Epoxy Resin
A process using low molecular weight epoxy resins with specific additives achieves a free BPA content below 1 ppm, addressing the issues of chemical and thermal resistance in epoxy resin coatings for food and beverage containers, ensuring compliance with safety and regulatory standards.
Patent Information
- Application Number
- JP2024526743
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-04
- Filing Date
- 2022-11-03
- Publication Date
- 2024-10-23
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing epoxy resins used in coatings for food and beverage containers contain bisphenol A (BPA), which is a suspected endocrine disruptor, and current replacements lack the necessary chemical and thermal resistance, leading to issues like corrosion and BPA migration, failing to meet safety and regulatory standards.
A process producing high molecular weight epoxy resins using low molecular weight epoxy resins based on BPA with specific additives, such as dicyclopentadiene diphenol oligomers, to achieve a free BPA content below 1 ppm, ensuring chemical and thermal resistance, and forming a continuous, non-porous coating that adheres well to surfaces.
The process significantly reduces BPA migration, maintains thermal and chemical resistance, and meets safety and regulatory standards by ensuring a free BPA content of less than 1 ppm, providing stable coatings for food and beverage containers.
Smart Images

Figure 2024538836000001 
Figure 2024538836000002 
Figure 2024538836000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing epoxy resins for use in coatings, composites and adhesives, which contain less than 2 ppm, preferably less than 1 ppm, of free bisphenol A (BPA), preferably less than 1 ppm after crosslinking with a curing agent.
[0002] Additionally, a cured high molecular weight epoxy resin composition having a free BPA content of the cured high molecular weight epoxy resin that is less than 1 ppm is also disclosed. [Background technology]
[0003] There is great pressure to eliminate the use of substances suspected of affecting the human hormonal system, so-called endocrine disruptors, especially in the packaging used for beverages, such as fruit juices, carbonated drinks and beer, as well as foodstuffs.
[0004] BPA remains one of the monomers used to make epoxy resins and, downstream, protective coatings for these containers. Currently, BPA is included in the list of substances of very high concern (SVHC). Its TDI limit (=tolerable daily intake) was set by the EFSA (=European Food Safety Authority) in January 2015 with a threshold of 4 micrograms per kg of body weight per day.
[0005] Companies that have successfully used BPA-based epoxy resins for the internal protection of food and beverage cans for over 70 years are now faced with the challenge of addressing relatively stringent requirements to not only meet the necessary limits on potential BPA migration, but also to satisfy legitimate consumer concerns and rights regarding health and environmental protection.
[0006] So far, epoxy resins used for coating metal containers and pipes, coating composite pipes for drinking water, packaging and preserving food and beverages have been aimed at protecting foodstuffs from corrosion products resulting from contact with food, which are often very aggressive, both in terms of organic acids in juices and basic amino acids that attack the glass and metal of the container. In addition, the coating also serves to protect the foodstuff from any material from the container itself, such as organic or metallic materials from the components used to manufacture the container. Primers applied directly to the container surface are used to provide further protection and ensure a reliable and uniform adhesion of the coating to the container. Such primers are designed not to peel off during processing of the container carrying the coating.
[0007] Thus, the corrosion products of deteriorated containers very often in the form of organic salts and complexes contaminate food and beverages with heavy metals, which, after ingestion, tend to pass through the digestive tract and accumulate in the fatty tissue of humans.
[0008] In a recent publication, Beverages 2019.5,3;doi:10.3390 / beverages 5010003 (MDPI Journal), it is clearly documented that migration of unreacted BPA from epoxy resins is below the current acceptable limits while keeping the free BPA concentration low after synthesis and maintaining the glass transition temperature (Tg). However, there is a need to maintain a high Tg of the cured system with sufficient network polymer density, thus reducing diffusion from the coating into the food and vice versa, from the food to the metal, which is a source of corrosion products.
[0009] It is also noted in this publication that these tests are relatively harmful since up to 20% ethanol was used and the elevated temperatures were 40°C and 60°C. Similarly, migration of BPA in epoxy interior protective coatings / varnishes in children's food cans was tested and still found to have 0.1-13 ppb of extractable BPA. It is therefore clear that the use of new approaches to the synthesis of high molecular weight epoxy resins, which relatively more minimize or preferably eliminate the content of unreacted BPA, is desirable to further reduce or eliminate migration of BPA into foods and beverages.
[0010] Therefore, there is an increasing effort to replace BPA-based two-component high molecular weight epoxy resins with polyester two-component resins, polyurethanes, polyamides, and thermoplastics in general, and other polymeric coatings.
