Composite having high thermal conductivity and method for producing said composite
The composite of an organic polymer with oriented hBN particles addresses the need for higher thermal conductivity in thermally conductive materials, achieving up to 20 W/mK in-plane conductivity for efficient heat management in electronic devices.
Patent Information
- Application Number
- JP2024522447
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-14
- Filing Date
- 2022-10-14
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-10-14
AI Technical Summary
There is a need to enhance the thermal conductivity and efficiency of thermally conductive polymer composites for effective thermal management in various industries, including consumer electronics, telecommunications infrastructure, LED lighting, hybrid and electric vehicles, and data centers.
A composite material is developed comprising an organic polymer with hexagonal boron nitride (hBN) particles dispersed throughout, where the hBN particles are oriented in-plane to achieve high thermal conductivity, with a volume fraction of hBN particles ranging from 40% to 90% and an in-plane thermal conductivity of at least 13.5 W/mK, achieved through alignment and surface functionalization of hBN particles.
The composite material exhibits enhanced thermal conductivity, reaching up to 20 W/mK in the in-plane direction, with improved packing density and alignment of hBN particles, effectively managing heat dissipation in electronic devices.
Smart Images

Figure 2024538459000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to composites comprising an organic polymer and ceramic particles, the ceramic particles including hexagonal boron nitride (hBN) particles dispersed throughout the organic polymer with a high degree of orientation, and methods of making the composites. [Background technology]
[0002] Thermally conductive polymer composites play an important role in various industries in the thermal management of electrical devices, since they can significantly reduce the operating temperature and extend the life of the devices by dissipating heat to avoid overheating. Typical industries in which thermally conductive polymer composites play an important role include consumer electronics (e.g., mobile phones, tablets), telecommunications infrastructure (e.g., cell towers), LED lighting, hybrid and electric vehicles (power modules), data centers (server boards, switches, monitoring modules, and power supplies), and solar cells.
[0003] There is a need for greater variety and efficiency of materials suitable for thermal management. [Brief description of the drawings]
[0004] The present disclosure may be better understood, and its numerous features and advantages made apparent to those skilled in the art by referencing the accompanying drawings.
[0005] [Figure 1A] FIG. 1A is a diagram showing platelet-type hBN particles, according to one embodiment. [Figure 1B] FIG. 1B includes a line drawing showing a cross-sectional side view of a composite having in-plane oriented hBN grains, according to one embodiment. [Figure 1C] FIG. 1C includes a line drawing illustrating a cross-sectional side view of a composite slice having hBN grains oriented in the through-plane direction, according to one embodiment. [Figure 2A] FIG. 2A includes a graph showing an X-ray spectrum of a composite including in-plane oriented hBN particles, according to one embodiment. [Figure 2B] Figure 2B is a graph showing the relationship between r and the orientation parameter η according to the March-Dorus method. [Figure 3A] FIG. 3A includes a graph showing the particle distribution of hBN particles contained in a composite, according to one embodiment. [Figure 3B] FIG. 3B includes a graph showing the particle distribution of hBN particles contained in a comparative composite. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0006] As used herein, the terms "comprises," "comprising," "includes," "including," "has," "having," or any other variations thereof, are intended to cover a non-exclusive inclusion. For example, a process, method, article, or apparatus that includes a list of features is not necessarily limited to only those features and may include other features that are not expressly listed or that are inherent to such process, method, article, or apparatus.
[0007] As used herein, unless clearly stated to the contrary, "or" refers to an inclusive or and not an exclusive or. For example, a condition A or B is satisfied by any one of the following: A is true (or exists) and B is false (or does not exist), A is false (or does not exist) and B is true (or exists), and both A and B are true (or exist).
[0008] Additionally, the use of "a" or "an" is used to describe elements and components described herein. This is done merely for convenience and to give a general sense of the scope of the invention. This description should be read to include one or at least one, and the singular also includes the plural, unless it is clear that otherwise is meant.
[0009] The present disclosure relates to a composite article comprising a composite including an organic polymer and ceramic particles including hexagonal boron nitride (hBN) particles distributed throughout the organic polymer, where an amount of hBN particles can range from 40 vol.% to 90 vol.% based on a total volume of the composite, where at least 90 vol.% of the ceramic particles can be hBN particles, and where an in-plane thermal conductivity of the composite can be at least 13.5 W / mK.
[0010] In one embodiment, the in-plane thermal conductivity of the composite can be at least 14.0 W / mK, or at least 14.5 W / mK, or at least 15.0 W / mK, or at least 15.5 W / mK, or at least 16.0 W / mK, or at least 16.5 W / mK, or at least 17.0 W / mK, or at least 17.5 W / mK, or at least 18.0 W / mK, or at least 18.5 W / mK, or at least 19.0 W / mK, or at least 19.5 W / mK, or at least 20 W / mK. In another aspect, the in-plane thermal conductivity can be 40 W / mK or less, or 35 W / mK or less, or 30 W / mK or less, or 25 W / mK or less.
