Composite having high thermal conductivity and method for producing said composite
A composite of oriented hexagonal boron nitride particles in an organic polymer addresses the need for more efficient thermal management materials, achieving high thermal conductivity and improved compatibility with organic polymers for enhanced heat dissipation.
Patent Information
- Application Number
- JP2024522446
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-14
- Filing Date
- 2022-10-14
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-10-14
AI Technical Summary
There is a need to enhance the thermal management materials in industries such as consumer electronics, telecommunications infrastructure, LED lighting, hybrid and electric vehicles, and data centers by increasing the variety and efficiency of thermally conductive polymer composites.
A composite is developed comprising an organic polymer and hexagonal boron nitride (hBN) particles with a high degree of orientation, achieved through mechanical exfoliation, surface functionalization, and alignment under pressure, resulting in a composite with in-plane thermal conductivity of at least 10 W/mK.
The composite achieves high thermal conductivity and improved compatibility with organic polymers, allowing for efficient heat dissipation and extended device life in various applications.
Smart Images

Figure 2024538458000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to composites comprising an organic polymer and ceramic particles, the ceramic particles including hexagonal boron nitride (hBN) particles dispersed throughout the organic polymer with a high degree of orientation, and methods of making the composites. [Background technology]
[0002] Thermally conductive polymer composites play an important role in various industries in the thermal management of electrical devices, since they can significantly reduce the operating temperature and extend the life of the devices by dissipating heat to avoid overheating. Typical industries in which thermally conductive polymer composites play an important role include consumer electronics (e.g., mobile phones, tablets), telecommunications infrastructure (e.g., cell towers), LED lighting, hybrid and electric vehicles (power modules), data centers (server boards, switches, monitoring modules, and power supplies), and solar cells.
[0003] There is a need for greater variety and efficiency of materials suitable for thermal management. [Brief description of the drawings]
[0004] The present disclosure may be better understood, and its numerous features and advantages made apparent to those skilled in the art by referencing the accompanying drawings.
[0005] [Figure 1A] FIG. 1A is a diagram showing platelet-type hBN particles, according to one embodiment. [Figure 1B] FIG. 1B includes a line drawing showing a cross-sectional side view of a composite having in-plane oriented hBN grains, according to one embodiment. [Figure 1C] FIG. 1C includes a line drawing showing a cross-sectional side view of a composite having hBN particles oriented in the through-plane direction, according to one embodiment. [Figure 2A] FIG. 2A includes a graph showing an X-ray spectrum of a composite including in-plane oriented hBN particles, according to one embodiment. [Figure 2B] Figure 2B is a graph showing the relationship between r and the orientation parameter η according to the March-Dorus method. [Diagram 3] FIG. 3 includes IR spectra of hBN particles before and after exfoliation and siliconization, according to one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0006] As used herein, the terms "comprises," "comprising," "includes," "including," "has," "having," or any other variations thereof, are intended to cover a non-exclusive inclusion. For example, a process, method, article, or apparatus that includes a list of features is not necessarily limited to only those features and may include other features that are not expressly listed or that are inherent to such process, method, article, or apparatus.
[0007] As used herein, unless clearly stated to the contrary, "or" refers to an inclusive or and not an exclusive or. For example, a condition A or B is satisfied by any one of the following: A is true (or exists) and B is false (or does not exist), A is false (or does not exist) and B is true (or exists), and both A and B are true (or exist).
[0008] Additionally, the use of "a" or "an" is used to describe elements and components described herein. This is done merely for convenience and to give a general sense of the scope of the invention. This description should be read to include one or at least one, and the singular also includes the plural, unless it is clear that otherwise is meant.
[0009] The present disclosure relates to a composite article comprising a composite including an organic polymer and ceramic particles including hexagonal boron nitride (hBN) particles distributed throughout the organic polymer, where the amount of hBN particles can be in the range of 20 vol.% to 40 vol.% based on a total volume of the composite, the amount of ceramic particles can be 50 vol.% or less based on a total volume of the composite, and the composite can include an in-plane thermal conductivity of at least 10 W / mK.
[0010] As used herein, the term hBN particles, unless otherwise indicated, refers to platelet-shaped hBN particles having an average length-to-thickness aspect ratio (L / T) of at least 5, as also shown in FIG. 1A.
[0011] As further used herein, the term "in-plane" refers to the xy directions of the composite. Figure IB shows a cross-section (10) of a composite in which the hBN particles (12) may be oriented (also referred to herein as aligned) in the xy directions of the composite, which is interchangeably referred to herein as "in-plane." In contrast, Figure 1C shows an embodiment of a composite slice in which the hBN particles (12) are aligned in the z direction, which is also interchangeably referred to herein as the "through-plane" or thickness direction of the composite.
[0012] In one embodiment, the composite of the present disclosure may be made by preparing a mixture including ceramic particles comprising hBN and an organic polymer, applying a layer of the mixture to a mold or support, performing an alignment procedure for the hBN particles, and solidifying and / or curing the organic polymer to form the composite.
[0013] In one embodiment, the alignment procedure can include applying pressure perpendicular to the in-plane directions (xy directions) of the layer of the mixture. In certain embodiments, the pressure can be applied by forming the layer on a 12" x 12" metal plate and applying pressure to the layer with a second metal plate of the same size, where the weight applied to the second metal plate can be at least 40,000 lbs, or at least 50,000 lbs, or at least 60,000 lbs, or at least 70,000 lbs. In further embodiments, the weight on the second plate can be 150,000 lbs or less.
