Crack-resistant Co-Ni-Cr-W-La alloy for powder-based additive manufacturing
A modified Co-Ni-Cr-W-La alloy with controlled composition and processing parameters addresses cracking issues in additive manufacturing, ensuring crack-free 3D printed articles with enhanced mechanical properties and efficiency.
Patent Information
- Application Number
- JP2024525886
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-05
- Filing Date
- 2022-11-04
- Publication Date
- 2024-10-29
AI Technical Summary
Conventional Co-Ni-Cr-W-La alloys used in additive manufacturing are prone to cracking due to internal stresses caused by temperature gradients during the laser welding process, leading to reduced productivity and increased costs from post-processing steps like Hot Isostatic Pressing.
A Co-Ni-Cr-W-La alloy with a modified chemical composition, including specific ranges of Ni, Cr, W, Si, Fe, Mn, B, C, and La, is used in powder form for additive manufacturing processes like SLM/L-PBF, DED/LMD, and EBM, with controlled laser volumetric energy density and layer thickness to minimize cracking without preheating or post-processing.
The alloy achieves crack-free or near-crack-free 3D printed articles with improved mechanical properties and reduced manufacturing time, overcoming the limitations of traditional alloys by maintaining structural integrity and enhancing productivity.
Smart Images

Figure 2024539713000001 
Figure 2024539713000002 
Figure 2024539713000003
Abstract
Description
[Technical field]
[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims the benefit under 35 USC § 119(e) of U.S. Provisional Application No. 63 / 276191, filed November 5, 2021, the disclosure of which is expressly incorporated herein by reference in its entirety.
[0002] FIELD OF THEINVENTION The present disclosure relates to producing three-dimensional metal articles by powder-based additive manufacturing such as selective laser melting (SLM), also known as laser-based powder bed fusion (L-PBF), direct energy deposition (DED) / laser metal deposition (LMD), or electron beam melting (EBM) processes. In particular, the present disclosure relates to a Co-Ni-Cr-W-La alloy having a modified chemistry compared to cast and / or wrought alloys of similar composition for producing crack-free or near crack-free parts and articles by SLM / L-PBF, LMD / DED, and EBM processes. [Background technology]
[0003] (Background information discussion) Due to the unique process of metal additive manufacturing, also known as 3D printing, using SLM / L-PBF (e.g., rapid solidification from the melt), traditional alloys are prone to cracking during 3D printing because these alloys were originally developed for forging, rolling, or casting processes, not the SLM / L-PBF process.
[0004] Often, when materials for additive manufacturing are required, those skilled in the art use known alloys that have been previously used in rolled, forged, or other wrought forms, including sheets, plates, bars, or castings. Frequently, the chemical composition of the wrought or cast alloy composition is copied into the powder material specifications for additive manufacturing, as in the case of conventional Co-Ni-Cr-W-La alloys. However, this can lead to macro- and / or micro-cracking issues with additively constructed laser welded metal articles.
[0005] A conventional alloy used in 3D printing is Haynes alloy 188. According to manufacturer information for the baseline wrought / cast of Haynes alloy 188, the alloy is classified as readily weldable by Gas Tungsten Arc (GTAW), Gas Metal Arc (GMAW), Shielded Metal Arc (SMAW), electron beam welding, and resistance welding techniques. See Haynes International-HAYNES 188 alloy, www.haynesintl.com / docs / default-source / pdfs / new-alloy-brochures / high-temperature-alloys / brochures / 188-brochure. Based on the manufacturer information, the basic alloy composition of Haynes alloy 188 is in the class of weldable materials. However, cracks have been observed in the 3D printing material during SLM / L-PBF processing of this conventional alloy. It is generally accepted that such cracks are primarily caused by internal stresses that build up in three-dimensional metal parts during the laser welding process (see Fraunhofer ILT, "Flying High with VCSEL Heating," press release, October 4, 2018).
[0006] The internal stresses are caused by temperature gradients within the generated part: at the laser spot, for example, temperatures above the melting point prevail, while the remaining areas of the part cool rapidly. Depending on the geometry and alloy, this temperature gradient can lead to cracks in the 3D printed material.
