Method for producing cellulose pulp

A method for producing high-quality cellulose dope from waste textiles by shredding, chemical separation, and filtration effectively addresses the challenges of recycling mixed cotton and synthetic fibers, enhancing the quality and versatility of cellulose production.

JP2024539053AInactive Publication Date: 2024-10-28インデュオ
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024523112
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-15
Filing Date
2022-10-12
Publication Date
2024-10-28
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The recycling of textiles containing a mixture of cotton and synthetic fibers is challenging due to their composition, leading to low-quality cellulose production and the presence of impurities, making them unsuitable for high-value applications.

Method used

A method involving shredding, chemical separation, filtration, and dissolution processes to produce high-quality cellulose dope from waste textiles, including steps to remove non-cellulosic components and impurities, such as using alkaline solutions and phase transfer catalysts to separate and purify cellulose fibers.

Benefits of technology

The method enables the production of high-quality cellulose dope with reduced impurities, expanding the availability of textiles for recycling and improving the quality of regenerated cellulose fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024539053000001_ABST
    Figure 2024539053000001_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing cellulose pulp from waste textiles containing cellulose fibers in a mass percentage of more than 50%, the method comprising the steps of shredding the waste textiles to obtain a first mixture of shredded fibers and residues, separating at least a portion of the non-cellulose components from the first mixture to obtain a second mixture having a mass percentage of cellulose fibers higher than the mass percentage of cellulose fibers in the first mixture, filtering the second mixture to recover a solid phase containing cellulose fibers, dissolving the cellulose fibers of the solid phase to obtain a cellulose pulp containing undissolved particles, and filtering the cellulose pulp to obtain the cellulose pulp separated from the undissolved particles.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to the field of producing dissolved cellulose dope, particularly cellulose dope made from waste textiles. [Background technology]

[0002] Worldwide, millions of tons of waste textile fibres are generated every year. For example, it is estimated that 85% of purchased clothing is discarded within one year of purchase. Much of this waste textile comprises waste textiles based on a mixture of cotton fibres and synthetic fibres, mainly polyester fibres. In the clothing industry, cotton-based clothing for example accounts for 35% of the market.

[0003] Cotton fibers are composed of cellulose, a naturally occurring polymer found in many plant species. Cellulose constitutes 35-50% of plant biomass, making it the most common compound in plant biomass. It is present in almost pure form and in fibrous form in cottonseed hairs. These cotton fibers are harvested from the cotton plant and consist of long intertwined cellulose polymer chains. These fibers are spun, colored, and finally woven, knitted, and assembled into textiles. Natural fibers, especially cotton-based fibers, are raw materials that are generally subject to price fluctuations due to climate change and political and socio-economic instability in major producing regions.

[0004] Cotton cultivation is a resource- and energy-intensive crop. For example, it is estimated that approximately 3000 liters of water are required to produce approximately 500 grams of cotton fiber. In addition, the cultivation of this plant requires extensive use of pesticides and large areas of cultivation, which generates large amounts of greenhouse gases. The cost of cotton production is rising due to the increasing demand for agricultural land, decreasing access to water, and a growing world population and therefore a growing demand for cotton. Thus, cotton production is seen as unsustainable, and it is assumed that cotton will not be profitable in the future.

[0005] Therefore, there is a need to find ways to reuse cotton from waste textiles that contain cotton. However, textiles that contain cotton are mainly present in the form of a mixture of cotton fibers and synthetic fibers. Therefore, in order to reuse cotton, it is necessary to separate the cotton from the synthetic fibers and chemicals potentially present in the textile. However, these textiles have the disadvantage that they are difficult to recycle due to their composition and the capacity of recycling methods. Therefore, textiles based on cotton and synthetic fibers are usually sold as second-hand goods or torn up for reuse as low-quality textiles.

[0006] However, some recent methods for recycling textiles based on cotton and synthetic fibers have shown better results. They are carried out by dissolving the cellulose of the cotton and isolating it from the synthetic fibers. The major drawback of this method is the low quality of the cellulose obtained. In fact, a large amount of impurities such as chemicals or synthetic fibers present in the waste textiles are present in the dissolved cellulose solution, degrading the quality of the regenerated cellulose fibers. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] International Publication No. 2021 / 181007 Summary of the Invention [Problem to be solved by the invention]

[0008] Therefore, there is a need to provide a method for recycling textiles, including cotton and synthetic fibers, among other materials, that allows for the production of higher quality cellulose dope. [Means for solving the problem]

[0009] The present disclosure improves the above situation.

[0010] A method for producing a cellulose dope from waste textiles containing cellulose fibers in a mass percentage of more than 50%, comprising the steps of: - S1 shredding waste textiles to obtain a first mixture of shredded fibres and residues; - S2 separating at least a portion of the non-cellulosic components from the first mixture to obtain a second mixture having a higher percentage by weight of cellulose fibers than the percentage by weight of cellulose fibers in the first mixture; - S3 filtering the second mixture to recover a solid phase comprising cellulose fibers; - S4 dissolving the cellulose fibers in the solid phase to obtain a cellulose dope containing undissolved particles; - S5 filtering the cellulose dope to obtain a cellulose dope separated from undissolved particles. A method is proposed which includes:

[0011] The method according to the invention makes it possible to obtain a high quality cellulose dope from waste textiles containing a large amount of non-cellulose fibers. This allows the utilization of a wider variety of textiles for recycling. The above-mentioned separation and filtration steps make it possible to obtain a cellulose dope of this quality thanks to the removal of the non-cellulose fibers.

