Preparation of high-speed superabsorbents with enhanced elastic behavior
The novel perforated plate design and monomer formulation in the extrusion process enhance the absorption rates and stability of superabsorbents, addressing thixotropic issues to improve the performance of personal hygiene products.
Patent Information
- Application Number
- JP2024520847
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-21
- Filing Date
- 2022-10-17
- Publication Date
- 2024-10-31
AI Technical Summary
Existing superabsorbent polymers face challenges in achieving high absorption rates while minimizing thixotropic behavior, which can lead to instability and leakage in personal hygiene products under external pressure.
A method involving the use of a novel perforated plate design in the extrusion process, with specific geometric parameters (5.5<2.10686036×(l/d) 0.774457 ×(V/A) -0.117802 <13.3) to control viscoelastic behavior, combined with a monomer mixture formulation that includes a blowing agent precursor to create a porous structure, resulting in a water-absorbing polymer with enhanced yield stress and absorption rates.
The method produces superabsorbents with improved yield stress (180 Pa to 254 Pa), increased absorption rates (FSR > 0.48 s to 0.88 s), and balanced property profiles, including higher centrifugal retention capacity and absorbency under pressure, while reducing thixotropic behavior, ensuring stability under load.
Smart Images

Figure 2024539848000006 
Figure 2024539848000007 
Figure 2024539848000008
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for preparing a water-absorbing polymer and to the water-absorbing polymer obtained thereby. [Background technology]
[0002] "Superabsorbent" is a common commercial term referring to polymer particles that can absorb large amounts of water without releasing the water under pressure. Other common terms are "superabsorbent materials" (SAMs), "superabsorbent polymers" (SAPs), or "absorbent gelling materials" (AGMs).
[0003] When superabsorbents absorb water, they expand rapidly. The water becomes trapped within the polymer network, and the hydrated superabsorbent forms a hydrogel. As well as water, superabsorbents can also absorb saline and many types of bodily fluids. This ability makes them an important component of personal hygiene products such as baby diapers and feminine care and incontinence products.
[0004] Superabsorbents are produced on a large industrial scale, with world production exceeding one million tonnes per year.
[0005] The technology of water-absorbing polymers can be derived from the following. Marcus Frank: Superabsorbents, Ullman Encyclopedia of Industrial Chemistry, published online: January 15, 2003, DOI:10.1002 / 14356007.f25_f01
[0006] The prevalent industrial process for manufacturing superabsorbents consists of the following basic steps: A monomer mixture is prepared. Its essential components are monomer, crosslinker, and initiator. Mainly, acrylic acid is selected as the monomer. As a solvent, water is also present in the monomer mixture. Other components may also be included, such as comonomers that will be included in the subsequent polymer, or auxiliary components that will not become part of the subsequent polymer.
[0007] The monomer mixture is fed into the reactor and polymerization is initiated by appropriate means depending on the type of initiator. During polymerization, the monomers build up polymer chains and are cross-linked by the cross-linking agent to form a three-dimensional polymer network. Water becomes trapped within the network. Thus, the reaction product is a hydrogel.
[0008] The hydrogel needs to be decomposed. This can be done directly in the reaction vessel using a stirrer (kneading reactor) and / or in one or more separate devices, so-called extruders or choppers.
[0009] In either case, the end of the degradation process is at least one extrusion vessel covered with a perforated plate through which the (pre-powdered) hydrogel is extruded, passing axially through the perforations to obtain the extruded hydrogel.
[0010] The extruded hydrogel is dried to expel the water from the polymer network. A solid polymer material is then obtained. The particle size of the polymer material then needs to be adjusted. This is done by grinding and sieving the solid polymer material to obtain a powder with a specific particle size between 150μm and 850μm.
[0011] The polymer powder is capable of absorbing water as a reversal of the drying process, but further finishing steps are required to improve performance.
[0012] Specifically, the powder is subjected to a surface cross-linking treatment. During surface cross-linking, the cross-linking density of the near-surface region of each particle increases. Thus, each particle obtains an egg-like core / shell structure with a soft core with a similar low cross-linking density and a hard shell with a higher cross-linking density. The core / shell structure greatly influences the absorption properties of the SAP.
[0013] Besides the absorption properties, other functions such as odor control, color stability, good storage and transport properties are adjusted during post-processing by adding further components to the polymer powder.
[0014] Superabsorbents are usually purchased by manufacturers of personal hygiene products. When making a purchasing decision, the overall performance profile of the superabsorbent is important. The required performance profile varies greatly depending on the type and purpose of the hygiene product. Over the past decades, numerous performance parameters have been established by market participants to compare the suitability of different SAP qualities for their applications. Some of these performance parameters are standardized by independent authorities, while others are defined by specific hygiene product manufacturers solely for their individual needs. In fact, in the real SAP market, both performance parameters are important. In addition, the patent literature is packed with parameters that have no impact whatsoever outside of specific patent rights.
[0015] In the present invention, the following performance parameters are of concern:
[0016] Storage modulus (G') The storage modulus represents the ratio of the shear stress (force) to the shear strain (deformation) of an elastic solid. G' is therefore a numerical representation of elasticity. Its units are Pascals. The higher the value, the harder the material. Elasticity is highly dependent on the water content. Dry SAP is relatively solid, whereas water-swollen SAP (hydrogels) exhibit viscoelastic behavior. G' is therefore measured in the swollen state. The amount of liquid absorbed by the probe is defined by the relevant method. The amount absorbed varies greatly from method to method, making it difficult to compare values obtained by different methods. Furthermore, the viscoelastic properties are recorded using oscillatory measurements that are influenced by other parameters. The methods used herein are defined below in the section "Gel Bed Rheology". In the (patent) literature, the following terms are used instead of storage modulus to describe the elasticity of SAP hydrogels: elastic modulus, storage modulus, gel strength, gel bed elasticity.
[0017] Yield stress (YS) The viscoelasticity of a hydrogel depends on time and stress (thixotropy). With increasing stress or constant stress over time, the elasticity decreases rapidly. The yield stress is the mechanical load applied at the moment when the elasticity of the hydrogel breaks down. Thus, the yield stress identifies the point at which the gel bed breaks down, the particles move relative to each other and the gel loses its elasticity. The higher the YS, the more elastic the material is, and the lower the YS, the less elastic the material is. The unit of yield stress is Pascal.
[0018] General articles dealing with the measurement of yield stress are available from: https: / / cdn.technologynetworks.com / TN / Resources / PDF / WP120416UnderstandYieldStressMeas.pdf
[0019] The method for measuring the yield stress used herein is defined in the "Gel Bed Rheology" section below. In practical applications, the yield stress is an important value that indicates reliability. The higher the value, the lower the risk of viscosity loss due to thixotropic behavior. A lower yield stress means that the adverse effects of thixotropy are less likely to be seen.
[0020] Free Swell Rate (FSR) This is a parameter relating to the rate of absorption of SAP in the absence of external pressure. It is constructed as the mass rate of absorbed urine per mass unit of SAP. It is expressed in seconds and is sometimes written as g / g*s. The higher the number, the faster the absorption rate. This parameter was established by a major diaper manufacturer. The test procedure is disclosed in EP 0 443 627 A1, page 12, lines 24 to 44.
[0021] Absorption of 20g / g (T20) This is a parameter related to the absorption rate of SAP in the absence of external pressure. It is configured as the time it takes for a certain amount of urine (20 g) to be absorbed by 1 g of SAP. The unit is seconds. The smaller the value, the faster the absorption rate. This parameter was established by another major diaper manufacturer. The test procedure is disclosed in paragraphs
[0027] to
[0071] of EP 2535697.
[0022] Centrifugal retention capacity (CRC) It is one of the oldest performance parameters of SAP. It refers to the capacity to absorb urine. It is expressed in g / g or [-]. The higher the value, the higher the capacity. This value is often called "tea bag capacity" because the test method uses tea bags that are officially filled with SAP. The test method involves centrifugation of the filled probe. However, the rotation speed, or centrifugal force G, chosen varies from time to time. Therefore, this value is only reliable for a specific rotation speed or G force. This method has been standardized by the industry association EDANA as standard test WSP 241.2(05).
[0023] Absorbency Under Pressure (AUP) It refers to the capacity to absorb urine when subjected to external pressure. Its unit is g / g or [-]. The higher the value, the higher the capacity. Different pressures are applied to the probe. Some use a pressure of 4.83 kPa (=0.7 psi, hence named AUP0.7), while others prefer a pressure of 2.07 kPa (=0.3 psi, hence named AUP0.3). Therefore, this value is only informative when a given pressure is applied. In this specification, AUP was measured at 4.83 kPa. The AUP value is also called "Absorbency Under Load (AUL)". This method is standardized by the industry association EDANA as standard test WSP 242.2(05).
[0024] Because the definitions of performance parameters change over time, it is not possible to compare specific values without considering the exact measurement methods used prior to that time period.
[0025] It is known that there are objective relationships and conflicts between the individual performance parameters. For example, measures to strengthen the AUP can result in a reduction in the CRC (see figure 7 of Frank cited above). Thus, developing a superabsorbent with improved behavior with respect to property X additionally implies not compromising property Y. A well-balanced property profile, optimized for the intended purpose of the SAP, is crucial.
[0026] A common mathematical approach to determining the balance of conflicting properties is to define an index as an arithmetic function of a number of property parameters. In the simplest case, the index is defined as the product of two parameters. If the value of the index is within a certain range, the property profile represented by the two parameters is balanced.
[0027] In the present case, thixotropic behavior and absorption rate were of interest. Specifically, an ultrafast superabsorbent was required that achieves an FSR value of at least 0.4 g / g / s or more. Such ultrafast superabsorbents are required for the construction of ultrathin diapers. A fast absorption rate together with permeability is key to replace a large amount of fluff in the diaper construction. With regard to viscoelasticity, it is beneficial if the hydrogel does not exhibit thixotropic behavior under the load applied during production, since this improves the processing efficiency during SAP production. In addition, it is undesirable for the gel bed to exhibit thixotropic properties in a diaper under load. Under prolonged external pressure, a swollen gel bed may suddenly lose its stability. This may result in leakage or poor rewetting behavior. Thus, a superabsorbent that does not exhibit thixotropy in the swollen state helps to improve the reliability of personal hygiene products. Swollen superabsorbents that do not exhibit thixotropy under the relevant loads behave like Newtonian fluids. Such viscoelastic behavior is desirable for the reasons mentioned above.
[0028] In order to improve the absorption rate value FSR, EP 2557095 proposes to adjust the mass specific energy required to contain the hydrogel within a certain range. The specific energy is calculated from the power consumption and efficiency factor of the grinding machine motor. Although the power consumption is easy to measure, EP 2557095 does not provide any information on how to measure the mechanical efficiency of the grinding machine. In paragraph
[0049] , it is stated that the efficiency can be inquired from the manufacturer of the gel grinding machine, but this is not true. Therefore, EP 2557095 does not teach the skilled person the details of the specific design of the grinding machine that will result in the desired efficiency.
[0029] The aim of EP 2951212 is to provide a SAP with improved FSR and CRC. The specific energy input during extrusion is limited to 60 kWh / t. The specific energy input is influenced by the extruder length to diameter ratio. Several extruder die dimensions are given, but their impact on FSR is not discussed.