[0014] In one embodiment, the method can include surface functionalizing the hBN particles prior to preparing the mixture. The surface functionalization can include exfoliating and activating the activated hBN particles to form activated hBN particles, and treating the activated hBN particles with an organic compound.
[0015] In one embodiment, activating can include introducing OH groups onto the outer surface of the hBN particles.
[0016] In certain aspects, exfoliation can be a mechanical process that can cut or exfoliate the hBN platelet particles to increase the surface area of the hBN particles. Activation of the hBN particles can be treating the hBN particles with an alkaline fluid, which may introduce OH groups onto the surface of the hBN particles by covalent bonding.
[0017] In certain embodiments, exfoliation and activation can occur simultaneously. In certain embodiments, exfoliation of the hBN particles can include ball milling using aqueous sodium hydroxide as the liquid medium.
[0018] The exfoliated and activated hBN particles can be further surface functionalized with an organic compound. In certain embodiments, the organic compound can be a polysiloxane, or polysilane, or silane compound containing silicon hydride groups, or any combination thereof.
[0019] In certain embodiments, chemically reacting the silane compound with the hBN particles can further include using a boron catalyst. In a non-limiting example, the boron catalyst can include tri(pentafluorophenyl)borane.
[0020] After exfoliation and activation of the hBN particles, a chemical reaction can take place between the introduced OH groups and a selected organic compound to covalently bond the organic compound to the surface of the hBN particles, also referred to herein as grafting.
[0021] In certain embodiments, the grafting of the surface of the hBN particles can be carried out using a polysiloxane containing silicone hydride groups as the organic compound. In certain aspects, the composite can include surface-functionalized hBN particles grafted with polysiloxane and a silicone polymer with the hBN particles distributed therein as the organic polymer.
[0022] The surface functionalization may not be limited to polysiloxane grafting, but may include any other monomer, oligomer, or polymer that can react with the introduced OH groups of the exfoliated hBN particles. Without being bound by theory, the grafted surface of the hBN particles may make the particles more compatible with organic polymer matrices, thereby allowing for lower processing viscosities, leading to easier alignment and improved homogeneous curing.
[0023] In some embodiments, the organic polymer of the composite can be a thermoplastic polymer or a thermoset polymer.
[0024] In certain embodiments, the organic polymer may be a polymerizable polymer that includes functional groups. In certain embodiments, curing of the polymerizable monomer may be required after and / or during compression molding.
[0025] Non-limiting examples of polymerizable polymers may include silicone polymers, or acrylate polymers, or epoxy polymers.
[0026] In a particular aspect, the polymerizable polymer can be a silicone polymer containing vinyl groups. In a non-limiting embodiment, the silicone polymer containing vinyl groups can be polymerized by crosslinking with a crosslinking agent. In one aspect, the weight percent ratio of the silicone polymer containing vinyl groups to the crosslinking agent can be 0.5-5, or 1-3, or 1-2.
[0027] In certain embodiments, the silicone polymer may have a molecular weight of at least 10,000 g / mol, at least 100,000 g / mol, at least 200,000 g / mol, at least 400,000 g / mol, or at least 700,000 g / mol. In other certain embodiments, the molecular weight of the silicone polymer may be 1,000,000 g / mol or less, or 800,000 g / mol or less, or 700,000 g / mol or less, or 500,000 g / mol or less, or 300,000 g / mol or less, or 100,000 g / mol or less.
[0028] In another particular embodiment, the organic polymer can be a thermoplastic polymer.Non-limiting examples of thermoplastic polymers can include polyethylene, polypropylene, polystyrene, polyurethane, polyacrylate, polyester, polycarbonate, polyimide, polybutylene terephthalate (PBT), polymethyl methacrylate (PMMA), polyethylene terephthalate (PET), polyamide, liquid crystal polymer (LCP), polyacrylonitrile (PAN), polyether ether ketone (PEEK), polyether ketone ketone (PEKK), polysulfone, polyether sulfone, polyphenylene oxide (PPO), polyetherimide, thermoplastic elastomer (TPE, olefin-based or styrenic), fluoropolymer such as polyvinylidene fluoride (PVDF), perfluoroalkoxyalkane (PFA), fluorinated ethylene propylene (FEP), or ethylene tetrafluoroethylene (ETFE), or any copolymer thereof, or any combination thereof.
[0029] In certain embodiments, the composite may include surface-functionalized hBN particles grafted with polysiloxane and, as the organic polymer, a silicone polymer in which the hBN particles are distributed.
[0030] In another particular embodiment, the hBN particles can be surface functionalized via fluorine surface functionalization and combined with a silicone polymer. Examples of fluorine surface functionalization can include plasma treatment with CF4, or CHF3, SF6, or C2F6.
[0031] In another embodiment, the organic polymer can be an epoxy polymer, and the hBN particles can be surface functionalized with an epoxy compound, or an amine, or a hydroxyl group. Non-limiting examples of introducing an epoxy compound can be plasma treatment with glycidyl methacrylate or plasma treatment with allyl glycidyl ether. Examples of amine functionalization can include plasma treatment with allylamine or 3-(aminopropyl)triethoxysilane.
