High-purity CR-W-MO-LA alloy for powder-based additive manufacturing
A modified Ni-Cr-W-Mo-La alloy with controlled particle size and reduced C and Si content, along with optimized parameters, addresses cracking issues in 3D printing, achieving crack-free articles efficiently and cost-effectively.
Patent Information
- Application Number
- JP2024525883
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-05
- Filing Date
- 2022-11-04
- Publication Date
- 2024-10-29
AI Technical Summary
Conventional Ni-Cr-W-Mo alloys, such as Haynes 230, are prone to cracking during 3D printing due to internal stresses caused by rapid temperature gradients, leading to inefficiencies and increased costs from preheating processes or additional treatments like hot isostatic pressing (HIP).
A modified Ni-Cr-W-Mo-La alloy with controlled particle size and reduced C and Si content, combined with optimized process parameters, to produce crack-free 3D printed articles without preheating or HIP.
The modified alloy composition and process parameters enable crack-free 3D printing across a wide range of parameters, enhancing productivity and reducing manufacturing costs by eliminating the need for preheating and HIP.
Smart Images

Figure 2024539712000001_ABST
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit under 35 U.S.C. Section 119(e) of U.S. Provisional Application No. 63 / 276,187, filed November 5, 2021, the disclosure of which is expressly incorporated herein by reference in its entirety. [Background technology]
[0002] Embodiments relate to techniques for producing three-dimensional metal articles via powder-based additive manufacturing, such as selective laser melting (SLM), also known as laser-based powder bed fusion (L-PBF), direct energy deposition (DED) / laser metal deposition (LMD) or electron beam melting (EBM) processes. Additionally, embodiments relate to Ni-Cr-W-Mo-La alloy, and in particular Ni-Cr-W-Mo-La alloy powder, which is similar to Haynes alloy 230, but with modified chemical composition and controlled grain size to produce crack-free or near crack-free parts via SLM / L-PBF, DED / LMD, and EBM processes.
[0003] Due to the unique process of metal additive manufacturing, also known as 3D printing, using SLM / L-PBF (e.g., rapid solidification from the melt), many conventional alloys are prone to cracking during 3D printing because these alloys are optimized for forging or casting processes and not the SLM / L-PBF process.
[0004] According to manufacturer information on standard wrought / cast commercial alloys such as Haynes alloy 230 (Brochure: Haynes 230 alloy; Ni-Cr-W-Mo alloy combining excellent high-temperature strength and oxidation resistance with excellent long-term stability and good fabricability; Haynes International Inc 2007), the alloy is readily weldable by a variety of techniques, including gas tungsten arc (GTAW), gas metal arc (GMAW), and resistance welding, which would place the basic alloy composition in the class of weldable materials. However, these welding techniques for which Haynes 230 alloy is favored are different from the welding processes in the additive manufacturing processes mentioned above. Thus, even though Haynes 230 alloy is classified as readily weldable, the very fast heating and cooling rates of the material during laser or electron beam welding lead to the formation of cracks in articles formed from Haynes 230 alloy in 3D printing processes. It is generally accepted that the cracks are primarily caused by internal stresses that build up within the parts during the laser or electron beam welding process. See Press Release: Flying High with VCSEL Heating; Fraunhofer ILT; October 4, 2018.
[0005] The internal stresses that build up in parts during 3D printing are caused by a temperature gradient within the generated component: within the laser spot, temperatures above the melting point prevail, while outside the laser spot, the component cools rapidly. Depending on the geometry and alloy, this temperature gradient can lead to cracks in the 3D printed material.
[0006] One conventional method of overcoming the cracking problem in Haynes 230 alloy or Haynes 230-like alloys involves heating the powder bed to high temperatures during the 3D printing process from the base plate of a powder additive manufacturing machine's build chamber, such as an SLM / L-PBF machine, or more effectively from the top of the machine's build chamber, to directly heat the layers that are now welded together, thereby avoiding or reducing the internal stresses within the article that ultimately lead to cracking. Using the latter, the temperature of the top layer can reach up to 900° C., high enough to avoid cracking.