[0030] EP 3070114 aims to improve the absorption properties of SAP, i.e. CRC and AUL. To achieve this, chopper die design rules are disclosed. However, no means are given to influence the absorption rate or thixotropy.
[0031] WO 2016 / 105119 also deals with the design of the chopper die. The shear stress during extrusion must be reduced in order to have less impact on the extractables. However, there is no mention of the subsequent viscoelastic behavior of the SAP.
[0032] EP 3067370 discloses a method for preparing SAPs with a specific gel strength. CRC, AUL, and FSR must be balanced. A relationship is established between the exit diameter of the extruder used and the gel strength. The number of exits of the extruder is not given.
[0033] US 2021 / 298962 deals with the manufacture of feminine hygiene absorbent products. In this process, a polymer gel is extruded using a pastry machine with a perforated plate with 12 holes with a hole diameter of 8 mm. The perforated plate had a thickness of 16 mm. The overall diameter of the perforated plate was not disclosed. The ratio of the inner length to the inner diameter of the extruder (L / D) was 4. This value relates to the bore of the extruder barrel of the pastry machine. However, the ratio of the length and diameter of the holes is not given.
[0034] EP 2565211 A1 relates to superabsorbents based on recent carbon sources. In an exemplary preparation, the hydrogel was finely ground by a meat chopper with a hole diameter of 8 mm. The length of the hole and the diameter of the plate are not given. The number of holes in the meat chopper is also not mentioned.
[0035] EP 3248993 A1 discloses a high-speed superabsorbent with low vortex value. During its preparation, the hydrogel is cut into chunks using a meat chopper. No further information on the meat chopper is given.
[0036] US 2007 / 060691 describes the use of a laboratory extruder from MADO GmbH to break up the hydrogel into small pieces. No detailed information on the machine parameters is given.
[0037] US 2014 / 312273 aims to produce water-absorbing polymers with improved swelling and faster liquid absorption rates while simultaneously maintaining the overall quality, and more specifically high permeability. During this process, the gel is ground in a meat grinder. The parameters of the meat grinder are not disclosed.
[0038] In EP 3406655 the balanced properties are T20, CRC and AUP. The cutting index is made up of the open area of the hole plate used, the screw speed and the solids content of the extruded hydrogel.
[0039] EP 2944376 and US 10130527 both disclose a method for producing a high-speed superabsorbent (T20=104 seconds) by forced agglomeration of two fractions of smaller polymer particles. The resulting superabsorbent is therefore considered to be mainly agglomerates. A structural disadvantage of agglomerated superabsorbents is their reduced mechanical strength. Agglomerated particles necessarily contain grain boundaries. These grain boundaries form fracture points within the particles. Under increasing mechanical stress, the agglomerates tend to break apart at the grain boundaries and deagglomerate. Thus, superabsorbents prepared by forced agglomeration are less stable than normal non-agglomerated monolithic superabsorbents. A further disadvantage of forced agglomeration as disclosed in EP 2944376 and US 10130527 is that it is an intensive process of extrusion / swelling / re-extrusion to produce a faster product. Implementation in a factory would be a clear capital expense. At first glance, the current prior art does not teach how one can positively influence both the absorption rate of a superabsorbent and the thixotropy of the corresponding hydrogel. [Prior art documents] [Patent documents]
[0040] [Patent Document 1] European Patent Application Publication No. 0443627 [Patent Document 2] European Patent Application Publication No. 2535697 [Patent Document 3] European Patent No. 2557095 [Patent Document 4] European Patent No. 2951212 [Patent Document 5] European Patent Application Publication No. 3070114 [Patent Document 6] International Publication No. 2016 / 105119 Brochure [Patent Document 7] European Patent No. 3067370 [Patent Document 8] US Patent Application Publication No. 2021 / 298962 [Patent Document 9] European Patent Application Publication No. 2565211 [Patent Document 10] European Patent Application Publication No. 3248993 [Patent Document 11] US Patent Application Publication No. 2007 / 060691 [Patent Document 12] US Patent Application Publication No. 2014 / 312273 [Patent Document 13] European Patent Application Publication No. 3406655 [Patent Document 14] European Patent Application Publication No. 2944376 [Patent Document 15] U.S. Pat. No. 1,013,0527 [Non-patent literature]
[0041] [Non-Patent Document 1] Marcus Frank: Superabsorbents, Ullman Encyclopedia of Industrial Chemistry, published online: January 15, 2003, DOI:10.1002 / 14356007.f25_f01 [Non-Patent Document 2] https: / / cdn.technologynetworks.com / TN / Resources / PDF / WP120416UnderstandYieldStressMeas.pdf Summary of the Invention [Problem to be solved by the invention]
[0042] It is therefore an object of the present invention to provide water-absorbing polymers with improved absorption rates and less thixotropic behavior, as well as methods for producing such polymers on an industrial scale. [Means for solving the problem]
[0043] This object was achieved in the following manner. (a) - at least one ethylenically unsaturated monomer having an acid group, which is optionally at least partially neutralized; - Water, at least one crosslinking agent, - at least one initiator or at least one component of an initiator system, optionally at least one ethylenically unsaturated comonomer polymerizable with said monomer, - optionally at least one water-soluble polymer, - optionally at least one blowing agent precursor, - additional ingredients, if necessary; providing a monomer mixture comprising: (b) providing a reactor having a reaction vessel; (c) preparing an extruder having an extrusion container, the extrusion container being covered with a perforated plate, the perforated plate having a plurality of through holes, each of the through holes having an equivalent diameter d and an axial length l, the total void area of the perforated plate being V, the total area of the perforated plate including the void area being A, and the shape of the perforated plate being in accordance with the requirements: 5.5<2.10686036×(l / d) 0.774457 ×(V / A) -0.117802 <13.3 and (d) carrying out polymerization in a reaction vessel by inverting the components of the monomer mixture to obtain a crosslinked polymer hydrogel; (e) optionally, chemically and / or physically modifying the hydrogel to obtain daughter products of the hydrogel; (f) transferring the hydrogel or daughter product thereof to the extrusion vessel; (g) optionally chopping the hydrogel or daughter products thereof within the extrusion vessel; (h) extruding the hydrogel or daughter product thereof from the extrusion vessel through the perforated plate, forcing the hydrogel or daughter product thereof axially through the through holes to obtain an extruded hydrogel; (i) optionally chemically and / or physically modifying the extruded hydrogel to obtain a daughter product of the extruded hydrogel; (k) drying the extruded hydrogel or daughter products thereof to obtain a solid polymeric material; (l) grinding the solid polymeric material to obtain a polymeric powder; (m) sieving the polymer powder to obtain at least one sized fraction of the polymer powder; (n) post-treating the sized fraction to obtain a water-absorbing polymer, the "post-treatment" step including at least one surface cross-linking step; A method for preparing a water-absorbing polymer comprising: Such a method is a first object of the present invention.
[0044] More precisely, the replacement of the conventional perforated plate in the conventional SAP manufacturing process with the novel perforated plate fulfilling the following requirements results in a water-absorbing polymer with a higher yield stress compared to a superabsorbent obtained by the conventional manufacturing process using the conventional perforated plate: Requirements: 5.5<2.10686036×(l / d) 0.774457 ×(V / A) -0.117802 <13.3 (In the above requirements, l represents the axial length of the hole in the perforated plate, d represents the equivalent diameter of the hole in the perforated plate, V represents the gap area of the perforated plate, A represents the total area of the perforated plate including the void area.) Therefore, the elasticity of the superabsorbent obtained by the present invention is maintained up to a higher load. Therefore, it is expected that the elasticity collapse due to thixotropic behavior will be observed under a load higher than that of the conventional one. The yield stress of the water-absorbent polymer obtained by the manufacturing method of the present invention is within the range of 180 Pa to 254 Pa.
[0045] In contrast to previous teachings regarding the geometry of extruder dies, current design rules incorporate two factors: the narrowness of the hole (l / d) and the porosity of the entire hole (V / A). These complex specifications allow for proper definition of the stresses within the hydrogel during extrusion to very precisely tune the viscoelastic behavior.
[0046] The current design rules were evaluated based on a comprehensive study of different perforated plates and their impact on SAP. Hydrogels were extruded with a large number of hole geometries and a large number of different hole counts. Water-absorbent polymers were produced from the extruded hydrogels using different perforated plates, and the performance parameters and rheology of the water-absorbent polymers were investigated. Several perforated plates were empirically found to have a positive impact on the desired performance parameters.
[0047] Next, the geometrical features of the identified perforated plates were intelligently analyzed to discover the similarities and related parameters. The chosen approach was based on the principle of describing physical effects using dimensionless numbers, according to the Pi theorem put forward by Edgar Buckingham (1867-1940). The hole fineness l / d and porosity V / A were found to be the dimensionless numbers that most affect the yield stress and absorption rate. Both quantities were combined in the form of a power function, each with a constant coefficient and an exponent. The constant coefficient and exponent quantities were adjusted using the least squares method to fit the useful perforated plate geometries found in the laboratory. Finally, the quality of the aligned approximation was verified using previously obtained experimental data. The suggested approximation turned out to be surprisingly feasible and simple.
[0048] According to the findings of the present invention, the yield stress and the absorption rate are substantially affected by two geometrical properties of the perforated plate, namely the hole narrowness l / d and the porosity V / A.
[0049] "Porosity" is the ratio of the area of voids within the plate, V, to the area A of the entire perforated plate exposed to the hydrogel.
[0050] The perforated plate that covers the extrusion vessel is necessarily perforated. It includes at least one orifice through which the hydrogel leaves the extrusion vessel during extrusion. The perforated plate may have multiple such holes. This should be the normal situation. In this specification, the entire set of holes is referred to as through holes, regardless of whether it is a single orifice or an array of multiple holes.
[0051] The void area is the sum of the total area of the holes through which the hydrogel is extruded. (The hole plate may have other holes through which the hydrogel is not extruded, for example, they may be screw holes to secure the hole plate to the extruder. Since no hydrogel is extruded through such holes, they have no effect on rheology or absorbency. Therefore, such holes are not taken into account when summing the void area.)
[0052] The cross section of the hole does not have to be constant in the axial direction: the hole may be tapered, in which case the area of the hole is determined at its narrowest point.
[0053] The area A of the perforated plate exposed to the hydrogel is the area of the part of the perforated plate that is subjected to the water pressure of the hydrogel, i.e., the area of the part in contact with the hydrogel. It does not include the part that is not in contact with the hydrogel, i.e., its bearing surface. However, the through holes are part of the area. Therefore, the area value is always greater than the blank area value. Therefore, the blank ratio is always less than 1.
[0054] The present invention assumes that the hole plate is planar. Therefore, all areas are simply measured in a plane. However, in some cases, the hole plate may have a three-dimensional design, such as a hemisphere. In that case, the area is calculated in a spatial domain rather than a planar projection. The reason is that the pressure profile of the hydrogel is performed spatially rather than projectionally.
[0055] The narrowness of the hole is the second characteristic of the perforated plate that affects the yield stress and absorption rate. The narrowness is defined as the ratio of the axial length of the hole, l, to the equivalent diameter of the hole, d, of the perforated plate. The higher the l / d ratio, the narrower the hole. In most cases, the narrowness is greater than 1, but stubby holes with l / d less than 1 are possible as well.