[0012] Other optional and non-limiting features are:

[0013] The waste textile may contain cellulosic fibers in a mass percentage of less than 85%, or even less than 80%.

[0014] The waste textiles may include cellulosic fibers, polyester fibers, and other types of synthetic fibers.

[0015] The above method may further include a step S0, prior to step S1 or simultaneously with step S1, of preparing waste fabric by removing hard parts such as buttons and zippers (hereinafter referred to as "smoothing").

[0016] Step S1 is carried out by a shredding device such as a knife shredder or a ball mill.

[0017] Step S2 may comprise a step of chemically separating a portion of the non-cellulosic components from the first mixture. Step S2 may be carried out by dissolving a portion of the non-cellulosic components of the first mixture. Dissolving a portion of the non-cellulosic components of the first mixture may be carried out by contacting the first mixture with an aqueous alkaline solution. The aqueous alkaline solution may be an aqueous alkaline solution containing hydroxide ions. The aqueous alkaline solution may comprise sodium hydroxide, calcium hydroxide or potassium hydroxide. The aqueous alkaline solution may be an aqueous alkaline solution based on sodium hydroxide, the mass percentage of which may be between 3 and 25%, in particular between 5 and 15%, preferably between 6 and 10%, more particularly 8%. Step S2 may be carried out at a temperature between 50 and 150°C, preferably between 70 and 100°C. More particularly, step S2 may be carried out at a temperature between 70 and 90°C in some cases or between 80°C and 100°C in some other cases. Step S2 may be carried out in a time interval of between 40 and 240 minutes, preferably between 40 and 90 minutes, more particularly between 90 minutes. In some cases, step S2 may be carried out in a time interval of between 15 and 240 minutes, preferably between 20 and 60 minutes, more particularly between 30 minutes. The alkaline aqueous solution may further contain a phase transfer catalyst. The phase transfer catalyst may be a quaternary ammonium, such as benzyltributylammonium chloride, methyltrioctylammonium bromide, or a mixture thereof, in particular benzyltributylammonium chloride. The mass percentage of the phase transfer catalyst may be between 0.1 and 2%, in particular between 0.5% and 2%. More particularly, the mass percentage of the phase transfer catalyst may be 0.7% in some cases, or between 1 and 2%, preferably between 1.25 and 1.75%, more particularly 1.61% in other cases.

[0018] The method may further comprise a step S2' of decolorizing the waste textile, said decolorization step may be before step S2 or after step S3.

[0019] The above method may further comprise a second chopping step S1' of chopping the second mixture, which may be after step S3.

[0020] The solid phase containing cellulose fibers obtained at the end of step S3 may contain materials other than chopped cellulose fibers in a mass percentage of less than 8%, preferably less than 5%, more particularly less than 2%.

[0021] Step S5 may be carried out using a filter having a pore size between 5 and 100 μm. In particular, the pore size may in some cases be between 10 and 50 μm, more particularly 19 μm, or in other cases be between 6 and 60 μm, more particularly 6 μm.

[0022] Step S4 is - a step S4-11 of contacting the solid phase containing cellulose fibers with an alkaline aqueous solution containing sodium hydroxide to obtain a solid phase of alkaline cellulose fibers; - step S4-12, pressing the solid phase of alkaline cellulose fibers to remove excess alkaline solution and obtain a compact solid phase of alkaline cellulose fibers; - a step S4-13 of grinding the solid phase of alkaline cellulose fibers obtained at the end of step S4-12 in order to obtain a solid phase of alkaline cellulose fibers less compact than the solid phase obtained at the end of step S4-12, - a step S4-14 of aging the solid phase containing alkaline cellulose fibers obtained at the end of step S4-13, - a step S4-15 of contacting the solid phase of aged alkaline cellulose fibers with carbon disulfide to obtain a solid phase of cellulose xanthate fibers; - a step S4-16 of contacting the solid phase of cellulose xanthate fibers with an aqueous alkaline solution containing sodium hydroxide to obtain a cellulose dope containing undissolved particles; and - a step S4-17 of maturing the cellulose dope containing undissolved particles; may include. The above method may further include a spinning step S6, which is carried out by a wet spinning method.

[0023] The chopped fibers and residue of the first mixture or the cellulose fibers of the solid phase containing cellulose fibers may be less than 1 mm in size. - step S4-21, contacting the solid phase containing cellulose fibers with an aqueous solution containing N-methylmorpholine N-oxide (NMMO); - Step S4-22 of evaporating the water contained in the aqueous solution containing (NMMO) and the solid phase containing cellulose fibers. may include: The above method may further include a spinning step S6, and the spinning step is carried out by a dry-jet wet spinning method.

[0024] The cellulose dope obtained at the end of step S5 may have a viscosity of 2 Pa·S or more.

[0025] Other features, details and advantages will become apparent upon reading the following detailed description and examining the accompanying drawings. [Brief description of the drawings]

[0026] [Figure 1] FIG. 1 is a schematic diagram illustrating the steps of a method according to the present invention for converting waste textile into a cellulose dope. [Diagram 2] 1 is a ternary graph whose axes represent the mass percentage of water, the mass percentage of cellulose, and the mass percentage of NMMO, respectively, and the evolution of these proportions during the implementation of the Lyocell process. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] <Definition> In the present invention, the cellulose dope is a state-of-the-art material known to those skilled in the art. It is usually a viscous solution containing cellulose molecules or molecules derived from cellulose dissolved in a solvent, and does not contain cellulose fibers. It is therefore possible for a person skilled in the art to clearly understand what the term "cellulose dope" refers to. In particular, a person skilled in the art understands that the "dissolving pulp" described, for example, in WO 2021 / 181007 is not a "cellulose dope". "Dissolving pulp" is in fact a material that is not flowable and contains interwoven cellulose fibers.

