Cold-rolled heat-treated steel sheet and its manufacturing method

A cold-rolled heat-treated steel sheet with a specific composition and manufacturing process addresses the challenge of achieving high strength, yield strength, and elongation, while maintaining weldability and forming compatibility, by utilizing controlled chemical elements and manufacturing steps.

JP2024538879AInactive Publication Date: 2024-10-24ARCELORMITTAL SA
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024525314
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-10-29
Publication Date
2024-10-24
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing high-strength and high-formability steel sheets lack the simultaneous achievement of strength exceeding 1440 MPa, yield strength greater than 1120 MPa, and total elongation of 6.5% or more, while maintaining good weldability and coating ability, as well as compatibility with forming processes.

Method used

A cold-rolled heat-treated steel sheet with specific chemical composition and microstructure, including 0.2% to 0.35% carbon, 0.5% to 1.5% manganese, and controlled proportions of other elements, combined with a manufacturing process involving hot rolling, annealing, and cold rolling to achieve the desired mechanical properties.

Benefits of technology

The solution achieves an ultimate tensile strength of more than 1440 MPa, yield strength greater than 1120 MPa, a YS/TS ratio of greater than 0.70, total elongation of 6.5% or more, and maintains good weldability and coating ability, ensuring compatibility with forming processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024538879000001
    Figure 2024538879000001
  • Figure 2024538879000002
    Figure 2024538879000002
  • Figure 2024538879000003
    Figure 2024538879000003
Patent Text Reader

Abstract

The present invention deals with a cold rolled heat treated steel sheet having, by weight percentage, 0.2%≦C≦0.35%, 0.5%≦Mn≦1.5%, 0.1%≦Si≦0.6%, 0%≦Al≦0.1%, 0.01%≦Ti≦0.1%, 0.0001%≦B≦0.010%, 0%≦P≦0.02%, 0%≦S≦0.03%, 0%≦N≦0.09%, and may contain optional elements, and the microstructure of the steel includes, by area percentage, at least 80% tempered martensite, 3-15% bainite, 1%-7% martensite, 0-12% ferrite, and 0-2% retained austenite.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cold-rolled steel sheet suitable as a steel sheet for vehicles. [Background technology]

[0002] Automotive parts must meet two contradictory requirements: ease of forming and strength. In recent years, in consideration of global environmental issues, automobiles have been given a third requirement: improved fuel efficiency. Therefore, automotive parts must now be made from materials with high formability to meet the criteria of ease of fitting into complex automotive assemblies, and at the same time, the strength must be improved for the crashworthiness and durability of the vehicle while reducing the vehicle's weight for improved fuel efficiency. In addition, steel parts must be weldable without liquid metal embrittlement.

[0003] Therefore, research and development efforts are being made to reduce the amount of material used in automobiles by increasing the strength of the materials. Conversely, increasing the strength of steel sheets reduces their formability, so there is a need to develop materials that have both high strength and high formability.

[0004] Prior research and development in the field of high strength and highly formable steel plates has resulted in several methods for producing high strength and highly formable steel plates, some of which are listed herein for the final evaluation of the present invention.

[0005] EP3561119 provides a tempered martensitic steel having a low yield ratio and excellent uniform elongation, and the tempered martensitic steel contains, by weight percent, 0.2-0.6% C, 0.01-2.2% Si, 0.5-3.0% Mn, 0.015% or less P, 0.005% or less S, 0.01-0.1% Al, 0.01-0.1% Ti, 0.05-0.5% Cr, 0. It contains 0.005-0.005% B, 0.05-0.5% Mo, 0.01% or less N, the balance being Fe and unavoidable impurities, has a yield ratio of 0.4-0.6, a product of tensile strength and uniform elongation (TS*U-El) of 10,000MPa% or more, and has a microstructure with 90% or more tempered martensite, 5% or less ferrite, and the balance being bainite, in terms of area ratio. However, the YS / TS ratio is not achieved. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] European Patent Application Publication No. 3561119 Summary of the Invention

[0007] Known prior art techniques for producing high strength and highly formable steel plates suffer from the deficiencies of one or the other. Thus, there is a need for a cold rolled steel plate having a strength of greater than 1440 MPa and a method for producing the same.