[0007] However, before the finished part can be removed from such a heated powder bed, it must be cooled to ambient temperature. Due to the low thermal conductivity of the powder bed, heating and cooling the powder bed requires a long time, resulting in a significant decrease in the productivity of the powder additive manufacturing process. Furthermore, expensive heating equipment and isolation and adaptation of the process chamber are required.
[0008] Another method to overcome the cracking problem in known Haynes 230 alloy or Haynes 230-like alloys is to apply a heat treatment at high external pressure and high temperature to close and repair the pores and cracks remaining in the 3D printed material. This is known as hot isostatic pressing (HIP). This process works to close internal pores and cracks, but cannot repair surface cracks. This process also adds an additional processing step to the 3D printing of the article, increasing manufacturing costs.
[0009] Therefore, it would be beneficial to provide an alloy similar to the Haynes 230 alloy composition that can be processed with an unheated or only slightly heated powder bed and does not require a 3D printing process step to repair cracks via HIP. Summary of the Invention
[0010] The embodiments described herein overcome the above-identified deficiencies in known technology by providing an alloy having an optimized chemical composition to control the grain size distribution of the alloy when provided as a powder for the SLM / L-PBF process of 3D printing.
[0011] In an embodiment, a modified nickel-based alloy with high contents of Cr and W for additive manufacturing of three-dimensional articles with reduced crack tendency is disclosed, as well as suitable process parameters for producing such articles. The composition of the powder according to the invention is based on a modified composition of the known commercially available prior art Haynes 230 alloy with (in wt%) 20.0-24.0 Cr, 13.0-15.0 W, 1.0-3.0 Mo, 0.3-1.0 Mn, 0.25-0.75 Si, 0.20-0.50 Al, 0.05-0.15 C, 0.005-0.05 La, max 3 Fe, max 5 Co, max 0.1 Ti, max 0.015 B, balance Ni, and unavoidable residual elements and impurities. Furthermore, although this known composition is available as a casting or forging material, the modified composition embodiment preferably relates to a material in the form of a powder, e.g. a mainly spherical powder.
[0012] The generally accepted known limits of max 0.75 wt% Si, max 1.0 wt% Mn and especially max 0.15 wt% C in the known Hayes 230 alloy, as well as the generally accepted known typical alloy contents of nominally 0.4 wt% Si, nominally 0.5 wt% Mn and especially nominally 0.1 wt% C, were all found to be too high for powders used in powder-based additive manufacturing such as SLM / L-PBF if crack-free or nearly crack-free three-dimensional articles of complex shapes are to be provided on a reliable basis. Furthermore, as discussed herein, according to embodiments, by strict control and modification of certain elements, such as modifying the C and Si content of the known Hayes 230 alloy composition to be 0.001≦C≦0.045 wt.% and 0.005≦Si≦0.20 wt.%, and controlling the particle size of the powder material to be 28≦D50≦38 μm, crack-free articles can be produced without pre-heat and without HIP in powder-based additive manufacturing processes, for example in SLM / L-PBF, DED / LMD or EBM machines, over a very wide range of process parameters.
[0013] In a preferred embodiment of the present invention, the alloy has a C content of 0.01-0.04 wt.% and a Si content of about 0.01-0.10 wt.%, and a D50 measured according to ASTM B822 of 28-38 μm.
[0014] The powder-based additive manufacturing process parameters are: a laser volume energy density Ed of 35-150 J / mm 3 In a preferred embodiment, the range is 60 to 110 J / mm 3 and more preferably, 65 to 100 J / mm 3 The range is selected to be:
[0015] The laser volumetric energy density is calculated as follows: E D = P / v h t, where P is the laser power in W, v is the laser surface scanning speed in mm / s, h is the hatch spacing in mm, and t is the layer thickness in mm of each of the welding powder layers in the powder-based additive manufacturing process.
[0016] In other embodiments, the thickness of each welding powder layer may be in the range of 0.01-0.1 mm, preferably 0.02-0.07 mm, and even more preferably 0.03-0.05 mm.