[0028] Waste textiles include any kind of textiles from two main sources: new waste textiles and manufacturing scraps from the textile industry, and used textiles from households or businesses. These textiles may be any kind of textiles, for example clothing, household linen, or rugs. Waste textiles as understood in the present invention usually include non-filamentary components, for example color pigments, and non-fibrous components, for example buttons or labels.

[0029] The present invention relates to a method for preparing a cellulose dope from waste textiles containing cellulose fibers in a mass percentage of more than 50%, comprising the steps of: - S1 shredding waste textiles to obtain a first mixture of shredded fibres and residues; - S2 separating at least a portion of the non-cellulosic components from the first mixture to obtain a second mixture having a higher mass percentage of cellulose fibers than the mass percentage of cellulose fibers in the first mixture; - S3 filtering the second mixture to recover a solid phase containing cellulose fibers; - S4 dissolving the cellulose fibers in the solid phase to obtain a cellulose dope containing undissolved particles; - S5 filtering the cellulose dope to obtain a cellulose dope separated from undissolved particles. The present invention relates to a method comprising the steps of:

[0030] The waste textiles are thus characterized by a mass percentage of cellulose fibres which can vary within a wide range. Thus, the method according to the invention has the advantage that it is applicable to many textiles whose total mass percentage of cellulose fibres is within the abovementioned range. This therefore makes it possible to avoid a sorting step prior to the above-mentioned method, which is required in conventional methods in order to collect only waste textiles containing a very high mass percentage of cellulose fibres.

[0031] The waste textile according to the invention may contain cellulosic fibers in a mass percentage of less than 85%, or even less than 80%.

[0032] Generally, cellulosic fibers are derived from cotton, which is mainly used in textile manufacturing. They may also be derived from other materials, such as viscose or lyocell.

[0033] The waste textiles may include cellulose fibers, polyester fibers, and other types of synthetic fibers. The waste textiles may also include non-textile parts (e.g. buttons, zippers, decorative elements).

[0034] Polyesters are a family of polymers whose repeating chain units contain ester functional groups (-C(O)-O-). Polyesters are commonly mixed with cellulosic fibers to improve the quality of the textiles. Indeed, textiles based on cellulosic and polyester fibers have the advantages of both types of fibers while mitigating their respective disadvantages. Examples of the most commonly used polyesters include semi-aromatic copolyesters, such as polyethylene terephthalate (PET) and copolymers of terephthalic acid and ethylene glycol. Those skilled in the art can determine which polymers belong to the polyester family.

[0035] Synthetic fibres other than polyester fibres are fibres made from synthetic materials. These synthetic materials are almost exclusively products obtained from hydrocarbons. Synthetic fibres other than polyester fibres may in particular be polyamide fibres, chlorofibres, acrylic fibres, vinyl fibres, elastane, aramid fibres or polyethylene fibres.

[0036] Reference is now made to Figure 1, which shows a schematic diagram of the steps of the method for preparing cellulose dope from waste textiles according to the present invention. The steps, including optional steps, are described in the order of completion.

[0037] The method for preparing the cellulose dope may further include a step S0 of smoothing the waste fabric before or simultaneously with step S1.

[0038] The smoothing step consists in particular of removing seams and hard points, such as buttons or zippers, from the waste textile. This step has the advantage of removing non-filamentary components from the waste textile. This smoothing step may be carried out manually or automatically, using a device that extracts the hard points.

[0039] According to one embodiment, the smoothing step S0 is carried out using a tear-off device, for example a Laroche Cadette or Laroche Exel type device.

[0040] Shredding process S1: According to the invention, the chopping step S1 comprises chopping waste textile material to obtain a first mixture of chopped fibres and residues.

[0041] The chopping step S1 in particular allows the waste textile to be chopped into powder and / or filaments. It is believed that the preliminary chopping of the waste textile ultimately improves the quality of the cellulose dope. After step S1, a first mixture of chopped fibers and residues in the form of powder and / or filaments is collected.

[0042] Step S1 can be carried out using a shredding device such as a knife shredder or a ball mill.

[0043] The above mentioned devices are particularly suitable for chopping fibrous materials such as waste textiles. These two types of devices make it possible to very well control the fineness of the chopped material.

[0044] The first mixture of chopped fibers and residue may also be washed, for example with water.

[0045] Separation process S2: According to the present invention, the separation step S2 includes separating at least a portion of the non-cellulosic components from the first mixture to obtain a second mixture having a higher mass percentage of cellulose fibers than the mass percentage of cellulose fibers in the first mixture.

[0046] This process thus makes it possible to collect a second mixture in which the proportion of non-cellulose fibres is reduced. This process has the advantage of being able to partially separate the cellulose fibres from the other components in the waste textile. Said fibres can thus be subjected to a treatment that allows the preparation of a cellulose dope, leading to the preparation of a cellulose dope of higher quality due to the higher concentration of cellulose.

[0047] Step S2 may be a step of chemically separating a portion of the non-cellulosic components from the first mixture.