[0008] The object of the present invention is to solve the above problems by making available a cold rolled, heat treated steel sheet which simultaneously has: - an ultimate tensile strength of at least 1440 MPa, preferably greater than 1470 MPa; - A yield strength of more than 1120 MPa, preferably more than 1130 MPa.

[0009] In a preferred embodiment, the cold rolled heat treated steel sheet has a total elongation of 6.5% or more.

[0010] In a preferred embodiment, the cold rolled heat treated steel sheet exhibits a YS / TS ratio of greater than 0.70.

[0011] Advantageously, such a steel may also have good suitability for forming, especially rolling, together with good weldability and coatability.

[0012] Another object of the invention is also to make available a manufacturing method for these plates that is robust to shifts in manufacturing parameters, while being compatible with conventional industrial applications.

[0013] The cold rolled, heat treated steel sheet of the present invention may be optionally coated with zinc or a zinc alloy, or aluminum or an aluminum alloy, to improve its corrosion resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Other features and advantages of the present invention will become apparent from the following detailed description of the invention.

[0015] Carbon is present in the steel in an amount between 0.2% and 0.35%. Carbon is a necessary element for retarding the formation of ferrite and bainite during cooling after annealing, thereby increasing the strength of the steel sheet. At a content below 0.2%, the steel of the invention will not have adequate tensile strength and ductility. On the other hand, if the carbon content exceeds 0.35%, the welds and heat-affected zones will be significantly hardened, and the mechanical properties of the welds will be impaired. The preferred limit of carbon is 0.22% to 0.33%, and the more preferred limit is 0.22% to 0.3%.

[0016] The manganese content of the steel of the present invention is 0.5%-1.5%. Manganese is a strength imparting element and more than 0.5% manganese is necessary to retard the formation of ferrite and to impart strength and hardenability to the steel sheet. Therefore, a higher percentage of manganese is preferred, such as 0.55-1.4%, more preferably 0.6%-1.3%. However, manganese exceeding 1.5% has adverse effects such as retarding the transformation from austenite to bainite during isothermal holding of the bainite transformation and reducing ductility. Also, manganese exceeding 1.5% leads to the formation of martensite beyond the target limit and thus to reduced elongation. Furthermore, a manganese content exceeding 1.5% leads to central segregation and also to reduced weldability of the steel. Furthermore, a high manganese content is detrimental in terms of hydrogen delayed fracture, which is an important criterion for steel manufacturers and the automotive industry.

[0017] The silicon content of the steel of the present invention is between 0.1% and 0.6%. Silicon is an element that contributes to strength improvement by solid solution strengthening. Silicon is a constituent that can delay the precipitation of carbides during cooling after annealing, therefore silicon promotes the formation of martensite. However, silicon is also a ferrite former and also increases the Ac3 transformation point, which pushes the annealing temperature to a higher temperature range, which is why the silicon content is kept at a maximum of 0.6%. A silicon content above 0.6% can also strengthen embrittlement, in addition silicon also impairs coatability. The preferred limit of silicon presence is between 0.1% and 0.5%, more preferably between 0.15% and 0.4%.

[0018] The aluminum content of the steel of the present invention is 0-0.1%. Aluminum can be added during steelmaking to deoxidize the steel and capture oxygen. Above 0.1%, the Ac3 point becomes high and productivity decreases. Also, within such ranges, aluminum combines with nitrogen in the steel to form aluminum nitrides, reducing the grain size, and aluminum also retards the precipitation of cementite, but in the present invention, when the aluminum content exceeds 0.1%, the amount and size of aluminum nitrides are detrimental to hole expansion and bending, and also pushes Ac3 into a higher temperature range that is industrially very expensive to achieve, and further causes grain coarsening during annealing and soaking. The preferred limit of aluminum is 0%-0.06%, more preferably 0%-0.05%.