[0011] As used herein, the term hBN particles, unless otherwise indicated, refers to platelet-shaped hBN particles having an average length-to-thickness aspect ratio (L / T) of at least 5, as shown in FIG. 1A. The hBN particles included in the composite may be unmodified or surface-modified. Unless specifically stated herein, the term hBN particles refers to both unmodified and surface-modified hBN particles.
[0012] As used further herein, the term "in-plane" refers to the xy directions of the composite. Figure IB shows a cross-section (10) of a composite in which hBN particles (12) are distributed throughout an organic polymer (14) and the hBN particles (12) may be oriented or aligned in the xy directions of the composite (which is interchangeably referred to herein as "in-plane"). In contrast, Figure 1C shows an embodiment of a composite slice in which the hBN particles (12) are aligned in the z direction, which is also interchangeably referred to herein as the "through-plane" or thickness direction of the composite.
[0013] In one embodiment, the composites of the present disclosure can be made by preparing a mixture comprising ceramic particles including hBN and an organic polymer, applying a layer of the mixture to a mold or support, performing an alignment procedure of the hBN particles, and solidifying and / or curing the organic polymer to form the composite. The mixture of hBN and the organic polymer can be a liquid mixture or a powder mixture.
[0014] In one embodiment, the alignment procedure may involve applying pressure perpendicular to the in-plane directions (xy directions) of the layer of the mixture.
[0015] In one embodiment, the hBN particles may have an average aspect ratio of the length (L) to the thickness (T) of the hBN particles of at least 5, or at least 7, or at least 10, or at least 20, or at least 30, or at least 40, or at least 50, or at least 60, or at least 70, or at least 80, or at least 90, or at least 100, or at least 110, or at least 120. In certain aspects, the aspect ratio may be 200 or less, or 120 or less, or 80 or less, or 50 or less, or 30 or less, or 15 or less.
[0016] In another embodiment, the hBN particles may have an average particle size (D50) of at least 1 micron, or at least 3 microns, or at least 5 microns, or at least 10 microns, or at least 15 microns, or at least 20 microns, or at least 25 microns, or at least 30 microns. In further aspects, the hBN particles may have an average particle size of 100 microns or less, or 50 microns or less, or 45 microns or less, or 40 microns or less, or 35 microns or less, or 30 microns or less, or 25 microns or less, or 20 microns or less, or 10 microns or less, or 5 microns or less.
[0017] In certain embodiments, the hBN particles of the composite may have a multimodal particle distribution, e.g., a bimodal or trimodal distribution. In certain aspects, the particle distribution may be a bimodal particle distribution (PSD).
[0018] In one embodiment, the particle size distribution of the hBN particles can include a first peak having a first peak maximum and a second peak having a second peak maximum, and the intensity ratio of the first peak maximum to the second peak maximum can be at least 1.5:1, or at least 2:1, or at least 2.5:1, or at least 3.0:1. In another embodiment, the intensity ratio of the first peak maximum to the second peak maximum can be 10:1 or less, or 7:1 or less, or 5:1 or less, or 4:1 or less, or 3.5:1 or less, or 3.0:1 or less.
[0019] In another embodiment, the distance between the first and second peak maxima of the hBN particle size distribution can be at least 20 microns, or at least 25 microns, or at least 30 microns, or at least 35 microns. In further embodiments, the distance between the first and second peak maxima can be 70 microns or less, or 60 microns or less, or 50 microns or less, or 40 microns or less, or 35 microns or less.
[0020] In yet another embodiment, the first peak maximum can correspond to an hBN particle size in the range of 8 microns to 13 microns, and the second peak maximum can correspond to an hBN particle size in the range of 35 to 50 microns.
[0021] In another embodiment, the difference between the average particle size (D50) and the median particle size of the hBN particles can be at least 2 microns, or at least 3 microns, or at least 4 microns, or at least 5 microns, or at least 6 microns, or at least 7 microns, or at least 8 microns, or at least 9 microns, or at least 10 microns. In further embodiments, the difference between the average particle size (D50) and the median particle size of the hBN particles can be 20 microns or less, or 15 microns or less, or 14 microns or less, or 13 microns or less, or 12 microns or less, or 11 microns or less, or 10 microns or less.
[0022] In certain embodiments, the average particle size (D50) of the hBN particles can range from 9 microns to 13 microns, and the median particle size can range from 15 microns to 25 microns.
[0023] In another embodiment, the 80th percentile of the hBN particle distribution (D90-D10) can be at least 15 microns, or at least 20 microns, or at least 25 microns, or at least 30 microns, or at least 35 microns, or at least 40 microns, or at least 45 microns, or at least 50 microns. In another embodiment, the 80th percentile of the hBN particle distribution (D90-D10) can be 80 microns or less, or 70 microns or less, or 60 microns or less, or 50 microns or less, or 45 microns or less, or 40 microns or less.
[0024] The organic polymer can be a thermoplastic polymer or a thermoset polymer.
[0025] In certain embodiments, the organic polymer may be a polymerizable polymer that includes functional groups. In certain embodiments, curing of the polymerizable monomer may be required after and / or during compression molding.