[0048] "Chemical separation process" is understood to mean a separation process using a chemical separation mechanism in which an element is separated by being transformed into one or more other elements, usually accompanied by a change of state. Chemical separation offers the advantage of being more efficient than mechanical separation and less damaging to the cellulose fibers. Indeed, mechanical separation processes are less suitable for waste textiles in which cellulose and synthetic fibers are intimately mixed, especially when they are spun together or woven together. Thus, chemical separation processes allow selective separation of one element of waste textiles from other elements due to the different chemical properties of the different elements.

[0049] According to one embodiment, step S2 is carried out by dissolving a portion of the non-cellulosic components of the first mixture.

[0050] This dissolution step makes it possible to produce a second mixture comprising a solid phase composed in particular of cellulose fibres and undissolved non-cellulosic fibres, and a liquid phase containing dissolved non-cellulosic fibres. Dissolution of some of the non-cellulosic components allows for a particularly more efficient separation, since the dissolved non-cellulosic components are in a separate phase from the phase of cellulose fibres.

[0051] According to one embodiment, dissolving a portion of the non-cellulosic components of the first mixture is carried out by contacting the first mixture with an aqueous alkaline solution.

[0052] The aqueous alkaline solution allows in particular the extraction of polyester fibres from the first mixture. Indeed, the contact of the fibres with the aqueous alkaline solution has the effect of dissolving the polyester and depolymerising it. In particular, PET depolymerises under the action of the aqueous alkaline solution, producing its constituent monomers: terephthalic acid and ethylene glycol. The action of the aqueous alkaline solution on the first mixture makes it possible to produce a liquid phase composed of the aqueous alkaline solution, terephthalic acid and ethylene glycol, and a solid phase composed of cellulose fibres and non-dissolved non-cellulose fibres. Generally, at the end of this step, an amount of polyester with a mass percentage of between 90 and 100%, preferably 100%, is removed.

[0053] The alkaline aqueous solution may be an alkaline aqueous solution containing hydroxide ions.

[0054] In the above cases, the aqueous alkaline solution may contain sodium hydroxide, calcium hydroxide, or potassium hydroxide.

[0055] Sodium hydroxide, calcium hydroxide, and potassium hydroxide are strong bases. Therefore, they make it possible to dissolve almost all, if not all, of the polyesters, especially PET. Thus, the solid phase composed of cellulose fibers and undissolved non-cellulose fibers does not contain polyesters, especially PET.

[0056] The molarity of the strong base in the aqueous solution may be between 1.25 and 3.75 mol / L, preferably between 1.5 and 2.5 mol / L, more particularly in some cases 2 mol / L or in some other cases 2.5 mol / L.

[0057] The aqueous alkali solution may be based on sodium hydroxide, the mass percentage of which may be between 5 and 15%, preferably between 6 and 10%, more particularly in some cases 8% or in other cases 10%.

[0058] The amount of aqueous alkaline solution can be selected depending on the amount of chopped fibers and residue. The greater the amount of chopped fibers and residue, the greater the amount of aqueous alkaline solution. The weight percentage of base in the aqueous alkaline solution is preferably selected such that the base is in excess relative to the weight of PET in the first mixture.

[0059] Step S2 may be carried out at a temperature between 50 and 150° C., preferably between 70 and 100° C. More specifically, step S2 may be carried out in some cases at a temperature between 70 and 90° C., or in some other cases at a temperature between 80 and 100° C.

[0060] The heating step of step S2 may be carried out by reflux heating.

[0061] Step S2 may be carried out for a time interval between 40 and 240 minutes, preferably between 40 and 90 minutes, more particularly for a time interval of 90 minutes. In one case, step S2 may be carried out for a time interval of between 15 and 240 minutes, preferably between 20 and 60 minutes, more particularly 30 minutes.

[0062] The time of step S2 may be selected so that nearly all, if not all, of the polyester fibers, especially the PET, are dissolved. If the time is too short, it is possible that most of the polyester may remain in a solid state.

[0063] The alkaline aqueous solution may further contain a phase transfer catalyst.

[0064] The use of phase transfer catalysts makes it possible to accelerate reactions, in particular chemical reactions that transform chemical species from one initial phase to another, for example from a solid phase to a liquid phase. The main phase transfer catalysts are phosphonium salts or quaternary ammonium salts. The addition of a phase transfer catalyst makes it possible not only to improve the yield, but also to reduce the degradation of the cotton by the base contained in the aqueous alkaline solution.

[0065] The phase transfer catalyst may be a quaternary ammonium, particularly benzyltributylammonium chloride (BTBAC), trioctylmethylammonium bromide (TOMAB), or a mixture thereof, particularly BTBAC.

[0066] The molar concentration of the phase transfer catalyst in the aqueous alkaline solution may be between 0.005 and 0.13 mol / L. In particular, this molar concentration may be between 0.04 and 0.08 mol / L, preferably between 0.05 and 0.075 mol / L, more particularly 0.07 mol / L, in some other cases between 0.025 and 0.07 mol / L, more particularly 0.025 mol / L.

[0067] For example, when the catalyst is BTBAC, the weight percentage of the phase transfer catalyst in the alkaline aqueous solution may be between 0.1 and 2%, in particular between 0.5% and 2%. More specifically, the weight percentage of BTBAC may be 0.7% in some cases, or between 1 and 2%, preferably between 1.25 and 1.75%, and more specifically 1.61% in other cases.

[0068] The method for preparing the cellulose dope according to the present invention may further comprise a step S2' of decolorizing the waste textile, said decolorizing step being before or after the separation step S2.

[0069] Said bleaching step makes it possible to bleach the waste textiles, i.e. to remove or inactivate the non-filamentous components used in coloured textiles, such as colour pigments, and thus to adjust the whiteness of the fibres of the first mixture or the second mixture by removing or decomposing the colouring agents.