[0032] In a further embodiment, the organic polymer can be polyethylene and the hBN particles can be subjected to fluorine surface functionalization or silane functionalization.
[0033] In yet another embodiment, the organic polymer can be a thermoplastic polyurethane (TPU) or polybutylene terephthalate (PBT), and the hBN particles can be functionalized with epoxy compounds, amines, or hydroxyl groups. In certain further embodiments, the PBT can also be surface functionalized by oxygen plasma treatment, air plasma treatment, treatment with boric acid / urea in combination with heat treatment, or treatment with boric acid / melamine in combination with heat treatment.
[0034] In certain aspects, the composites of the present disclosure may have an in-plane thermal conductivity of at least 10 W / mK, with a corresponding amount of hBN particles of 39 vol.% or less, or 38 vol.% or less, or 37 vol.% or less, or 36 vol.% or less, or 35 vol.% or less, or 34 vol.% or less, or 33 vol.% or less, or 32 vol.% or less, or 31 vol.% or less, or 30 vol.% or less, or 29 vol.% or less, or 28 vol.% or less, or 25 vol.% or less.
[0035] In certain embodiments, a majority of the ceramic particles contained within the composite can be hBN particles, for example, at least 90 volume %, or at least 92 volume %, or at least 94 volume %, or at least 96 volume %, or at least 98 volume %, or at least 99 volume %, based on the total volume of the ceramic particles. In certain embodiments, the ceramic particles can consist essentially of hBN particles, which as used herein means having 0.5 volume % or less of ceramic particles that are not hBN particles.
[0036] The orientation of the hBN particles in the composite (also referred to herein as exchangeable alignment of the hBN particles) can be measured by performing X-ray diffraction and analyzing the X-ray spectrum according to the March-Dauer method (see detailed description in the Examples). It has been found that the March-Dauer orientation parameter η can be a suitable quantitative expression to characterize the degree of alignment of the hBN particles dispersed in the composite. Good alignment is considered in this disclosure to be a March-Dauer orientation parameter η of at least 50%. In certain embodiments, the March-Dauer orientation parameter of the hBN particles in the composite can be at least 52%, or at least 54%, or at least 56%, or at least 58%, or at least 60%.
[0037] As further demonstrated in the examples, it has surprisingly been found that a specific combination of mechanical exfoliation and chemical treatment of hBN particles prior to functionalization with organic compounds can result in thermal conductivities of at least 10 W / mK at hBN concentrations of less than 40 vol.%.
[0038] In one embodiment, the hBN particles may have an average aspect ratio of the length (L) to the thickness (T) of the hBN particles of at least 5, or at least 7, or at least 10, or at least 20, or at least 30, or at least 40, or at least 50, or at least 60, or at least 70, or at least 80, or at least 90, or at least 100, or at least 110, or at least 120. In certain aspects, the aspect ratio may be 200 or less, or 120 or less, or 80 or less, or 50 or less, or 30 or less, or 15 or less.
[0039] In another embodiment, the hBN particles may have an average particle size (D50) of at least 1 micron, or at least 3 microns, or at least 5 microns, or at least 10 microns, or at least 15 microns, or at least 20 microns, or at least 25 microns, or at least 30 microns. In further aspects, the hBN particles may have an average particle size of 100 microns or less, or 50 microns or less, or 45 microns or less, or 40 microns or less, or 35 microns or less, or 30 microns or less, or 25 microns or less, or 20 microns or less, or 10 microns or less, or 5 microns or less.
[0040] In certain embodiments, the hBN particles of the composite may have a multimodal particle distribution, e.g., a bimodal or trimodal distribution. In certain aspects, the particle distribution may be a bimodal particle distribution (PSD).
[0041] In one embodiment, the particle size distribution of the hBN particles can include a first peak having a first peak maximum and a second peak having a second peak maximum, and the intensity ratio of the first peak maximum to the second peak maximum can be at least 1.5:1, or at least 2:1, or at least 2.5:1, or at least 3.0:1. In another embodiment, the intensity ratio of the first peak maximum to the second peak maximum can be 10:1 or less, or 7:1 or less, or 5:1 or less, or 4:1 or less, or 3.5:1 or less, or 3.0:1 or less.
[0042] In another embodiment, the distance between the first and second peak maxima of the hBN particle size distribution can be at least 20 microns, or at least 25 microns, or at least 30 microns, or at least 35 microns. In further embodiments, the distance between the first and second peak maxima can be 70 microns or less, or 60 microns or less, or 50 microns or less, or 40 microns or less, or 35 microns or less.
[0043] In yet another embodiment, the first peak maximum can correspond to an hBN particle size in the range of 8 microns to 13 microns, and the second peak maximum can correspond to an hBN particle size in the range of 35 to 50 microns.
[0044] In another embodiment, the 80th percentile of the hBN particle distribution (D90-D10) can be at least 15 microns, or at least 20 microns, or at least 25 microns, or at least 30 microns, or at least 35 microns, or at least 40 microns, or at least 45 microns, or at least 50 microns. In another embodiment, the 80th percentile of the hBN particle distribution (D90-D10) can be 80 microns or less, or 70 microns or less, or 60 microns or less, or 50 microns or less, or 45 microns or less, or 40 microns or less.