[0017] The embodiment relates to a Ni-Cr-W-Mo-La alloy material powder for additive manufacturing, the alloy material powder having a composition of 18.0-22.0 wt% Cr, 12.0-15.0 wt% W, 1.0-3.0 wt% Mo, 0.15-0.75 wt% Al, 0.005-0.05 wt% La, 0.001≦C≦0.045 wt%, 0.005≦Si≦0.20 wt%, the balance Ni, and unavoidable residual elements and impurities. The powder has a particle size distribution generally between 10 and 100 μm.
[0018] According to an embodiment, the powder may include spherical particles.
[0019] According to an embodiment, the composition may further include greater than 0 wt.% and less than 5 wt.% Fe, greater than 0 wt.% and less than 7 wt.% Co, greater than 0 wt.% and less than 0.5 wt.% Ti, greater than 0 wt.% and less than 0.020 wt.% B, and greater than 0 wt.% and less than or equal to 0.25 wt.% Mn.
[0020] In yet other embodiments, the Mn content may be greater than 0 wt.% and less than 0.10 wt.%.
[0021] In other embodiments, the Si content may be 0.005≦Si≦0.10 wt.%.
[0022] According to another embodiment, the powder may be a substantially spherical powder with a particle size distribution of 10-50 μm and a D50 of 28-38 μm.
[0023] In an embodiment, the additive manufacturing process for producing a three-dimensional article using the above-described embodiment of the alloy material powder has a melting point of 30 to 150 J / mm 3 in the range of 60 to 110 J / mm 3 in the range of 65 to 100 J / mm 3 The additive manufacturing process includes combining laser parameters of laser power, laser surface scanning speed, hatch distance, and build layer thickness to generate a laser volumetric energy density for 3D printing the material in the range of 0.01 to 0.1 mm. Further, the layers are applied with each layer thickness in the range of 0.01 to 0.1 mm, and the additive manufacturing process includes a selective laser melting process, a laser-based powder bed fusion process, a direct energy deposition process, a laser metal deposition process, or an electron beam melting process.
[0024] An embodiment relates to an alloy material powder for additive manufacturing processes comprising 0.001≦C≦0.045 wt.% and 0.005≦Si≦0.20 wt.%. The powder has a particle size distribution generally between 10 and 100 μm.
[0025] An embodiment relates to a method for three-dimensional printing of an article having a crack-free structure, the method comprising: supplying successive layers of a powder having a particle size distribution generally between 10 and 100 μm to a powder additive manufacturing process having a composition including 0.001≦C≦0.045 wt.% and 0.005≦Si≦0.20 wt.%; and applying a volumetric energy density of 38.7 J / mm3 to 152.29 J / mm3 to the successive layers of powder.
[0026] According to an embodiment, the powder composition may further include 18.0-22.0 wt% Cr, 12.0-15.0 wt% W, 1.0-3.0 wt% Mo, 0.15-0.75 wt% Al, 0.005-0.05 wt% La, >0 wt% and up to 5 wt% Fe, >0 wt% and up to 7 wt% Co, >0 wt% and up to 0.5 wt% Ti, >0 wt% and up to 0.020 wt% B, and >0 wt% and less than 0.25 wt% Mn, with the balance Ni, and unavoidable residual elements and impurities. Further, the additive manufacturing process may include one of a selective laser melting (SLM) process, a laser-based powder bed fusion (L-PBF) process, a direct energy deposition (DED) / laser metal deposition (LMD) process, or an electron beam melting (EBM) process. The volumetric energy density (ED) can be determined from the formula: ED=P / v·h·t, where P is the laser power in W, v is the laser surface scanning speed, h is the hatch spacing, and t is the layer thickness of each of the weld powder layers. The powder based additive manufacturing process involves combining the laser parameters of laser power, laser surface scanning speed, hatch distance, and build layer thickness. The powder can be a roughly spherical powder with a particle size distribution of 10-50 μm and a D50 of 28-38 μm.