[0011] for example: US Pat. No. 7,682,674 discloses a coating composition based on PVC and acrylic resins. US Patent Application Publication No. 2003 / 0170396 discloses compositions based on epoxy novolac resins. WO 2010 / 100122 describes compositions based on epoxidized vegetable oils. WO 2012 / 091701 discloses epoxidized glycols containing hydrogenated BPA. US Pat. No. 9,139,690 discloses compositions based on epoxidized cycloaliphatic diols. US Patent No. 9,150,685 discloses diglycidyl ethers of 2-phenyl-1,3-propanediol in mixtures with BADGE (=bisphenol A diglycidyl ether), or BFDGE (=bisphenol F diglycidyl ether), or their hydrogenated variants. However, corrosion has always remained a problem. In WO 2021 / 024033, bisphenol A or F is fully replaced with oligomers of dicyclopentadiene diphenol (DCPD). However, all BPA replacement options offered so far have problems with chemical and thermal resistance and therefore do not meet the required properties of epoxy resins based on substituted BPA, which unfortunately may contain up to several thousand ppm of unreacted BPA.
[0012] Thus, existing processes for producing safe epoxy resins are based on excluding the use of standard BPA / BPF epoxy resins and instead using cycloaliphatic and aliphatic glycidyl ethers or glycidyl esters, or combinations thereof, and adducts containing polyphenols, or adducts of polyphenols with phenol and mono-, di- or polycyclopentadiene, or epoxidized derivatives thereof, alkylated or arylated bisphenols, or epoxidized derivatives thereof, as well as, for example, epoxidized sugars and oils.
[0013] However, as mentioned above, these materials have final properties that are disadvantageous and / or problematic for most applications, particularly with regard to glass transition temperature after curing, relatively poor chemical and corrosion resistance, and also relatively poor strength properties.
[0014] The formation of higher molecular weight adducts of these resins due to the cycloaliphatic or aliphatic hydroxyl, glycidyl, or glycidyl ester reactive groups is also relatively difficult and problematic, often requiring the use of increased amounts of phase transfer catalysts, and has a significant adverse effect on end-use properties, primarily related to the softening point of powder coating binders, and generally on reactivity; pot life; time to reach handling strength of coatings, composites, and adhesives; chemical resistance; thermal resistance; and associated creep resistance.
[0015] Furthermore, these products are often offered as replacements for the BPA / BPF-based high molecular weight epoxy resins originally used to treat the surfaces of containers that come into contact with drinking water and foodstuffs. Toxicity and endocrine disrupting studies for these replacements are often not yet available for many published materials. Summary of the Invention [Problem to be solved by the invention]
[0016] The drawbacks of the prior art of replacing only BPA-based epoxy resins with the above BPA-free resins and polymers are overcome by the process of the present invention for the production of chemically and thermally resistant epoxy resins and systems with various types of hardeners, for the treatment of the interior surfaces of metal containers, pipes and surfaces for drinking water and food, and possibly other protective coatings (e.g. in the medical field, for example syringe barrel coatings, etc.), with environmental protection against free BPA. [Means for solving the problem]
[0017] The subject of the present invention is a high molecular weight epoxy resin composition produced from a low molecular weight epoxy resin based on BPA with an epoxy equivalent weight of 172 to 500 g / mol, comprising: (a) dicyclopentadiene diphenol oligomers, and / or monomers, and / or polymers, and / or (b) bisphenol F or S or Z or C, or polyalkyl BPF, alkyl biphenol, polyalkyl biphenol, or polyalkyl BPA, and / or (c) a mixture of phenolic substances (a) and (b), and / or (d) aliphatic, cycloaliphatic, and aromatic polyacids, or their anhydrides, and / or (e) aliphatic and / or alicyclic and / or aromatic polyhydric alcohols or polyphenols, and / or (f) a mixture of monomers according to (a), (d), and (e); Here, the content of free BPA in the final high molecular weight epoxy resin is less than 2 ppm, preferably less than 1 ppm.
[0018] A method for producing an epoxy resin having a free BPA content of the cured high molecular weight epoxy resin that is less than 1 ppm is also disclosed.
[0019] These formulations and resulting coatings should not only reduce or prevent migration of BPA into foodstuffs and the external environment, but also, for example: - Form a continuous (homogeneous, non-porous, pinhole-free, fish-eye-free) coating film on surfaces that come into contact with drinking water and foodstuffs; - Excellent adhesion to a variety of surfaces used in the packaging and transport of beverages and foodstuffs; - and avoids delamination of the coating in the presence of contents within the package, and - Stability, which means no formation of debris, - Furthermore, there must be no sensory changes in preserved foods and beverages, medicines, and other applications; - And it must meet the user's requirements. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] In an embodiment of the present invention, the invention encompasses low molecular weight basic BPA epoxy resins, i.e. resins with an epoxy index of 0.2-0.58 epoxy equivalent per 100 g of resin or epoxy equivalent weight EEW of 172-500 g / mol, which are also reacted with DCPD diphenol oligomers, tetramethyl bisphenol F, optionally terephthalic acid, isophthalic acid, cyclohexane dicarboxylic acid, bisphenol Z, bisphenol F, 4,4'-biphenol, dimethylresorcinol, and mixtures thereof, with the required results in the application.