[0045] In certain embodiments, a majority of the ceramic particles contained within the composite can be hBN particles, for example, at least 90 volume %, or at least 92 volume %, or at least 94 volume %, or at least 96 volume %, or at least 98 volume %, or at least 99 volume %, based on the total volume of the ceramic particles. In certain embodiments, the ceramic particles can consist essentially of hBN particles, which as used herein means having 0.5 volume % or less of ceramic particles that are not hBN particles.
[0046] Surprisingly, it has been observed that certain surface-functionalized hBN particles can be dispersed in organic polymers with a high degree of orientation already at hBN concentrations of up to 40% by volume, based on the total volume of the composite, such that a thermal conductivity of the composite of at least 10 W / mK can be obtained.
[0047] Many different aspects and embodiments are possible. Some of these aspects and embodiments are described herein. After reading this specification, a person skilled in the art will understand that these aspects and embodiments are merely illustrative and do not limit the scope of the present invention. The embodiment may be according to any one or more of the embodiments listed below.
[0048] Embodiment Embodiment 1. A composite article comprising a composite comprising an organic polymer and ceramic particles comprising hexagonal boron nitride (hBN) particles distributed throughout the organic polymer, The amount of hBN particles is in the range of 20% to 40% by volume based on the total volume of the composite; the amount of ceramic particles is 50 volume percent or less based on the total volume of the composite; The composite article, wherein the composite has an in-plane thermal conductivity of at least 10 W / mK.
[0049] Embodiment 2. The composite article of embodiment 1, wherein the in-plane March-Dauer orientation parameter η of the hBN particles in the composite is at least 50%, or at least 51%, or at least 52%, or at least 53%, or at least 54%, or at least 55%, or at least 56%, or at least 57%, or at least 58%, or at least 59%, or at least 60%, or at least 61%, or at least 62%, or at least 63%, or at least 64%, or at least 65%.
[0050] Embodiment 3. The composite article of any one of the preceding embodiments, wherein the average aspect ratio of the length to thickness of the hBN particles is at least 5, or at least 10, or at least 20, or at least 30, or at least 40, or at least 50, or at least 60, or at least 70, or at least 80, or at least 90, or at least 100, or at least 110, or at least 120.
[0051] Embodiment 4. The composite article of any one of the preceding embodiments, wherein the average aspect ratio of the hBN particles is 200 or less, or 120 or less, or 80 or less, or 50 or less.
[0052] Embodiment 5. The composite article of any one of the preceding embodiments, wherein the hBN particles have an average particle size (D50) of at least 1 micron, or at least 3 microns, or at least 5 microns, or at least 10 microns, or at least 15 microns, or at least 20 microns, or at least 25 microns, or at least 30 microns, or at least 35 microns.
[0053] Embodiment 6. The composite article of any one of the preceding embodiments, wherein the hBN particles have an average particle size of 100 microns or less, or 70 microns or less, or 50 microns or less, or 45 microns or less, or 40 microns or less, or 35 microns or less, or 30 microns or less, or 25 microns or less, or 20 microns or less, or 10 microns or less, or 5 microns or less.
[0054] Embodiment 7. The composite article of any one of the preceding embodiments, wherein the hBN particles have a multimodal distribution.
[0055] Embodiment 8. The composite article of embodiment 7, wherein the hBN particles comprise a combination of three different particle size ranges.
[0056] Embodiment 9. The composite article of embodiment 7 or 8, wherein the hBN particles comprise a first portion of hBN particles having an average particle size of 3 to 7 microns, a second portion of hBN particles having an average particle size of 12 to 20 microns, and a third portion of hBN particles having an average particle size of 25 to 35 microns.
[0057] Embodiment 10. The composite article of embodiment 9, wherein the volume ratio of the first portion to the second and third portions is in the range of 0.7:1.0:1.3 to 1.3:1.0:0.7, or 0.8:1.0:1.2 to 1.2:1.0:0.8, or 0.9:1.0:1.1 to 1.1:1.0:0.9.
[0058] Embodiment 11. The composite article of any one of the preceding embodiments, wherein the composite has an electrical volume resistivity of at least 1.0E+12, or at least 1.0E+13, or at least 1.0E+14.
[0059] Embodiment 12. The composite article of any one of the preceding embodiments, wherein the organic polymer of the composite comprises a thermoplastic polymer or a thermoset polymer.
[0060] Embodiment 13. The composite article of embodiment 14, wherein the organic polymer comprises a silicone polymer, an acrylate polymer, a polyurethane, an epoxide polymer, a polyamide, a polyimide, a liquid crystal polymer (LCP), a fluoropolymer, a polyethylene, a polypropylene, a polystyrene, a polyester, a polycarbonate, a polybutylene terephthalate (PBT), a polyethylene terephthalate (PET), a polyamide, a liquid crystal polymer (LCP), a polyacrylonitrile (PAN), a polyetheretherketone (PEEK), a polyetherketoneketone (PEKK), a polysulfone, a polyethersulfone, a polyphenylene oxide (PPO), a polyetherimide, a thermoplastic elastomer (TPE, olefinic or styrenic), a polyvinylidene fluoride (PVDF), a perfluoroalkoxyalkane (PFA), a fluorinated ethylene propylene (FEP), an ethylene tetrafluoroethylene (ETFE), or any copolymer thereof, or any combination thereof.
[0061] Embodiment 14. The composite article of any one of the preceding embodiments, wherein the organic polymer comprises a silicone polymer.
[0062] Embodiment 15. The composite article of embodiment 16, wherein the organic polymer consists essentially of a silicone polymer.