[0007] In the Fraunhofer press release mentioned above, the conventional approach to solving the cracking problem in Co-Ni-Cr-W-La alloys is explained by heating the powder bed at high temperatures during the 3D printing process, either from the base plate of the build chamber of the SLM / L-PBF machine, or more effectively from the top of the machine's build chamber by directly heating the layers being actively welded, which avoids or reduces the internal stresses in the article that ultimately lead to cracking. Using the latter heating process, the temperature in the top layer can reach up to 900°C, which is high enough to avoid cracking.
[0008] However, before a finished part can be removed from such a heated powder bed, it must be cooled to ambient temperature. Due to the low thermal conductivity of the powder bed, heating and cooling of the powder bed requires a significant amount of time, leading to a significant decrease in the productivity of the SLM / L-PBF process. Furthermore, expensive heating equipment, insulation, and adaptation of the process chamber are required in this conventional process. Currently available commercial SLM / L-PBF machines have limited capabilities to provide powder bed heating at high temperatures.
[0009] Another approach to solving the cracking problem in Ni- and Co-based alloys during additive manufacturing is to apply a heat treatment at high external pressure and high temperature to close and repair any remaining porosity and cracks formed in the 3D printed material. This is known as Hot Isostatic Pressing (HIP). HIP is effective at closing internal pores and cracks, but does not repair all surface cracks. This HIP approach also involves an additional processing step to the 3D printing of the article, which increases the manufacturing cost.
[0010] Therefore, there is a need to provide a Co-Ni-Cr-W-La alloy similar to wrought / cast materials that is in powder form and can be processed in an unheated or slightly heated powder bed, which does not require a post-3D printing processing step to repair cracks by pressurized heat treatment, such as hot isostatic pressing. Summary of the Invention
[0011] The embodiments provide a Co-based alloy with high Ni, Cr, and W content for powder-based additive manufacturing of three-dimensional articles, and a process for manufacturing such articles, with significantly reduced tendency to form cracks in the microstructure during additive manufacturing in a powder bed. In an embodiment of the present disclosure, the Co-Ni-Cr-W-La alloy composition comprises a powder having the following chemical composition: 20.0 to 24.0% by weight of Ni, 20.0 to 24.0 wt.% Cr, 13.0 to 16.0 wt.% W, 0.2 to 0.5% by weight of Si, 0 to 3% by weight of Fe, >0-1.25 wt.% Mn, 0 to 0.015% by weight of B, >0% by weight of C, >0 wt.% La, and Residual amount of Co, as well as unavoidable residual elements and impurities.
[0012] In an embodiment, the alloy composition is available as a wrought material having a C (Carbon) content in the range of 0.05-0.15 wt.% and a La (Lanthanum) content in the range of 0.02-0.12 wt.%. In another embodiment, the alloy composition is provided as a powder material. As a powder material, the alloy composition can be used in powder-based additive manufacturing such as SLM / L-PBF, DED / LMD, or EBM, with a typical particle size distribution in the range of 10-100 μm, which rarely leads to cracks being formed in the article by the process.
[0013] In one embodiment of the present disclosure, the carbon content is 0.05 to 0.15% by weight. In a preferred embodiment of the present disclosure, the carbon content is 0.05 to 0.10% by weight. In another embodiment of the present disclosure, the carbon content is 0.01 to 0.05% by weight. In yet another embodiment of the present disclosure, the carbon content is 0.01 to 0.04% by weight. In another embodiment of the present disclosure, the carbon content is 0.01 to 0.03% by weight.
[0014] In an exemplary embodiment, the alloy composition comprises a ratio of C / La that produces crack-free or nearly crack-free articles by a laser-based powder bed additive manufacturing process without preheating and without HIP over a range of processing parameters.
[0015] The inventors have found that the commonly accepted content ranges of C and La in wrought alloy compositions of conventional Co-Ni-Cr-W-La alloys have unacceptably wide C / La ratios for powder-based additive manufacturing if crack-free or nearly crack-free three-dimensional articles of complex shapes are intended to be consistently provided. For the typical content ranges of C and La in conventional Co-Ni-Cr-W-La alloys, the theoretical minimum ratio of C / La (C / La) is: min is 0.42, the theoretical maximum ratio (C / La) max is 7.50. The ratio of C and La in the nominal content range of conventional Co-Ni-Cr-W-La alloy compositions is (C / La) nom =0.10 / 0.03=3.33.