[0056] If the holes extend vertically through the perforated plate, the axial length will be equal to the thickness of the perforated plate.
[0057] The cross section of the hole does not necessarily have to be circular. The cross section of the hole may be of other shapes. To characterize the size of an orifice of any shape, the equivalent diameter is used. The equivalent diameter d of a single hole is defined as the diameter of an imaginary circle that has the same area as the cross section of the actual hole. If the hole in the plate is circular, the equivalent diameter is equal to the actual diameter of the hole. If the hole in the plate is non-circular, the cross section area of the hole is measured. Then, an imaginary circle with the same area as the actual inner diameter is imaged. The calculated diameter of the imaginary circle is defined as the equivalent diameter of the actual shape. For example, if the hole is a square with side length s, the equivalent diameter is calculated as d = 1.1288 x s. If the hole is a hexagon with side length a, the equivalent diameter is calculated as d = 1.8188 * x a.
[0058] In the simplest case, the equivalent diameter of all holes is equal. However, it is also possible to provide perforated plates with holes of different sizes. In such a case, the individual equivalent diameter has to be ascertained for each individual hole. The equivalent diameter of the entire through hole is the arithmetic median of all the individual equivalent diameters. The same approach applies if the through hole contains holes of different shapes.
[0059] In the simplest case, the extruder consists of just one single perforated plate. However, there are known choppers with a series of perforated plates located downstream of the extrusion vessel. In such cases, only the shape of the last perforated plate that actually caps the extrusion vessel is relevant for application of the design rules of the present invention, since the pressure drop is the highest at the last downstream perforated plate.
[0060] Thanks to the design rules of the present invention it is now possible to provide a perforated plate which produces a defined stress regime during extrusion, so that the viscoelastic behavior of the superabsorbent can be easily controlled in the desired way without further trial and error.
[0061] A further effect of the defined stress regime during extrusion is the evaporation of water trapped within the polymer network due to high pressure and frictional heat. The steam generated within the hydrogel expands and a porous structure is formed. The latter is preserved during drying, so that the subsequent superabsorbent acquires a porous morphology. Thanks to the porosity, the surface area of the superabsorbent is enlarged, which ultimately increases the absorption rate.
[0062] According to a preferred embodiment of the present invention, the monomer mixture is made with the following formulation: - at least partially neutralized acrylic acid: 10% to 70% by weight -Water: 30%~80% by weight - Crosslinking agent: 0.05% to 5% by weight - Initiator: 0.1% to 1% by weight - Comonomer: 0% by weight - Water-soluble polymer: 0% by weight -Precursor of foaming agent: 0% to 1% by weight -Other ingredients: 0% to 20% by weight
[0063] All percentages above are based on the total weight of the monomer mixture. All percentages add up to 100% by weight. A content of 0 means that the relevant component has not been added to the monomer mixture. A content ranging from 0 to a percentage greater than 0 means that the relevant component may be included as required. The term "additional components" includes components that are not monomers, water, crosslinkers, initiators, comonomers, water-soluble polymers, or blowing agent precursors.
[0064] This preferred formulation has been well proven to result in a water-absorbing polymer with high yield stress, fast absorption rate, and additional beneficial properties.
[0065] Preferably, the monomer mixture contains a precursor of a blowing agent. The amount of the precursor is within a range of 1000 ppm to 1500 ppm based on the weight of the monomer mixture. The unit ppm is 10 -6 The precursor is a material that reacts upon polymerization to produce a gas. The gas blows out of the monomer mixture upon polymerization to produce a foam-like hydrogel. The gas becomes trapped in the pores of the hydrogel. Thus, the effective blowing agent is not the precursor, but the gas produced. The precursor must not react with the monomer or comonomer that will be incorporated into the polymer chain. Rather, the precursor is intended to react independently of the polymerization reaction. Precursors that meet these requirements are selected from the group consisting of sodium carbonate, potassium carbonate, ammonium carbonate, ammonium carbamate, magnesium carbonate, calcium carbonate, barium carbonate, lithium carbonate, sodium bicarbonate, potassium bicarbonate, ammonium bicarbonate, magnesium bicarbonate, calcium bicarbonate, barium bicarbonate, 3-oxopentanedioic acid, and urea. The gas produced by these precursors and acting as a blowing agent is most often carbon dioxide.
[0066] The porous structure of the hydrogel expanded by the blowing agent is maintained in the superabsorbent afterwards. The porosity increases the absorption rate. Therefore, the blowing agent improves the water evaporation effect during extrusion.
[0067] Within the method of the present invention, the formulation of the monomer mixture includes at least one compound that acts as a crosslinker. Otherwise, a three-dimensional polymer network will not be formed. It is possible to use several different substances, each of which acts as a crosslinker. The total amount of all crosslinkers in the monomer mixture is preferably more than 10 mmol and less than 50 mmol, based on 1 mole of monomer. The unit millimolar is 10 -3 The total amount of crosslinkers is expressed as moles. When only one crosslinker is included, the total amount of crosslinkers is equal to the amount of a single crosslinker. If the total amount of crosslinkers is less than 10 millimoles, the crosslink density may be insufficient and the strength of the gel may be compromised. Conversely, if the total amount of crosslinkers is more than 50 millimoles, the gel strength may be abnormally high. Extrusion of very stiff hydrogels through the hole plate of the present invention requires a huge amount of energy. Friction increases and the hydrogel may be thermally damaged.
[0068] The method of the present invention includes a surface cross-linking step, which increases the cross-link density of the polymer powder in the area near the surface of each powder particle. Thus, the particles acquire a core / shell structure. Several methods are known in the field of superabsorbent polymer manufacturing technology for achieving such a core-shell structure. The surface cross-linking method best suited for the present process includes adding at least one surface cross-linking agent and, optionally, at least one further component to a sized fraction of the polymer powder or its daughter product to obtain a mixture, and subjecting the mixture to a heat treatment to increase the cross-link density in the surface area of the polymer powder.
[0069] The method of the present invention uses at least one reactor for carrying out the polymerization and at least one extruder for extruding the hydrogel. According to a preferred embodiment of the present invention, the reactor and the extruder are provided structurally separate. Thus, dedicated equipment is used to carry out each of the polymerization and extrusion steps. Preferably, a belt reactor with an endless running belt, which serves as a reaction vessel, is used for the polymerization, and a meat chopper is used to carry out the extrusion step. Alternatively, both reaction and extrusion functions may be carried out in one combined device. A well-known type of equipment that integrates both reaction and extrusion steps is the kneading reactor.
[0070] The second object of the present invention is a water-absorbing polymer having a yield stress (YS) in the range of 180 Pa to 254 Pa. This water-absorbing polymer is obtained by the method of the present invention. The yield stress is measured according to the gel bed rheology method defined herein. It is noted that a yield stress in the above range can be obtained by conventional manufacturing methods as well. However, by using the perforated plate of the present invention, a higher yield stress can be obtained without changing the formulation of the monomer mixture.
[0071] The superabsorbent obtained by the method of the present invention has a porous structure due to the evaporation of water during extrusion. The porosity improves the absorption rate of the superabsorbent. Specifically, the water-absorbing polymer obtained by the method of the present invention meets all of the following performance parameters: (a) a free swell rate (FSR) greater than 0.48 seconds and less than 0.88 seconds, as measured according to the FSR Method defined herein; (b) an uptake of 20 g / g (T20) greater than 62 seconds and less than 125 seconds, as measured according to the k(t) method defined herein; Superabsorbents that achieve FSR and T20 values within this range are considered "ultrafast."
[0072] A further feature of the superabsorbents obtained by the method of the present invention is a balanced property profile in terms of gel strength and absorption rate. Gel strength is quantified by the storage modulus G', measured according to the gel bed rheology method disclosed herein. The beneficial property balance is indicated by a product of storage modulus and free swell rate (G' x FSR) greater than 2666 Pa·s and less than 5106 Pa·s.
[0073] The superabsorbents prepared according to the method of the present invention obtain good properties in terms of speed and elasticity, without adversely affecting other performance parameters. For example, the water-absorbing polymers obtained by the method of the present invention satisfy both of the following performance parameters: (a) Centrifuge retention capacity (CRC) of 25.8 g / g to 29.9 g / g, measured in accordance with EDANA standard test WSP 241.2(5). (b) Absorbency under pressure (AUP) at 4.83 kPa (0.7 psi) of 23.0 g / g to 25.6 g / g, as measured in accordance with EDANA WSP 242.2(5).
[0074] The particle size distribution of the obtained water-absorbent polymer is preferably adjusted to the following particle size distribution. -600μm~710μm: 5% by weight -500μm~600μm: 30% by weight -300μm~500μm: 50% by weight -150μm~300μm: 15% by weight
[0075] The above percentages are target values. Reasonable deviations from the above target values are allowed, so the particle size distribution may be as follows: -600μm~710μm: More than 0% by weight and less than 10% by weight - 500μm~600μm: More than 20% by weight and less than 40% by weight - 300μm~500μm: More than 40% by weight and less than 60% by weight - 150μm~300μm: more than 5% by weight and less than 25% by weight In both cases, all percentages within the particle size distribution add up to 100% by weight. The above particle size distribution is adjusted by sieving.
[0076] The water-absorbing polymers prepared according to the invention are almost dry because they have undergone a drying process. Specifically, the moisture trapped in the polymer network immediately after polymerization has been expelled during drying. Thus, after drying, the material is no longer considered a hydrogel. In industrial processes, hydrogels are not completely dried, since drying to the point of complete removal of moisture would consume a large amount of energy. Thus, some moisture remains in the final product. To avoid a sticky final product, the moisture content needs to be limited. In a preferred embodiment, the water-absorbing polymers of the invention have a moisture content of up to 10% by weight, or up to 7% by weight, or up to 5% by weight, or up to 3% by weight. In the field of superabsorbents, the moisture content is usually measured according to EDANA standard NWSP230.0.R2(19).
[0077] It is worth mentioning that the water-absorbing polymer obtained by the method of the present invention contains two particle types, namely monolith particles and agglomerated particles. Monolith particles are composed of only one polymer particle, whereas agglomerated particles are composed of at least two polymer particles attached to each other. In this process, inorganic particles attached to the polymer are not taken into account. Thus, agglomerates can be identified by visible grain boundaries between polymer particles, whereas monolith particles are completely devoid of polymer grain boundaries. Particle agglomeration is a notorious phenomenon in superabsorbents. However, those skilled in the art of superabsorbents use a distinction between forced agglomeration to avoid smaller particles (fine particles) and undesired agglomeration that leads to oversize of particles.
[0078] The method aims to avoid agglomeration. Therefore, the aggregate portion in the water-absorbing particle of the present invention is very small. Specifically, the ratio r of the number of monolith particles to the number of aggregate particles is more than 20, or more than 32, or more than 50, or more than 80, or more than 126, or more than 200, or more than 500. The method of calculating the ratio r is as follows:
[0079] Thanks to the predominance of monolithic particles, the superabsorbent of the invention has adequate mechanical strength.
[0080] Furthermore, the process of the present invention creates conditions within the extruder where speeds can be achieved in a single push without the expense of agglomeration, thus allowing for the production of high speed superabsorbents with less capital expenditure.