[0026] Non-limiting examples of polymerizable polymers may include silicone polymers, or acrylate polymers, or epoxy polymers.
[0027] In a particular aspect, the polymerizable polymer can be a silicone polymer containing vinyl groups. In a non-limiting embodiment, the silicone polymer containing vinyl groups can be polymerized by crosslinking with a crosslinking agent. In one aspect, the weight percent ratio of the silicone polymer containing vinyl groups to the crosslinking agent can be 0.5-5, or 1-3, or 1-2.
[0028] In certain embodiments, the silicone polymer may have a molecular weight of at least 10,000 g / mol, at least 100,000 g / mol, at least 200,000 g / mol, at least 400,000 g / mol, or at least 700,000 g / mol. In other certain embodiments, the molecular weight of the silicone polymer may be 1,000,000 g / mol or less, or 800,000 g / mol or less, or 700,000 g / mol or less, or 500,000 g / mol or less, or 300,000 g / mol or less, or 100,000 g / mol or less.
[0029] In another particular embodiment, the organic polymer can be a thermoplastic polymer.Non-limiting examples of thermoplastic polymers can include polyethylene, polypropylene, polystyrene, polyurethane, polyacrylate, polyester, polycarbonate, polyimide, polybutylene terephthalate (PBT), polymethyl methacrylate (PMMA), polyethylene terephthalate (PET), polyamide, liquid crystal polymer (LCP), polyacrylonitrile (PAN), polyether ether ketone (PEEK), polyether ketone ketone (PEKK), polysulfone, polyether sulfone, polyphenylene oxide (PPO), polyetherimide, thermoplastic elastomer (TPE, olefin-based or styrenic), fluoropolymer such as polyvinylidene fluoride (PVDF), perfluoroalkoxyalkane (PFA), fluorinated ethylene propylene (FEP), or ethylene tetrafluoroethylene (ETFE), or any copolymer thereof, or any combination thereof.
[0030] In one embodiment, the hBN particles may be surface functionalized before combining them with an organic polymer. For example, the surface functionalization of the hBN particles may include oxygen plasma treatment, or silane surface functionalization, or fluorine surface functionalization, or epoxy surface functionalization, or amine surface functionalization, or hydroxyl surface functionalization. Surface functionalization of the hBN particles may be advantageous to obtain higher solid loading of the hBN particles in the organic polymer. In certain aspects, prior to surface functionalization, the hBN particles may be subjected to exfoliation and / or activation by treatment with an OH-introducing compound.
[0031] In certain embodiments, the organic polymer can be silicone, and the hBN particles can be surface functionalized with silane, or via oxygen plasma treatment, or via fluorine surface functionalization. Non-limiting examples of silane compounds can include SiH4 or aminosilane. Examples of fluorine surface functionalization can include plasma treatment with CF4, or CHF3, SF6, or C2F6.
[0032] In another embodiment, the organic polymer can be an epoxy polymer, and the hBN particles can be surface functionalized with an epoxy compound, or an amine, or a hydroxyl group. Non-limiting examples of introducing an epoxy compound can be plasma treatment with glycidyl methacrylate or plasma treatment with allyl glycidyl ether. Examples of amine functionalization can include plasma treatment with allylamine or 3-(aminopropyl)triethoxysilane.
[0033] In a further embodiment, the organic polymer can be polyethylene and the hBN particles can be subjected to fluorine surface functionalization or silane functionalization.
[0034] In yet another embodiment, the organic polymer can be a thermoplastic polyurethane (TPU) or polybutylene terephthalate (PBT), and the hBN particles can be functionalized with epoxy compounds, amines, or hydroxyl groups. In certain further embodiments, the PBT can also be surface functionalized by oxygen plasma treatment, air plasma treatment, treatment with boric acid / urea in combination with heat treatment, or treatment with boric acid / melamine in combination with heat treatment.
[0035] In certain embodiments, a majority of the ceramic particles contained within the composite can be hBN particles, for example, at least 90 volume %, or at least 92 volume %, or at least 94 volume %, or at least 96 volume %, or at least 98 volume %, or at least 99 volume %, based on the total volume of the ceramic particles. In certain embodiments, the ceramic particles can consist essentially of hBN particles, which as used herein means having 0.5 volume % or less of ceramic particles that are not hBN particles.
[0036] The orientation of the hBN particles in the composite (also referred to herein as exchangeable alignment of the hBN particles) can be measured by performing X-ray diffraction and analyzing the X-ray spectrum according to the March-Dauer method (see detailed description in the Examples). It has been found that the March-Dauer orientation parameter η can be a suitable quantitative expression to characterize the degree of alignment of the hBN particles dispersed in the composite. Good alignment is considered in this disclosure to be a March-Dauer orientation parameter η of at least 50%. In certain embodiments, the March-Dauer orientation parameter of the hBN particles in the composite can be at least 52%, or at least 54%, or at least 56%, or at least 58%, or at least 60%.
[0037] As further demonstrated in the Examples, it has surprisingly been discovered that certain size variations of the hBN particles contained in the composite can contribute to a significant increase in the thermal conductivity of the composite.