[0016] In the embodiment of the present disclosure, the C / La content ratio in the Co-Ni-Cr-W-La alloy embodiment is 0.1-2, preferably 0.1-1.5, and more preferably 0.1-1.
[0017] In an advantageous embodiment of the present disclosure, the Co-Ni-Cr-W-La alloy in powder form has a C / La ratio of <1.75 to achieve crack-free printing in powder-based additive manufacturing processes such as SLM / L-PBF.
[0018] In an exemplary embodiment of the present disclosure, the laser-based powder bed additive manufacturing process parameters achieve a dense structure exhibiting a small amount of porosity in the final structure, such as <0.10% by volume, which translates to a relative density of >99.90% of the produced metal article. In an exemplary embodiment, the laser volumetric density E D 50~150J / mm 3 , preferably 75 to 100 J / mm 3 , more preferably 80 to 90 J / mm 3 is within the range.
[0019] The laser volumetric energy density is calculated as follows: E D =P / (vht) where P is the laser power in watts, v is the laser surface scanning speed in mm / s, h is the hatch spacing in mm, and t is the layer thickness in mm of each of the welding powder layers formed during the powder-based additive manufacturing process.
[0020] In another embodiment of the present disclosure, the layer thickness of each welding powder layer in the additively manufactured metal part is in the range of 0.01-0.1 mm, preferably in the range of 0.02-0.07 mm.
[0021] Embodiments are directed to an alloy powder for powder-based additive manufacturing comprising a powder comprising 20-24 wt% Ni, 20-24 wt% Cr, 13-16 wt% W, 0.2-0.50 wt% Si, >0 wt% Mn, >0 wt% C, >0 wt% La, and balance Co. The ratio of C to La content in the powder is 0.1-1.75.
[0022] According to an embodiment, the C content may be 0.01 to 0.05% by weight.
[0023] According to an embodiment, the powder may have a particle size distribution of 10 to 120 μm.
[0024] In another embodiment, the powder has a spherical morphology and a particle size distribution between 10 and 50 μm and a D50 between 25 and 35 μm.
[0025] According to yet other embodiments, the powder may further comprise >0-3 wt.% Fe, >0-1.25 wt.% Mn, and >0-0.015 wt.% B.
[0026] In yet another embodiment, a method for additively manufacturing a three-dimensional article can include subjecting the alloy powder according to claim 1 to a powder-based additive manufacturing process with a laser volume energy density calculated by ED=P / vht, where P is the laser power, v is the laser surface scanning speed, h is the hatch spacing, and t is the layer thickness of each welding powder layer. The laser volume energy density ED for printing a three-dimensional article is 50-150 J / rnm 3 , preferably 75 to 100 J / rnm 3 , more preferably 80 to 90 J / rnm 3 Furthermore, at least one welding powder layer may be applied, and the layer thickness of each welding powder layer may be in the range of 0.01-0.1 mm, preferably in the range of 0.02-0.07 mm.
[0027] Embodiments are directed to a method for three-dimensional printing of an article having a crack-free structure, the method comprising: supplying successive layers of Co-Ni-Cr-W-La alloy powder to a powder-based additive manufacturing process, the Co-Ni-Cr-W-La alloy powder having a composition including C and La such that the ratio of the C content in weight percent to the La content in weight percent is less than 1.75; 3 ~150J / mm 3 to successive layers of the powder.
[0028] According to an embodiment, the C content of the Co-Ni-Cr-W-La alloy powder composition may be 0.01-0.05 wt %.
[0029] According to another embodiment, the Co-Ni-Cr-W-La alloy powder composition may further include 20-24 wt% Ni, 20-24 wt% Cr, 13-16 wt% W, 0.2-0.50 wt% Si, and >0 wt% Mn. The Co-Ni-Cr-W-La alloy powder composition may further include >0-3.0 wt% Fe, >0-1.25 wt% Mn, and >0-0.015 wt% B.
[0030] In an embodiment, the additive manufacturing process may include one of a selective laser melting (SLM) process, a laser-based powder bed fusion (L-PBF) process, a direct energy deposition (DED) / laser metal deposition (LMD) process, or an electron beam melting (EBM) process.