[0063] Embodiment 16. The composite article of any one of embodiments 16 or 17, wherein the silicone polymer has a molecular weight of at least 10,000 g / mol, at least 100,000 g / mol, at least 200,000 g / mol, at least 400,000 g / mol, or at least 700,000 g / mol.
[0064] Embodiment 17. The composite article of any one of embodiments 16-18, wherein the silicone polymer has a molecular weight of 1,000,000 g / mol or less, or 800,000 g / mol or less, or 700,000 g / mol or less, or 500,000 g / mol or less, or 300,000 g / mol or less, or 100,000 g / mol or less.
[0065] Embodiment 18. The composite article of any one of the preceding embodiments, wherein the composite further comprises a surfactant.
[0066] Embodiment 19. The composite article of embodiment 17, wherein the amount of the surfactant is at least 0.1% by weight and no more than 5% by weight.
[0067] Embodiment 20. The composite article of embodiment 27 or 28, wherein the surfactant is a polysiloxane.
[0068] Embodiment 21. The composite article of any one of the preceding embodiments, wherein the amount of hBN particles is 92 vol.%, or at least 94 vol.%, or at least 96 vol.%, or at least 98 vol.%, or at least 99 vol.%, based on the total volume of the ceramic particles.
[0069] Embodiment 22. The composite article of any one of the preceding embodiments, wherein the ceramic particles of the composite consist essentially of hBN particles.
[0070] Embodiment 23. The composite article of any one of the preceding embodiments, wherein the amount of hBN particles is 39 vol.% or less, or 38 vol.% or less, or 37 vol.% or less, or 36 vol.% or less, or 35 vol.% or less, based on the total volume of the composite.
[0071] Embodiment 24. The composite article of any one of the preceding embodiments, wherein the amount of hBN particles is at least 21 vol.%, or at least 22 vol.%, or at least 23 vol.%, or at least 24 vol.%, or at least 25 vol.%, or at least 26 vol.%, or at least 27 vol.%, or at least 28 vol.%, or at least 29 vol.%, or at least 30 vol.%, or at least 31 vol.%, or at least 32 vol.%, or at least 33 vol.%, or at least 34 vol.%, based on the total volume of the composite.
[0072] Embodiment 25. The composite article of any one of the preceding embodiments, wherein the thermal conductivity of the composite is at least 10.5 W / mK, or at least 11.0 W / mK, or at least 11.5 W / mK, or at least 12 W / mK, or at least 12.5 W / mK, or at least 13.0 W / mK, or at least 13.5 W / mK, or at least 14 W / mK, or at least 14.5 W / mK, or at least 15.0 W / mK, or at least 15.5 W / mK, or at least 16 W / mK, or at least 16.5 W / mK, or at least 17.0 W / mK, or at least 17.5 W / mK, or at least 18 W / mK, or at least 18.5 W / mK, or at least 19.0 W / mK, or at least 19.5 W / mK, or at least 20 W / mK.
[0073] Embodiment 26. The composite article of any one of the preceding embodiments, wherein the thermal conductivity of the composite is 40 W / mK or less, or 30 W / mK or less, or 20 W / mK or less.
[0074] Embodiment 27. A composite article according to any one of the preceding embodiments, wherein the surface of the hBN particles is functionalized with an organic compound.
[0075] Embodiment 28. The composite article of embodiment 27, wherein the organic compound is selected from polysiloxanes, polysilanes, silanes, or any combination thereof.
[0076] Embodiment 29. The composite article of embodiment 28, wherein the organic compound is a polysiloxane.
[0077] Embodiment 30. The composite article of any one of embodiments 27-29, wherein the organic compound is covalently bonded to the surface of the hBN particles.
[0078] Embodiment 31. The composite article of any one of embodiments 25-26, wherein the polysiloxane has a molecular weight of at least 100 and not more than 100,000.
[0079] Embodiment 32. The composite article of embodiment 27, wherein the organic compound comprises a fluorine-containing compound, an epoxy compound, or an amine.
[0080] Embodiment 33. A method of forming a composite article, comprising: preparing a mixture of ceramic particles and an organic polymer, the ceramic particles comprising hBN particles, the amount of the hBN particles being in the range of 20-40 vol.% based on the total weight of the dispersion, and the total amount of the ceramic particles being 50 vol.% or less based on the total volume of the composite; applying a layer of the mixture to a mold or substrate; carrying out an alignment procedure of hBN particles; and solidifying and / or curing the organic polymer or organic polymerizable material to form a composite. The method wherein the in-plane thermal conductivity of the composite is at least 10 W / mK.
[0081] Embodiment 34. The method of embodiment 33, further comprising surface functionalizing the hBN particles prior to preparing the mixture.
[0082] Embodiment 35. The method of embodiment 34, wherein the surface functionalization comprises exfoliating and activating hBN particles to form activated hBN particles, and treating the activated hBN particles with an organic compound.
[0083] Embodiment 36 The method of embodiment 35, wherein the activation comprises introducing OH groups onto the outer surface of the hBN particles.
[0084] Embodiment 37 The method according to embodiment 34 or 35, wherein stripping and activation are performed simultaneously.
[0085] Embodiment 38. The method of any one of embodiments 34 to 37, wherein the exfoliation comprises ball milling.