[0038] Many different aspects and embodiments are possible. Some of these aspects and embodiments are described herein. After reading this specification, a person skilled in the art will understand that these aspects and embodiments are merely illustrative and do not limit the scope of the present invention. The embodiment may be according to any one or more of the embodiments listed below.
[0039] Embodiment Embodiment 1. A composite comprising an organic polymer and ceramic particles comprising hexagonal boron nitride (hBN) particles distributed throughout the organic polymer, wherein the amount of hBN particles ranges from 40% to 90% by volume based on the total volume of the composite; At least 90% by volume of the ceramic particles are hBN particles; The composite article, wherein the composite has an in-plane thermal conductivity of at least 13.5 W / mK.
[0040] Embodiment 2. The composite article of embodiment 1, wherein the in-plane March-Dollase orientation parameter η of the hBN particles within the composite is at least 50%.
[0041] Embodiment 3. The composite article of embodiment 1 or 2, wherein the March-Dollase orientation parameter η is at least 52%, or at least 54%, or at least 56%, or at least 58%, or at least 60%.
[0042] Embodiment 4. The composite article of any one of embodiments 1-3, wherein the in-plane thermal conductivity of the composite is at least 14.0 W / mK, or at least 14.5 W / mK, or at least 15.0 W / mK, or at least 15.5 W / mK, or at least 16.0 W / mK, or at least 16.5 W / mK, or at least 17.0 W / mK, or at least 17.5 W / mK, or at least 18.0 W / mK, or at least 18.5 W / mK, or at least 19.0 W / mK, or at least 19.5 W / mK, or at least 20 W / mK.
[0043] Embodiment 5. The composite article of any one of embodiments 1-4, wherein the in-plane thermal conductivity of the composite is 40 W / mK or less, or 35 W / mK or less, or 30 W / mK or less, or 25 W / mK or less.
[0044] Embodiment 6. The composite article of any one of the preceding embodiments, wherein the average aspect ratio of the length to thickness of the hBN particles is at least 5, or at least 10, or at least 20, or at least 30, or at least 40, or at least 50, or at least 60, or at least 70, or at least 80, or at least 90, or at least 100, or at least 110, or at least 120.
[0045] Embodiment 7. The composite article of any one of the preceding embodiments, wherein the average aspect ratio of the hBN particles is 200 or less, or 120 or less, or 80 or less, or 50 or less, or 30 or less, or 15 or less.
[0046] Embodiment 8. The composite article of any one of the preceding embodiments, wherein the hBN particles have an average particle size (D50) of at least 1 micron, or at least 3 microns, or at least 5 microns, or at least 10 microns, or at least 15 microns, or at least 20 microns, or at least 25 microns, or at least 30 microns.
[0047] Embodiment 9. The composite article of any one of the preceding embodiments, wherein the hBN particles have an average particle size of 100 microns or less, or 50 microns or less, or 45 microns or less, or 40 microns or less, or 35 microns or less, or 30 microns or less, or 25 microns or less, or 20 microns or less, or 10 microns or less, or 5 microns or less.
[0048] Embodiment 10. A composite article of any one of the preceding embodiments, wherein the hBN particles have a multimodal particle distribution.
[0049] Embodiment 11. The composite article of embodiment 10, wherein the hBN particles comprise a bimodal particle distribution.
[0050] Embodiment 12. A composite article according to any one of embodiments 10-11, wherein the particle size distribution of the hBN particles comprises a first peak having a first peak maximum and a second peak having a second peak maximum, and the intensity ratio of the first peak maximum to the second peak maximum is at least 1.5:1, or at least 2:1, or at least 2.5:1, or at least 3.0:1.
[0051] Embodiment 13. A composite article according to any one of embodiments 10-12, wherein the particle size distribution of the hBN particles comprises a first peak having a first peak maximum and a second peak having a second peak maximum, and the intensity ratio of the first peak maximum to the second peak maximum is 10:1 or less, or 7:1 or less, or 5:1 or less, or 4:1 or less, or 3.5:1 or less, or 3.0:1 or less.
[0052] Embodiment 14. The composite article of embodiment 12 or 13, wherein the distance between the first peak maximum and the second peak maximum is at least 20 microns, or at least 25 microns, or at least 30 microns, or at least 35 microns.
[0053] Embodiment 15. The composite article of any one of embodiments 12-14, wherein the distance between the first peak maximum and the second peak maximum is 70 microns or less, or 60 microns or less, or 60 microns or less, or 50 microns or less, or 40 microns or less, or 35 microns or less.
[0054] Embodiment 16. The composite article of any one of embodiments 12-15, wherein the first peak maximum corresponds to a particle size in the range of 8 microns to 13 microns and the second peak maximum corresponds to a particle size in the range of 35 to 50 microns.
[0055] Embodiment 17. A composite article according to any one of embodiments 10 to 16, wherein the difference between the average particle size (D50) and the median particle size of the hBN particles is at least 2 microns, or at least 3 microns, or at least 4 microns, or at least 5 microns, or at least 6 microns, or at least 7 microns, or at least 8 microns, or at least 9 microns, or at least 10 microns.