[0027] Other exemplary embodiments and advantages of the present invention can be ascertained by reviewing the present disclosure and accompanying drawings. [Brief description of the drawings]
[0028] The present invention will be further described in the following detailed description with reference to the several drawings, in which like reference numerals represent like parts throughout the several views, and in which: [Figure 1A]FIG. 1A shows an optical microscope image of a cross section parallel to the build plate of a machine, and FIG. 1B shows an optical microscope image of a cross section perpendicular to the build plate of a machine, illustrating severe cracks on a cross-sectional surface of an article produced in a powder-based additive manufacturing process such as a standard SLM / L-PBF system from a Ni-Cr-W-Mo-La alloy in spherical powder form having a chemical composition according to the prior art. [Figure 1B] FIG. 1A shows an optical microscope image of a cross section parallel to the build plate of a machine, and FIG. 1B shows an optical microscope image of a cross section perpendicular to the build plate of a machine, illustrating severe cracks on a cross-sectional surface of an article produced in a powder-based additive manufacturing process such as a standard SLM / L-PBF system from a Ni-Cr-W-Mo-La alloy in spherical powder form having a chemical composition according to the prior art. [Figure 2A] 2A and 2B show a crack-free cross-sectional surface of an article produced from a Ni-Cr-W-Mo-La alloy in spherical powder form having a chemical composition according to an embodiment, in a powder-based additive manufacturing process such as a standard SLM / L-PBF system, where FIG. 2A is an optical microscope image showing a cross section perpendicular to the machine build plate and parallel to the build direction in an etched state, FIG. 2B is a scanning electron microscope (SEM) image of the cross section perpendicular to the machine build plate, and FIG. 2C is an SEM image of the cross section parallel to the build direction. [Figure 2B] 2A and 2B show a crack-free cross-sectional surface of an article produced from a Ni-Cr-W-Mo-La alloy in spherical powder form having a chemical composition according to an embodiment, in a powder-based additive manufacturing process such as a standard SLM / L-PBF system, where FIG. 2A is an optical microscope image showing a cross section perpendicular to the machine build plate and parallel to the build direction in an etched state, FIG. 2B is a scanning electron microscope (SEM) image of the cross section perpendicular to the machine build plate, and FIG. 2C is an SEM image of the cross section parallel to the build direction. [Figure 2C]2A and 2B show a crack-free cross-sectional surface of an article produced from a Ni-Cr-W-Mo-La alloy in spherical powder form having a chemical composition according to an embodiment, in a powder-based additive manufacturing process such as a standard SLM / L-PBF system, where FIG. 2A is an optical microscope image showing a cross section perpendicular to the machine build plate and parallel to the build direction in an etched state, FIG. 2B is a scanning electron microscope (SEM) image of the cross section perpendicular to the machine build plate, and FIG. 2C is an SEM image of the cross section parallel to the build direction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] The details shown in this specification are examples and are intended only as illustrative descriptions of embodiments of the present invention, and are presented to provide what is believed to be the most useful and easily understood explanation of the principles and conceptual aspects of the present invention. In this regard, no attempt has been made to show the structural details of the present invention in more detail than is necessary for a fundamental understanding of the present invention, and the description taken together with the drawings will make clear to those skilled in the art how some forms of the present invention may be embodied in practice.
[0030] Table 1 shows comparative chemical compositions of various known Ni-Cr-W-Mo-La alloys (commonly referred to as Haynes 230 alloy, which is commercially available in wrought or cast form). Specifically, Table 1 shows the compositions of known Haynes 230 alloy (Ni-Cr-W-Mo) from Haynes International (see Brochure: Haynes 230 alloy; a Ni-Cr-W-Mo alloy that combines excellent high temperature strength and oxidation resistance with excellent long term stability and good workability; Haynes International Inc 2007), Ulrich Metals (see www.ulbrich.com / alloys / haynes-230-uns-n06230), and NeoNickel (see www.neonickel.com).
[0031] [Table 1]
[0032] Table 2 shows comparative examples of known Ni-Cr-W-Mo-La alloys supplied in the form of powders having particle sizes of about 10-100 μm for powder bed additive manufacturing in the SLM / L-PBF process. In particular, Table 2 shows the composition of alloy powders similar to Haynes 230 alloy, such as AMPERPRINT 0211 from Hoganas (www.hoganas.com), TRUFORM 230 from Praxair Surface Technologies (www.praxairsurfacetechnology.com), and METCOADD H23X-A from Oerlikon Metco AG.