[0086] Embodiment 39. The method of any one of embodiments 35 to 38, wherein the organic compound is a polysiloxane, or polysilane, or silane compound containing silicon hydride groups, or any combination thereof.
[0087] Embodiment 40. The method of embodiment 39, wherein the treating comprises chemically reacting the hBN particles with an organic compound.
[0088] Embodiment 41. The method of embodiment 40, wherein chemically reacting the hBN particles with an organic compound comprises using a boron catalyst.
[0089] Embodiment 42. The method of embodiment 41, wherein the boron catalyst comprises tri(pentafluorophenyl)borane.
[0090] Embodiment 43. The method of any one of embodiments 33 to 42, wherein the alignment step comprises applying pressure to the layer of the mixture.
[0091] Embodiment 44. The method of embodiment 43, wherein the pressure is adjusted such that the degree of in-plane March-Dorus orientation parameter of the cured composite is at least 50%.
[0092] Embodiment 45. The method of embodiment 43 or 44, wherein the pressure is at least 2 MPa, or at least 100 MPa, or at least 500 MPa. EXAMPLES
[0093] The following non-limiting examples illustrate the invention.
[0094] Example 1 Preparation of activated hBN powder
[0095] To prepare activated hBN (hBN containing OH groups on the surface) for use as starting material for silane functionalization, different treatments were performed.
[0096] In all the series of experiments carried out, hBN particles with an average particle size of 30 microns and an aspect ratio of 8–10 were used as starting material and subjected to different types of exfoliation in combination with the introduction of OH groups on the outer surface of the hBN particles before surface functionalization with silanes.
[0097] Stripping and activation with NaOH (sample BN1) hBN powder was exfoliated using a PQ-N4 planetary ball mill (Across International) loaded with zirconia beads. The ratio of hBN powder to zirconia beads was approximately 50:1. For milling, 200 g of hBN powder was mixed with 500 mL of 2 M NaOH and milled at 200 rpm for 12 h. The mill speed was then increased to 400 rpm and milled for an additional 12 or 24 h. After milling, the zirconia beads were removed and the hBN platelets were rinsed with dilute HCl solution and washed with water by vacuum filtration until a neutral pH was obtained. The final powder was dried in a vacuum oven at 50-60 °C.
[0098] Peeling in neutral solvent (sample BN2) The same experiment as above was carried out to prepare sample BN1, except that neutral water (deionized water) was used.
[0099] Sonication and polydopamine (PDA) treatment (sample BN3) Exfoliation was achieved by mixing 200 g of hBN powder and 300 mL of isopropyl alcohol (IPA) together in a FlackTek Speedmixer, followed by sonication for 30 minutes.
[0100] The exfoliated hBN was further subjected to PDA functionalization to introduce hydroxyl groups onto the surface of the hBN particles.
[0101] PDA functionalization was performed by immersing 20 g of exfoliated hBN in a solution of 8 g of dopamine hydrochloride, 300 mL of Tris buffer solution (10 mM, pH 8.5), and 100 mL of ethanol solution. The mixture was stirred for 12 h at room temperature under light protection. The treated hBN powder was separated by centrifugation at 4000 rpm for 15 min, washed with deionized water and ethanol, and dried at 60 °C for 12 h.
[0102] O2 plasma activation (sample BN4) Plasma treatment of the hBN powder was carried out using a Pico-SR-PCCE-C low-pressure plasma reactor manufactured by Diener Electronics Co. It is known that during oxygen plasma treatment, hydroxyl groups are grafted onto the surface of the hBN plate.
[0103] Plasma treatment was performed for 12 min with a batch size of 15 g hBN in a 50% O2 / 50% air mixture at a pressure of 0.3 mbar and a power of 100 W. The combination of O2 and air was chosen to introduce water vapor for hydroxyl formation in the plasma gas.
[0104] Glycidyl methacrylate plasma polymerization (sample BN5) Glycidyl methacrylate (GMA) is an epoxy-functional monomer that can be polymerized by plasma-enhanced chemical vapor deposition (PECVD). The application of power of 40 W or more promotes the opening of the epoxide ring and the generation of hydroxyl groups.
[0105] Plasma activation of the hBN powder was performed using air gas at a power of 100 W and a pressure of 0.3 mbar for 5 minutes.
[0106] Example 2 Functionalization of activated hBN particles by the Piers-Rubinsztajn reaction The activated hBN powder samples of Example 1 (BN1, BN2, BN3, BN4, and BN5) were subjected to functionalization by silicification via the Piers-Rubinsztajn reaction according to the following procedure: 50 g of activated hBN powder was dispersed in 300 mL of anhydrous toluene in a 500 mL round-bottom flask equipped with a reflux condenser under N2 atmosphere, to which 30 mg of the catalyst tris(pentafluorophenyl)borane-B(CF5)3- in 1 mL of toluene was added under stirring. In addition, the flask contained glass beads (number 40, diameter 6 mm) to promote the reaction at the interface of the glass beads and to break the hBN stacks formed during the peeling. After adding the catalyst, 4.0 mL of silicon hydride (DMS-H11 from Gelest) was slowly added to the reaction mixture, followed by continued stirring at a temperature of 60 °C for 12 hours.
[0107] The reaction mixture was then filtered and the siliconized hBN particles were washed with toluene and IPA to remove non-grafted silicone.