[0070] Step S2' can be achieved by decolorization by oxidation, decolorization by reduction, decolorization by acid or base treatment, or decolorization by enzymatic decolorization, preferably decolorization by oxidation, decolorization by reduction, or decolorization by acid or base treatment.

[0071] Step S2' may be carried out in two, three, four or five steps.

[0072] The process of step S2' may be selected from the group consisting of an acid treatment, a sodium hydroxide treatment, a hydrogen peroxide treatment, an ozone treatment, and a sodium dithionite treatment.

[0073] The method for preparing a cellulose dope according to the present invention may further include a second chopping step S1' of chopping the second mixture, said second chopping step may be after step S3.

[0074] This second chopping step of chopping the second mixture makes it possible to adjust in particular the fineness of chopping of the solid phase so that the dissolution step S4 can be easily carried out. This step is carried out after the filtration step S3. If the method comprises a decolorization step S2' after step S2, the chopping step S1' is preferably carried out after the decolorization step S2'.

[0075] Step S1' can be carried out by a shredding device such as a knife shredder or a ball mill.

[0076] Filtration step S3: According to the present invention, a filtering step S3 includes filtering the second mixture to recover a solid phase containing cellulose fibers and other materials.

[0077] The filtration step S3 makes it possible to separate the solid phase from the liquid phase of the second mixture to recover the solid phase more concentrated in cellulose fibres.

[0078] Step S3 may be performed with a filter having smaller pores than the fineness of chopping achieved in step S1 or step S1'.

[0079] Preferably, the solid phase containing cellulose fibers obtained at the end of step S3 contains materials other than cellulose fibers in a mass percentage of less than 8%, preferably less than 5% and more particularly less than 2%.

[0080] These materials other than cellulose fibers may in particular be polyamide, elastane, wool or silk. These materials do not dissolve in step S2 and therefore remain in the solid phase. Thus, the mass percentage of materials other than cellulose fibers is very low, making it possible to prepare a high quality cellulose dope with a low content of impurities.

[0081] The solid phase containing the cellulose fibers may further be washed, for example with an aqueous solution of acetic acid, then it may be filtered and then washed, for example with distilled water, then it may be filtered and then dried.

[0082] Melting process S4: According to the invention, the dissolving step S4 comprises dissolving the solid phase cellulose fibers to obtain a cellulose dope containing undissolved particles.

[0083] The dissolving step S4 allows the cellulose fibers to be dissolved to recover the cellulose dope. The cellulose dope contains undissolved particles, such as the above-mentioned impurities that did not react during the dissolving step, and dissolved particles. The undissolved impurities are small, but still need to be removed from the cellulose dope.

[0084] The dissolution step may be carried out in two ways, according to two processes known to those skilled in the art: the "viscose" process, which is described first, and the "lyocell" process, which is described second.

[0085] Dissolving step S4 by viscose process According to the viscose process, step S4 comprises: - a step S4-11, called mercerization, in which the solid phase containing cellulose fibers is contacted with an aqueous alkaline solution containing sodium hydroxide to obtain a solid phase of alkaline cellulose fibers; - step S4-12, which involves pressing the solid phase of alkaline cellulose fibers to remove excess alkaline solution and obtain a dense solid phase of alkaline cellulose fibers, the mass percentage of cellulose being between 20 and 40%, preferably between 25% and 35%, more particularly about 30%, - a step S4-13 of comminuting the solid phase of alkaline cellulose fibres obtained at the end of step S4-12 in order to obtain a solid phase of alkaline cellulose fibres having a lower density than the solid phase obtained at the end of step S4-12, i.e. a density between 80 and 180 g / L, - a step S4-14 of aging the solid phase containing alkaline cellulose fibers obtained at the end of step S4-13, - a step S4-15 of contacting the solid phase of aged alkaline cellulose fibers with carbon disulfide to obtain a solid phase of cellulose xanthate fibers; - a step S4-16 of contacting the solid phase of cellulose xanthate fibers with an aqueous alkaline solution containing sodium hydroxide to obtain a cellulose dope containing undissolved particles; and - Step S4-17 of maturing the cellulose dope containing undissolved particles Includes.

[0086] In step S4-11, the solid-phase cellulose fibers are reacted with an aqueous alkaline solution. Preferably, the base contained in the aqueous alkaline solution is a strong base. This step allows the cellulose fibers to be impregnated with the base contained in the aqueous alkaline solution, thereby producing alkaline cellulose fibers that are swollen compared to the cellulose fibers alone.

[0087] The mass of sodium hydroxide may be selected such that it is in excess relative to the mass of the solid phase containing the cellulose fibers, which ensures maximum swelling of the cellulose fibers. The aqueous alkaline solution of step S4-11 may be an aqueous alkaline solution based on sodium hydroxide, with the mass percentage of sodium hydroxide being between 15 and 25%.

[0088] Step S4-11 may be carried out at a temperature between 30 and 50° C., for a time interval between 20 and 60 minutes.

[0089] The solution is pressurized in step S4-12 to remove excess sodium hydroxide, and is ground in step S4-13. The alkaline cellulose fibers are then aged in an oxygen atmosphere in step S4-14 for, for example, 3 hours 40 minutes, or in some cases 15 hours 30 minutes.

[0090] In step S4-15, the alkaline cellulose fibers are treated by contacting them with carbon disulfide to form cellulose xanthate fibers.