[0033] [Table 2]
[0034] A fair review of Tables 1 and 2 reveals that all of the known Ni-Cr-W-Mo-La alloy compositions listed, regardless of whether the compositions are supplied in powder form for SLM / L-PBF processes or in cast or wrought form, specify 0.05≦C≦0.15 wt.%, 0.25≦Si≦0.75 wt.%, and 0.30≦Mn≦1.00 wt.%, or describe a typical mid-spec (nominal) composition of C=nominal 0.1 wt.%, Si=nominal 0.4 wt.%, and Mn=nominal 0.5 wt.%.
[0035] The embodiments also relate to nickel-based alloys having high contents of Cr and W. However, in contrast to known Ni-Cr-W-Mo-La compositions described in Tables 1 and 2, the Ni-Cr-W-Mo-La compositions according to the embodiments are modified to reduce the crack propensity of the articles when used in powder-based additive manufacturing of three-dimensional articles. Thus, the modified composition of the Ni-Cr-W-Mo-La powder according to the embodiment has the same specifications (wt%) as the known composition: 20.0-24.0 Cr, 13.0-15.0 W, 1.0-3.0 Mo, 0.20-0.50 Al, 0.005-0.05 La, max. 3 Fe, max. 5 Co, max. 0.1 Ti, max. 0.015 B, but the modified composition of the embodiment also includes strict control and modification of additional elements such as 0.001≦C≦0.045 wt%, 0.005≦Si≦0.20 wt%, and ≦0.25 wt% Mn, balance Ni, as well as unavoidable residual elements and impurities. Additionally, the modified composition of the embodiment further includes controlling the particle size of the powder material to have a D50 of 28 μm or more and 38 μm or less.
[0036] The modified compositions of the embodiments have demonstrated superior results over known compositions in that they are capable of producing crack-free articles by powder-based additive manufacturing processes without preheating and HIP over a very wide range of process parameters.
[0037] Example 1: A metal alloy according to the prior art composition shown in Tables 1 and 2, with the actual composition of Cr=20.5 wt%, W=13.6 wt%, Mo=2.0 wt%, Mn=0.35 wt%, Si=0.42 wt%, Al=0.3 wt%, C=0.09 wt%, La=0.02 wt%, Fe=1.0 wt%, Co=0.3 wt%, Ti=0.06 wt%, B=0.006 wt%, balance Ni, and unavoidable residual elements and impurities, was produced by melting and gas atomization to obtain a roughly spherical powder with particles generally sized about 10-50 μm with a D50 of 37 μm. This known metal alloy powder was used in SLM / L-PBF powder bed additive manufacturing to provide a 3D printed article using an EOS M280 machine supplied by EOS GmbH-Electro Optical Systems. 72.5 J / mm 3 A volumetric energy density of was applied to process 3D printing material with a build layer thickness of 0.040 mm.
[0038] As seen in Figures 1A and 1B, which are optical microscope images showing severe cracking that can be observed in the article, the as-fabricated structure of this 3D printed material contains numerous cracks as seen in cross sections parallel to the base plate of the M280 machine (Figure 1A) and perpendicular to the base plate of the M280 machine (Figure 1B). The alloys mentioned above also have a high thermal conductivity of 55-75 J / mm 3 We printed using various process parameters with the volumetric energy density E (Ed) adjusted within the range of 0.01 μm to 0.1 μm, but we were unable to obtain a crack-free structure for this known composition in the full range of parameters investigated.
[0039] Although known Ni-Cr-W-Mo-La alloy compositions similar to the Haynes 230 alloy used in this example are derived from cast or wrought Haynes 230 alloy compositions that are classified as readily weldable by conventional welding techniques, it has been found that when a crack-free or nearly crack-free structure for a 3D printed article is required, the cast or wrought Haynes 230 alloy compositions are not suitable for producing a 3D printed article by the SLM / L-PBF process.
[0040] To overcome these shortcomings identified in structures formed from the prior art Haynes 230 alloy composition, embodiments relate to the modification of the known alloy, where tighter control of the specific constituent elements in the known alloy composition is provided, to achieve crack-free structures of 3D printed articles from such modified alloy. In particular, it could be demonstrated that the contents of C, Si, and Mn in the known composition are too high to use the powder in SLM / L-PBF for crack-free surface structures.
