Poly(butyl acrylate)-based transparent and stretchable electrochromic element composition and method for producing electrochromic member

The use of poly(butyl acrylate) and specific additives in electrochromic elements addresses electrolyte leakage issues, enhancing light transmittance, elasticity, and moisture resistance, facilitating flexible display applications.

JP2024538490AActive Publication Date: 2024-10-23KOREA UNIV OF TECH & EDUCATION IND UNIV COOPERATION FOUND
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024514130
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-14
Filing Date
2021-12-08
Publication Date
2024-10-23
Estimated Expiration
2041-12-08

AI Technical Summary

Technical Problem

Conventional electrochromic elements face issues with electrolyte leakage and require additional protective layers to prevent water vaporization, limiting their use in flexible displays.

Method used

A composition for an electrochromic element using poly(butyl acrylate) as a light-transparent polymer resin, combined with a crosslinking agent, initiator, ionic liquid, and electrochromic substances, which includes specific ratios of polyethylene glycol dimethacrylate, 1-hydroxycyclohexyl phenyl ketone, 1-butyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide, and various electrochromic materials like MHV, DHV, and TFMFPhV, to enhance light transmittance, elasticity, and flexibility.

Benefits of technology

The solution provides electrochromic elements with improved light transmittance, elasticity, and moisture resistance, enabling applications in various fields while simplifying the manufacturing process and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024538490000001_ABST
    Figure 2024538490000001_ABST
Patent Text Reader

Abstract

The present invention relates to a composition for an electrochromic device having transparency and elasticity based on poly(butyl acrylate) and a method for producing an electrochromic member. The composition for an electrochromic device according to an embodiment of the present invention includes a light-transmitting polymer resin, a cross-linking agent, an initiator, an ionic liquid, and an electrochromic material, and the light-transmitting polymer resin is poly(butyl acrylate).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composition for an electrochromic device having transparency and elasticity based on poly(butyl acrylate) and a method for producing an electrochromic member. [Background technology]

[0002] The electrochromic element contains an electrochromic material and changes color depending on the voltage applied from the outside. Various materials such as polymer compounds and metal oxides are used for the electrochromic material, and the color changes reversibly depending on the voltage applied to the electrodes.

[0003] Recently, the application of such color-changing elements has been expanding, for example, to smart window systems that block outside views and sunlight, and to automotive glass that displays information such as maps and text.

[0004] Conventional electrochromic elements use liquid electrochromic materials, which causes electrolyte leakage problems and limits their use in flexible displays. Recently, solidified water-based electrolytes have been developed, but they require an additional protective layer to prevent water from evaporating easily. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Korean Patent No. 10-2078481 Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a composition for electrochromic elements having optical transparency and elasticity, and a method for producing an electrochromic member.

[0007] Also, various electrochromic materials can be used to realize various colors.

[0008] In addition, since it has moisture resistance and flexibility, it can be applied in various fields.

[0009] Furthermore, the manufacturing method is simple, which makes it possible to increase production efficiency and reduce manufacturing costs. [Means for solving the problem]

[0010] The composition for an electrochromic device according to an embodiment of the present invention includes a light-transmitting polymer resin, a cross-linking agent, an initiator, an ionic liquid, and an electrochromic material, and the light-transmitting polymer resin is poly(butyl acrylate).

[0011] The crosslinking agent may be polyethylene glycol dimethacrylate, and the content of the crosslinking agent may be 1 to 2 parts by weight based on 100 parts by weight of the light-transmitting polymer resin.

[0012] The initiator may be 1-hydroxycyclohexyl phenyl ketone, and the content of the initiator may be 0.5 to 2 parts by weight based on 100 parts by weight of the light-transmitting polymer resin.

[0013] The ionic liquid may be 1-butyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide, and the content of the ionic liquid may be 150 to 250 parts by weight based on 100 parts by weight of the light-transmitting polymer resin.

[0014] The anode redox compound may further be included in an amount of 1 to 8 parts by weight based on 100 parts by weight of the polymer resin.

[0015] The color-changing material may be MHV, and the content of the color-changing material may be 8 to 15 parts by weight based on 100 parts by weight of the light-transmitting polymer resin.