[0081] A further advantage of the method of the present invention is that the extrusion conditions are adjusted so that the shear stress applied to the hydrogel during extrusion is small enough not to cause the thixotropic behavior of the subsequent superabsorbent.By following the design rules of the present invention for determining the shape of the perforated plate, the shear stress is ensured to be smaller than the critical shear stress that causes thixotropy.Therefore, the water-absorbing polymer prepared by the method of the present invention behaves like a Newtonian fluid (in the swollen state).
[0082] As a Newtonian fluid, the superabsorbent prepared by the method of the present invention shows a linear relationship between shear stress and strain as long as the shear stress is less than the yield stress.When a level of stress is applied that exceeds the yield stress, the swollen superabsorbent shows thixotropic behavior.However, since the superabsorbent of the present invention achieves a high yield stress, Newtonian behavior is expected for sanitary applications.
[0083] Thus, the water-absorbing polymers of the present invention are characterized by a linear relationship between shear stress and strain, which is valid for shear stress values lower than the yield stress. Shear stress and strain are measured according to the gel bed rheology method defined below.
[0084] Further properties of viscoelastic substances that behave like Newtonian fluids can be derived from a diagram showing the relationship between the storage modulus and the loss modulus versus strain. For non-thixotropic substances, the storage modulus and the loss modulus lines do not intersect. Specifically, the storage modulus is greater than the loss modulus. As the strain increases, both curves approach each other. If the strain exceeds the intersection of the storage modulus and the loss modulus curves, thixotropic behavior is expected. The location of the intersection can be 100% strain, or even better, 1000% strain. The lower limit of strain below which thixotropy is not observed is 1%, or even 0.1%.
[0085] Thus, the water-absorbing polymers of the present invention are also characterized in that the storage modulus (G') is greater than the loss modulus (G'') as long as the water-absorbing polymer is strained in the range of 0.1% to 1000%, or 1% to 100%. The strain is measured according to the Gel Bed Rheology Method defined below.
[0086] Explanation of the whole process The present invention will now be described in detail by way of example with reference to the following figures. FIG. 1: Flowchart of the method for producing the water-absorbing polymer of the present invention. FIG. 2: View of the perforated plate of the invention, namely front view and cross section FIG. 3: SEM image of SAP particles obtained by the method of the present invention. Figure 4: SEM image of SAP particles obtained by conventional method (prior art)
[0087] Figure 1 shows the process flow chart of the method of the present invention for preparing water-absorbing polymer. This can also be considered as a schematic diagram of the manufacturing plant for carrying out the method of the present invention.
[0088] In its minimum configuration, the plant consists of seven functional units (a) to (g), which are arranged to form a production strand. Each functional unit essentially performs one step of the process. An overview of the steps in the process and the associated functional units is given in Table 1. Table 1: Overview of steps and functional units in the method
[0089] [Table 1]
[0090] Basically, all functional units are provided structurally separate in dedicated machines. However, some functional units may combine several manufacturing steps in one multifunctional machine. This is described separately. Between all functional units, suitable conveying means are arranged for the material transport from unit to unit. Conventional conveyors known in the technology of superabsorbent manufacturing are chosen. In FIG. 1, the conveying means are represented by arrows.
[0091] First, an ethylenically unsaturated monomer 1, at least one crosslinking agent 2 and at least one initiator 3 are mixed in a receiver (a) to obtain a monomer mixture 4. The ethylenically unsaturated monomer 1 is administered in liquid form, i.e. as an aqueous monomer solution. The crosslinking agent 2 and the initiator 3 are also administered in the form of a solution. Due to the use of water as a solvent for the active ingredients, the monomer mixture contains a significant amount of water.
[0092] Preferred ethylenically unsaturated monomers are α-, β-unsaturated acids, preferably α-, β-unsaturated carboxylic or sulfonic acids, including acrylic acid, methacrylic acid, crotonic acid, isocrotonic acid, itaconic acid, fumaric acid, maleic acid and 2-acrylamido-2-methyl-1-propanesulfonic acid. Although these acids can be used in their acidic form, it is more preferred to use the α-, β-ethylenically unsaturated acids in at least partially neutralized form, as alkali metal and / or ammonium salts, including sodium and potassium salts.
[0093] Neutralization is conveniently accomplished by contacting the aqueous monomer solution with a sufficient amount of base to neutralize 10% to 95% of the acid groups present in the acid monomers. Neutralization may be performed in the receiver 1 or beforehand. Additionally, neutralization may be performed after polymerization, so-called gel neutralization. Preferably, the amount of base is sufficient to neutralize 40% to 85%, most preferably 55% to 80%, of the groups present in the monomers. Suitable compounds useful for neutralizing the acid groups of the monomers include bases that sufficiently neutralize the acid groups without adversely affecting the polymerization process. Examples of such compounds include alkali metal hydroxides, alkali metal carbonates, and alkali metal bicarbonates.
[0094] In the method of the present invention, the monomer mixture contains at least about 10% by weight, more preferably at least about 25% by weight, and even more preferably from about 45% to about 99.9% by weight of α-,β-unsaturated carboxylic and / or sulfonic acids. The above acidic groups may preferably be present, at least partially, in the form of sodium and / or potassium and / or ammonium salts.
[0095] The acidic groups are preferably neutralized to at least about 25 mol%, more preferably at least about 50 mol%, even more preferably from about 50 mol% to less than 90 mol%, more preferably from about 50 mol% to less than 80 mol%.
[0096] The monomer mixture may also include a mixture of the above-mentioned preferred monomers. In addition, the monomer mixture may include additional ethylenically unsaturated monomers in an amount of up to 60% by weight. Examples include, but are not limited to, acrylamide, methacrylamide, maleic anhydride, alkyl esters or amides of the above-mentioned monomers (e.g., methyl (meth)acrylate, (meth)acrylamide, hydroxyethyl (meth)acrylate, and hydroxypropyl (meth)acrylate, or (meth)acrylates of polyethylene glycol methyl ether, etc.). When at least one additional monomer is included, such monomer is referred to herein as "comonomer".
[0097] The monomer mixture further comprises at least one crosslinker 2 for crosslinking the polymer network, i.e., a network crosslinker. Suitable crosslinkers are those having at least two ethylenically unsaturated double bonds, those having at least one ethylenically unsaturated double bond and at least one functional group reactive towards acidic groups, and those having at least two functional groups reactive towards acidic groups, or mixtures thereof.
[0098] Suitable covalent network crosslinking agents include compounds having 2 to 4 groups selected from the group consisting of CH2=CHCO-, CH2=C(CH3)CO-, and CH2=CH-CH2- in one molecule. Examples of crosslinkers include diallylamine, triallylamine, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, diacrylates and dimethacrylates of trimethylolpropane and pentaerythritol, triacrylates and trimethacrylates of trimethylolpropane and pentaerythritol, tetraacrylates and tetramethacrylates of pentaerythritol, allyl methacrylate, tetraallyloxyethane, and acrylates of highly ethoxylated derivatives of trimethylolpropane or pentaerythritol having 3 to 30 ethylene oxide units, such as highly ethoxylated trimethylolpropane triacrylate or tetraacrylate and tetramethacrylate of pentaerythritol. Other suitable crosslinkers are monoallyl ether polyether monoacrylates, such as polyethylene glycol monoallyl ether acrylate (PEG-MAE-AE). Particularly preferred are ester-type crosslinkers such as highly ethoxylated trimethylolpropane triacrylate (HE-TMPTA) having between about 3 and about 30 EO units per molecule, allyl-type crosslinkers, and crosslinkers having both acrylate and allyl functionalities in the same molecule, such as polyethylene glycol monoallyl ether acrylate (PEG-MAE-AE).
[0099] As a bifunctional or polyfunctional agent capable of reacting with the acidic groups of the polymer backbone at elevated temperatures to form crosslinks, polyethylene glycol, preferably polyethylene glycol (PEG) that is liquid or pasty at room temperature (21°C to 25°C), such as PEG600, may be used.
[0100] These network crosslinkers are distinct from, and not to be confused with, the surface crosslinkers described below. Mixtures of the aforementioned network crosslinkers may be used as well.
[0101] Said network crosslinking agent renders the water-absorbent polymer water-insoluble, despite its water-swelling properties. The preferred amount of crosslinking agent is determined by the desired degree of absorbent capacity and the desired strength of retention of absorbed liquid, i.e., the desired absorbency under pressure (AUP) or absorbency under load (AUL), respectively. The crosslinking agent is advantageously used in an amount ranging from 0.05 to 5% by weight, based on the total weight of the ethylenically unsaturated monomers used. More preferably, the amount ranges from 0.4% to 0.5% by weight. Usually, when an amount of more than about 5% by weight is used, the crosslink density of the polymer becomes too high, resulting in a decrease in the absorbent capacity. When the crosslinking agent is used in an amount less than 0.05% by weight, the crosslink density of the polymer usually becomes too low, resulting in a sticky polymer when in contact with the liquid to be absorbed, resulting in a decrease in the initial absorption rate.
[0102] The network crosslinker may preferably be soluble in the aqueous solution of the ethylenically unsaturated monomers, but may simply be dispersed in said solution, optionally in the presence of a dispersing agent. Examples of suitable dispersing agents include carboxymethylcellulose suspending aids, methylcellulose, hydroxypropylcellulose, and polyvinyl alcohol. Such dispersing agents are advantageously provided in a concentration of 0.0005 to 0.1% by weight, based on the total weight of the ethylenically unsaturated monomers.
[0103] Preferably, the aforementioned one or more crosslinking agents may be used in combination with a fairly small amount of polyhydric alcohol. Preferably, the monomer mixture further comprises at least one polyhydric alcohol as an additional crosslinking agent in an amount of at least 50 ppm, more preferably 100-1000 ppm, based on the total weight of the ethylenically unsaturated monomers. The polyhydric alcohol preferably comprises glycerin, preferably used in an amount of 100-1000 ppm, based on the total weight of the ethylenically unsaturated monomers, more preferably only comprising said glycerin.
[0104] The monomer mixture 4 further comprises at least one polymerization initiator 3 .
[0105] Conventional vinyl addition polymerization initiators may be used for the polymerization of the water-soluble monomers and the crosslinking agent. To initiate the polymerization, free radical polymerization initiators that are sufficiently soluble in the monomer solution are preferred. For example, water-soluble persulfates such as potassium persulfate, ammonium persulfate, sodium persulfate, and even alkali metal persulfates, hydrogen peroxide, and water-soluble azo compounds such as 2,2'-azobis-(2-amidinopropane) hydrochloride may be used. The so-called redox initiator system is composed of two elements, namely an oxidizing element and a reducing element. The monomer mixture may be composed of only one element of the initiator system in the first step, and in the second step, the second element of the initiator system is added to start the polymerization. Hydrogen peroxide or sodium persulfate, which can be used as the oxidizing element of the redox initiator system, may be combined with a reducing element such as a sulfite, an amine, or ascorbic acid. The amount of initiator used may preferably range from 0.1% to about 1% by weight, preferably from about 0.1% to about 0.5% by weight, based on the total weight of the ethylenically unsaturated monomers.