[0056] Embodiment 18. A composite article or method according to any one of embodiments 10 to 17, wherein the difference between the average particle size (D50) and the median particle size of the hBN particles is 20 microns or less, or 15 microns or less, or 14 microns or less, or 13 microns or less, or 12 microns or less, or 11 microns or less, or 10 microns or less.
[0057] Embodiment 19. The composite article of any one of embodiments 10-18, wherein the 80th percentile distribution value (D90-D10) of the hBN particles is at least 15 microns, or at least 20 microns, or at least 25 microns, or at least 30 microns, or at least 35 microns, or at least 40 microns, or at least 45 microns, or at least 50 microns.
[0058] Embodiment 20. A composite article according to any one of embodiments 10 to 19, wherein the 80th percentile distribution value (D90-D10) of the hBN particles can be 80 microns or less, or 70 microns or less, or 60 microns or less, or 50 microns or less, or 45 microns or less, or 40 microns or less.
[0059] Embodiment 21. A composite article according to any one of embodiments 10 to 20, wherein the hBN particles have a particle size D90 value of at least 30 microns, or at least 35 microns, or at least 40 microns, or at least 45 microns, or at least 50 microns, or at least 55 microns, or at least 60 microns.
[0060] Embodiment 22. A composite article according to any one of embodiments 10 to 20, wherein the hBN particles have a particle size D90 value of 120 microns or less, or 110 microns or less, or 90 microns or less, or 80 microns or less, or 70 microns or less, or 60 microns or less, or 55 microns or less.
[0061] Embodiment 23. A composite article according to any one of embodiments 10 to 22, wherein the hBN particles have a particle size D50 value of at least 6 microns, or at least 7 microns, or at least 8 microns, or at least 9 microns, or at least 10 microns, or at least 11 microns, or at least 12 microns, or at least 13 microns, or at least 15 microns, or at least 20 microns.
[0062] Embodiment 24. A composite article according to any one of embodiments 10 to 22, wherein the hBN particles have a particle size D50 value of 40 microns or less, or 35 microns or less, or 30 microns or less, or 25 microns or less, or 20 microns or less, or 15 microns or less.
[0063] Embodiment 25. A composite article according to any one of embodiments 10 to 24, wherein the hBN particles have a particle size D10 value of at least 1 micron, or at least 2 microns, or at least 30 microns, or at least 4 microns, or at least 5 microns, or at least 6 microns.
[0064] Embodiment 26. A composite article according to any one of embodiments 10 to 24, wherein the hBN particles have a particle size D10 value of 12 microns or less, or 10 microns or less, or 8 microns or less, or 6 microns or less, or 4 microns or less, or 2 microns or less.
[0065] Embodiment 27. A composition described in any one of embodiments 10 to 26, wherein the average particle size (D50) of the hBN particles is in the range of 9 microns to 13 microns and the median particle size is in the range of 15 microns to 25 microns.
[0066] Embodiment 28. The composite article of any one of the preceding embodiments, wherein the composite has an electrical volume resistivity of at least 1.0E+12, or at least 1.0E+13, or at least 1.0E+14.
[0067] Embodiment 29. The composite article of any one of the preceding embodiments, wherein the organic polymer of the composite comprises a thermoplastic polymer or a thermoset polymer.
[0068] Embodiment 30. The composite article of embodiment 29, wherein the organic polymer comprises a silicone polymer, an acrylate polymer, a polyurethane, an epoxide polymer, a polyamide, a polyimide, a liquid crystal polymer (LCP), a fluoropolymer, a polyethylene, a polypropylene, a polystyrene, a polyester, a polycarbonate, a polybutylene terephthalate (PBT), a polyethylene terephthalate (PET), a polyamide, a liquid crystal polymer (LCP), a polyacrylonitrile (PAN), a polyetheretherketone (PEEK), a polyetherketoneketone (PEKK), a polysulfone, a polyethersulfone, a polyphenylene oxide (PPO), a polyetherimide, a thermoplastic elastomer (TPE, olefinic or styrenic), a polyvinylidene fluoride (PVDF), a perfluoroalkoxyalkane (PFA), a fluorinated ethylene propylene (FEP), an ethylene tetrafluoroethylene (ETFE), or any copolymer thereof, or any combination thereof.
[0069] Embodiment 31. The composite article of any one of the preceding embodiments, wherein the organic polymer comprises a silicone polymer.
[0070] Embodiment 32. The composite article of embodiment 24, wherein the organic polymer consists essentially of a silicone polymer.
[0071] Embodiment 33. The composite article of any one of embodiments 24 or 25, wherein the silicone polymer has a molecular weight of at least 10,000 g / mol, at least 100,000 g / mol, at least 200,000 g / mol, at least 400,000 g / mol, or at least 700,000 g / mol.
[0072] Embodiment 34. The composite article of any one of embodiments 24-26, wherein the silicone polymer has a molecular weight of 1,000,000 g / mol or less, or 800,000 g / mol or less, or 700,000 g / mol or less, or 500,000 g / mol or less, or 300,000 g / mol or less, or 100,000 g / mol or less.