[0021] As seen in the structure below, for example, resins reacted with, for example, dicyclopentadiene diphenol oligomers are preferably synergistically utilized in combination with compounds or oligomers having aromatic and / or aliphatic structures, which preferably have high hydrophobicity and hydrolytic stability. Additionally, the phenolic groups provide high monomer conversion during resin synthesis and crosslinking, and preferably high functionality and branching are preferably utilized when the hardener-utilizing polymer network is formed, while also maintaining advantageous application properties, such as solubility in methyl ethyl ketone for spray applications, fast drying and adhesion to substrates, advantageous drying at elevated temperatures for excellent cure to provide the required glass transition temperature and chemical and thermal durability, etc.
[0022] The process of the present invention produces modified, low molecular weight epoxy resins based on BPA, having unreacted BPA content less than 5 ppm, by reacting with dicyclopentadiene polyphenol dimers and / or oligomers of the following structure, or optionally with other monomers, such as polycarboxylic acids and their anhydrides, alkylated bisphenols, such as tetramethylbisphenol F, novolaks, etc., such that the final reaction product, after curing with a hardener, contains free BPA well below the acceptable and often detection limit of 1 ppm, thus meeting the previously known safety, toxicological, environmental and technical requirements.
[0023] [ka]
[0024] In particular, all basic application requirements of the resulting materials, both for powder coatings, solution coatings and composites, can be met for their desired applications if the amount of unreacted BPA after curing is less than 1 ppm, which is close to the natural background and makes it possible to meet all currently required standards for food and water extractables.
[0025] Therefore, an embodiment of the present invention is to provide a formulation that substantially reduces the free BPA content in the uncured resin, without hardener and / or other additives, to a level that fully meets all current hygiene and environmental regulations, such as in the case of formula (1) using DCPD diphenol oligomers:
[0026] [ka]
[0027] Here, R 1 and / or R 2 are independently -CH3, -H, =C6H 10 , -R.
[0028] Preferably, a molecular weight of 500 to 2000 daltons, preferably 1000 to 6000 daltons, is achieved.
[0029] In another embodiment of the present invention, where alkaline hydrolysis is not taken into consideration, as shown in formula (2), the modification of BADGE is carried out by using organic polyacids such as isophthalic acid, phthalic acid or its anhydride, terephthalic acid, adipic acid or its anhydride, succinic acid or its anhydride, maleic acid or its anhydride, fumaric acid, cyclohexanedicarboxylic acid, methyltetrahydrophthalic acid, methylhexahydrophthalic acid, hexahydrophthalic acid, tetrahydrophthalic acid, etc.
[0030] TIFF2024538836000003.tif61161
[0031] Advantageously, another formulation is contemplated, in which the formulations described by formula (1) and formula (2) are combined, thereby achieving the required optimum performance properties by mutual combination of monomers with BPA type low molecular weight epoxy resins.
[0032] The advantage of the above solution is that it allows to use existing technical equipment and processes for producing medium and high molecular weight BPA type epoxy resins in the temperature range of 50°C to 250°C, the usual standard amounts of catalysts based on onium salts, such as ammonium salts, phosphonium salts, and other catalysts commonly used in the above reactions, are in the range of 0.001 to 5% by weight, the standard molar ratios of reactants are given by their reactivity depending on the catalyst used and the softening point of the resulting resin, and either flaky strips or final transfer of the resin in solution with the desired reactive or non-reactive solvent or solvent mixture, or aqueous dispersion of the desired drying property and viscosity. Preferred onium salt catalysts are selected from: ethyltriphenylphosphonium bromide, ethyltriphenylphosphonium chloride, triphenylphosphine, benzyltributylammonium chloride, benzyltriethylammonium chloride, benzyltrimethylammonium chloride, tetrabutylammonium bromide, tetramethylammonium chloride, tetramethylammonium bromide, tetrabutylammonium hydrogen sulfate, trioctylmethylammonium chloride, benzyltriethylammonium bromide, tetraethylammonium chloride, trimethylamine, phosphonium halide salts, and the like.
[0033] The curing process for resins produced according to the present invention is the same as that used for standard BPA resins, using reactive sites such as epoxy groups, hydroxyl groups, or other introduced groups such as amine or amide type groups depending on the end use of the application such as coatings, composites, adhesives, etc. This curing process also significantly reduces the level of unreacted BPA in the entire system by the following reaction with epoxy groups, or salt formation with amines, amides, or hydrogen bonding with polar groups in the cured material.
[0034] In another embodiment of the present invention, a hardenable composition of high molecular weight epoxy resin is prepared. The hardenable composition of high molecular weight epoxy resin includes a hardener and a high molecular weight epoxy resin in an amount of 10 to 97% by weight.
[0035] The curing agents used to produce the curable high molecular weight epoxy resin compositions according to the present invention are selected from polyetheramines, aliphatic, cycloaliphatic, heterocyclic, and aromatic polyamines, and / or their cycloaliphatic, aliphatic, and aromatic epoxides, urea derivatives, and adducts with dicyandiamide.