[0108] As proof that the silicone chains were grafted onto the hBN particles, DRIFT IR measurements were performed on a siliconized BN1 powder sample. The IR spectrum (see Figure 3, spectrum 3) clearly shows the characteristic peaks of Si-CH3 and Si-O-Si expected from the grafting reaction, thereby confirming the success of the grafting. In comparison, IR spectra 1 and 2 shown in Figure 3 were made from pre-functionalized hBN particles, before functionalization (1) and before functionalization and after exfoliation and activation (2).
[0109] Table 1 summarizes the different types of hBN powders used in the experiments to form hBN-silicone composites.
[0110] Preparation of hBN-silicone composites After siliconization of the activated hBN powder samples, composites were prepared using silicone polymer as a matrix to disperse the hBN particles.
[0111] The following procedure was followed: A mixture was prepared by mixing 34% by volume of the hBN particle sample with silicone rubber (AB specialty Andigum H110-0) and the crosslinker 2,4-dichlorobenzoyl peroxide (50% in polydimethylsiloxane; Gelest). The weight percent ratio of crosslinker to silicone was about 1-1.5. The mixture further contained 2% by weight of Siltech silicone surfactant and 3% by weight of Evonik VS10000. The dispersion was mixed in a Brabender mixture at room temperature for about 40 minutes.
[0112] Composites were made from the prepared hBN dispersion by pouring a layer of the dispersion mixture onto a metal plate and pressing it to a desired thickness by applying a pressure of 34-46 MPa for 20 minutes. Specifically, pressing was performed between two 12" x 12" metal plates with a weight of 60,000 lbs. The desired thickness was created by pressing the mixture between two metal plates containing shims as spacers with the desired sheet thickness of 0.32 mm. After cold pressing, the pressed material (sheet) was cured in an oven at 120 °C for 4 minutes.
[0113] Table 2 provides an overview of the samples prepared, indicating the type of hBN activation and the measured thermal conductivity of the composites formed. [Table 1]
[0114] The data summarized in Table 2 show that a surprising increase in thermal conductivity can be achieved when hBN powder is activated via exfoliation in a ball mill in the presence of NaOH solution. This appears to be the best activation for efficient siliconization and also has a strong effect on the formation of hBN-containing composites with silicone polymers, with the resulting composites having high thermal conductivity.
[0115] In sample E1, a material with a high thermal conductivity of 10.8 W / mK was obtained with an hBN content of only about 34 volume % based on the total volume of the composite.
[0116] Example 3 Composites are made in the same way as in Example 2 for sample E1, except that different volumetric amounts of hBN are used. The volumetric amounts are varied at 25%, 30%, and 38% by volume. Thermal conductivity is measured, and the March-Dorus orientation parameter is measured.
[0117] Example 4 A composite is formed in the same manner as Sample E1 in Example 2, except that low-polyethylene is used as the organic polymer. Thermal conductivity and March-Dorus orientation parameter are measured.
[0118] Example 5 A number of composite sheets obtained in Example 2 for sample E1 are added to a multi-layer stack of sheets before curing, the stack is compressed by applying pressure and then heat treated to effect curing of the silicone polymer.
[0119] From the pressed and cured multilayer laminate, a 0.5 mm thick composite slice is cut with a diamond wire. The composite slice is analyzed for thermal conductivity in its thickness direction (z). The thermal conductivity throughout the thickness direction (z direction, also called the through-plane direction) of the composite slice has been measured and is expected to be at least 90% of the in-plane thermal conductivity of the multilayer composite of sample E1. A diagram of a composite slice with hBN particles (14) oriented in the through-plane direction is shown in Figure 1C.
[0120] Thermal Conductivity Measurement Thermal conductivity was measured using a transient planar source device (TPS 2500 S, Hot Disk Instruments). The instrument and measurements are designed by placing a temperature sensor between two samples of the test material, introducing a heat pulse to the surface of the test sample, measuring the temperature change, and calculating the thermal conductivity based on it. The temperature sensor was a Paton-insulated Hot Disk® sensor model 5501 (radius 6.4 mm). The heat pulse was varied in the range of 60-150 mW for 3-15 seconds to ensure that the conductivity value remained constant independent of the pulse parameters. The measurements were performed according to the Hot Disk Thermal Constants Analyser Instruction Manual (2015-04-15) from Hot Disk®. A slab module was used for the measurement of in-plane thermal conductivity, and anisotropic method was applied for the measurement of through-plane thermal conductivity.
[0121] Measurement of the March-Dauras orientation parameter η X-ray diffraction analysis was performed to determine the degree of orientation (also referred to herein as alignment) of the hBN particles within the composite. For in-plane oriented hBN platelets, the primary plane of interest was the in-plane direction parallel to the surface (e.g., the (002) plane). First, 2D XRD spectra were obtained after spot diffraction of the sample on a Bruker D8 diffractometer using focused Cu Kα radiation (λ = 1.5418 Å) in step scan mode at angular positions ranging from 10° to 80°. One-dimensional (1D) XRD spectra were then obtained by integration of the 2D spectrum using a built-in function in EVA software from Bruker. The Rietveld peak fitting method was used to compare the (002) peak intensity of the oriented hBN pattern to a non-oriented hBN database pattern to obtain a quantifiable measure of orientation. An XRD spectrum showing the (002) peak is shown in Figure 2A. As more (002) hBN planes align parallel to the surface, the relative intensity of the (002) experimental peak increases compared to the database peak.