[0073] Embodiment 35. The composite article of any one of the preceding embodiments, wherein the composite further comprises a surfactant.
[0074] Embodiment 36. The composite article of embodiment 35, wherein the amount of surfactant is at least 0.1 wt%, at least 0.5 wt%, or at least 1 wt%, or at least 2 wt%, or at least 3 wt%, or at least 4 wt%, based on the total weight of the composite.
[0075] Embodiment 37. The composite article of embodiment 35, wherein the amount of surfactant is 7 wt.% or less, or 5 wt.% or less, or 3 wt.% or less, or 2 wt.% or less, based on the total weight of the composite.
[0076] Embodiment 38. The composite article of any one of embodiments 35 to 37, wherein the surfactant is a polysiloxane.
[0077] Embodiment 39. The composite article of any one of the preceding embodiments, wherein the ceramic particles of the composite comprise 92 vol.%, or at least 94 vol.%, or at least 96 vol.%, or at least 98 vol.%, or at least 99 vol.% hBN particles based on the total volume of the ceramic particles.
[0078] Embodiment 40. The composite article of any one of the preceding embodiments, wherein the ceramic particles of the composite consist essentially of hBN particles.
[0079] Embodiment 41. A composite article according to any one of the preceding embodiments, wherein the surface of the hBN particles comprises a functionalizing compound.
[0080] Embodiment 42. The composite article of embodiment 41, wherein the functionalizing compound comprises a silane compound, or an epoxy compound, or an amine compound, or a fluorine compound, or a hydroxyl group.
[0081] Embodiment 43. The composite article of any one of the preceding embodiments, wherein the composite is a sheet having a thickness of at least 25 microns, or at least 50 microns, or at least 100 microns, or at least 300 microns, or at least 500 microns, or at least 1000 microns, or at least 5000 microns.
[0082] Embodiment 44. The composite article of any one of the preceding embodiments, wherein the composite is a sheet having a thickness of 10,000 microns or less, or 5,000 microns or less, or 1,000 microns or less.
[0083] Embodiment 45. A method of forming a composite article, comprising: Preparing a mixture of ceramic particles and an organic polymer, the ceramic particles comprising at least 90 volume percent hBN particles based on the total volume of the ceramic particles, the amount of hBN particles being in the range of 40 volume percent to 90 volume percent based on the total volume of the mixture; applying a layer of the mixture to a mold or substrate; carrying out an alignment procedure of hBN particles; solidifying and / or curing the organic polymer to form a composite; The method wherein the in-plane thermal conductivity of the composite is at least 13.5 W / mK.
[0084] Embodiment 46 The method of embodiment 43, wherein the alignment step comprises applying pressure to the layer of the mixture.
[0085] Embodiment 47. The method of embodiment 44, wherein the pressure is adjusted such that the degree of in-plane March-Dorus orientation parameter of the composite after solidification and / or curing is at least 50%.
[0086] Embodiment 48. The method of embodiment 44 or 45, wherein the pressure is at least 2 MPa, or at least 100 MPa, or at least 500 MPa.
[0087] Embodiment 49. The method of any one of embodiments 43 to 46, wherein the organic polymer is a polymerizable polymer containing a functional group.
[0088] Embodiment 50. The method of embodiment 47, wherein the polymerizable polymer comprises a silicone polymer, or an acrylate polymer, or an epoxy polymer.
[0089] Embodiment 51. The method of embodiment 48, wherein the polymerizable polymer is a silicone polymer containing vinyl groups.
[0090] Embodiment 52. The method of any one of embodiments 43 to 49, wherein the mixture is essentially free of a dispersing liquid.
[0091] Embodiment 53. The method of embodiment 43, wherein the mixture is a dry powder mixture.
[0092] Embodiment 54. The method of any one of embodiments 43 to 51, further comprising surface functionalizing the hBN particles prior to preparing the mixture.
[0093] Embodiment 55. The method of embodiment 52, wherein the surface functionalization of the hBN particles comprises oxygen plasma treatment, or silane surface functionalization, or fluorine surface functionalization, or epoxy surface functionalization, or amine surface functionalization, or hydroxyl surface functionalization.
[0094] Embodiment 56 The method of embodiment 53, wherein the surface functionalization comprises a silane surface functionalization and the organic polymer comprises a silicone polymer. EXAMPLES
[0095] The following non-limiting examples illustrate the invention.
[0096] Example 1 Preparation of hBN-silicone composites Mixtures were prepared by mixing the hBN particle samples with silicone rubber (AB specialty Andigum H110-0) and the crosslinker 2,4-dichlorobenzoyl peroxide (50% in polydimethylsiloxane; Gelest). The weight percent ratio of crosslinker to silicone was about 1-1.5. The mixtures further contained 2 wt.% Siltech silicone surfactant and 3 wt.% Evonik VS10000. Mixing of the dispersions was performed at room temperature in a Brabender mixture for about 40 minutes. In all experiments in Example 1, the amount of hBN was 64% by volume based on the total volume of the liquid mixture.