[0019] Titanium is an element added to the steel of the invention in an amount of 0.01% to 0.1%, preferably 0.01% to 0.09%. The formation of carbides, nitrides and carbonitrides is suitable for imparting strength to the steel according to the invention by precipitation hardening during the resulting annealing soaking temperature range after full annealing becomes finer, leading to hardening of the product. However, titanium contents exceeding 0.1% are not preferred for the invention, since titanium consumes carbon by forming a large amount of precipitates, which tend to reduce the ductility of the steel.

[0020] Boron is an essential element and can be added in an amount of 0.0001% to 0.010%, preferably 0.001% to 0.004%, to harden the steel. Boron blocks said nitrides to form boron nitrides, which give the steel of the invention strength. Boron also gives the steel of the invention hardenability. However, it has been found that the addition of more than 0.010% boron significantly reduces the rollability of the steel sheet. Further boron segregation can occur at the grain boundaries, which is detrimental to formability.

[0021] The phosphorus content of the steel of the invention is limited to 0.02%. Phosphorus is a hardening element in solid solution. Small amounts of phosphorus, at least 0.002%, can therefore be advantageous, but phosphorus also has its negative effects, such as reduced spot weldability and hot rollability, due in particular to its tendency to segregate at grain boundaries or co-segregate with manganese. For these reasons, its content is preferably limited to a maximum of 0.015%.

[0022] Sulfur is not an essential element, but may be present in the steel as an impurity. The lower the sulfur content, the better, but from the viewpoint of production costs, it is 0.03% or less, preferably 0.005% at most. Furthermore, if higher sulfur is present in the steel, it will combine with Mn and Ti to form sulfides, which will adversely affect the bending, hole expansion and elongation of the steel of the present invention.

[0023] Nitrogen is limited to 0.09% to avoid degradation of the material over time and to minimize the precipitation of nitrides during solidification, which is detrimental to the mechanical properties of the steel.

[0024] Molybdenum is an optional element and is present in the steel of the present invention in an amount of 0% to 0.9%. Molybdenum plays an effective role in improving hardenability and hardness, and when added in an amount of at least 0.01%, it retards the formation of ferrite and bainite during cooling after annealing. Mo is also beneficial for the toughness of hot rolled products, making them easier to manufacture. However, the addition of molybdenum excessively increases the cost of adding alloying elements, so for economic reasons, its content is limited to 0.9%. The preferred limit for molybdenum is 0% to 0.7%, more preferably 0% to 0.6%.

[0025] Chromium is an optional element in the steel of the present invention and is present in amounts between 0% and 0.6%. Chromium provides strength and hardening to the steel, but if used in amounts greater than 0.5%, it will detract from the surface finish of the steel. The preferred limits for chromium are 0.01% to 0.5%, more preferably 0.01% to 0.4%.

[0026] Niobium is an optional element and may be present in the range of 0% to 0.09%, preferably 0.001% to 0.08%, more preferably 0.01% to 0.07%. The formation of carbonitrides is suitable for imparting strength to the steel according to the invention by precipitation hardening during the resulting annealing soaking temperature range after full annealing becomes finer, leading to hardening of the product. However, when the niobium content exceeds 0.09%, the consumption of carbon by niobium by forming a large amount of carbonitrides is not preferred for the invention, since a large amount of carbonitrides tends to reduce the ductility of the steel.

[0027] Vanadium is an optional element that may be added to the steel of the present invention in amounts between 0% and 0.1%, preferably between 0.001% and 0.1%. Like niobium, vanadium plays a role in hardening, since it participates in carbonitrides. But it also participates in forming VN, which appears during solidification of the cast product. The amount of V is limited to 0.1% to avoid coarse VN, which is detrimental to hole expansion. If the vanadium content is less than 0.001%, vanadium does not have any effect on the steel of the present invention.

[0028] In order to increase the strength and improve the corrosion resistance of the steel of the present invention, 0% to 2% copper may be added as an optional element. To obtain such effects, a minimum of 0.01% copper is preferable. However, if the copper content exceeds 2%, the surface morphology may deteriorate.