[0106] In addition, the monomer mixture may contain one or more chelating agents to control the rate of initiation and polymerization, which may otherwise rise to undesirable levels due to impurities present in the monomer mixture, such as heavy metal ions, especially iron ions. The chelating agent may preferably be selected from organic polyacids, phosphoric polyacids, and their salts. Preferably, the chelating agent may be selected from nitrilotriacetic acid, ethylenediaminetetraacetic acid, cyclohexanediaminetetraacetic acid, diethylenetriaminepentaacetic acid, ethyleneglycol-bis-(aminoethylether)-N,N,N'-triacetic acid, N-(2-hydroxyethyl)-ethylenediamine-N,N,N'-triacetic acid, triethylenetetraaminehexaacetic acid, tartaric acid, citric acid, iminodisuccinic acid, gluconic acid, and their salts. A commercially available chelating agent is the pentasodium salt of diethylenetriaminepentaacetic acid.
[0107] Furthermore, the monomer mixture 4 may contain water-soluble polymers such as, for example, polyvinyl alcohol, polyvinylpyrrolidone, polyglycols, polyacrylic acids, starches, starch derivatives, and water-soluble or water-swellable cellulose ethers. When polyvinyl alcohol (PVA) is used, the latter may be partially or completely hydrolyzed. When water-soluble polymers are used, they may be preferably used in an amount of up to about 10% by weight, relative to the ethylenically unsaturated monomers. Such water-soluble polymers may also be used as graft groups for the monomers to be polymerized.
[0108] Furthermore, the monomer mixture 4 may contain recycled fines 11. Fines 11 are considered as particles produced by the present process. They are too small for the desired application defined by the product specification. Polymer particles having a particle size of less than 250 μm, preferably less than 200 μm, are defined as fines according to the present invention. Most fines 11 are generated by grinding (e) of the solid polymer material 7 after polymerization or by attrition of the dried polymer. Thus, said undesired product fraction is removed from the polymer but can be recycled by adding it to the monomer mixture 4 before polymerization.
[0109] In addition, the monomer mixture 4 may contain a precursor of a blowing agent. In particular, carbonates or bicarbonates are useful precursors. During polymerization, such substances decompose to carbon dioxide, the actual blowing agent capable of foaming the polymerization mixture. Examples of blowing agent precursors include sodium carbonate, potassium carbonate, ammonium carbonate, ammonium carbamate, magnesium carbonate, calcium carbonate, barium carbonate, lithium carbonate, sodium bicarbonate, potassium bicarbonate, ammonium bicarbonate, magnesium bicarbonate, calcium bicarbonate, barium bicarbonate, 3-oxopentanedioic acid, urea. The precursor may be added in granular form or dissolved in an aqueous solution.
[0110] Furthermore, other additives may be added to the monomer mixture, which may be selected from, but are not limited to, water-insoluble organic or inorganic powders such as alkali metal chlorates, water-insoluble metal oxides such as silica or zinc oxide, surfactants, dispersing aids, water-soluble metal salts such as silver salts, aluminum sulfate or aluminum lactate, odor control agents such as magnesium salts or calcium salts, or further processing aids such as modified non-ionic polypropylene waxes.
[0111] Once the monomer mixture 4 is produced from the above components, it is transferred to the reaction vessel of reactor (b).
[0112] It should be noted that the monomer mixture 4 may be made in the reaction vessel instead of in the receiver (a). It is also possible that the monomer mixture is made partially in the receiver (a) and partially in the reactor (b). In particular, the initiator 3 may be added to the reaction vessel. When a redox initiator system is used, one component of the initiator system is added to the receiver (a) and the second component is added to the reactor (b).
[0113] It is also possible, and even preferred, to use equipment in which both the receiver (a) and the reactor (b) are integrated in one device. Examples of such integrated devices are belt reactors or kneading reactors. These reactor types are referred to in the encyclopedia article cited at the beginning.
[0114] For the present invention, it does not matter whether the receiver (a) and the reactor (b) are structurally separate or integrated, although for ease of understanding, both functional units are shown separately in this specification.
[0115] In the reaction vessel of the reactor (b), the liquid monomer mixture is polymerized to obtain a paste-like hydrogel 5. During the course of this reaction, the monomers are bonded to polymer chains and crosslinked into a three-dimensional network by the crosslinker. Water, which was initially used as a solvent for the monomers, is trapped within the network. The polymer network with trapped water within is considered to be the hydrogel 5. Depending on the formulation of the monomer mixture, the hydrogel 5 may contain up to 70% water by weight. Alternatively, the hydrogel 5 may contain 30% to 70% water by weight, or 40% to 60% water by weight.
[0116] Optionally, the hydrogel 5 may be subjected to further physical and / or chemical treatment to obtain a daughter product of the hydrogel 5. Such treatment may be neutralization if the monomers were used in acidic form. In addition, functional additives may be added. In the case of the present invention, such treatment is not relevant.
[0117] However, the key step of the method of the invention is the subsequent extrusion. For this purpose, the hydrogel 5 (or its daughter products) is fed into an extruder (c), whose function is to break the hydrogel 5 into small fragments and to subject it to a defined stress regime in order to affect the elasticity and the absorption rate of the water-absorbing polymer 12 thereafter.
[0118] To perform this function, the extruder is provided with an extrusion vessel covered with a perforated plate having a plurality of through holes, the perforated plate being disclosed in detail below. The hydrogel is introduced into the extrusion vessel through an inlet. Inside the extrusion vessel is at least one mechanical actuator which exerts pressure on the hydrogel towards the perforated plate. The through holes are the only outlet of the extrusion vessel in the direction of pressure, so that the hydrogel is extruded from the extrusion vessel through the through holes.
[0119] In the simplest case, a single worm is used as the actuator. The worm extends axially through the extrusion vessel and reaches the perforated plate. The worm rotates so that its flight carries the hydrogel towards the perforated plate. The flight pitch can increase downstream to gradually compress the hydrogel. Optionally, the worm can be equipped with knives rotating in a plane perpendicular to the axis of the worm to break down the hydrogel. Such rotating knives can be located at various positions along the axial direction of the worm, for example, just behind the entrance of the extrusion vessel, at the end of the extrusion vessel in front of the perforated plate, or even outside the extrusion vessel behind the perforated plate. The structure of an extruder with one worm and possibly rotating knives is very similar to a meat chopper (also known as meat mincer) used in the food industry to process minced meat.
[0120] Alternatively, the extruder may be configured similarly to extruders with one or two screws, such as those used to compound plastics. Such extruders are often structurally combined with kneading-type reactors, in which case the device acting as both reactor and extruder has a single cavity that combines the functions of a reaction vessel and an extrusion vessel.
[0121] Finally, it is possible to use a device similar to an injection molding machine to extrude the hydrogel. The actuator of such a device is configured as an axially movable plunger that pushes the hydrogel towards a perforated plate. The plunger can be axially rotatable and equipped with flights. Such an actuator can be used as an axially movable worm, integrating the cinematics of the plunger with the cinematics of the worm.
[0122] The design of the actuator chosen is not relevant to the present invention, as long as it is able to apply pressure to the hydrogel towards the perforated plate. The perforated plate acts as the strongest hydraulic resistor for the hydrogel in the viscoelastic flow of the hydrogel downstream of the extrusion vessel, so that the stress on the hydrogel is essentially defined by the shape of the perforated plate. The influence of the actuator is relatively small. This is why the design of the actuator is not so important. The strong compression during extrusion affects the viscoelastic behavior of the hydrogel in such a way that the yield stress of the later superabsorbent is strengthened. In addition, part of the water contained in the polymer network of the hydrogel evaporates. As soon as the hydrogel passes through the through holes, the steam is released from the hydrogel into the atmosphere. The steam acts as a foaming agent that gives the extruded hydrogel 6 a porous structure for accelerating the speed. This effect can also be observed and heard. The hydrogel emerging from the orifice is noticeably expanded with a sizzling sound.
[0123] If desired, the extruded hydrogel 6 may undergo additional physical and / or chemical modifications to obtain its daughter products.
[0124] In the next step, the extruded hydrogel 6 (or its daughter products) is fed to a dryer (d), where the trapped water is expelled from the polymer network and a solid polymer material 7 is obtained. The drying is not complete; the residual water content of the solid polymer material 7 leaving the dryer (d) is preferably between 4% and 7% by weight. The design of the dryer is of no importance for the method of the invention; for example, a circulating belt dryer can be used. This dryer type is referred to in the encyclopedia article cited at the beginning.
[0125] The solid polymer material 7 leaving the dryer (d) is then fed to a grinder (e). In the grinder (e), the solid polymer material 7 is ground into a polymer powder 8. The particle size distribution of the polymer powder 8 can be very broad and include very fine to very coarse particles.
[0126] For use in hygiene products, the water-absorbing polymers must have a limited particle size distribution, for example in the range of 150 μm to 850 μm. To adapt the polymer powder 8 to this exemplary specification, a sieve (f) is used. In the simplest configuration, the sieve (f) comprises two sieve decks arranged vertically and extending horizontally, which define the finest and coarsest particle sizes. For example, the first sieve at the top has a mesh size that allows all particles with a particle size less than 850 μm to pass. The second sieve deck at the bottom has a mesh that allows fine particles with a particle size less than 150 μm to pass. The polymer powder 8 is fed onto the first sieve deck. From the top of the second sieve deck, a fraction 9 of the polymer powder is collected from the sieve (9) with the desired particle size distribution in the range of 150 μm to 850 μm. The coarse particles 10 that could not pass the first sieve are returned to the grinder (e). The particulates 11 that pass through the second sieve deck are recycled to the monomer mixture 4. Alternatively, the particulates 11 can be mixed into the hydrogel 5 or agglomerated in a separate process (not shown).
[0127] Fraction 9 of the polymer powder with the desired particle size distribution can basically be used as an absorbent. However, such a base material does not meet the requirements to be included in modern hygiene products as a superabsorbent. In particular, the absorbency and permeability under pressure are still insufficient. In order to achieve the desired performance profile, fraction 9 is sent to a post-treatment section (g).
[0128] In the post-treatment section (g), the polymer powder fraction 9 may be subjected to several chemical and / or physical treatments to obtain a water-absorbing polymer 12 with final properties.
[0129] Within the post-treatment section (g), at least one surface cross-linking operation is carried out. Surface cross-linking is a chemical reaction that increases the cross-link density of the polymer in the region near the surface of the granules. Due to this procedure, the particles acquire an egg-like core / shell structure. The core of the SAP particles retains a relatively low cross-link density and is therefore relatively soft. However, the shell is relatively hard due to a higher degree of cross-linking. The core / shell structure of the polymer particles improves the absorbency and permeability under pressure of the water-absorbing polymer 12.
[0130] For surface crosslinking, the polymer particles are contacted with a preferably organic chemical surface crosslinking agent. The surface crosslinking agent is preferably contacted with the polymer particles in the form of a liquid surface crosslinking cocktail comprising the surface crosslinking agent and a solvent, especially if it is not liquid under the surface crosslinking conditions. In addition to water, suitable solvents are especially water-miscible organic solvents, such as methanol, ethanol, 1-propanol, 2-propanol, 1,2-propanediol, 1,3-propanediol, 1-butanol, 2-butanol, tert-butanol, iso-butanol, or mixtures of organic solvents, or mixtures of water with one or more of these organic solvents. Water is most preferred as solvent. In the surface crosslinking cocktail, the surface crosslinking agent shall be present in an amount ranging from 5 to 75% by weight, in particular from 10 to 50% by weight, more in particular from 15 to 40% by weight, based on the total weight of the surface crosslinking cocktail.