[0016] The color-changing material may be DHV, and the content of the color-changing material may be 10 to 20 parts by weight based on 100 parts by weight of the light-transmitting polymer resin.

[0017] The color-changing material may be TFMFPhV, and the content of the color-changing material may be 1 to 10 parts by weight based on 100 parts by weight of the light-transmitting polymer resin.

[0018] The electrochromic element according to an embodiment of the present invention includes a first electrode, a second electrode, and an electrochromic element layer that changes color in response to a voltage applied between the first electrode and the second electrode, and the electrochromic element layer includes the composition for electrochromic elements described above.

[0019] A method for manufacturing an electrochromic member according to an embodiment of the present invention includes a step of mixing a light-transmitting polymer resin, a crosslinking agent, an initiator, an ionic liquid, and an electrochromic material to prepare a mixture.

[0020] In the step of preparing the mixture, the content of the crosslinker may be 1 to 2 parts by weight, the content of the initiator may be 0.5 to 2 parts by weight, and the content of the ionic liquid may be 150 to 250 parts by weight, based on 100 parts by weight of the polymer resin. Effect of the Invention

[0021] The composition for electrochromic element and the method for manufacturing an electrochromic member according to the embodiments of the present invention may have light transmittance and elasticity.

[0022] Also, various electrochromic materials can be used to realize various colors.

[0023] In addition, since it has moisture resistance and flexibility, it can be applied in various fields.

[0024] Furthermore, the manufacturing method is simple, which makes it possible to increase production efficiency and reduce manufacturing costs. [Brief description of the drawings]

[0025] [Figure 1] 4 shows the results of evaporation tests for ion gels 1 to 6. [Diagram 2]4 shows the results of tensile strength-strain measurements for ion gels 1 to 6. [Diagram 3] FIG. 1 is a Nyquist diagram showing impedance experiment results. [Figure 4] FIG. 1 is a diagram showing the results of measurement by cyclic voltammetry. [Diagram 5] FIG. 1 is a diagram showing the results of measurement by cyclic voltammetry. [Figure 6] FIG. 1 is a diagram showing the results of measurement by cyclic voltammetry. [Figure 7] FIG. 13 is a diagram showing the measurement results of light absorptance. [Figure 8] FIG. 13 is a diagram showing the measurement results of light absorptance. [Figure 9] FIG. 13 is a diagram showing the measurement results of light absorptance. [Figure 10] Photographs showing the results of bleaching and coloring experiments. [Figure 11] Photographs showing the results of bleaching and coloring experiments. [Figure 12] Photographs showing the results of bleaching and coloring experiments. [Figure 13] FIG. 13 is a diagram showing the measurement results of light transmittance. [Figure 14] FIG. 13 is a diagram showing the measurement results of light transmittance. [Figure 15] FIG. 13 is a diagram showing the measurement results of light transmittance. [Figure 16] FIG. 1 shows optical density versus charge density profile. [Figure 17] FIG. 1 shows optical density versus charge density profile. [Figure 18] FIG. 1 shows optical density versus charge density profile. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] Hereinafter, preferred embodiments of the present invention will be described with reference to the accompanying drawings. However, the embodiments of the present invention may be modified into various other forms, and the scope of the present invention is not limited to the embodiments described below. Furthermore, the embodiments of the present invention are provided to more completely explain the present invention to those having average knowledge in the relevant technical field. Therefore, the shapes and sizes of elements in the drawings may be exaggerated for clearer explanation, and elements represented by the same reference numerals in the drawings are the same elements. Furthermore, the same reference numerals are used throughout the drawings for parts having similar functions and actions. In addition, throughout the specification, "including" a certain element means that it may further include other elements, rather than excluding other elements, unless otherwise specified to the contrary.

[0027] Composition for electrochromic element The composition for an electrochromic device according to an embodiment of the present invention includes a light-transmitting polymer resin, a cross-linking agent, an initiator, an ionic liquid, and an electrochromic material, and the light-transmitting polymer resin is poly(butyl acrylate).

[0028] By using poly(butyl acrylate) (PBA) as the main polymer, the material may have optical transparency, flexibility, and elasticity. In particular, by using the crosslinker, initiator, and ionic liquid used in the embodiments of the present invention together, these properties may be further improved. The molecular formula of the poly(butyl acrylate) is (CH 12 O2) n (n is a natural number) and its chemical formula is as shown in the following Chemical Formula 1. The molecular weight of the poly(butyl acrylate) is not particularly limited, but may be 20,000 to 100,000.