[0029] The optional addition of nickel in an amount of 0-2% can increase the strength and toughness of the steel of the present invention. A minimum of 0.01% is preferred to achieve this effect. However, if its content exceeds 2%, nickel can cause a decrease in ductility.

[0030] Calcium is an optional element that may be added to the steel of the present invention in an amount of 0% to 0.005%, preferably 0.001% to 0.005%. Calcium is added to the steel of the present invention as an optional element, especially during inclusion treatment. Calcium contributes to the smelting of the steel by supplementing the sulfur content, which has a negative effect on the spheroidization of the steel.

[0031] Other elements such as cerium, magnesium or zirconium can be added individually or in combination in the following proportions: Ce≦0.1%, Mg≦0.05% and Zr≦0.05%. Up to the maximum content levels indicated, these elements make it possible to refine the inclusion particles during solidification.

[0032] The balance of the steel composition consists of iron and unavoidable impurities resulting from processing.

[0033] The microstructure of the steel sheet according to the present invention comprises, by area percentage, at least 80% tempered martensite, 3% to 15% bainite, 1% to 7% martensite, 0% to 12% ferrite, and 0 to 2% retained austenite.

[0034] The surface fraction of a phase in the microstructure is measured by the following method: a sample is cut from the steel sheet, polished and etched with reagents known per se to reveal the microstructure. The cross section is then examined using a scanning electron microscope, for example a scanning electron microscope with a field emission gun ("FEG-SEM"), in secondary electron mode at a magnification of more than 5000 times.

[0035] The fraction of ferrite is determined by SEM observation after etching with Nittal or picral / Nittal reagents. The retained austenite is determined by XRD and the partitioned martensite by dilatometry tests according to SMC V Van Bohemen and J. Sietsma in the publication Metallurgical and Materials transactions, Vol. 40A, May 2009-1059.

[0036] The tempered martensite constitutes at least 80% of the microstructure by area fraction. It originates from martensite, which is formed on cooling after annealing, in particular below the Ms temperature, more specifically below Ms-10°C. Such martensite is tempered during holding at a tempering temperature Ttemper between 200°C and Ms-10°C. The tempered martensite of the present invention imparts ductility and strength to such steel. Preferably, the content of tempered martensite is between 80% and 95%, more preferably between 80% and 90%.

[0037] Bainite is present in an amount of 3% to 15%. In the framework of the present invention, bainite may include carbide-free bainite and / or lath bainite and granular bainite. When present, lath bainite is in the form of laths with a thickness of 1 micron to 5 microns. When present, carbide-free bainite has a very low density of carbides and is less than 100 μm. 2 Bainite has less than 100 carbides per area unit and may contain island austenite. When present, granular bainite is a grain form with carbides present intragranularly. Bainite provides improved elongation. The preferred presence of bainite is 3% to 12%, more preferably 3% to 11%.

[0038] The ferrite constitutes 0% to 12% of the microstructure in terms of area fraction of the steel of the present invention. The ferrite imparts strength and elongation to the steel of the present invention. The ferrite of the present steel may include polygonal ferrite, lath ferrite, acicular ferrite, plate ferrite or epitaxial ferrite. The ferrite of the present invention is formed during cooling after annealing. However, if the content of ferrite is more than 10% in the steel of the present invention, the hardness difference with hard phases such as tempered martensite, martensite, bainite, etc. becomes large, the local ductility decreases, and the total elongation and yield strength decrease, so that both the yield strength and the total elongation cannot be obtained at the same time. The preferred limit of the ferrite of the present invention is 0% to 11%, more preferably 0% to 10%.

[0039] Martensite constitutes 1% to 7% of the microstructure by area fraction. In the present invention, fresh martensite is formed by cooling the cold rolled steel sheet after overaging. Martensite imparts ductility and strength to the steel of the present invention. However, if the presence of fresh martensite exceeds 10%, it imparts excess strength but reduces elongation beyond the allowable limit of the steel of the present invention, because fresh martensite has the same amount of carbon content as retained austenite and therefore fresh martensite is brittle and hard. Therefore, the preferred limit of fresh martensite for the steel of the present invention is 1% to 6%, more preferably 1% to 5%.