[0036] Furthermore, the curing agents used to produce the curable high molecular weight epoxy resin compositions according to the present invention are also based on polyamides and aminoamides based on aliphatic, cycloaliphatic, heterocyclic, and aromatic amines and polyamines and / or their adducts with cycloaliphatic, and aliphatic, dimeric, and polymeric aliphatic mono- and di- and polycarboxylic acids.
[0037] Preferred amino curing agents are also selected from dicyandiamide (DICY), isophoronediamine (IPDA), diethylenetriamine (DETA), triethylenetetramine (TETA), bis(p-aminocyclohexyl)methane (PACM), ethylenediamine (EDA), tetraethylenepentamine (TEPA), polyoxypropylenediamine, polyoxypropylenetriamine, polyetheramine D230, T403, etc., diaminodiphenylmethane (DDM), diaminodiphenylsulfone (DDS), 2,4-diamino-1-methylcyclohexane, 2,6-diamino-1-methylcyclohexane, 2,4-diamino-3,5-diethyltoluene, 2,6-diamino-3,5-diethyltoluene, 3,3',5,5'-tetramethyl-4,4'-diaminobiphenyl and 3,3'-dimethyl-4,4'-diaminodiphenyl, and aminoplast resins, etc.
[0038] Furthermore, the curing agents used to produce the curable high molecular weight epoxy resin compositions according to the present invention are also based on polyamides and aminoamides: polyesters, anhydrides, i.e. aliphatic, cycloaliphatic, heterocyclic and aromatic, polyanhydrides and polyacids, and / or their adducts with cycloaliphatic, aliphatic and aromatic epoxides.
[0039] Preferred anhydride hardeners are selected from: hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, endomethylenetetrahydrophthalic anhydride, methylnadic anhydride, methylbutenyltetrahydrophthalic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, cyclohexanetricarboxylic anhydride, methylcyclohexenedicarboxylic anhydride, methylcyclohexanetetracarboxylic dianhydride, maleic anhydride, phthalic anhydride, succinic anhydride, dodecenylsuccinic anhydride, octyloxy ... ctenylsuccinic anhydride, pyromellitic anhydride, trimellitic anhydride, alkylstyrene-maleic anhydride copolymer, chlorendic anhydride, polyazelaic anhydride, benzophenone tetracarboxylic anhydride, ethylene glycol bisanhydrotrimellitate, glycerol trimellitate, glycerol bis(anhydrotrimellitate) monoacetate, benzophenone tetracarboxylic acid, polyadipic anhydride, polysebacic anhydride, poly(ethyloctadecanedioic) anhydride, poly(phenylhexadecanedioic) anhydride, HET anhydride, norbornane-2,3-dicarboxylic anhydride.
[0040] Additionally, curing agents used to produce the curable high molecular weight epoxy resin compositions according to the present invention may also be based on melamine, urea, and phenol formaldehyde resins, novolacs, and polyphenols such as dicyclopentadiene diphenol.
[0041] Preferred hardeners are selected from phenol-formaldehyde, resorcinol-formaldehyde, catechol-formaldehyde, hydroquinone-formaldehyde, cresol-formaldehyde, chloroglucinol-formaldehyde, pyrogallol-formaldehyde, melamine-formaldehyde, urea-formaldehyde.
[0042] The curing process of the resins produced according to the present invention further employs curing agents based on masked or unmasked polyisocyanates and also based on Lewis bases such as trimethylamine, quinuclidine, pyridine, tetrahydrothiophene, and / or trimethylphosphine, and Lewis acids such as FeCl3, AlCl3, SbCl5, SnCl4, TiCl4, BF3, SO2Cl2, and / or metal triflate complexes.
[0043] Another embodiment of the present invention includes a process for producing a curable high molecular weight epoxy resin, said curable high molecular weight epoxy resin being produced by using a composition of high molecular weight epoxy resin based on BPA, with an epoxy equivalent weight of 172-500 g / mol, and a selected curing agent, and oligomers, monomers, and / or polymers of dicyclopentadiene diphenol, and / or bisphenol F or S or Z or C, or polyalkyl BPF, alkyl biphenol, polyalkyl biphenol, or polyalkyl BPA, and / or mixtures of the above phenolic substances, and / or aliphatic, cycloaliphatic, and aromatic polyacids, or anhydrides thereof, and / or aliphatic, and / or cycloaliphatic, and / or aromatic polyhydric alcohols, or polyphenols, and / or mixtures of the above monomers, wherein the content of free BPA in the final high molecular weight epoxy resin is less than 2 ppm, preferably less than 1 ppm. EXAMPLES
[0044] Production of resin according to the present invention
[0045] Example 1
[0046] A four-neck flask equipped with a stirrer, thermometer, reflux condenser, inert gas inlet, and heating nest was charged with the following: - 262.89 g of low molecular weight epoxy resin having an epoxy equivalent weight of 192 g / mol of epoxy groups, 137.1 g of dicyclopentadiene diphenol oligomers with an equivalent weight of 168 g / mol, and - ethyltriphenylphosphonium bromide addition catalyst in an amount of 0.05%.