[0131] The polymer particles are preferably brought into contact with the liquid surface cross-linking cocktail by thoroughly mixing the cocktail with the polymer particles. Suitable mixing devices for applying the surface cross-linking cocktail onto the polymer particles are Patterson-Kelly mixers, DRAIS turbulent mixers, Lödige mixers, Leberg mixers, screw mixers, plate mixers or fluidized bed mixers, as well as continuously operating vertical mixers (Schugi mixers) in which the polymer structure is mixed at high frequency by rotating blades. In addition, mixing devices equipped with heated paddles (Nara mixers) may be used.
[0132] In the surface crosslinking, the polymer particles are preferably contacted with at most 20% by weight, in particular at most 15% by weight, more particularly at most 10% by weight, very particularly at most 5% by weight of the solvent. The percentages given are based on the weight of the polymer particles.
[0133] The surface crosslinking agents used in the method according to the invention are preferably understood to be compounds having at least two functional groups capable of reacting with the functional groups of the polymer structure in a condensation reaction (=condensation crosslinking agent), an addition reaction or a ring-opening reaction. Examples of these functional groups include alcohol functional groups, amino functional groups, aldehyde functional groups, glycidic functional groups, isocyanate functional groups, carbonate functional groups or epichloro functional groups. The following compounds are preferred as surface crosslinking agents in the method according to the invention:
[0134] Polyols, such as polyethylene glycols, such as ethylene glycol, diethylene glycol, triethylene glycol and tetraethylene glycol, polypropylene glycols, such as propylene glycol, dipropylene glycol, tripropylene glycol or tetrapropylene glycol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 2,4-pentanediol, 1,6-hexanediol, 2,5-hexanediol, glycerin, polyglycerin, trimethylolpropane, polyoxypropylene, oxyethylene-oxypropylene block copolymers, sorbitan fatty acid esters, polyoxyethylenesorbitan fatty acid esters, pentaerythritol, polyvinyl alcohol and sorbitol, amino alcohols, such as ethanolamine, diethanolamine, triethanolamine or propanolamine, polyamine compounds, such as ethylenediamine, diethylenetriamine, triethylenetetraamine, tetraethylenepentamine or pentaerythritol, pentaethylenehexamine, polyglycidyl ether compounds, such as ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, glycerin diglycidyl ether, glycerin polyglycidyl ether, pentaerythritol polyglycidyl ether, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, hexanediol glycidyl ether, trimethylolpropane polyglycidyl ether, ethers, sorbitol polyglycidyl ethers, phthalic acid diglycidyl esters, adipic acid diglycidyl ethers, 1,4-phenylene bis(2-oxazoline), glycidol, polyisocyanates, preferably diisocyanates such as 2,4-toluene diisocyanate and hexamethylene diisocyanate, 2,2-bishydroxymethylbutanol-tris[3-(1-aziridinyl)propionate], 1,6-hexamethyl-enediethyleneurea and diphenylmethane-bis-4,4'-N,Polyaziridine compounds such as N'-diethylene urea, halogen epoxides such as epichloro- and epibromohydrin and α-methyl epichlorohydrin, alkylene carbonates such as 1,3-dioxolan-2-one (ethylene carbonate), 4-methyl-1,3-dioxolan-2-one (propylene carbonate), 4,5-dimethyl-1,3-dioxolan-2-one, 4,4-dimethyl-1,3-dioxolan-2-one, xolan-2-one, 4-ethyl-1,3-dioxolan-2-one, 4-hydroxymethyl-1,3-dioxolan-2-one, 1,3-dioxan-2-one, 4-methyl-1,3-dioxan-2-one, 4,6-dimethyl-1,3-dioxan-2-one, 1,3-dioxolan-2-one, poly-1,3-dioxolan-2-one, polyquaternary amines such as condensation products from dimethylamine and epichlorohydrin. Further preferred surface crosslinking agents are further polyoxazolines such as 1,2-ethylenebisoxazoline, crosslinkers having silane groups such as γ-glycidoxypropyltrimethoxysilane and γ-aminopropyltrimethoxysilane, oxazolidinones such as 2-oxazolidinone, bis- and poly-2-oxazolidine, and diglycol silicates.
[0135] Among these compounds, examples of the surface crosslinking agent include diethylene glycol, triethylene glycol, polyethylene glycol, glycerol, polyglycerol, propylene glycol, diethanolamine, triethanolamine, polyoxypropylene, oxyethylene-oxypropylene block copolymer, sorbitan fatty acid ester, polyoxyethylene sorbitan fatty acid ester, trimethylolpropane, pentaerythritol, polyvinyl alcohol, sorbitol, 1,3-dioxolan-2-one (ethylene glycol), Particularly preferred are condensation crosslinkers such as 4-methyl-1,3-dioxolan-2-one (propylene carbonate), 4,5-dimethyl-1,3-dioxolan-2-one, 4,4-dimethyl-1,3-dioxolan-2-one, 4-ethyl-1,3-dioxolan-2-one, 4-hydroxymethyl-1,3-dioxolan-2-one, 1,3-dioxan-2-one, 4-methyl-1,3-dioxan-2-one, 4,6-dimethyl-1,3-dioxan-2-one and 1,3-dioxan-2-one.
[0136] After contacting the polymer particles with the surface cross-linking agent, they are heated to a temperature in the range of 50° C. to 300° C., preferably 75° C. to 275° C., in particular 150° C. to 250° C. As a result, the outer regions of the polymer structure are preferably more highly cross-linked than the inner regions. The duration of the heat treatment is limited by the risk of destroying the desired property profile of the polymer structure by the action of heat.
[0137] Beyond surface cross-linking, the post-treatment section (g) may include further physical and / or chemical treatments to improve the final properties of the water-absorbing polymer 12. Examples of such optional operations are rewetting or the addition of special additives. Rewetting can be done with water and / or polyethylene glycol. Examples of special additives include odor control agents, permeability enhancers, anti-cucking additives, flow modifiers, surfactants, viscosity modifiers, urine stability enhancers, dust-repellent additives, and color stabilizers.
[0138] Examples of odor control agents include cyclodextrins, zeolites, inorganic or organic salts. Zinc peroxide is yet another odor control agent.
[0139] Further additives are chelating agents such as ethylenediaminetetraacetic acid (EDTA), ethyleneglycoltetraacetic acid (EGTA), diethylenetriaminepentaacetic acid (DTPA), nitrile(methylene)triphosphonic acid, ethylenediamine-tetra(methylenephosphonic acid (EDTMP), diethylene-triamine-penta(methylenephosphonic acid (DTPMP), 1,3-diaminopropane-N,N,N',N'-tetraacetic acid, Na2-ethanediglycine (HEIDA), Baypure CX100, citric acid, etc.
[0140] Further additives include weak oxidizers such as hydrogen peroxide, zinc peroxide, potassium peroxide, urea hydrogen peroxide, percarbonates, persulfates, Eureco LX, Eureco derivatives, and the like.
[0141] Further additives are pH adjusters such as organic acids, inorganic acids, odor control additives (salicylic acid and its salts, silver, zinc salts, glutamic acid, tartaric acid, benzoic acid, lactic acid, cysteine hydrochloride, zeolites, cyclodextrins), natural odor control additives (1,2,3,4,6-penta-O-{3,4-dihydroxy-5-[(3,4,5-trihydroxybenzoyl)oxy]benzoyl}-D-glucopyranose (tannic acid), gallic acid, Catappa extract (termeria catappa), walnut leaves, hawthorn tea, ginkgo biloba).
[0142] Additionally, additives that enhance the whiteness of the polymer or long term color stability against darkening, yellowing, or browning, etc., may be added during post-processing. Such additives are well known in the art and include antioxidants, sulfur and phosphorus containing compounds, chelating agents, optical brighteners, etc. Preferred additives for color stability are 2-hydroxy-2-sulfonatoacetic acid, bisulfites, phosphonates, ethylenediaminetetraacetic acid, ethylenediamine-N,N'-disuccinic acid, diethylenediaminepentaacetic acid, salts and derivatives thereof, and mixtures thereof.
[0143] Examples of permeation enhancers are salts containing a divalent or higher cation of a metal and at least one organic base as anion. The divalent or higher cation of a metal is selected from the group consisting of Mg2+, Ca2+, Ba2+, Al3+, Fe2+, Fe3+, Ga3+, Ti4+, Zr4+, Cu2+ and Zn2+, most preferably Al3+. The organic base is an at least partially deprotonated mono-, di- or tricarboxylic acid, with deprotonated monocarboxylic acids being particularly preferred. Hydroxycarboxylic acids are also preferred, with at least partially deprotonated mono-, di- or tri-hydroxycarboxylic acids being particularly preferred, with monohydroxycarboxylic acids being particularly preferred. Particularly preferred anions are the corresponding bases, in particular of the following acids: anisic acid, benzoic acid, formic acid, valeric acid, citric acid, glyoxylic acid, glycolic acid, glycerol phosphate, glutaric acid, chloroacetic acid, chloropropionic acid, cinnamic acid, succinic acid, acetic acid, tartaric acid, lactic acid, pyruvic acid, fumaric acid, propionic acid, 3-hydroxypropionic acid, malonic acid, maleic acid, butyric acid, isobutyric acid, imidinoacetic acid, malic acid, isothioic acid, methylmaleic acid, adipic acid, itaconic acid, crotonic acid, oxalic acid, salicylic acid, gluconic acid, gallic acid, sorbic acid, gluconic acid, fatty acids, in particular stearic acid and adipic acid, and p-oxybenzoic acid. Of these bases, tartrates and lactates are very preferred, and lactates are most preferred. The most preferred permeation enhancer is aluminum lactate. Aluminum sulfate is also a preferred polyvalent metal salt. The polyvalent metal salt can be aluminum sulfate, such as hydrated aluminum sulfate (e.g., aluminum sulfate having 12-14 waters of hydration). The polyvalent metal salt can be aluminum lactate. Mixtures of polyvalent metal salts can be used.
[0144] It is preferred that a further anion different from the organic base is present in the permeation enhancer. The anion is preferably an inorganic base. The inorganic base is preferably a deprotonated inorganic acid. As such acids, in particular acids capable of releasing two or more protons are considered. These include in particular acids containing sulfur, nitrogen or phosphorus, with sulfur or phosphorus acids being particularly preferred. Sulfur-containing acids, in particular sulfuric acid and therefore as their salts, sulfates have proven to be particularly satisfactory as bases. It is preferred to use a further salt containing aluminum sulfate as the permeation enhancer. Preferably, at least 50% by weight, in particular at least 75% by weight and more particularly 100% by weight of the salt is based on aluminum sulfate. The two different anions can be used in a ratio of 1:100 to 100:1, preferably in a ratio of 1:10 to 10:1, in particular in a ratio of 1:5 to 5:1.