[0097] In a series of experiments conducted, the hBN particles were varied by using a combination of hBN powders with different average (D50) particle sizes. The following hBN powders were used: hBN-1 with a D50 size of 5.5 microns, hBN-2 with a D50 size of 16 microns, and hBN-3 with a D50 size of 30 microns. These are also summarized in Table 1. [Table 1]
[0098] After preparing the hBN-containing polymer mixture, composites were made by sandwiching the compound between two metal plates and then pressing it at a pressure of 2-110 MPa for 20 minutes to a predetermined thickness of about 0.35 mm. Specifically, pressing was performed between two 12" x 12" metal plates with a weight of 60,000 pounds. The predetermined thickness was obtained by pressing the mixture between two metal plates containing shims as spacers with the desired sheet thickness. After cold pressing, the pressed sheet (sheet) was cured in a 120°C oven for 4 minutes to harden the silicone polymer.
[0099] From the data summarized in Table 2, it can be seen that with a total amount of hBN of 68 volume %, a high thermal conductivity of 18.3 W / mK was achieved for the combination of hBN1, hBN2, and hBN3 powders. In contrast, the measured thermal conductivity was much lower when using the combination of hBN1 and hBN2 (Comparative Sample C1) or only powder hBN1 (Comparative Sample C2). Without being bound by theory, the surprising advantage of the hBN powder combination of Sample E1 may be related to the optimized alignment and improved packing density of the hBN particles within the formed composite.
[0100] A graph of particle size distribution (PSD) measurements for a 1:1:1 mixture of hBN1 / hBN2 / hBN3 is shown in Figure 3A. The PSD is seen to be a bimodal distribution. The first peak maximum is at 10.1 microns, which is very close to the D50 particle size of 11.5 microns, while the second peak is located further away at 44.9 microns. The intensity ratio between the first and second peaks is between 2.98 and 1.0.
[0101] In contrast, the PSD of comparative sample C1 (see FIG. 3B) shows a unimodal distribution, with the D50 value and the D median being very close to each other (1.3 microns). [Table 2]
[0102] Example 2 The experiment is carried out as described in Example 1 for sample E1, except that the total amount of hBN in the liquid mixture is varied: 45% by volume (sample E2), 55% by volume (sample E3), and 70% by volume (sample E5). The thermal conductivity has been measured and is expected to be greater than 15 W / mK.
[0103] Example 3 The experiments are carried out as described in Example 1 for sample E1, except that the organic polymer is changed to TPU (sample E5) and BMP (sample E6). The thermal conductivity has been measured and is expected to be greater than 15 W / mK.
[0104] Example 4 A number of composite sheets obtained in Example 1 for sample E1 are added to a multi-layer stack of sheets before curing, the stack is compressed by applying pressure and then heat treated to effect curing of the silicone polymer.
[0105] From the pressed and cured multilayer laminate, a 0.5 mm thick composite slice is cut with a diamond wire. The composite slice is analyzed for thermal conductivity in its thickness direction (z). The thermal conductivity throughout the thickness direction (z direction, also called the through-plane direction) of the composite slice has been measured and is expected to be at least 90% of the in-plane thermal conductivity of the multilayer composite of sample E1. A diagram of a composite slice with hBN particles (14) oriented in the through-plane direction is shown in Figure 1C.
[0106] Thermal Conductivity Measurement Thermal conductivity was measured using a transient planar source device (TPS 2500 S, Hot Disk Instruments). The instrument and measurements are designed by placing a temperature sensor between two samples of the test material, introducing a heat pulse to the surface of the test sample, measuring the temperature change, and calculating the thermal conductivity based on it. The temperature sensor was a Paton-insulated Hot Disk® sensor model 5501 (radius 6.4 mm). The heat pulse was varied in the range of 60-150 mW for 3-15 seconds to ensure that the conductivity value remained constant independent of the pulse parameters. The measurements were performed according to the Hot Disk Thermal Constants Analyser Instruction Manual (2015-04-15) from Hot Disk®. A slab module was used for the measurement of in-plane thermal conductivity, and anisotropic method was applied for the measurement of through-plane thermal conductivity.
[0107] Measurement of the March-Dauras orientation parameter η X-ray diffraction analysis was performed to determine the degree of orientation (also referred to herein as alignment) of the hBN particles within the composite. For in-plane oriented hBN platelets, the primary plane of interest was the in-plane direction parallel to the surface (e.g., the (002) plane). First, 2D XRD spectra were obtained after spot diffraction of the sample on a Bruker D8 diffractometer using focused Cu Kα radiation (λ = 1.5418 Å) in step scan mode at angular positions ranging from 10° to 80°. One-dimensional (1D) XRD spectra were then obtained by integration of the 2D spectrum using a built-in function in EVA software from Bruker. The Rietveld peak fitting method was used to compare the (002) peak intensity of the oriented hBN pattern to a non-oriented hBN database pattern to obtain a quantifiable measure of orientation. An XRD spectrum showing the (002) peak is shown in Figure 2A. As more (002) hBN planes align parallel to the surface, the relative intensity of the (002) experimental peak increases compared to the database peak.