[0029] [ka]

[0030] The crosslinking agent functions to improve mechanical properties such as hardness and elasticity and to provide chemical stability by forming crosslinks between the chains of the light-transmitting polymer. The crosslinking agent may be preferably polyethylene glycol dimethacrylate (PEGDA) to provide elasticity and flexibility by bonding with the light-transmitting polymer. The molecular formula of the polyethylene glycol dimethacrylate is C3H5C(O)(OCH2CH2). n It is OC(O)C3H5 (n is a natural number), and the chemical formula can be the following Chemical Formula 2.

[0031] [ka]

[0032] The content of the crosslinking agent may be 1 to 2 parts by weight, preferably 1 to 1.4 parts by weight, based on 100 parts by weight of the light-transmitting polymer resin. If the content of the crosslinking agent is too high, the light transmittance may decrease, and if the content of the crosslinking agent is too low, the mechanical properties of the manufactured color-changing element member may decrease.

[0033] The initiator serves to induce a polymerization reaction between the light-transmitting polymer and the crosslinking agent. The initiator may be 1-hydroxycyclohexyl phenyl ketone (PI). The molecular formula of 1-hydroxycyclohexyl phenyl ketone is HOC6H. 10 COC6H5, and its chemical formula can be represented by Chemical Formula 3 below.

[0034] [ka]

[0035] The content of the initiator may be 0.5 to 2 parts by weight, preferably 0.8 to 1.2 parts by weight, based on 100 parts by weight of the light-transmitting polymer resin. If the content of the initiator is too high, there may be a problem of reduced flexibility and stretchability, and if the content of the initiator is too low, there may be a problem of reduced strength.

[0036] Ionic liquids generally maintain a non-volatile state at 100° C. and improve the movement of ions and electrons in the electrochromic material. The ionic liquid may be 1-butyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide (BMIM TFSI). The molecular formula of 1-butyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide is C 10 H 15 It is F6N3O4S2 and its chemical formula is shown in Chemical Formula 4 below.

[0037] [ka]

[0038] The content of the ionic liquid may be 150 to 250 parts by weight, preferably 180 to 220 parts by weight, based on 100 parts by weight of the light-transmitting polymer resin. If the content of the ionic liquid is too low, the ionic conductivity of the ion gel may decrease, and if the content is too high, the light transmittance may decrease.

[0039] In one embodiment, the composition for an electrochromic device may further include an anode redox compound, which may be any one of ferrocene and dimethylferrocene, and is preferably dimethylferrocene. The dimethylferrocene may be represented by the following Formula 5:

[0040] [ka]

[0041] The content of the anode redox compound may be 1 to 8 parts by weight based on 100 parts by weight of the polymer resin.

[0042] An electrochromic material is a material that changes its color by changing the wavelength that it absorbs depending on an externally applied voltage. In the embodiments of the present invention, the electrochromic material may be variously used depending on the color to be realized.

[0043] To realize a red or magenta color, the electrochromic material may be 1-heptyl-[4,4'-bipyridine](hexafluorophosphate) (MHV[PF6]), which may be represented by Chemical Formula 6.

[0044] [ka]

[0045] In this case, the content of the color-changing material may be 8 to 15 parts by weight, more preferably 13 to 15 parts by weight, based on 100 parts by weight of the light-transmitting polymer resin. If the content deviates from this range, problems such as poor color realization or shortened lifespan may occur.

[0046] To realize a blue or cyan color, the electrochromic material may be 1,1'-diheptyl-[4,4'-bipyridine]bis(hexafluorophosphate) (DHV[PF6]2). The 1,1'-diheptyl-[4,4'-bipyridine]bis(hexafluorophosphate) may be represented by Chemical Formula 7.

[0047] [ka]

[0048] In this case, the content of the color-changing material may be 10 to 20 parts by weight, more preferably 16 to 18 parts by weight, based on 100 parts by weight of the light-transmitting polymer resin. If the content deviates from this range, problems such as poor color realization or shortened lifespan may occur.