[0031] According to yet other embodiments, the volumetric energy density (ED) may be determined from the equation: ED=P / v·h·t, where P is the laser power in W, v is the laser surface scanning speed, h is the hatch spacing, and t is the layer thickness of each of the welding powder layers in the powder-based additive manufacturing process.
[0032] According to yet another embodiment, the powder may have a spherical morphology and a particle size distribution of 10-50 μm and a D50 of 25-35 μm. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] Prior art Co-Ni-Cr-W-La alloy compositions, whether in solid wrought or powder form, require carbon (C) and lanthanum (La) contents, independent of each other, with C in the range of 0.05% to 0.15% by weight and lanthanum in the range of 0.02% to 0.12% by weight. Typical or nominal contents of the elements in prior art Co-Ni-Cr-W-La compositions include contents of C=0.10% by weight and La=0.03% by weight. Typical contents of C and La in prior art Co-Ni-Cr-W-La compositions are (C / La) max = 7.50 and (C / La) min=0.42, whereas the nominal contents of C and La in the prior art Co-Ni-Cr-W-La compositions are in the range of (C / La) nom = 3.33 content ratio.
[0034] These ranges have been found by the inventors to be unacceptably wide for use in powder-based additive manufacturing if crack-free or nearly crack-free articles are intended to be produced. EXAMPLES
[0035] Comparative Example 1 A prior art Co-Ni-Cr-W-La composition with an actual composition of Ni=22.1 wt%, Cr=22.2 wt%, W=14.6 wt%, Si=0.38 wt%, Fe=0.2 wt%, P<0.01 wt%, S<0.01 wt%, B<0.001 wt%, C=0.09 wt%, La=0.02 wt%, with the balance of Co and unavoidable residual elements and impurities, was produced by melting and gas atomization to provide particles typically around 20-50 μm in size and a mostly spherical powder with a D50 of 33 μm and a D90 of 49 μm. This material was used in an SLM / L-PBF powder bed additive manufacturing process, producing a powder with an industry standard L-PBF machine and 85 J / mm 3 A volumetric energy density of 1000 keV was used to produce a 3D printed article.
[0036] The 3D printed article produced according to Comparative Example 1 showed some cracks in the as-constructed state and was not further tested for mechanical properties. Table 1 below shows that the prior art Co-Ni-Cr-W-La composition of Comparative Example 1 has a C / La content ratio of 4.50 for the produced 3D printed article.
[0037] As shown in Table 1, even though the prior art Co-Ni-Cr-W-La alloy composition is classified as readily weldable by conventional welding techniques, the chemical composition of powders containing this prior art Co-Ni-Cr-W-La alloy is not suitable for producing 3D printed articles by powder-based additive processing where crack-free or nearly crack-free structures are required or even desired.
[0038] [Table 1]
[0039] One aspect of the present disclosure and embodiments is to solve the problems presented by prior art Co-Ni-Cr-W-La alloy compositions by identifying the interdependence of specific elements / components and their relationships in specific amounts / contents in the presently disclosed Co-Ni-Cr-W-La alloy compositions, thereby providing crack-free structures when 3D printed in powder-based additive manufacturing. However, the embodiments are not limited to the explicitly disclosed examples, and are understood to include any embodiment proposed according to the present disclosure that solves the problems presented by prior art Co-Ni-Cr-W-La compositions without departing from the spirit and scope of the embodiments. Furthermore, as shown in Table 1, the contents of certain elements in known Co-Ni-Cr-W-La alloy compositions, such as C and La, as well as the content ratio of C / La in these prior art Co-Ni-Cr-W-La alloy compositions, are not effective for avoiding cracks in 3D printed articles by powder-based additive manufacturing.
[0040] Example 1 A metal alloy according to a preferred embodiment of the present disclosure was produced by melting and gas atomization to produce a generally spherical powder with particles of approximately 20-50 μm size, a D50 of 32 μm, and a D90 of 48 μm. The chemical composition of this Example 1 metal alloy was Ni=21.7 wt%, Cr=21.7 wt%, W=14.1 wt%, Fe=0.2 wt%, Mn=0.5 wt%, Si=0.36 wt%, C=0.06 wt%, La=0.04 wt%, B<0.006 wt%, P<0.01 wt%, S<0.01 wt%, with the balance being Co and unavoidable residual elements and impurities. This material was used in SLM / L-PBF powder bed additive manufacturing using an industry standard L-PBF machine and 85 J / mm 3 The 3D printed article was produced using a volumetric energy density of 1.001 to 1.001. Table 1 shows that the C / La content ratio of the metal alloy of Example 1 was 1.50 for the produced 3D printed article.