[0040] Retained austenite is an optional microstructure that may be present in steel at 0% to 2%.

[0041] The cold rolled steel sheet according to the invention can be produced by any suitable method. A preferred method consists in providing a semi-finished casting of steel having the chemical composition according to the invention. Casting can be carried out in ingots or continuously in the form of thin slabs or thin strip, i.e. with thicknesses ranging from about 220 mm for slabs to several tens of millimeters for thin strip.

[0042] For example, a slab is considered a semi-finished product. The slab having the above chemical composition is produced by continuous casting, and the slab is preferably subjected to a soft reduction directly during casting to ensure the elimination of center segregation and porosity reduction. The slab provided by the continuous casting process can be used directly at high temperature after continuous casting, or it can be first cooled to room temperature and then reheated for hot rolling.

[0043] The temperature of the slabs subjected to hot rolling should preferably be at least 1000° C., preferably above 1150° C. and below 1300° C. If the temperature of the slab is below 1150° C., excessive loads will be applied to the rolling mill, and the temperature of the steel may drop to the ferrite transformation temperature during the finish rolling, so that the steel is rolled with transformed ferrite in its structure. Moreover, the temperature should not exceed 1300° C., as this is industrially expensive.

[0044] The temperature of the slab is high enough to allow hot rolling to be completed entirely in the austenitic field and for the final hot rolling temperature to remain above 850° C. It is necessary that the final rolling be performed above 850° C., because below this temperature the rollability of the steel sheet is significantly reduced.

[0045] The sheet thus obtained is then cooled to a temperature of 680°C or less at a cooling rate of at least 5°C / s. Preferably, the cooling rate is less than or equal to 100°C / s and higher than 10°C / s. The hot rolled steel sheet is then coiled at a coiling temperature of less than 680°C, preferably between 500°C and 680°C, more preferably between 520°C and 670°C. The coiled hot rolled steel sheet is then cooled, preferably to room temperature. The hot rolled sheet can then be subjected to an optional descaling process, such as pickling, to remove scale formed during hot rolling and ensure that the surface of the hot rolled steel sheet is free of scale before the hot rolled steel sheet is subjected to an optional hot band annealing.

[0046] The hot rolled sheet may be subjected to an optional hot band annealing at a temperature between 350°C and 750°C for 1 to 96 hours. The temperature and time of such hot band annealing are selected to ensure softening of the hot rolled sheet and to facilitate cold rolling of the hot rolled steel sheet. The hot rolled sheet may then be subjected to an optional descaling process, such as pickling, to remove scale formed during the hot band annealing.

[0047] Next, the hot-rolled steel sheet is cooled to room temperature, and then cold-rolled at a rolling reduction of 35 to 90% to obtain a cold-rolled steel sheet.

[0048] The cold rolled steel sheet is then subjected to annealing to impart the desired microstructure and mechanical properties to the steel of the present invention.

[0049] In the annealing, the cold rolled steel sheet is heated from room temperature to a soaking temperature TA of Ac3+10°C to Ac3+150°C at a heating rate HR1 of 1°C / sec to 30°C / sec. The heating rate HR1 is 1°C / sec to 20°C / sec, more preferably 1°C / sec to 10°C / sec. The preferred TA temperature is 800°C to 900°C.

[0050] The cold rolled steel sheet is then held at the annealing soaking temperature TA for 100-1000 seconds to ensure sufficient transformation to form 100% austenite at the end of the soak. The cold rolled steel sheet is then cooled at an average cooling rate CR1 of 5°C / s-200°C / s, preferably 8°C / s-100°C / s, more preferably 10°C / s-70°C / s, to a cooling stop temperature range CS1 of Ms-Ms-150°C, preferably 200°C-350°C, more preferably 220°C-330°C. The steel is held at the CS1 temperature for a time of 1 s-500 s. During this cooling step, the martensite of the present invention is formed. If the CS1 temperature is higher than Ms-40°C, the steel of the present invention has too much austenite which is detrimental to the total elongation, and if CS1 is lower than Ms-150°C, the amount of fresh martensite is too high and the total elongation target is not achieved.