[0145] The color stabilizing additives may be selected from alkali metal sulfites or bisulfites, ammonium sulfite, sodium metabisulfite, ammonium bisulfite, sulfinic acids, 2-hydroxy-2-sulfinatoacetic acid, 2-hydroxy-2-sulfonatoacetic acid, or sulfonic acids, and salts or derivatives of the foregoing.
[0146] Rewetting or addition of special additives may occur before and / or during and / or after surface crosslinking. At the end of post-treatment section (g), a salable water-absorbing polymer 12 is obtained.
[0147] As already mentioned above, the geometry of the perforated plate is key to the success of the invention. A simplified diagram of the perforated plate 13 is shown in Figure 2. On the left is a front view and on the right is a cross-sectional view.
[0148] The perforated plate 13 is substantially flat and circular. It is made of steel. The perforated plate 13 has a hole 14 in its center. The hole 14 is used as a bearing for a worm of an extruder (not shown). Furthermore, the perforated plate 13 has a number of through holes 15 that serve as orifices for discharging the hydrogel from an extrusion container covered by the perforated plate 13. The perforated plate 13 is surrounded by a flange collar 16. The flange collar 16 is designed to fasten the perforated plate 13 to an extruder in order to cover the extrusion container of the extruder. For this purpose, the flange collar 16 is provided with flange holes 17 arranged in a circle. The flange collar 16 is fastened to the extruder by bolts (not shown) extending through the flange holes 17.
[0149] According to the invention, the perforated plate 13 follows the following design rules: 5.5<2.10686036×(l / d) 0.774457 ×(V / A) -0.117802 <13.3
[0150] In the formula, l represents the axial length of the through hole 15. As shown in FIG. 2, the through hole 15 extends through the perforated plate 13 perpendicular to its plane, and the axial length l of the through hole 15 is the same as the thickness of the perforated plate 13.
[0151] The equivalent diameter d of the through hole is the second variable in the formula. The perforated plate 13 illustrated in Figure 2 has through holes with a circular cross section, so the equivalent diameter d of the through hole is equal to the circular diameter of the through hole. If the through holes are non-circular or of a different size, d should be calculated as described in the general disclosure section.
[0152] The variable V represents the gap area of the hole plate. It is the sum of the cross-sectional areas of all the through-holes through which the hydrogel passes. Since no hydrogel passes through the central hole 14, the cross-sectional area of the hole 14 is not considered part of the gap area. For the hole plate 13 illustrated in FIG. 2, there are five circular through-holes, each with a diameter d, so the gap area is V=5 / 4×π×d 2It is calculated as follows.
[0153] Finally, the total area A of the hole plate 13 is a design rule variable. The total area is the area of the face of the hole plate in contact with the hydrogel, including the void area. For the hole plate 13 illustrated in FIG. 2, the total area A is A=1 / 4×π×(DW), where D is the diameter of the hole plate (without flange collar 16) and W is the diameter of the central hole 14. 2 The flange collar 16 and the central hole 14 are not considered part of the total area since they do not contact the hydrogel.
[0154] In the case of the perforated plate 13 shown in FIG. 2, the conditional formula 2.10686036×(l / d) 0.774457 ×(V / A) -0.117802 is 7.94. Therefore, this perforated plate 13 satisfies the design rules of the present invention and is therefore suitable for use in the method of the present invention for producing the water-absorbing polymer of the present invention.
[0155] An image of the water-absorbing polymeric particles of the invention taken by scanning electron microscope (SEM) at 500x magnification is reproduced in Figure 3. Its structure is characterized by a particular porosity caused by the evaporation of water during the extrusion step of the manufacturing method of the invention. This porosity is the possible reason for the increased absorption rate. However, the viscoelastic behavior cannot be derived from the SEM image. To evaluate this, gel bed rheological measurements are necessary.
[0156] Figure 4 reproduces an SEM image of a conventional SAP particle prepared according to a conventional manufacturing method (prior art), which is less porous and therefore not as fast as the SAP particle of the present invention shown in Figure 3.
[0157] Test procedure definition Within this disclosure, the following procedures are used to measure product characteristics.
[0158] Centrifuge Retention Volume (CRC) Method As specified in EDANA Standard Test WSP 241.2(05), available at edana.org / publications.
[0159] Absorbance Under Pressure (AUP) Method As specified in EDANA Standard Test WSP242.2(05). The procedure is available at edana.org / publications. The pressure to be applied will be 4.83 kPa (=0.7 psi).
[0160] Free Swell Rate (FSR) Method for Measuring FSR As defined in EP 0 443 627 A1, page 12, lines 24 to 44.
[0161] K(t) method to measure uptake of 20g / g (T20) As defined in paragraphs
[0027] to
[0071] of European Patent Application Publication No. 2535697.
[0162] Gel bed rheology method to measure storage modulus G', loss modulus G'', strain ε, shear stress σ, and yield stress YS Gel bed rheology was performed using an Anton Paar rheometer equipped with a building material cell and corresponding vanes (tools).
[0163] In addition to other values, the rheometer can measure the strain ε, the storage modulus G′, the loss modulus G″, and the shear stress σ.
[0164] The prescribed particle size distribution of the SAP probe was adjusted so that 5% was greater than 600μm-710μm, 30% was greater than 500μm, 50% was greater than 300μm, and 15% was greater than 150μm. Dry SAP with the above particle size distribution was added to a building material cell (BMC) and mounted on the rheometer before swelling with saline. After adding the SAP, the BMC was tapped lightly to create a uniform and level SAP bed at the bottom. The amount of SAP added corresponded to a swelling of 90% of the CRC value of the sample using a total of 250g of 0.9% saline. The amount of SAP was calculated as follows: for CRC=29g / g, SAP amount=(250g) / (29g / g×90%)=9.58g.
[0165] The addition of saline to the SAP in BMC was added to the vane shaft using a separatory funnel at a rate of approximately 10 g / sec. This was important to minimize disturbance of the SAP bed, reduce noise in the data, and ensure an excess of saline was provided during addition (the rate of saline addition was faster than the rate of swelling of the SAP). The rheometer test profile was started when the saline was added to the vane shaft. A total of 50 minutes elapsed between the addition of the saline and the amplitude sweep interval portion where the yield stress was measured.
[0166] Two different rheometer test profiles were used between the two test runs but were very similar.
[0167] Interval 1: Time sweep, 0.1% strain, 1Hz oscillation, 270 data points every 5.6 seconds (=25 minutes) Interval 2: Time sweep, no distortion / oscillation, 270 data points every 5.6 seconds (=25 minutes) Interval 3: Amplitude sweep, logarithmic shear stress ramp from 0.1 to 10,000 Pa, 150 data points every 8.6 s (= 22 min), with conditional termination of test if strain exceeds 400%.
[0168] Maximum normal force F_N maxand the maximum storage modulus G' can be extracted directly from the time sweep and is defined as the maximum value obtained in the test. The yield stress is determined by analyzing the decrease in storage modulus with increasing stress. If the decrease in storage modulus is more than 25 Pa (absolute) and 1% (relative), both based on a consistent basis, the corresponding shear stress is considered as the yield stress (YS).
[0169] Ratio of monolith particles to agglomerates Three random samples of 10 g each were taken from the mass of water-absorbing polymer to be probed, i.e. taken from separate locations within the mass, i.e. from different locations within the mass.
[0170] From the first sample, at least 501 particles are randomly selected. The selected particles are visually inspected using an optical microscope. For each particle, the inspector determines whether the particle appears agglomerated or monolithic. Agglomerated particles n 1 and monolith particle m 1 Count and record the number of m 1 and 1 Ratio of 1 Calculate r for the second sample. 2 Calculate the r of the third sample. 3 This procedure is repeated for each to calculate
[0171] The ratio of monolith particles to aggregate particles, r, is r 1 , r 2 , r 3 It is defined as the arithmetic mean of r = (r 1 +r 2 +r 3 ) / 3
[0172] Experimental Data Preparation of water-absorbing polymer probes Water-absorbing polymer probes were prepared according to the general procedure disclosed below. To the extent that process parameters were varied, the varied parameters are represented by variables named $n, where n is a natural number between 1 and 12.
[0173] General Procedure Prepare a monomer mixture containing 1440 g of acrylic acid neutralized to 74 mol % with sodium hydroxide solution (1848.5 g, 32% sodium hydroxide solution), $1 g of deionized water, $2 g of polyethylene glycol 300 diacrylate (62.1%), $3 g of polyethylene glycol 450 monoallyl ether acrylate (68.6%), and $4 g of 10% aqueous sodium carbonate. Remove dissolved oxygen from the monomer mixture by degassing with nitrogen and cool to a starting temperature of approximately 4 °C.
[0174] After the initiation temperature is reached, the initiator solution (1.35 g sodium persulfate in 10 g deionized water, 0.315 g 35% hydrogen peroxide solution in 2 g deionized water, and 0.068 g ascorbic acid in 5 g deionized water) is added. An exothermic polymerization reaction occurs. The final temperature is approximately 105°C.
[0175] After a post-reaction time of 20 minutes, the resulting hydrogel was minced in a laboratory meat mincer (Mado® Primus, motor power: about 2.2 kW). About 5% of the resulting hydrogel was extruded from the meat mincer using a circular hole plate (plate diameter: 80 mm, hole diameter: $6 mm, hole length: $7, number of holes: $8) with many similar cylindrical holes.
[0176] The hydrogel extruded from the meat mincer was then dried at 170 °C for 20 min in a laboratory belt dryer (FAU type-2-430 / 200 / 2800 / 250, SO3045; LINN HIGH TERM GmbH WERK II).
[0177] The dried polymeric material was coarsely ground and then crushed using a cutting mill (Retsch lab catting mill SM 100) with a total width of 1.5 mm, sieved and sized to a powder with a particle size of 150 μm to 700 μm (d50: approximately 350 μm). From each sample, a defined particle size distribution was adjusted: 5% > 600 μm to 710 μm, 30% > 500 μm, 50% > 300 μm and 15% > 150 μm. The samples were then homogenized for at least 3 min on a turbulent overhead shaker.