[0041] Example 2 A metal alloy according to another embodiment of the present disclosure was produced by melting and gas atomization to provide a mostly spherical powder with particles generally sized between about 20-50 μm, and a D50 of 32 μm and a D90 of 49 μm. The chemical composition of the metal alloy was Ni=22.1 wt%, Cr=22.3 wt%, W=14.4 wt%, Fe=0.2 wt%, Mn=0.2 wt%, Si=0.39 wt%, C=0.10 wt%, La=0.08 wt%, B<0.010 wt%, P<0.01 wt%, S<0.01 wt%, with the balance being Co and unavoidable residual elements and impurities. As shown in Table 1, the metal alloy of this Example 2 has a content ratio of C / La=1.25 and a melting point of 85 J / mm 3 The 3D printed articles were then used in SLM / L-PBF powder bed additive manufacturing to produce 3D printed articles using an industry standard L-PBF machine with a volumetric energy density of 1000 nm. The articles produced showed no cracks in their as-built structures and the samples were subsequently heat treated and tested for mechanical properties at room and elevated temperatures.
[0042] 3D printed samples produced from material according to Example 2 were heat treated at 1177°C for 45 minutes, followed by rapid cooling in air. The heat treated material was then machined into test specimens with a diameter at a gauge length of 6.41 mm, and then subjected to testing to determine the tensile properties of the material according to ASTM E8-16a at 20°C, 537°C and 649°C. As shown in Table 2 below, the material produced according to Tester 2 exhibited superior yield strength and ultimate tensile strength compared to data for wrought materials such as those specified in AMS 5608G. The ductility values (elongation at break) of the material also show elevated values indicating good construction and resulting crack-free structure of this material.
[0043] [Table 2]
[0044] In addition, the anisotropy of the materials described in Examples 1 and 2, which is the difference between the strength and ductility of samples built with the principal axes Y and Z parallel and perpendicular to the L-PBF machine build plate, is relatively low, which is beneficial.
[0045] Since the Co-Ni-Cr-W-La alloys described in Examples 1 and 2 are intended for use at high temperatures, creep tests in the form of so-called stress-rupture tests were typically carried out in accordance with the requirements of AMS 5608G for plates of Co-Ni-Cr-W-La material, which requires a minimum life of 23 hours under a stress of 76 MPa at a temperature of 927° C. for commercial materials. The stress was increased by 13.8 MPa every 8 to 10 hours.
[0046] The results of the stress-rupture tests are shown in Table 3. As shown in Table 3, the requirements of commercially available wrought materials are exceeded for the alloy composition according to Example 2, which is attributed to the sound and crack-free structure of the material produced according to Example 2.
[0047] [Table 3]
[0048] The present invention is not limited to the embodiments and examples described above. For example, the disclosed Co-Ni-Cr-W-La alloy is not only suitable for SLM / L-PBF processes, but also for powder nozzle additive manufacturing processes, also called laser metal deposition (LMD) or direct energy deposition (DED) as well as electron beam melting (EBM) processes, with the advantages described.
[0049] Furthermore, because at least the invention is disclosed herein in a manner that enables it to be made and used by disclosure of certain exemplary embodiments, for purposes of simplicity or efficiency, the invention can be practiced in the absence of any additional elements or additional structure not specifically disclosed herein.
[0050] It should be noted that the foregoing examples are provided for illustrative purposes only and are not to be construed as limiting the present invention in any way. Although the present invention has been described with reference to exemplary embodiments, it is understood that the terms used herein are terms of description and illustration, rather than terms of limitation. Changes may be made within the scope of the appended claims, as currently described and amended, without departing from the scope and spirit of the present invention in its aspects. Although the present invention has been described herein with reference to specific means, materials, and embodiments, the present invention is not intended to be limited to the details disclosed herein, but rather the present invention extends to all functionally equivalent structures, methods, and uses as are within the scope of the appended claims.