[0047] Stirring was started and the reaction mixture was heated to a temperature of 140° C. under an inert nitrogen stream and reacted for 4 hours while controlling the content of epoxide groups. After the reaction was completed, the product had an epoxy equivalent weight of 685 g / mol of epoxy groups, a softening point of 103° C., and a viscosity of a 40% (by weight) solution in butyl glycol of 283 mPas.
[0048] Analysis of free BPA content in epoxy resins was performed by high performance liquid chromatography (HPLC) using an Agilent 1260 Infinity II liquid chromatograph with an Agilent Poroshell 120 EC-C18 2.7 μm 4.6 × 100 mm column. The mobile phase consisted of 60% methanol and 40% water (for samples, the resin was washed from the column with pure tetrahydrofuran (THF) for 10 min). The flow rate of the mobile phase was 1 ml / min. Samples were prepared as solutions in THF with a concentration of about 10 mg / ml. The mobile phase consisted of 60% methanol and THF. The concentrations of the calibration solutions were in the range of about 0.1-9 exp.-5 mg / ml and the dosage was 3 μl.
[0049] There were nine calibration solutions, each dosed in duplicate. Samples were prepared in triplicate, with each solution dosed in duplicate. The free BPA content in the prepared epoxy resin was below the detection limit, i.e., less than 1 ppm.
[0050] Further analysis of the free BPA content in the resulting epoxy resin was carried out using a quantitative test developed by Solvias AG, "Method for the determination of Bisphenol-A in the solid epoxy resins by LC / MS" (Standard No. CSOP-0724_01). The free BPA content in the resulting epoxy resin was less than 1 ppm.
[0051] Example 2
[0052] A four-neck flask equipped with a stirrer, thermometer, reflux condenser, inert gas inlet, and heating nest was charged with the following: - 294.9 g of low molecular weight epoxy resin having an epoxy equivalent weight of 192 g / mol of epoxy groups, 105.1 g of dicyclopentadiene diphenol oligomer with an equivalent weight of 168 g / mol, and - ethyltriphenylphosphonium bromide addition catalyst in an amount of 0.05%.
[0053] Stirring was started and the reaction mixture was heated to a temperature of 140° C. under an inert nitrogen stream and reacted for 4 hours while controlling the content of epoxide groups. After the reaction was completed, the product had an epoxy equivalent weight of 450 g / mol of epoxy groups, a softening point of 91° C., and a viscosity of a 40% (by weight) solution in butyl glycol of 151 mPas.
[0054] The content of free BPA was analyzed by HPLC using a calibration for BPA (according to Example 1) with a detection limit of less than 1 ppm.
[0055] Example 3
[0056] A four-neck flask equipped with a stirrer, thermometer, reflux condenser, inert gas inlet, and heating nest was charged with the following: - 237.7 g of low molecular weight epoxy resin having an epoxy equivalent weight of 192 g / mol of epoxy groups, 162.3 g of dicyclopentadiene diphenol oligomers with an equivalent weight of 168 g / mol, and - ethyltriphenylphosphonium bromide addition catalyst in an amount of 0.1%.
[0057] Stirring was started and the reaction mixture was heated to a temperature of 180° C. under an inert nitrogen stream and reacted for 6 hours while controlling the content of epoxide groups. After the reaction was completed, the product had an epoxy equivalent weight of 1482 g / mol of epoxy groups, a softening point of 128° C., and a viscosity of a 40% (by weight) solution in butyl glycol of 76 mPas.
[0058] The content of free BPA was analyzed by HPLC using a calibration for BPA (according to Example 1) with a detection limit of less than 1 ppm.
[0059] Example 4
[0060] A four-neck flask equipped with a stirrer, thermometer, reflux condenser, inert gas inlet, and heating nest was charged with the following: - 227 g of low molecular weight epoxy resin having an epoxy equivalent weight of 192 g / mol of epoxy groups, 173 g of dicyclopentadiene diphenol oligomers with an equivalent weight of 168 g / mol, and - ethyltriphenylphosphonium bromide addition catalyst in an amount of 0.1%.
[0061] Stirring was started, and the reaction mixture was heated to a temperature of 190°C under an inert nitrogen flow and reacted for 6 hours while controlling the content of epoxide groups. After the reaction was completed, the product had an epoxy equivalent of 2655 g / mol of epoxy groups and a softening point of 151°C.
[0062] The content of free BPA was analyzed by HPLC using a calibration for BPA (according to Example 1) with a detection limit of less than 1 ppm.
[0063] Example 5
[0064] A four-neck flask equipped with a stirrer, thermometer, reflux condenser, inert gas inlet, and heating nest was charged with the following: - 227 g of low molecular weight epoxy resin having an epoxy equivalent weight of 192 g / mol of epoxy groups, - 50 g of isophthalic acid, and - ethyltriphenylphosphonium bromide addition catalyst in an amount of 0.05%.