[0108] Peak fitting of the XRD patterns was performed using Topas quantitative software from Bruker. The Topas software has a built-in refinement function to determine the March-Dorus parameters using the March-Dorus function W(α). See Eq. (1) below.
number
[0109] The preferred orientation η(r) as a function of the March-Dauer parameter r can be calculated according to the following equation (2):
number
[0110] The graph in Figure 2B shows the relationship between the March-Dorus parameter r and the degree of preferred orientation η(r), also referred to herein as the "March-Dorus orientation parameter η." The solid line in the graph shows the actual measured curve, and the dashed line is a simplified linear trend line conversion of the curve.
[0111] Measurement of electrical volume resistivity The electrical resistivity of the samples was measured according to ASTM D257.
[0112] Measurement of particle size distribution of hBN particles The particle size distribution of hBN particles was measured by laser scattering using a Horiba Laser Scattering Particle Size Distribution Analyzer LA-950. The expressions median size (D50) and average size are used according to the HORIBA manual definition.
[0113] In the foregoing specification, the concepts have been described with reference to specific embodiments. However, those skilled in the art will recognize that various modifications and changes can be made without departing from the scope of the invention as set forth in the following claims. The specification and figures are therefore to be regarded in an illustrative rather than a restrictive sense, and all such modifications are intended to be included within the scope of the invention.
Claims
1. 1. A composite article comprising a composite comprising an organic polymer and ceramic particles comprising hexagonal boron nitride (hBN) particles distributed throughout the organic polymer, the amount of said hBN particles ranges from 40 vol.% to 90 vol.% based on the total volume of said composite; at least 90% by volume of the ceramic particles are hBN particles; The composite article, wherein the composite has an in-plane thermal conductivity of at least 13.5 W / mK.
2. 2. The composite article of claim 1, wherein the hBN grains in the composite have an in-plane March-Dollase orientation parameter η of at least 50%.
3. 10. The composite article of claim 1, wherein the composite has an in-plane thermal conductivity of at least 16.0 W / mK.
4. 4. The composite article of any one of claims 1 to 3, wherein the hBN particles have an average length-to-thickness aspect ratio of at least 5.
5. 10. The composite article of claim 1, wherein the hBN particles have an average particle size (D50) of at least 1 micron and no greater than 100 microns.
6. 6. The composite article of claim 5, wherein the hBN particles comprise a multimodal particle distribution.
7. 7. The composite article of claim 6, wherein the particle size distribution of the hBN particles comprises a first peak having a first peak maximum and a second peak having a second peak maximum, and an intensity ratio of the first peak maximum to the second peak maximum is at least 2:1 and not more than 10:
1.
8. 7. The composite article of claim 6, wherein the distance between said first peak maximum and said second peak maximum is at least 20 microns and not more than 70 microns.
9. 7. The composite article of claim 6, wherein the first peak maximum corresponds to a grain size in the range of 8 microns to 13 microns and the second peak maximum corresponds to a grain size in the range of 35 to 50 microns.
10. 7. The composite article of claim 6, wherein the difference between the average particle size (D50) and the median particle size of the hBN particles is at least 5 microns.
11. 10. The composite article of claim 1, wherein the composite has an electrical volume resistivity of at least 1.0E+12, or at least 1.0E+13, or at least 1.0E+14.
12. The composite article of claim 1 , wherein the organic polymer of the composite comprises a thermoplastic polymer or a thermoset polymer.
13. 15. The composite article of claim 14, wherein the organic polymer comprises a silicone polymer, an acrylate polymer, a polyurethane, an epoxide polymer, a polyamide, a polyimide, a liquid crystal polymer (LCP), a fluoropolymer, a polyethylene, a polypropylene, a polystyrene, a polyester, a polycarbonate, a polybutylene terephthalate (PBT), a polyethylene terephthalate (PET), a polyamide, a liquid crystal polymer (LCP), a polyacrylonitrile (PAN), a polyetheretherketone (PEEK), a polyetherketoneketone (PEKK), a polysulfone, a polyethersulfone, a polyphenylene oxide (PPO), a polyetherimide, a thermoplastic elastomer (TPE, olefinic or styrenic), a polyvinylidene fluoride (PVDF), a perfluoroalkoxyalkane (PFA), a fluorinated ethylene propylene (FEP), an ethylene tetrafluoroethylene (ETFE), or any copolymer thereof, or any combination thereof.
14. The composite article of claim 14 , wherein the organic polymer comprises a silicone polymer.
15. 10. The composite article of claim 1, wherein the composite is a sheet having a thickness of at least 25 microns and no greater than 5000 microns.
Citation Information
Patent Citations
Heat-conductive sheet
JP2012039060A
Resin composition and method for producing the same
JP2016108457A
Composition containing boron nitride aggregated particle, and molding using composition containing boron nitride aggregated particle
JP2016135732A
High aspect ratio boron nitride, method, and composition containing the same
JP2017510540A
Hexagonal boron nitride powder, method for producing the same, resin composition and resin sheet
JP2018104260A