[0051] The cold-rolled steel sheet is then cooled to room temperature at a cooling rate of at least 1° C. / sec to obtain a cold-rolled heat-treated steel sheet.

[0052] The resulting cold rolled heat treated steel sheet can then be optionally coated by any of the known methods. The coating can be made with zinc or a zinc-based alloy, or with aluminum or an aluminum-based alloy.

[0053] To ensure degassing of the coated product, an optional post-batch annealing, preferably at 170-210°C for 12-30 hours, can be performed after coating the product, followed by cooling to room temperature to obtain the cold-rolled coated steel sheet. EXAMPLES

[0054] The following tests and examples presented herein are non-limiting in nature and must be considered for illustrative purposes only, showing the advantageous features of the invention, explaining the importance of the parameters selected by the inventors after extensive experimentation, and further establishing the properties that may be achieved by the steel according to the invention.

[0055] Samples of steel sheets according to the invention and several comparative grades of steel sheets were prepared using the compositions summarized in Table 1 and the processing parameters collected in Table 2. The corresponding microstructures of these steel sheets are summarized in Table 3 and the properties are summarized in Table 4.

[0056] Table 1 lists steels having compositions expressed in weight percent, and also lists the Ac3 and Ms for each steel, where the Ac3 and Ms temperatures are calculated from the formula derived by Andrews published in Journal of the Iron and Steel Institute, 203, 721-727, 1965.

[0057] Ac3(℃)=910-203×(%C)^(1 / 2)-15.2×(%Ni)+44.7×(%Si)+104×(%V)+31.5×(%Mo)+13.1 ×(%W)-30×(%Mn)-11×(%Cr)-20×(%Cu)+700×(%P)+400×(%Al)+120×(%As)+400×(%Ti).

[0058] Ms(℃)=539-423×(%C)-30.4×(%Mn)-12.1×(%Cr)-17.7×(%Ni)-7.5×(%Mo)

[0059] [Table 1]

[0060] Table 2 summarizes the annealing process parameters performed on the steels in Table 1.

[0061] Furthermore, before the annealing treatment of the steels of the present invention and the reference examples, the samples were heated to a temperature of 1150° C. to 1300° C. and hot rolled. All trials were cold rolled with a cold rolling reduction of 55%.

[0062] [Table 2]

[0063] Table 3 summarizes the results of tests carried out according to standards on different microscopes, such as scanning electron microscopes, to measure the microstructural composition, in area fraction, of both the steel of the invention and the reference trials.

[0064] [Table 3]

[0065] From the above table it can be seen that all trials according to the invention meet the microstructure target, which is not the case for the reference examples.

[0066] Table 4 summarizes the mechanical and surface properties of both the inventive and reference steels.

[0067] <Table 4: Mechanical properties of the trials> The yield strength YS, tensile strength TS and total elongation TE are measured according to the ISO standard ISO 6892-1 published in October 2009.

[0068] [Table 4]

[0069] From the above table, it can be seen that the tests according to the invention all meet the target properties, which is not the case for the reference examples.

Claims

1. 2. A cold rolled heat treated steel sheet comprising the following elements expressed in weight percent: 0.2%≦C≦0.35%, 0.5%≦Mn≦1.5%, 0.1%≦Si≦0.6%, 0%≦Al≦0.1%, 0.01%≦Ti≦0.1%, 0.0001%≦B≦0.010%, 0%≦P≦0.02%, 0%≦S≦0.03%, 0%≦N≦0.09% and any of the following elements: 0%≦Cr≦0.6%, 0%≦Nb≦0.09%, 0%≦Mo≦0.9%, 0%≦V≦0.1%, 0%≦Ni≦2%, 0%≦Cu≦2%, 0%≦Ca≦0.005%, 0%≦Ce≦0.1%, 0%≦Mg≦0.05%, 0%≦Zr≦0.05% and the balance of the composition is composed of iron and unavoidable impurities resulting from processing, and the microstructure of the steel includes, by area percentage, at least 80% tempered martensite, 3 to 15% bainite, 1% to 7% martensite, 0 to 12% ferrite, and 0 to 2% retained austenite.