[0065] Stirring was started, and the reaction mixture was heated to a temperature of 140°C under an inert nitrogen flow and reacted for 4 hours while controlling the content of epoxide groups. After the reaction was completed, the product had an epoxy equivalent of 470 g / mol of epoxy groups and a softening point of 82°C.
[0066] The content of free BPA was analyzed by HPLC using a calibration for BPA (according to Example 1) with a detection limit of less than 1 ppm.
[0067] Example 6
[0068] A four-neck flask equipped with a stirrer, thermometer, reflux condenser, inert gas inlet, and heating nest was charged with the following: - 227 g of low molecular weight epoxy resin having an epoxy equivalent weight of 192 g / mol of epoxy groups, - 50 g of cyclohexanedicarboxylic acid, and - ethyltriphenylphosphonium bromide addition catalyst in an amount of 0.05%.
[0069] Stirring was started, and the reaction mixture was heated to a temperature of 140°C under an inert nitrogen flow and reacted for 4 hours while controlling the content of epoxide groups. After the reaction was completed, the product had an epoxy equivalent of 455 g / mol of epoxy groups and a softening point of 75°C.
[0070] The content of free BPA was analyzed by HPLC using a calibration for BPA (according to Example 1) with a detection limit of less than 1 ppm.
[0071] Example 7
[0072] A four-neck flask equipped with a stirrer, thermometer, reflux condenser, inert gas inlet, and heating nest was charged with the following: - 227 g of low molecular weight epoxy resin having an epoxy equivalent weight of 192 g / mol of epoxy groups, - 56g terephthalic acid, - 56 g of dicyclopentadiene diphenol oligomer with an equivalent weight of 168 g / mol, - ethyltriphenylphosphonium bromide addition catalyst in an amount of 0.05%.
[0073] Stirring was started, and the reaction mixture was heated to a temperature of 180°C under an inert nitrogen flow and reacted for 6 hours while controlling the content of epoxide groups. After the reaction was completed, the product had an epoxy equivalent of 1967 g / mol of epoxy groups and a softening point of 135°C.
[0074] The content of free BPA was analyzed by HPLC using a calibration for BPA (according to Example 1) with a detection limit of less than 1 ppm.
[0075] Example 8
[0076] A four-neck flask equipped with a stirrer, thermometer, reflux condenser, inert gas inlet, and heating nest was charged with the following: - 227.0 g of low molecular weight epoxy resin having an epoxy equivalent weight of 192 g / mol of epoxy groups, - 137 g of tetramethylbisphenol F with an equivalent weight of 128.17 g / mol, - ethyltriphenylphosphonium bromide addition catalyst in an amount of 0.05%.
[0077] Stirring was started and the reaction mixture was heated to a temperature of 200° C. under an inert nitrogen flow and reacted for 6 hours while controlling the content of epoxide groups. After the reaction was completed, the product had an epoxy equivalent weight of 3264 g / mol of epoxy groups, a softening point of 155° C., and a viscosity of a 40% (by weight) solution in butyl glycol of 151 mPas.
[0078] The content of free BPA was analyzed by HPLC using a calibration for BPA (according to Example 1) with a detection limit of less than 1 ppm.
[0079] Example 9
[0080] A four-neck flask equipped with a stirrer, thermometer, reflux condenser, inert gas inlet, and heating nest was charged with the following: - 227.0 g of low molecular weight epoxy resin having an epoxy equivalent weight of 192 g / mol of epoxy groups, - 101 g of bisphenol Z with an equivalent weight of 134.18 g / mol, - ethyltriphenylphosphonium bromide addition catalyst in an amount of 0.05%.
[0081] Stirring was started and the reaction mixture was heated to a temperature of 140° C. under an inert nitrogen flow and reacted for 4 hours while controlling the content of epoxide groups. After the reaction was completed, the product had an epoxy equivalent weight of 767 g / mol of epoxy groups, a softening point of 105° C., and a viscosity of a 40% (by weight) solution in butyl glycol of 305 mPas.
[0082] The content of free BPA was analyzed by HPLC using a calibration for BPA (according to Example 1) with a detection limit of less than 1 ppm.
[0083] Example 10
[0084] A four-neck flask equipped with a stirrer, thermometer, reflux condenser, inert gas inlet, and heating nest was charged with the following: - 227.0 g of low molecular weight epoxy resin having an epoxy equivalent weight of 192 g / mol of epoxy groups, - 102.5 g of 4,4'-biphenol with an equivalent weight of 93.1 g / mol, - ethyltriphenylphosphonium bromide addition catalyst in an amount of 0.05%.
[0085] Stirring was started, and the reaction mixture was heated to a temperature of 200°C under an inert nitrogen flow and reacted for 4 hours while controlling the content of epoxide groups. After the reaction was completed, the product had an epoxy equivalent of 2030 g / mol of epoxy groups and a softening point of 145°C.