Claims
1. 1. An alloy powder for powder-based additive manufacturing, comprising: A powder comprising: 20 to 24 wt.% Ni; 20 to 24 wt.% Cr; 13-16 wt.% W; 0.2 to 0.50 wt.% Si; >0 wt.% Mn; >0 wt.% C; >0 wt.% La; and a balance of Co, The alloy powder, wherein the ratio of the C to La content in the powder is 0.1 to 1.
75.
2. 2. The alloy powder according to claim 1, wherein the C content is 0.01 to 0.05 wt. %.
3. The alloy powder of claim 1, wherein the powder has a particle size distribution of 10 to 120 μm.
4. 2. The alloy powder of claim 1, wherein the powder has a spherical morphology and a particle size distribution of 10-50 μm and a D50 of 25-35 μm.
5. The powder is >0-3 wt.% Fe; >0-1.25 wt.% Mn; 2. The alloy powder of claim 1, further comprising: >0-0.015 wt.% B.
6. 1. A method for additive manufacturing of a three-dimensional article, comprising:
13. A method for producing an additive manufacturing process comprising: subjecting the alloy powder of claim 1 to a powder-based additive manufacturing process having a laser volumetric energy density calculated by: E D = P / v.h.t, where P is the laser power, v is the laser surface scanning speed, h is the hatch spacing, and t is the layer thickness of each welding powder layer; The laser volumetric energy density E for printing the three-dimensional object D However, 50 to 150 J / mm 3 That is, the method.
7. The laser volumetric energy density E for printing the three-dimensional object D However, 75 to 100 J / mm 3 The method according to claim 6, wherein
8. The laser volumetric energy density E for printing the three-dimensional object D However, 80 to 90 J / mm 3 The method according to claim 6, wherein
9. The method of claim 6, wherein at least one welding powder layer is applied, and the layer thickness of each welding powder layer is in the range of 0.01 to 0.1 mm.
10. The method of claim 6, wherein the layer thickness of each welding powder layer is in the range of 0.02 to 0.07 mm.
11. 1. A method for three dimensional printing of an article having a crack free structure, comprising: providing successive layers of Co-Ni-Cr-W-La alloy powder to a powder-based additive manufacturing process, the Co-Ni-Cr-W-La alloy powder having a composition including C and La such that a ratio of the C content in weight percent to the La content in weight percent is less than 1.75; 50 J / mm 3 ~150 J / mm 3 and applying a volumetric energy density of said powder to said successive layers of said powder.
12. The method according to claim 11, wherein the C content of the Co-Ni-Cr-W-La alloy powder composition is 0.01-0.05 wt%.
13. 12. The method of claim 11, wherein the Co-Ni-Cr-W-La alloy powder composition further comprises 20-24 wt.% Ni, 20-24 wt.% Cr, 13-16 wt.% W, 0.2-0.50 wt.% Si, and >0 wt.% Mn.
14. 14. The method of claim 13, wherein the Co-Ni-Cr-W-La alloy powder composition further comprises >0-3.0 wt.% Fe, >0-1.25 wt.% Mn, and >0-0.015 wt.% B.
15. 12. The method of claim 11 , wherein the additive manufacturing process comprises one of a selective laser melting (SLM) process, a laser-based powder bed fusion (L-PBF) process, a direct energy deposition (DED) / laser metal deposition (LMD) process, or an electron beam melting (EBM) process.
16. The volumetric energy density (E D ) is determined from the following equation: E D = P / v h t, 12. The method of claim 11 , wherein P is laser power in W, v is laser surface scanning speed, h is hatch spacing, and t is a layer thickness of each of the j welding powder layers in the powder-based additive manufacturing process.
17. 12. The method of claim 11, wherein the powder has a spherical morphology and a particle size distribution between 10 and 50 μm and a D50 μm between 25 and 35.
Citation Information
Patent Citations
Co-based alloy used for combustion chamber components, and preparation method thereof
CN106756404A
SMTGH5188 spherical powder for 3D printing, and preparation method and application of SMTGH5188 spherical powder for 3D printing
CN112024869A
Preparation method of GH5188 cobalt-based high-temperature alloy powder for 3D printing
CN112809010A
Crack-free nickel-based superalloy and component design method and preparation method thereof
CN113073235A
Alloy material, product using said alloy material, and fluid machine having said product
WO2019088157A1