[0041] Example 2: The metal alloy according to the embodiment has a real chemical composition of Cr=19.9 wt%, W=13.4 wt%, Mo=2.0 wt%, Mn=0.01 wt%, Si=0.02 wt%, Al=0.18 wt%, C=0.01 wt%, La<0.005 wt%, Fe=0.1 wt%, Co=0.02 wt%, balance Ni, and unavoidable residual elements and impurities, and was produced by melting and gas atomization to obtain a roughly spherical powder with particles generally sized about 10-50 μm with a D50 of 30 μm. The metal alloy was processed in SLM / L-PBF powder bed additive manufacturing using an EOS M290 machine supplied by EOS GmbH-Electro Optical Systems, with selected process parameters of volumetric energy density Ed to perform a total of 35 3D printing processes, where the utilized volumetric energy density was 38.7 J / mm 3 ~152.29J / mm 3 It was decided.
[0042] The 3D printed materials or articles were investigated in the as-printed state for defects commonly associated with the SLM / L-PBF process, such as holes and cracks. Different levels of porosity were observed for 35 3D printing trials, but no cracks were observed. Table 3 below shows selected results such as number of cracks, porosity, and maximum pore size (in μm) for various parameter fields investigated with Ni-Cr-W-Mo-La alloys having compositions according to embodiments.
[0043] [Table 3]
[0044] Example 3: The Ni-Cr-W-Mo-La alloy in spherical powder form having the composition of the alloy described in Example 2, i.e., the chemical composition according to the embodiment, was used in SLM / L-PBF powder bed additive manufacturing to produce 3D printed articles using an EOS M290 machine supplied by EOS GmbH-Electro Optical Systems. 3 A volumetric energy density of 0.040 mm was applied to fabricate the material with a build layer thickness of 0.040 mm. The resulting microstructure of this 3D printed material is shown in Figures 2A-2C, and no cracks are observed.
[0045] FIG. 2A shows an optical microscope image of a cross-section of the 3D printed material in the as-etched state in a plane perpendicular to the build plate and parallel to the build direction. Individual laser weld tracks are visible in this image. FIG. 2B and FIG. 2C show scanning electron microscope (SEM) images of the cross-sections perpendicular to the machine build plate and parallel to the build direction, respectively. As can be seen from FIG. 2A-C, the resulting structure is dense and crack-free.
[0046] Compared to the structure produced in Example 2, the parameters selected to achieve this exemplary structure can be considered optimized, since not only is the structure crack-free, but the printed material structure according to this example exhibits low as-produced porosity values of 0.024%, corresponding to a 99.97% density of the structure, and a maximum pore size of only 17.86 μm. Thus, the material composition and process parameters of Example 3 represent a preferred embodiment of the present invention.
[0047] Example 4: A metal alloy according to the embodiment having a real chemical composition of Cr=20.0 wt%, W=13.6 wt%, Mo=1.9 wt%, Mn=0.0002 wt%, Si=0.085 wt%, Al=0.21 wt%, C=0.0046 wt%, La=0.023 wt%, Fe=0.035 wt%, Co=0.129 wt%, balance Ni, and unavoidable residual elements and impurities, was produced by melting under vacuum and gas atomizing to obtain a roughly spherical powder with particles generally about 10-50 μm and D50 of 31 μm. The metal alloy was produced using an EOS M290 machine supplied by EOS GmbH-Electro Optical Systems at 60.0 J / mm 3 ~75.0J / mm 3 The material was processed in standard SLM / L-PBF powder bed additive manufacturing with process parameters selected to perform six test 3D prints with a volumetric energy density E adjusted to 6. The six test 3D prints were produced for part density and tensile property samples.