2. 2. The cold rolled heat treated steel sheet according to claim 1, wherein said composition comprises 0.22% to 0.33% carbon.

3. 3. The cold rolled heat treated steel sheet according to claim 1 or 2, wherein the composition comprises 0.55% to 1.4% manganese.

4. The cold rolled heat treated steel sheet according to any one of claims 1 to 3, wherein the composition comprises 0% to 0.06% aluminum.

5. The cold rolled heat treated steel sheet according to any one of claims 1 to 4, wherein the composition comprises 0.1% to 0.5% silicon.

6. The cold rolled heat treated steel sheet according to any one of claims 1 to 5, wherein the martensite is 1% to 6%.

7. The cold rolled heat treated steel sheet according to any one of claims 1 to 7, wherein the tempered martensite is 80% to 95%.

8. 9. The cold rolled heat treated steel sheet according to any one of the preceding claims, wherein the sheet has an ultimate tensile strength of at least 1440 MPa and a yield strength of at least 1120 MPa.

9. A method for producing a cold-rolled heat-treated steel sheet comprising the following successive steps: - Providing a steel composition according to any one of claims 1 to 5, - reheating said semi-finished product to a temperature between 1000°C and 1300°C, - rolling said semi-finished product in the austenitic range with a hot rolling finishing temperature above 850 ° C to obtain a hot rolled steel sheet; - cooling the sheet at a cooling rate of at least 5°C / s to a coiling temperature of not more than 680°C and coiling the hot-rolled sheet; - cooling the hot rolled sheet to room temperature; - optionally subjecting said hot rolled steel plate to a descaling process; - optionally subjecting the hot rolled steel sheet to annealing; - optionally subjecting said hot rolled steel plate to a descaling process; - cold rolling the hot rolled steel sheet at a rolling reduction of 35 to 90% to obtain a cold rolled steel sheet; - then heating said cold-rolled steel sheet from room temperature to a temperature TA of Ac3+10°C to Ac3+150°C at a heating rate HR1 of 1°C / s to 30°C / s and holding it for 100 to 1000 seconds; - cooling the cold-rolled steel sheet from TA to a temperature CS1 of from Ms to Ms-150°C at a cooling rate CR1 of from 5°C / s to 200°C / s; - then holding the cold-rolled steel sheet at the CS1 temperature for 1 to 500 seconds; - followed by cooling to room temperature at a cooling rate of at least 1°C / s to obtain a cold rolled heat treated steel sheet.

10. The method of claim 9, wherein the coiling temperature is between 680°C and 500°C.

11. The method according to claim 9 or 10, wherein CS1 is from 200°C to 350°C.

12. The method according to any one of claims 9 to 11, wherein HR1 is from 1°C / s to 20°C / s.

13. The method according to any one of claims 9 to 12, wherein TA is between 800°C and 900°C.

14. Use of a steel sheet obtainable according to any one of claims 1 to 8 or produced by the method according to any one of claims 9 to 13 for the manufacture of structural parts of a vehicle.

Citation Information

Patent Citations

  • Method for producing high-strength cold-rolled steel sheet with excellent steel sheet shape

    JP2013227657A

  • Cold-rolled steel sheet and method for producing the same

    JP2016008310A

  • Cold rolled and heat treated steel sheet and a method of manufacturing thereof

    WO2019092577A1

  • A cold rolled martensitic steel and a method of martensitic steel thereof

    WO2020250098A1

  • Tempered martensitic steel having low yield ratio and excellent uniform elongation, and manufacturing method therefor

    EP3561119A1