[0091] The mass of carbon disulfide may affect the dissolution of the cellulose fibers. The mass of carbon disulfide is preferably equal to at least 30% of the initial mass of the solid phase containing the cellulose fibers. The mass ratio of carbon disulfide to alkaline cellulose fibers is preferably between 0.2 and 0.5.

[0092] The time of step S4-15 influences the conversion of cellulose xanthate fibers. The time of step S4-15 is therefore selected so as to obtain a high conversion of cellulose fibers to cellulose xanthate fibers. The gamma value of the cellulose xanthate fibers is between 25 and 50%, preferably between 30 and 45%. The temperature also influences the conversion of the alkaline cellulose fibers to cellulose xanthate fibers. The temperature is selected so that carbon disulfide is present in gaseous form during step S4-15. Thus, step S4-15 can be carried out at a temperature between 25 and 50° C., in particular between 25 and 35° C., for a time interval between 100 and 200 minutes. These operating conditions are suitable for carrying out step S4-15 under vacuum.

[0093] Step S4-16 dissolves the cellulose xanthate fibers by contacting them with an aqueous alkaline solution. The cellulose xanthate then exists in a viscous paste form called cellulose dope. This cellulose dope also contains the dissolved and undissolved impurities mentioned above.

[0094] According to one embodiment, the aqueous alkaline solution of step S4-16 is an aqueous alkaline solution based on sodium hydroxide, the mass percentage of sodium hydroxide being between 2 and 15%, in particular between 5 and 15%.

[0095] Dissolution of cellulose xanthate fibers is achieved by contacting and mixing cellulose xanthate with a base. Those skilled in the art know how to adjust the concentration of the base to obtain a cellulose dope containing a mass percentage of cellulose between 5 and 12% and a mass percentage of base between 2 and 8%, in particular between 4 and 6%. Preferably, the base selected is sodium hydroxide.

[0096] According to one embodiment, step S4-16 is carried out at a temperature between 0 and 10° C., for a time interval between 150 and 200 minutes.

[0097] In step S4-17, the cellulose dope is allowed to stand for, for example, 16 hours after step S4-16.

[0098] Dissolving step S4 by Lyocell process When the dissolution step S4 is carried out by the Lyocell process, it is necessary that during the chopping step S1 or after the chopping step S1', if carried out, the waste textile is chopped in such a way that the fibre size of the first mixture of chopped fibres and residues or the second mixture when the chopping step S1' is carried out is less than 1 mm.

[0099] In such a case, step S4 is - a step S4-21 of contacting the solid phase containing cellulose fibers with an aqueous solution containing N-methylmorpholine N-oxide (NMMO), - a step S4-22 of evaporating a part of the water contained in the aqueous solution containing NMMO and cellulose in order to dissolve the cellulose and obtain a cellulose dope; Includes.

[0100] Step S4-21 involves contacting the cellulose fibers with an aqueous solution containing NMMO to obtain a solution containing water, NMMO, and cellulose, as well as impurities, thereby dispersing the cellulose fibers and facilitating the subsequent reaction.

[0101] The mass percentage of NMMO may preferably be selected to be close to the zone where dissolution of cellulose in NMMO is possible. The mass percentage of NMMO in the aqueous solution is preferably between 60 and 90%, preferably between 70 and 80%, more particularly 76%.

[0102] Step S4-22 dissolves the cellulose by evaporating water from the aqueous solution containing NMMO. After the water has evaporated, a cellulose dope containing the above-mentioned dissolved and undissolved impurities is obtained.

[0103] FIG. 2 shows a ternary graph whose axes represent the mass percentage of water, the mass percentage of cellulose, and the mass percentage of NMMO, respectively, and the evolution of these proportions during the Lyocell process.

[0104] The shaded area represents the dissolution range of cellulose in NMMO. Point a) represents the mixture containing cellulose fibers and water before dissolution. By reducing the amount of water, the mixture moves to point b) which is within the dissolution range and the cellulose dissolves. During dissolution of the cellulose, the amount of NMMO decreases until point c) is reached where NMMO has completely reacted with the cellulose. Thus, the mixture at point c) contains water and cellulose. An evaporation step S4-22 evaporates the water to concentrate the cellulose until point d) is reached.

[0105] The pulp has a different viscosity depending on which step S4 has been performed: if the pulp is obtained at the end of step S4-22, it has a much higher viscosity than at the end of step S4-17.

[0106] Filtration step S5: According to the present invention, step S5 includes filtering the cellulose dope to obtain the cellulose dope separated from undissolved particles.

[0107] The filtering step S5 filters the cellulose dope obtained at the end of the dissolving step S4 to recover the cellulose dope containing pulp-like cellulose and dissolved impurities. In this way, the undissolved impurities are separated from the cellulose dope, making it possible to obtain a higher quality cellulose dope. The cellulose dope obtained at the end of step S5 still contains a trace amount of dissolved impurities.

[0108] Step S5 may in particular be carried out by means of a filter through which the cellulose dope passes. The filter may have pores with a size between 5 and 100 μm, in particular between 5 and 54 μm, preferably between 10 and 50 μm, more particularly 19 μm or, in some cases, 6 μm. Such pore size corresponds to a mesh size between 150 and 3000 mesh, in particular between 270 and 3000 mesh, preferably between 300 and 1500 mesh, more particularly 789 mesh or, in some cases, 2500 mesh.

[0109] Preferably, the filter is a metal filter, in particular made of wire mesh, and the pores have a rectangular shape. The size of the pores therefore corresponds to the size of the rectangular pores. The fineness of the pores of such a filter advantageously allows removing almost all undissolved impurities from the cellulose dope. Advantageously, the cellulose dope obtained is of high quality.