[0048] The produced 3D printed materials / articles were investigated in the as-printed state for defects (e.g., holes and cracks) as commonly associated with the SLM / L-PBF process. The materials were further tested for tensile properties at room temperature and 900 °C (according to ASTM E8M-21 after heat treatment at 1177 °C for 1 hour followed by rapid cooling in nitrogen). Cracks and pores in the printed materials / articles were investigated using high resolution image analysis. Results showed no cracks and few pores as confirmed by high levels of material density, better than 99.99%, in all five test prints with Ed ranging from 66.7 to 75.0. For the fabrication of hardware for tensile testing, an Ed of 60.0 was selected for 3D printing.
[0049] Table 4 has a D50 of 31 μm and is 60.0 J / mm 34 shows the results of tensile tests at room temperature (25° C.) and at high temperature (900° C.) according to ASTM E8M for products / articles manufactured using a standard SLM / L-PBF system (EOS M290 machine supplied by EOS GmbH-Electro Optical Systems) from powder of Ni-Cr-W-Mo-La alloy with a chemical composition according to the embodiment applying a volumetric energy density of 1000 nm. From the tensile test results in Table 4 below, it can be seen that a very high level of ductility is achieved for the test, represented by the elongation at break value, which is a typical sign of a very successful 3D printing run for the material. Furthermore, there seems to be little difference between the results obtained for two different test directions, perpendicular or parallel to the build layer, i.e., Z and XY, which is an additional advantage of the material according to the embodiment.
[0050] [Table 4]
[0051] Therefore, cracks in materials / articles produced from Ni-Cr-W-Mo-La alloys in additive manufacturing processes can be limited by controlling the C, Si, and Mn content of the alloy within the disclosed ranges of 0.001≦C≦0.045 wt%, 0.005≦Si≦0.20 wt%, and Mn≦0.25 wt%, which have been shown to be suitable for producing crack-free 3D printed articles.
[0052] Of course, embodiments are not limited to the examples explicitly described, and in this regard, it is expected that the disclosed Ni-Cr-W-Mo-La alloys are not only suitable for SLM / L-PBF processes, but also for other known powder nozzle additive manufacturing processes, such as laser metal deposition (LMD) or direct energy deposition (DED), as well as electron beam melting (EBM) processes, without departing from the advantages described herein.
[0053] 5941 It should be noted that the foregoing examples are provided for illustrative purposes only and should not be construed as limiting the present invention. Although the present invention has been described with reference to exemplary embodiments, it is understood that the terms used herein are terms of description and illustration, rather than terms of limitation. Changes may be made within the purview of the appended claims, as currently stated and amended, without departing from the scope and spirit of the present invention in its aspects. Although the present invention has been described herein with reference to particular means, materials and embodiments, the present invention is not intended to be limited to the details disclosed herein. Rather, the present invention extends to all functionally equivalent structures, methods and uses, as fall within the scope of the appended claims.
Claims
1. 1. A Ni-Cr-W-Mo-La alloy material powder for additive manufacturing, comprising: 18.0 to 22.0 wt.% Cr, 12.0 to 15.0 wt.% W, 1.0 to 3.0 wt.% Mo, 0.15 to 0.75 wt.% Al, 0.005 to 0.05% by weight of La, More than 0.001 to less than 0.045 wt.% C, More than 0.005 to less than 0.20 wt.% Si; A Ni-Cr-W-Mo-La alloy material powder comprising a balance of Ni and unavoidable residual elements and impurities, said powder having a particle size distribution generally between 10 and 100 μm.
2. 2. The Ni-Cr-W-Mo-La alloy raw material powder according to claim 1, wherein the powder comprises spherical particles.
3. The composition comprises: More than 0% and less than 5% by weight of Fe; More than 0 wt. % and less than 7 wt. % Co; greater than 0 wt.% and less than 0.5 wt.% Ti; greater than 0% and less than 0.020% by weight of B, and 2. The Ni--Cr--W--Mo--La alloy raw material powder according to claim 1, further comprising more than 0 wt. % and not more than 0.25 wt. % Mn.
4. 2. The Ni--Cr--W--Mo--La alloy raw material powder according to claim 1, wherein the Mn content is more than 0 wt. % and less than 0.10 wt. %.
5. The Si 2. The Ni--Cr--W--Mo--La alloy raw material powder according to claim 1, wherein the content is 0.005≦Si≦0.10% by weight.