[0086] The content of free BPA was analyzed by HPLC using a calibration for BPA (according to Example 1) with a detection limit of less than 1 ppm.
[0087] Example 11
[0088] A four-neck flask equipped with a stirrer, thermometer, reflux condenser, inert gas inlet, and heating nest was charged with the following: - 100.0 g of low molecular weight epoxy resin having an epoxy equivalent weight of 192 g / mol of epoxy groups, - 25 g of bisphenol F with an equivalent weight of 100.12 g / mol, - 30 g of dicyclopentadiene diphenol oligomer with an equivalent weight of 294.55 g / mol, - ethyltriphenylphosphonium bromide addition catalyst in an amount of 0.05%.
[0089] Stirring was started and the reaction mixture was heated to a temperature of 140° C. under an inert nitrogen flow and reacted for 4 hours while controlling the content of epoxide groups. After the reaction was completed, the product had an epoxy equivalent weight of 806 g / mol of epoxy groups, a softening point of 101° C., and a viscosity of a 40% (by weight) solution in butyl glycol of 315 mPas.
[0090] The content of free BPA was analyzed by HPLC using a calibration for BPA (according to Example 1) with a detection limit of less than 1 ppm.
[0091] Example 12
[0092] A four-neck flask equipped with a stirrer, thermometer, reflux condenser, inert gas inlet, and heating nest was charged with the following: - 235.0 g of low molecular weight epoxy resin having an epoxy equivalent weight of 192 g / mol of epoxy groups, - 77 g of dimethylresorcinol with an equivalent weight of 69.08 g / mol, - ethyltriphenylphosphonium bromide addition catalyst in an amount of 0.05%.
[0093] Stirring was started, and the reaction mixture was heated to a temperature of 190°C under an inert nitrogen flow and reacted for 4 hours while controlling the content of epoxide groups. After the reaction was completed, the product had an epoxy equivalent of 2022 g / mol of epoxy groups and a softening point of 140°C.
[0094] The content of free BPA was analyzed by HPLC using a calibration for BPA (according to Example 1) with a detection limit of less than 1 ppm.
[0095] Example 13
[0096] A powder coating composition based on epoxy resin according to Example 1 was produced by using a carboxyl-containing polyester hardener Crylcoat 340 with an acid value of 75 mg KOH / g. TiO2 pigment (Kronos 2160), BlacFixe F filler with a volume concentration (PVC) of 15% by volume, benzoin as an antifoaming agent, and Resiflow PV-85 as a flow promoter were further added.
[0097] [Table 1]
[0098] The resulting composition was extruded twice, ground to a particle size of 20-80 microns, and electrostatically sprayed onto a grounded metal plate, which was then cured at 180° C. for 20 minutes.
[0099] [Table 2]
[0100] Free BPA content in the mill-cured coatings was analyzed by HPLC after extraction in a Soxhlet apparatus with tetrahydrofuran, using a calibration for BPA (according to Example 1) with a detection limit of less than 1 ppm. .
[0101] Example 14
[0102] A coating composition for use as a protective coating for metal containers was prepared by dissolving a 45% by weight solution of the epoxy resin prepared according to Example 4 in a mixture of methyl isobutyl ketone and Dowanol PM, and further mixing with melamine-formaldehyde resin Cymel 303 in a ratio of 70 parts epoxy binder and 30 parts Cymel 303 hardener. TiO2 pigment (Kronos 2160), BlacFixe F filler at a volume concentration (PVC) of 15% by volume, Byk A 530 as an antifoaming agent, and Disperbyk 163 as a dispersing additive were further added. The resulting composition was cured at 140°C for 30 minutes.
[0103] [Table 3]
[0104] [Table 4]
Claims
1. A high molecular weight epoxy resin composition comprising a BPA-based low molecular weight epoxy resin having an epoxy equivalent weight of 172 to 500 g / mol and: (a) oligomers and / or monomers and / or polymers of dicyclopentadiene diphenol, and / or (b) bisphenol F or S or Z or C, or polyalkyl BPF, alkyl biphenol, polyalkyl biphenol, or polyalkyl BPA, and / or (c) a mixture of phenolic materials (a) and (b), and / or (d) aliphatic, cycloaliphatic, and aromatic polyacids or their anhydrides, and / or (e) aliphatic and / or alicyclic and / or aromatic polyhydric alcohols or polyphenols, and / or (f) a mixture of monomers according to (a), (d), and (e); and The content of free BPA in the final high molecular weight epoxy resin is less than 2 ppm, preferably less than 1 ppm; A high molecular weight epoxy resin composition.
2. 2. The high molecular weight epoxy resin composition according to claim 1, wherein the average molecular weight of the high molecular weight epoxy resin composition is in the range of 1,000 to 6,000 daltons.