[0110] When the cellulose dope is obtained at the end of step S4-22, it has a relatively high viscosity. It may be advantageous to heat the cellulose dope and apply pressure to help force the cellulose dope through the filter.

[0111] Preferably, the cellulose dope obtained at the end of step S5 has a viscosity higher than 2 Pa·S.

[0112] If the cellulose dope is obtained according to the viscose process, the viscosity may be measured according to the ISO 12058-1:2018 standard using a steel ball with a diameter of 14 mm, a stopwatch, and at a temperature of 20° C.

[0113] When the cellulose dope is obtained according to the Lyocell process, its viscosity may be measured according to the ISO 6721-10:2015 standard by oscillatory rheometry using a parallel plate configuration with plates of 25 mm diameter, plates spaced 1 mm apart, carried out at 90° C. and choosing a traction of 0.5%.

[0114] If the cellulose dope obtained at the end of step S5 is pre-dissolved by viscose process, the above method for preparing cellulose dope may further include a spinning step S6, which is carried out by wet spinning method.

[0115] According to one embodiment, when the cellulose dope obtained at the end of step S5 is pre-dissolved by the Lyocell process, the above-mentioned method for preparing cellulose dope may further include a spinning step S6, which is carried out by a dry-jet wet spinning method.

[0116] Fiber spinning is a conventional method for forming polymer filaments and its two variations, wet spinning and dry-jet wet spinning, are known to those skilled in the art.

[0117] The spinning process consists of extruding a polymer solution, also called spin dope. The extrusion is carried out through the capillary of a die. If the melting temperature of the polymer is higher than its decomposition temperature, the polymer must be spun in solution to form fibers, also called wet spinning. If the method used is wet spinning, the polymer solution is extruded directly in a coagulation bath, whereas in dry-jet wet spinning, the polymer solution is extruded into an evaporation chamber before being immersed in a coagulation bath.

[0118] It is also possible to regenerate fibres using the cellulose dope prepared by the method of the invention in other ways, in particular by coating. EXAMPLES

[0119] Example 1a: Preparation of cellulose dope using dissolution step by viscose process Shredding process S1: 20 g of waste textile containing 60% mass percentage of cellulose fibers is placed in a knife shredder. The waste textile is shredded and a first mixture of shredded fibers and residues having a size of less than 2 cm is collected.

[0120] Separation process S2: 20 g of the mixture of chopped fibers and residue is introduced into 2 kg of an aqueous solution containing 8% by weight of sodium hydroxide and 1.61% by weight of BTBAC, previously heated to 90° C. The solution is kept at 90° C. for 1.5 hours and stirred at 100 rpm.

[0121] Filtration step S3: The solution is filtered to recover a solid phase containing cellulose fibers. The solid phase is washed in a 2 wt% acetic acid bath for 10 minutes. The solution is then filtered to recover a solid phase containing cellulose fibers. The solid phase is washed in a distilled water bath for 10 minutes. The solution is then filtered to recover a solid phase containing cellulose fibers, which is then dried in an oven at 105°C.

[0122] Melting process S4: Process S4-11: 3 g of the solid phase containing cellulose fibers are introduced into 100 g of an aqueous solution containing 18% by weight of sodium hydroxide, previously heated to 40° C. The solution is kept at 40° C. for 40 minutes, while being stirred at 100 rpm.

[0123] Process S4-12: The solution is pressurized to remove excess sodium hydroxide until 9 g of alkaline cellulose fiber is recovered.

[0124] Process S4-13: Alkaline cellulose fibers are crushed.

[0125] Process S4-14: They are then aged in the presence of oxygen at 50° C. for 3 hours 40 minutes.

[0126] Process S4-15: The alkaline cellulose fibers are placed in a closed reactor under a hood at 32° C. 3 g of carbon disulfide are introduced into the reactor. The reactor is placed under vacuum and left to stand for 2.5 hours to produce cellulose xanthate fibers.

[0127] Process S4-16: 18 g of an aqueous solution containing 8% by weight of sodium hydroxide is introduced into the reactor. The reactor is left to stand for 10 minutes. The contents of the reactor are stirred at 5° C. for 3 hours to dissolve the cellulose xanthate fibers.

[0128] Process S4-17: The cellulose dope is then withdrawn from the reactor and placed under a hood in a container covered with a perforated film at room temperature for 16 hours.

[0129] Filtration step S5: The cellulose dope is placed in a device capable of pressure filtration. The filter has a rectangular hole with a side length of 19 μm. Then, a pressure of 5 bar is applied to force the cellulose dope through the filter.

[0130] Example 1b: Preparation of cellulose dope using dissolution step by viscose process The procedure carried out in Example 1a is carried out in Example 1b with the following modifications: During the separation step S2: 400 g of aqueous solution instead of 2 kg, the solution is maintained at 90° C. for 40 minutes instead of 1.5 hours. During step S4-14: the ground alkaline cellulose fibers are aged in the presence of oxygen at 30° C. instead of 50° C. for 15 hours 30 minutes instead of 3 hours 40 minutes. During the filtration step S5: the filter pores have a side length of 6 μm.

[0131] Example 2: Preparation of cellulose dope using dissolution step by Lyocell process Based on the method described in Example 1b, it is possible to modify step S4 of dissolving the cellulose fibers.

[0132] Shredding process S1: As in Example 1.

[0133] Separation process S2: As in Example 1.