6. 2. The Ni-Cr-W-Mo-La alloy material powder of claim 1, wherein the powder is a substantially spherical powder having a particle size distribution of 10-50 μm and a D50 of 28-38 μm.
7. 13. An additive manufacturing process for producing a three-dimensional article from the alloy material of claim 1, comprising: 30-150J / mm 3 3D printing the material in a range of 0.1 to 0.5 nm.
8. The laser volume energy density is 60 to 110 J / mm 3 8. The additive manufacturing process for the additive manufacturing of three-dimensional articles according to claim 7, wherein the range of
9. The laser volume energy density is 65 to 100 J / mm 3 8. The additive manufacturing process for the additive manufacturing of three-dimensional articles according to claim 7, wherein the range of
10. 8. An additive manufacturing process for the additive manufacturing of three-dimensional articles according to claim 7, wherein the layers are applied with each layer thickness in the range of 0.01 to 0.1 mm.
11. 8. The additive manufacturing process for additive manufacturing of three-dimensional articles according to claim 7, wherein said additive manufacturing process comprises a selective laser melting process.
12. 8. The additive manufacturing process for additive manufacturing of three-dimensional articles according to claim 7, wherein said additive manufacturing process comprises a laser based powder bed fusion process.
13. 8. The additive manufacturing process for additive manufacturing of three-dimensional articles according to claim 7, wherein the additive manufacturing process comprises a direct energy deposition process.
14. 8. The additive manufacturing process for additive manufacturing of three-dimensional articles according to claim 7, wherein said additive manufacturing process comprises a laser metal deposition process.
15. 8. The additive manufacturing process for additive manufacturing of three-dimensional articles according to claim 7, wherein said additive manufacturing process comprises an electron beam melting process.
16. 1. An alloy material powder for an additive manufacturing process, comprising: 0.001≦C≦0.045 wt.%, and 1. An alloy material powder comprising: 0.005≦Si≦0.20 wt. %, said powder having a particle size distribution generally between 10 and 100 μm.
17. 1. A method for three dimensional printing of an article having a crack free structure, comprising: providing successive layers of a powder having a particle size distribution generally between 10 and 100 μm to a powder additive manufacturing process having a composition including 0.001≦C≦0.045 wt.% and 0.005≦Si≦0.20 wt.%; and applying 38.7 J / mm 3 ~152.29J / mm 3 and applying a volumetric energy density of
18. 18. The method of claim 17, wherein the powder composition further comprises 18.0-22.0 wt.% Cr, 12.0-15.0 wt.% W, 1.0-3.0 wt.% Mo, 0.15-0.75 wt.% Al, 0.005-0.05 wt.% La, >0 wt.% and up to 5 wt.% Fe, >0 wt.% and up to 7 wt.% Co, >0 wt.% and up to 0.5 wt.% Ti, >0 wt.% and up to 0.020 wt.% B, and >0 wt.% and less than 0.25 wt.% Mn, with balance Ni and unavoidable residual elements and impurities.
19. 20. The method of claim 17, wherein the additive manufacturing process comprises one of a selective laser melting (SLM) process, a laser-based powder bed fusion (L-PBF) process, a direct energy deposition (DED) / laser metal deposition (LMD) process, or an electron beam melting (EBM) process.
20. The volumetric energy density E is determined from the following formula: E D =P / v・h・t、 18. The method of claim 17, wherein P is laser power in W, v is laser surface scanning speed, h is hatch distance, and t is layer thickness of each of the welding powder layers, and the powder based additive manufacturing process comprises combining the laser parameters of laser power, laser surface scanning speed, hatch distance, and build layer thickness:
21. 18. The method of claim 17, wherein the powder is an approximately spherical powder with a particle size distribution of 10-50 μm and a D50 of 28-38 μm.
Citation Information
Patent Citations
Nickel-base high temperature alloy and manufacturing method, component and application thereof
CN111500898A
SMTGH3230 spherical powder for 3D printing, and preparation method and application of SMTGH3230 spherical powder for 3D printing
CN112024870A
Methods for additively manufacturing turbine engine components via binder jet printing with nickel-chromium-tungsten-molybdenum alloys
US20190247921A1