3. 3. The high molecular weight epoxy resin composition of claim 1 or 2, wherein the BPA-based low molecular weight epoxy resin comprises a diglycidyl ether of bisphenol A.
4. 4. A composition of the cured high molecular weight epoxy resin of any one of claims 1 to 3, which has been cured with a hardener, and the cured high molecular weight epoxy resin has a free BPA content of less than 1 ppm.
5. The curing agent is: (a) polyetheramines, aliphatic, cycloaliphatic, heterocyclic, and aromatic polyamines, and / or their cycloaliphatic, aliphatic, and aromatic adducts with epoxides, urea derivatives, and dicyandiamide, and / or (b) polyesters, anhydrides, i.e. aliphatic, cycloaliphatic, heterocyclic and aromatic polyanhydrides and polyacids, and / or their adducts with cycloaliphatic, aliphatic and aromatic epoxides, and / or (c) polyamides and aminoamides based on aliphatic, cycloaliphatic, heterocyclic, and aromatic amines, polyamines, and their adducts with cycloaliphatic, dimeric, and polymeric aliphatic mono-, di-, and polycarboxylic acids, and / or (d) melamine, urea, and phenol formaldehyde resins, novolacs, and polyphenols such as dicyclopentadiene diphenol, and / or (e) a masked or unmasked polyisocyanate; and / or (f) Lewis bases and acids; The composition of claim 4, wherein the curing agent is selected from the group consisting of:
6. 6. The cured high molecular weight epoxy resin composition of claim 4 or 5, wherein the proportion of resin is 10 to 97% by weight, the remainder of the composition being the curing agent.
7. 1. A method for producing a high molecular weight BPA-based epoxy resin, comprising: reacting a low molecular weight BPA-based epoxy resin having an epoxy equivalent weight of 172-500 g / mol with a (a) oligomers and / or monomers and / or polymers of dicyclopentadiene diphenol, and / or (b) bisphenol F or S or Z or C, or polyalkyl BPF, alkyl biphenol, polyalkyl biphenol, or polyalkyl BPA, and / or (c) a mixture of phenolic materials (a) and (b), and / or (d) aliphatic, cycloaliphatic, and aromatic polyacids, or anhydrides thereof, and / or (e) aliphatic and / or alicyclic and / or aromatic polyhydric alcohols or polyphenols; and / or (f) a mixture of monomers according to (a), (d), and (e); and reacting in the presence of a catalyst based on an ammonium salt or a phosphonium salt at a temperature in the range of 50 to 250° C., The process wherein the free BPA content of the resulting high molecular weight epoxy resin is less than 2 ppm, preferably less than 1 ppm.
8. The ammonium or phosphonium salt based catalyst comprises: Ethyl triphenylphosphonium bromide, ethyl triphenylphosphonium chloride triphenylphosphine, benzyl tributyl ammonium chloride, benzyl triethyl ammonium chloride, benzyl trimethyl ammonium chloride, tetrabutyl ammonium bromide, tetramethyl ammonium chloride, tetramethyl ammonium bromide, tetrabutyl ammonium hydrogen sulfate, trioctyl methyl ammonium chloride, benzyl triethyl ammonium bromide, tetraethyl ammonium chloride, trimethyl amine, halogenated phosphonium salts, etc.
8. A method for producing the high molecular weight epoxy resin of claim 7, selected from the group consisting of:
9. 7. A method for producing a composition comprising the cured high molecular weight epoxy resin of claim 5 or 6, wherein the resin is cured with a curing agent, and the final free BPA content of the cured high molecular weight epoxy resin is less than 1 ppm.
10. The curing agent is (a) polyetheramines, aliphatic, cycloaliphatic, heterocyclic, and aromatic polyamines, and / or their cycloaliphatic, aliphatic, and aromatic adducts with epoxides, urea derivatives, and dicyandiamide, and / or (b) polyesters, anhydrides, i.e. aliphatic, cycloaliphatic, heterocyclic and aromatic polyanhydrides and polyacids, and / or their adducts with cycloaliphatic, aliphatic and aromatic epoxides, and / or (c) polyamides and aminoamides based on aliphatic, cycloaliphatic, heterocyclic, and aromatic amines, polyamines, and their adducts with cycloaliphatic, dimeric, and polymeric aliphatic mono-, di-, and polycarboxylic acids, and / or (d) melamine, urea, and phenol formaldehyde resins, novolacs, and polyphenols such as dicyclopentadiene diphenol, and / or (e) a masked or unmasked polyisocyanate; and / or (f) Lewis bases and acids is a hardener based on The cured high molecular weight epoxy resin contains less than 1 ppm of free BPA. The method of claim 9.
Citation Information
Patent Citations
JP1975005760A
Epoxy resin composition and powder coating material
JP1998036637A
Production method of high-molecular-weight epoxy resin
JP2001172362A
Solid materials prepared from epoxy resins and phenolic hydroxyl-containing materials
US4394497A
A modified epoxy resin
WO2021024033A1