[0049] To realize a green hue, the electrochromic material may be 3-fluoro-4-(trifluoromethyl)phenyl-[4,4'-bipyridine]hexafluorophosphate (TFMFPhV[PF6]2). The 3-fluoro-4-(trifluoromethyl)phenyl-[4,4'-bipyridine]hexafluorophosphate may be represented by Chemical Formula 8.

[0050] [ka]

[0051] In this case, the content of the color-changing material may be 1 to 10 parts by weight, more preferably 6 to 8 parts by weight, based on 100 parts by weight of the light-transmitting polymer resin. If the content deviates from this range, problems such as poor color realization or shortened lifespan may occur.

[0052] Electrochromic element The electrochromic element according to an embodiment of the present invention includes a first electrode, a second electrode, and an electrochromic element layer that changes color in response to a voltage applied between the first electrode and the second electrode, and the electrochromic element layer includes an electrochromic member manufactured using the above-mentioned composition for electrochromic elements.

[0053] The first and second electrodes are not particularly limited and may be made of materials commonly used in electrical devices, but may be made of ITO glass or ITO-PEN, etc., because they have optical transparency, flexibility, and stretchability.

[0054] The electrochromic element layer may include the composition for electrochromic element described above, and may be prepared in an appropriate size and thickness by the preparation method described below.

[0055] Manufacturing method of electrochromic member A method for manufacturing an electrochromic member according to an embodiment of the present invention includes a step of mixing a light-transmitting polymer resin, a crosslinking agent, an initiator, an ionic liquid, and an electrochromic material to prepare a mixture.

[0056] The light-transmitting polymer resin, the crosslinking agent, the initiator, the electrochromic material, and the ionic liquid mixed in the step of preparing the mixture are the same as those described above.

[0057] In the step of preparing the mixture, the content of the crosslinker may be 1 to 2 parts by weight, the content of the initiator may be 0.5 to 2 parts by weight, and the content of the ionic liquid may be 150 to 250 parts by weight, based on 100 parts by weight of the polymer resin.

[0058] In one embodiment, the step of preparing the mixture may include a step of curing the mixture, which may be performed by irradiating with UV light, preferably with a wavelength of 100 to 400 nm, for 2 to 30 minutes.

[0059] Manufacturing example: Manufacturing of PBA mixed ion gel Ion gel 1 0.5g of PBA as a polymer resin, 0.006g of PEGDA as a crosslinking agent, and 0.005g of PI as an initiator were mixed and then photocured for 10 minutes using a UV curing device with a wavelength of 365 nm.

[0060] Ion Gel 2 The same procedure was followed as for ion gel 1, except that 0.25 g of BMIM TFSI was further added to ion gel 1.

[0061] Ion Gel 3 The same procedure was followed as for ion gel 1, except that 0.5 g of BMIM TFSI was further added to ion gel 1.

[0062] Ion Gel 4 The same procedure was followed as for ion gel 1, except that 0.75 g of BMIM TFSI was further added to ion gel 1.

[0063] Ion Gel 5 The same procedure was followed as for ion gel 1, except that 1.0 g of BMIM TFSI was further added to ion gel 1.

[0064] Ion Gel 6 The same procedure was followed as for ion gel 1, except that 1.25 g of BMIM TFSI was further added.

[0065] Experimental example: Evaporation test Ion gels 1 to 6 were cut to a certain size, and the weights of the corresponding samples were measured while maintaining them at room temperature for 30 days under conditions of 20 to 27°C and 19 to 40% RH. Figure 1 shows the results of this experiment. Referring to Figure 1, it can be seen that there is no change in weight even if the content of ionic liquid in the ion gel increases.

[0066] Experimental example: Tensile strength-strain measurement Measurements were performed on ion gels 1 to 6 using a universal testing machine (UTM, Tinius Olsen, H5KT) according to ASTM D638 type V. Figure 2 shows the results of this experiment. Referring to Figure 2, it can be seen that the tensile strength decreases as the content of ionic liquid increases. Ion gel 5 has the most suitable flexibility and elasticity, while ion gel 6 has too low tensile strength and is easily torn, making it difficult to use as an electrochromic element. Therefore, it is determined that the most suitable amount of ionic liquid for ion gel 5 is 200 parts by weight per 100 parts by weight of the light-transmitting polymer.