[0122] Peak fitting of the XRD patterns was performed using Topas quantitative software from Bruker. The Topas software has a built-in refinement function to determine the March-Dorus parameters using the March-Dorus function W(α). See Eq. (1) below.
number
[0123] The preferred orientation η(r) as a function of the March-Dauer parameter r can be calculated according to the following equation (2):
number
[0124] The graph in Figure 2B shows the relationship between the March-Dorus parameter r and the degree of preferred orientation η(r), also referred to herein as the "March-Dorus orientation parameter η." The solid line in the graph shows the actual measured curve, and the dashed line is a simplified linear trend line conversion of the curve.
[0125] Measurement of electrical volume resistivity The electrical resistivity of the samples was measured according to ASTM D257.
[0126] Measurement of particle size distribution of hBN particles The particle size distribution of hBN particles was measured by laser scattering using a Laser Scattering Particle Size Distribution Analyzer LA-950 manufactured by Horiba. The expressions median size (D50) and average size are used according to the HORIBA manual definition.
[0127] In the foregoing specification, the concepts have been described with reference to specific embodiments. However, those skilled in the art will recognize that various modifications and changes can be made without departing from the scope of the invention as set forth in the following claims. The specification and figures are therefore to be regarded in an illustrative rather than a restrictive sense, and all such modifications are intended to be included within the scope of the invention.
Claims
1. 1. A composite article comprising a composite comprising an organic polymer and ceramic particles comprising hexagonal boron nitride (hBN) particles distributed throughout the organic polymer, the amount of said hBN particles ranges from 20 vol.% to 40 vol.% based on the total volume of said composite; the amount of the ceramic particles is 50 volume percent or less based on the total volume of the composite; The composite article, wherein the composite has an in-plane thermal conductivity of at least 10 W / mK.
2. 2. The composite article of claim 1, wherein the hBN grains in the composite have an in-plane March-Dollase orientation parameter η of at least 50.
3. 2. The composite article of claim 1, wherein the hBN particles have an average aspect ratio of length (L) to thickness (T) of at least 5.
4. 10. The composite article of claim 1, wherein the hBN particles have an average particle size (D50) of at least 1 micron and no greater than 70 microns.
5. 10. The composite article of claim 1, wherein the composite has an electrical volume resistivity of at least 1.0E+12.
6. The composite article of claim 1 , wherein the organic polymer of the composite comprises a thermoplastic polymer or a thermoset polymer.
7. 7. The composite article of claim 6, wherein the organic polymer comprises a silicone polymer, an acrylate polymer, a polyurethane, an epoxide polymer, a polyamide, a polyimide, a liquid crystal polymer (LCP), a fluoropolymer, a polyethylene, a polypropylene, a polystyrene, a polyester, a polycarbonate, a polybutylene terephthalate (PBT), a polyethylene terephthalate (PET), a polyamide, a liquid crystal polymer (LCP), a polyacrylonitrile (PAN), a polyetheretherketone (PEEK), a polyetherketoneketone (PEKK), a polysulfone, a polyethersulfone, a polyphenylene oxide (PPO), a polyetherimide, a thermoplastic elastomer (TPE, olefinic or styrenic), a polyvinylidene fluoride (PVDF), a perfluoroalkoxyalkane (PFA), a fluorinated ethylene propylene (FEP), an ethylene tetrafluoroethylene (ETFE), or any copolymer thereof, or any combination thereof.
8. The composite article of claim 7 , wherein the organic polymer comprises a silicone polymer.
9. 9. The composite article of any one of claims 1 to 8, wherein the amount of the hBN particles is at least 92 volume %, based on the total volume of the ceramic particles.
10. 10. The composite article of claim 1, wherein the surface of the hBN particles is functionalized with an organic compound.
11. 11. The composite article of claim 10, wherein the organic compound is selected from a polysiloxane, a polysilane, a silane, or any combination thereof.
12. 1. A method of forming a composite article, comprising: preparing a mixture of ceramic particles and an organic polymer, the ceramic particles comprising hBN particles, the amount of the hBN particles being in the range of 20-40 vol.% based on the total weight of the dispersion, and the total amount of ceramic particles being 50 vol.% or less based on the total volume of the composite; applying a layer of said mixture to a mold or substrate; performing an alignment procedure for hBN particles; and solidifying and / or curing the organic polymer or organic polymerizable material to form a composite. wherein the composite has an in-plane thermal conductivity of at least 10 W / mK.
13. 13. The method of claim 12, further comprising surface functionalizing the hBN particles prior to preparing the mixture.
14. 14. The method of claim 13, wherein surface functionalization comprises exfoliating and activating the hBN particles to form activated hBN particles, and treating the activated hBN particles with an organic compound, the organic compound comprising a polysiloxane, or polysilane, or silane compound containing silicon hydride groups, or any combination thereof.
15. 15. The method of claim 14, wherein the exfoliating comprises ball milling and the activating comprises introducing OH groups onto the surface of the hBN particles.
Citation Information
Patent Citations
Boron nitride composition having enhanced function and composition made therewith
JP2007182369A
Mixed boron nitride composition and method for producing the same
JP2010505729A
Electrically insulating thermally conductive resin composition and method for producing the same
JP2016017086A
High aspect ratio boron nitride, method, and composition containing the same
JP2017510540A
Heat-conductive composite material, heat-conductive filler, and production method of the same