[0134] Filtration step S3: As in Example 1.

[0135] Shredding process S1': The solid phase containing cellulose fibres is shredded using a knife shredder to obtain a solid phase containing cellulose fibres less than 1 mm in size.

[0136] Melting process S4: Process S4-21:116 g of an aqueous solution containing NMMO at a mass percentage of 50% is placed in a pear-shaped flask of a rotary evaporator. 39 g of water is removed by evaporating the water under vacuum at 99° C. 10 g of the solid phase containing cellulose fibers is introduced into the pear-shaped flask together with 0.26 g of propyl gallate.

[0137] Process S4-22: The contents of the eggplant flask are evaporated under vacuum using a rotary evaporator to remove 15 g of water.

[0138] Filtration step S5: The cellulose dope, which has been preheated to 110°C, is placed in a device capable of pressure filtration. The filter holes are rectangular with a side length of 19 μm. Then, a pressure of 15 bar is applied to pass the cellulose dope through the filter. [Explanation of symbols]

[0139] - S0 smoothing process - S1 Shredding process - S1' Shredding process - S2 separation process - S2' Decolorization process - S3 filtration process - S4 melting process - S4-11 Contacting with an alkaline aqueous solution - S4-12 Pressurizing alkaline cellulose - S4-13 Alkaline cellulose crushing process - S4-14 Aging process of alkaline cellulose - S4-15 Contacting with carbon disulfide - S4-16 Contacting with an alkaline aqueous solution - S4-17 Cellulose dope maturation process - S4-21 Contacting with an aqueous NMMO solution - S4-22 Evaporation process - S5 filtration process - S6 spinning process

Claims

1. A method for producing a cellulose dope from waste textiles containing cellulose fibers in a mass percentage of more than 50%, comprising the steps of: (S1) shredding waste textile fabrics to obtain a first mixture of shredded fibers and residue; (S2) separating at least a portion of the non-cellulosic components from the first mixture to obtain a second mixture having a higher mass percentage of cellulose fibers than the mass percentage of cellulose fibers in the first mixture; (S3) filtering the second mixture to recover a solid phase comprising cellulose fibers; (S4) dissolving the solid phase cellulose fibers to obtain a cellulose dope containing undissolved particles; and (S5) filtering the cellulose dope to obtain a cellulose dope separated from undissolved particles. A method for producing a cellulose dope comprising the steps of:

2. Step (S4) - a step (S4-11) of contacting the solid phase containing cellulose fibers with an alkaline aqueous solution containing sodium hydroxide to obtain a solid phase of alkaline cellulose fibers; - applying pressure to the solid phase of alkaline cellulose fibers to remove excess alkaline solution and obtain a dense solid phase of alkaline cellulose fibers (S4-12); - a step (S4-13) of comminuting the solid phase of alkaline cellulose fibers obtained at the end of step (S4-12) in order to obtain a solid phase of alkaline cellulose fibers having a lower density than the solid phase obtained at the end of step (S4-12), - a step (S4-14) of ageing the solid phase comprising alkaline cellulose fibers obtained at the end of step (S4-13), - contacting the solid phase of the aged alkaline cellulose fibers with carbon disulfide to obtain a solid phase of cellulose xanthate fibers (S4-15); - contacting the solid phase of cellulose xanthate fibers with an aqueous alkaline solution containing sodium hydroxide to obtain a cellulose dope containing undissolved particles (S4-16); and - maturing the cellulose dope containing undissolved particles (S4-17); The method for producing the cellulose dope according to claim 1 , comprising:

3. Step (S4) - contacting the solid phase comprising cellulose fibres with an aqueous solution comprising N-methylmorpholine N-oxide (NMMO) (S4-21); and - A step (S4-22) of evaporating the water contained in the aqueous solution containing (NMMO) and the solid phase containing cellulose fibers; The method for producing the cellulose dope according to claim 1 , comprising:

4. The method for producing a cellulose dope according to any one of claims 1 to 3, wherein the waste textile contains cellulose fibers in a mass percentage of less than 85%.

5. The method for producing a cellulose dope according to any one of claims 1 to 4, wherein step (S2) is carried out by contacting the first mixture with an alkaline aqueous solution to dissolve a portion of the non-cellulose components of the first mixture.

6. The method for producing a cellulose dope according to claim 5, wherein the aqueous alkali solution is an aqueous alkali solution based on sodium hydroxide, the mass percentage of said sodium hydroxide being between 3 and 25%.

7. The method for producing a cellulose dope according to claim 5 or 6, wherein step (S2) is carried out at a temperature between 50 and 150°C.

8. The method for producing a cellulose dope according to any one of claims 5 to 7, wherein step (S2) is carried out for a time interval between 15 and 240 minutes.

9. The method for producing a cellulose dope according to any one of claims 5 to 8, wherein the alkaline aqueous solution contains a phase transfer catalyst, and the phase transfer catalyst is a quaternary ammonium.

10. 10. The method for producing a cellulose dope according to claim 9, wherein the quaternary ammonium is benzyltributylammonium chloride, methyltrioctylammonium bromide, or a mixture thereof.

11. The method for producing a cellulose dope according to claim 10, wherein the quaternary ammonium is benzyltributylammonium chloride, and the mass percentage of benzyltributylammonium chloride is between 0.1 and 2%.

12. The method for producing a cellulose dope according to any one of claims 1 to 11, wherein step (S5) is carried out using a filter having a pore size between 5 and 100 µm.

Citation Information

Patent Citations

  • Separation of polycotton blends

    WO2021181007A1