[0067] Experimental example: Measurement of ionic conductivity The electrochromic members produced in the examples and comparative examples were placed between platinum electrodes, and the impedance spectrum was measured using an impedance spectrometer. Figure 4 is a Nyquist diagram showing the experimental results.

[0068] Manufacturing example: Manufacturing of electrochromic materials Example 1 0.5g of PBA as polymer resin, 0.006g of PEGDA as crosslinker, 0.005g of PI as initiator, 1g of BMIM TFSI as ionic liquid, 0.04g of MHV[PF6] as electrochromic material, and 0.022g of dimethylferrocene as anode redox compound were mixed. Then, it was photocured for 10 min in a UV curing machine with a wavelength of 365 nm.

[0069] Example 2 The same procedure as in Example 1 was repeated, except that 0.05 g of MHV[PF6] and 0.029 g of dimethylferrocene were added.

[0070] Example 3 The same procedure as in Example 1 was repeated, except that 0.06 g of MHV[PF6] and 0.036 g of dimethylferrocene were added.

[0071] Example 4 The same procedure as in Example 1 was repeated, except that 20.06 g of DHV[PF6] and 0.022 g of dimethylferrocene were used instead of MHV[PF6].

[0072] Example 5 The same procedure as in Example 4 was repeated, except that 20.07 g of DHV[PF6] and 0.027 g of dimethylferrocene were added.

[0073] Example 6 The same procedure as in Example 4 was repeated, except that 20.086 g of DHV[PF6] and 0.0319 g of dimethylferrocene were added.

[0074] Example 7 The same procedure as in Example 1 was repeated, except that 20.00965 g of TFMFPhV[PF6] and 0.005352 g of dimethylferrocene were used instead of MHV[PF6].

[0075] Example 8 The same procedure as in Example 7 was repeated, except that 0.0193 g of TFMFPhV[PF6]2 and 0.0107 g of dimethylferrocene were added.

[0076] Example 9 Example 7 The same procedure as in Example 7 was carried out, except that 0.0399 g of TFMFPhV[PF6]2 and 0.022 g of dimethylferrocene were added.

[0077] Manufacturing example: Manufacturing of electrochromic elements The electrochromic member prepared above was cut to 10 mm wide and 20 mm long, placed on ITO glass, and a spacer having a thickness of 100 μm was placed on the edge of the electrochromic member, and then the top was covered with another ITO glass. The electrochromic elements thus prepared were defined as Examples 10 to 18 corresponding to Examples 1 to 9 of the electrochromic member, respectively.

[0078] Experimental example: Cyclic voltammetry measurement 20mVs using a potential tester (biologics, SP240) -1 Current / potential curves were obtained by cyclic voltammetry for Examples 10 to 18 under the conditions above. Figure 4 shows the experimental results for Examples 10 to 12, Figure 6 shows the experimental results for Examples 13 to 15, and Figure 6 shows the experimental results for Examples 16 to 18. Referring to Figures 4 to 6, it can be seen that the higher the content of the electrochromic material, the clearer the change in current.

[0079] Experimental example: Measuring light absorption rate For Examples 12, 15, and 18, a UV-Vis Spectrometer (Perkin Elmer, Lambda 465) was used to measure in the range of 400 to 800 nm. Figures 7 to 9 are diagrams showing the experimental results for Examples 12, 15, and 18, respectively. Referring to Figures 7 to 9, Example 12 has the highest absorptance at wavelengths of 552 nm, Example 15 has the highest absorptance at wavelengths of 605 nm, and Example 18 has the highest absorptance at wavelengths of 649 nm, and it can be seen that the light absorptance is adjusted depending on the applied voltage.

[0080] Experimental example: Bleaching and coloring experiment Voltage was applied to Examples 10 to 18 to observe how each color was realized. Figures 10 to 12 are photographs showing the experimental results of Examples 10 to 12, Examples 13 to 15, and Examples 16 to 18, respectively. Referring to Figures 10 to 12, it can be seen that colors are realized depending on each electrochromic material, and that clearer colors are realized in Examples 12, 15, and 18.

