type silica-alumina molecular sieve; Preferably, step (2) has the following characteristics: the hydrogenation active metal source is selected from soluble compounds of the metal, preferably selected from metal chlorides, nitrates, or combinations thereof; The concentration of the solution of the hydrogenation active metal source is 1.5 to 50 g / L, preferably 2 to 45 g / L, based on the mass of the hydrogenation active metal; The solution of the hydrogenation active metal source is added dropwise to the H-type silica-alumina molecular sieve; and the mass ratio of the hydrogenation active metal in the solution of the hydrogenation active metal source to the H-type silica-alumina molecular sieve is 0.002-0.015:1, for example 0.005-0.02:1; The method according to any one of claims 7 to 9, comprising one or more of the following:

11. The hydrocarbylation process comprises mixing and reacting the hydrogenation active metal-supported product with a hydrocarbylation reagent in a solvent; said hydrocarbylating agent is selected from methyltrimethoxysilane, dimethyldimethoxysilane, ethyltrimethoxysilane, diethyldimethoxysilane, propyltrimethoxysilane, isopropyltrimethoxysilane, phenyltrimethoxysilane, tolyltrimethoxysilane, phenylsilanetriol, tolylsilanetriol, diphenylsilanediol, or combinations thereof, preferably selected from dimethyldimethoxysilane, diethyldimethoxysilane, isopropyltrimethoxysilane, phenyltrimethoxysilane, tolyltrimethoxysilane, phenylsilanetriol, tolylsilanetriol, or combinations thereof; Preferably, the hydrocarbylation process has the following characteristics: The solvent is ethanol, toluene or a combination thereof; the mass ratio of the product carrying the hydrogenation active metal, the hydrocarbylating reagent and the solvent is 1:(0.05-0.45):(5-55), preferably 1:(0.06-0.40):(6-50); The reaction conditions for the hydrocarbylation process include a reaction temperature of 40 to 110° C., preferably 70 to 110° C., and a reaction time of 6 to 48 hours, preferably 8 to 24 hours; The method according to any one of claims 7 to 10, comprising one or more of the following:

12. The reduction is carried out using a reducing gas, preferably hydrogen, and the conditions of the reduction are preferably a reduction temperature of 300 to 450° C., a reduction time of 3 to 6 hours, and a volumetric space velocity of the reducing gas of 40 to 200 h -1 The method according to any one of claims 7 to 11, comprising:

13. 7. Use of the hydrogenation-acid catalyst bifunctional catalyst according to any one of claims 1 to 6 in a hydroconversion reaction of a hydrocarbon, comprising contacting and reacting a hydrocarbon feedstock with said catalyst in the presence of hydrogen, preferably said hydroconversion reaction being selected from a benzene hydroalkylation reaction and an alkane hydroisomerization reaction.

14. contacting and reacting the hydrogenation-acid catalyst bifunctional catalyst of any one of claims 1 to 6 with benzene in the presence of hydrogen to obtain cyclohexylbenzene; Preferably, the reaction conditions include: a mass ratio of benzene to catalyst is 8-40, preferably 10-40; a reaction temperature is 100-220° C., preferably 120-200° C.; a reaction time is 2-8 hours, preferably 2.5-6 hours; and a hydrogen pressure is 0.8-2.5 MPa, preferably 1.0-2.5 MPa.

15. contacting and reacting linear alkanes in the presence of hydrogen with the hydrogenation-acid catalyst bifunctional catalyst of any one of claims 1 to 6 to obtain an isomerization product; The linear alkane is a C8 or higher linear alkane, preferably a C8 to C20 linear alkane, more preferably a C8 to C12 linear alkane; Preferably, the reaction conditions include a mass ratio of linear alkane to catalyst of 10 to 100, preferably 10 to 50; a reaction temperature of 250 to 400° C., preferably 300 to 400° C.; a reaction time of 3 to 10 hours, preferably 4 to 10 hours; and a hydrogen pressure of 2.5 to 5.0 MPa, preferably 3.0 to 4.0 MPa.

Citation Information

Patent Citations

  • A method of preparing phenylcyclohexane by hydroalkylation

    CN105439802A

  • Method for preparing cyclohexyl benzene through hydrogenation alkylation

    CN106518602A

  • Method for preparing catalyst for preparation of phenylcyclohexane through benzene hydrogenation

    CN109999893A

  • Method for synthesizing cyclohexylbenzene

    CN110563543A

  • Method for producing cyclohexylbenzene

    JP2010535822A