[0081] Experimental example: Light transmittance experiment The transmittance of light having wavelengths of 525, 605, and 649 nm was measured for Examples 10 to 18, respectively. In this case, the change in light transmittance was observed while coloring and bleaching were performed by applying and cutting off a voltage. Figures 13 to 15 are photographs showing the experimental results of Examples 10 to 12, Examples 13 to 15, and Examples 16 to 18, respectively. Referring to Figures 13 to 15, it can be seen that the higher the content of the electrochromic material, the greater the change in light transmittance, and in particular, the changes in light transmittance of Examples 12, 15, and 18 were very excellent.

[0082] Experimental Example: Optical Density vs. Charge Density Analysis The coloring efficiency (η) was calculated by analyzing the relationship between optical density and charge density for Examples 10 to 18 under conditions of 606 nm and -1.0 V. Figures 16 to 18 are photographs showing the experimental results of Examples 10 to 12, Examples 13 to 15, and Examples 16 to 18, respectively. Referring to Figures 16 to 17, it can be seen that the higher the content of the electrochromic material, the higher the coloring efficiency (η).

[0083] The present invention is not limited by the above-described embodiments and the accompanying drawings, but is limited by the appended claims. Therefore, various substitutions, modifications, and changes can be made by a person skilled in the art without departing from the technical spirit of the present invention as set forth in the claims, and such modifications and changes are also within the scope of the present invention.

Claims

1. A light-transmitting polymer resin; A cross-linking agent; An initiator; an ionic liquid; and electrochromic materials, The electrochromic element composition, wherein the light-transmitting polymer resin is poly(butyl acrylate).

2. 2. The composition for an electrochromic device according to claim 1, wherein the crosslinking agent is polyethylene glycol dimethacrylate, and the content of the crosslinking agent is 1 to 2 parts by weight based on 100 parts by weight of the light-transmitting polymer resin.

3. 2. The composition for an electrochromic device according to claim 1, wherein the initiator is 1-hydroxycyclohexyl phenyl ketone, and the content of the initiator is 0.5 to 2 parts by weight based on 100 parts by weight of the light-transmitting polymer resin.

4. 2. The composition for an electrochromic device according to claim 1, wherein the ionic liquid is 1-butyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide, and the content of the ionic liquid is 150 to 250 parts by weight based on 100 parts by weight of the light-transmitting polymer resin.

5. 2. The composition for an electrochromic device according to claim 1, further comprising an anode redox compound in an amount of 1 to 8 parts by weight based on 100 parts by weight of the polymer resin.

6. 2. The composition for an electrochromic device according to claim 1, wherein the color-changing material is MHV, and the content of the color-changing material is 8 to 15 parts by weight based on 100 parts by weight of the light-transmitting polymer resin.

7. 2. The composition for an electrochromic device according to claim 1, wherein the color-changing material is DHV, and the content of the color-changing material is 10 to 20 parts by weight based on 100 parts by weight of the light-transmitting polymer resin.

8. 2. The composition for an electrochromic device according to claim 1, wherein the color-changing material is TFMFPhV, and the content of the color-changing material is 1 to 10 parts by weight based on 100 parts by weight of the light-transmitting polymer resin.

9. A first electrode; A second electrode; an electrochromic element layer that changes color in response to a voltage applied by the first and second electrodes; The electrochromic element layer comprises the composition for electrochromic elements according to claim 1 .

10. A method for producing an electrochromic member, comprising the steps of mixing a light-transmitting polymeric resin, a crosslinking agent, an initiator, an ionic liquid, and an electrochromic material to produce a mixture.

11. In the step of producing the mixture, The content of the crosslinking agent is 1 to 2 parts by weight based on 100 parts by weight of the polymer resin, The content of the initiator is 0.5 to 2 parts by weight, The method of claim 10, wherein the content of the ionic liquid is 150 to 250 parts by weight.

Citation Information

Patent Citations

  • Mesoporous network electrodes for electrochemical cells

    JP2004533702A

  • Electrochromic device containing a solid or quasi-solid electrolyte layer and method for manufacturing the same

    JP2016507082A

  • Gel electrolyte and electrochromic device

    JP2017090677A

  • Electrochromic photochromic optical article

    JP2021121822A

  • Electrochromic Compound, Electrochromic Device, and, Method of Driving Electrochromic Device

    KR1020180099415A