[0178] Three portions of 50 g of each of these mixtures were coated with a solution containing $9 g of surface cross-linking agent $10, 1.5 g of deionized water, $11 g of aluminum lactate (30% aqueous solution), and 12 g of aluminum sulfate x 14 hydrate. According to this procedure, a syringe (0.45 mm needle) is used to apply the solution to the polymeric material powder in the mixer. The coated powder is then heated at a temperature of 180° C. for 30 minutes in a drying cabinet. The three surface cross-linked polymeric materials are then combined. [Brief description of the drawings]
[0179] [Figure 1] 1 shows a process flow chart of the method of the present invention for preparing a water-absorbing polymer. [Diagram 2] 1A and 1B are views of a perforated plate of the present invention, namely a front view and a cross-sectional view. [Diagram 3] 1 is a SEM image of SAP particles obtained by the method of the present invention. [Figure 4] 1 is a SEM image of SAP particles obtained by a conventional method (prior art). [Figure 5-1-A] FIG. 1 shows shear stress / strain. [Figure 5-2-A] FIG. 1 shows shear stress / strain. [Figure 5-3-A] FIG. 1 shows shear stress / strain. [Fig. 5-4-A] FIG. 1 shows shear stress / strain. [Figure 5-5-A]FIG. 1 shows shear stress / strain. [Fig. 5-6-A] FIG. 1 shows shear stress / strain. [Fig. 5-7-A] FIG. 1 shows shear stress / strain. [Fig. 5-8-A] FIG. 1 shows shear stress / strain. [Fig. 5-9-A] FIG. 1 shows shear stress / strain. [Fig. 5-10-A] FIG. 1 shows shear stress / strain. [Fig. 5-11-A] FIG. 1 shows shear stress / strain. [Fig. 5-12-A] FIG. 1 shows shear stress / strain. [Fig. 5-13-A] FIG. 1 shows shear stress / strain. [Fig. 5-14-A] FIG. 1 shows shear stress / strain. [Fig. 5-15-A] FIG. 1 shows shear stress / strain. [Figure 5-1-B] FIG. 13 is a diagram showing coefficient / distortion. [Figure 5-2-B] FIG. 13 is a diagram showing coefficient / distortion. [Fig. 5-3-B] FIG. 13 is a diagram showing coefficient / distortion. [Fig. 5-4-B] FIG. 13 is a diagram showing coefficient / distortion. [Figure 5-5-B] FIG. 13 is a diagram showing coefficient / distortion. [Fig. 5-6-B] FIG. 13 is a diagram showing coefficient / distortion. [Fig. 5-7-B] FIG. 13 is a diagram showing coefficient / distortion. [Fig. 5-8-B] FIG. 13 is a diagram showing coefficient / distortion. [Fig. 5-9-B] FIG. 13 is a diagram showing coefficient / distortion. [Fig. 5-10-B] FIG. 13 is a diagram showing coefficient / distortion. [Fig. 5-11-B] FIG. 13 is a diagram showing coefficient / distortion. [Fig. 5-12-B] FIG. 13 is a diagram showing coefficient / distortion. [Fig. 5-13-B] FIG. 13 is a diagram showing coefficient / distortion. [Fig. 5-14-B]FIG. 13 is a diagram showing coefficient / distortion. [Fig. 5-15-B] FIG. 13 is a diagram showing coefficient / distortion. EXAMPLES
[0180] This experimental example was obtained by changing parameters $1 to $12 of the general process described above according to Table 2. The changed parameters are as follows: $1 amount of deionized water [g] $2 Amount of crosslinker polyethylene glycol (PEG) [g] $3 Amount of crosslinker monoallyl ether acrylate (MAE-AE) [g] $4 Amount of foaming agent precursor sodium carbonate [g] (Without foaming agent, $4=0) $5 Amount of gel obtained from the recipe used in this example [%] (If you make two examples from one recipe, $5=50, (If you create one example from one recipe, you get $5=100) $6 Hole diameter [mm] (= equivalent diameter d) $7 Hole length [mm] (= axial length l) $8 Number of holes in perforated plate [-](=n) $9 Amount of surface cross-linking agent [g] $10 Name of substance used as surface crosslinking agent [-] $11 Amount of permeability enhancer aluminum lactate used [g] $12 Amount of permeability enhancer aluminum sulfate 14-hydrate used [g]
[0181] Characterization of the example experiment Since the general procedure includes all the essential steps of the method of the invention, only the shape of the perforated plate is decisive for characterizing the examples. If the geometric parameters of a particular example meet the requirements of the design rules of the invention, then the example is inventive. If not, the respective example is a comparative example.
[0182] Based on the variables $6, $7, and $8, which represent the equivalent diameter d, axial length l, and number of holes, the conditional formula 2.10686036 × (l / d) 0.774457 ×(V / A) -0.117802 The void area V is calculated using the formula n×π / 4×d 2 The area A is calculated using the formula π / 4×80 2 mm 2 Therefore, the void ratio V / A is n×d 2 / 6400mm -2 It is calculated as follows.
[0183] The calculated value of this conditional expression was used to evaluate the inventiveness of each experimental example. If the value of the conditional expression is greater than 5.5 and less than 13.3, the experimental example is inventive. Otherwise, the experimental example is a comparative example. The results are shown in Table 3.
[0184] Performance data evaluation The performance parameters CRC, AUP, T20, FSR, YS and G' of the water-absorbing polymer particles obtained in Experimental Examples 1 to 15 were measured according to the method defined above. The product of the storage modulus and the free swelling rate (G' x FSR) was calculated for each experimental example. The results are shown in Table 4.
[0185] In addition to YS and G', the loss modulus G'', shear stress σ and strain ε of all examples were measured with a rheometer according to the gel bed methodology. For each example, the obtained values were plotted in two different diagrams. The first diagram shows the evolution of the shear stress with respect to the strain (shear stress-strain diagram) and the second diagram shows the evolution of the storage modulus and loss modulus with respect to the strain (modulus-strain diagram).
[0186] The figures are summarized in Figure 5. The correlation between the actual figure names, figure types, and experimental examples can be derived from Table 5.
[0187] Consideration The examples have been shown to achieve a higher yield stress than the comparative examples made from the same recipe. Thus, the shape of the perforated plate does indeed have a positive effect on the elasticity of the product. It is expected that the superabsorbents obtained by the method of the invention will withstand a higher load before collapsing than superabsorbents made from the same recipe but extruded without the method of the invention.
[0188] Moreover, the T20 value of the inventive probe is lower than that of the comparative example made from the same recipe.Thus, the inventive shape of the perforated plate affects the absorption rate of the product.
[0189] Finally, the product of storage modulus G' and free swelling rate FSR of the examples is improved compared to the comparative examples made from the same recipe, indicating a better balance of product properties for the SAP made using the perforated plate of the present invention.
[0190] These findings hold for a variety of recipe monomer mixtures, and therefore the effect of the hole plate geometry appears decisive.
[0191] Furthermore, the figure shows that the prepared experimental examples behave like Newtonian fluids over a wide range of strains:
[0192] In Newtonian or non-thixotropic materials there is a linear relationship between shear stress and shear rate or strain, whereas in thixotropic materials there is a non-linear relationship.
[0193] For example, M. Dinkgreve et al. show how the stress-strain curves of thixotropic materials become highly nonlinear at low shear forces and strains. See, for example, Figure 11 in Dinkgreve et al. M. Dinkgreve et al.: On different methods of measuring yield stress, Journal of Non-Newtonian Fluid Mechanics 238 (2016), pp. 233-241, DOI 10.1016 / j.jnnfm.2016.11.001.
[0194] The materials obtained by the experimental examples do not show this behavior: they all show a linear relationship between shear stress and strain.
[0195] The horizontal lines in each graph of Figure 5-*-A represent the calculated yield stress for each sample test run. As can be seen from these graphs, the shear stress vs. strain curves do not show thixotropic behavior in the linear region (curves below the horizontal line), so the standard definition of yield stress can be applied. In each case, the shear stress becomes nonlinear only after the yield stress (horizontal line). Above the yield stress, the material no longer behaves Newtonianally. Since the examples achieve a higher YS, the inventive material is Newtonian under higher loads than the non-inventive material.
[0196] The materials prepared in the examples also do not exhibit thixotropic behavior as evidenced by the storage modulus (G') and loss modulus (G'') versus strain curves. Thixotropic materials typically have storage modulus and loss modulus curves that intersect as the viscosity of the material is changed by shear or stress. This is G'=G''. This is shown in Figures 10a and 10b of the cited paper by M. Dinkgreve et al. In these figures, all of the thixotropic materials show a loss modulus that intersects with the storage modulus. This is a result of the thixotropic behavior of the materials tested in that paper. The storage modulus and loss modulus curves of the materials prepared in the examples do not exhibit this behavior. Figure 5-*-B shows the G' and G'' curves for all 15 examples. There is a point where G' and G'' can intersect only at high strain values where the test is essentially terminated due to "breakage" of the gel. This is in contrast to the behavior in Figures 10a and 10b described in the paper.
[0197] Furthermore, repeated measurements of the samples are found to be highly reproducible and consistent. Measurements of very low strain values contain noise, but this is a typical phenomenon of vibration measurements at low strain values. Three test runs were performed for each sample and the yield stress of each test run was measured. The values were then averaged and presented in Table 4.
[0198] Thus, extrusion of a hydrogel through a perforated plate following the disclosed design rules has been demonstrated to reduce the deleterious effects of thixotropy and increase the absorption rate of superabsorbents made from the hydrogel. Table 2: Values of variables according to the current experimental example
[0199] [Table 2]
[0200] EC: Ethylene carbonate PD: 1,3-propanediol Table 3: Calculated results of properties of perforated plate
[0201] [Table 3]
[0202] Table 4: Performance data evaluation results
[0203] [Table 4]
[0204] (Comparative Example): Comparative Example, (Example): Example
[0205] Table 5: Correlation between figures and experimental examples
[0206] [Table 5]
[0207] sign a Receiver b. Reactor c. Extruder d dryer e Crusher f sieve g Post-processing section 1. Monomer 2. Crosslinking Agent 3. Initiator 4. Monomer mixture 5. Hydrogels 6. Extruded Hydrogels 7 Solid Polymer Materials 8. Polymer Powder 9 Polymer Powder Fractions 10 coarse grain 11 Fine particles 12 Water-absorbent polymer 13 Perforated Plate 14 holes 15 Through Hole 16 Flange collar 17 Flange hole d equivalent diameter of through hole l Axial length of through hole D diameter of perforated plate W Hole diameter
Claims
1. (a) - at least one ethylenically unsaturated monomer having an acid group, which is optionally at least partially neutralized, - Water, at least one cross-linking agent, at least one initiator, or at least one component of an initiator system, optionally at least one ethylenically unsaturated comonomer polymerizable with said monomer, - optionally at least one water-soluble polymer, - optionally at least one blowing agent precursor, - additional ingredients, if necessary; providing a monomer mixture comprising: (b) providing a reactor having a reaction vessel; (c) preparing an extruder having an extrusion vessel, the extrusion vessel being covered with a perforated plate, the perforated plate having a plurality of through holes, each of the through holes having an equivalent diameter d and an axial length 1, a total void area of the perforated plate formed by the through holes is V, and a total area of the perforated plate including the void area is A; (d) carrying out polymerization in a reaction vessel by inverting the components of the monomer mixture to obtain a crosslinked polymer hydrogel; (e) optionally, chemically and / or physically modifying the hydrogel to obtain daughter products of the hydrogel; (f) transferring said hydrogel or daughter product thereof to said extrusion vessel; (g) optionally chopping said hydrogel or daughter products thereof within said extrusion vessel; (h) extruding the hydrogel or daughter product thereof from the extrusion vessel through the perforated plate to force the hydrogel or daughter product thereof axially through the through holes to obtain an extruded hydrogel; (i) optionally, chemically and / or physically modifying the extruded hydrogel to obtain a daughter product of the extruded hydrogel; (k) drying the extruded hydrogel or daughter products thereof to obtain a solid polymeric material; (l) grinding the solid polymeric material to obtain a polymeric powder; (m) sieving the polymer powder to obtain at least one sized fraction of the polymer powder; (n) post-treating the sized fraction to obtain a water-absorbing polymer, the "post-treatment" step including at least one surface cross-linking step; Including, The shape of the perforated plate meets the requirements: 5.5<2.10686036×(l / d) 0.774457 × (V / A) -0.117802 <13.3 A method for preparing a water-absorbing polymer, wherein the water-absorbing polymer is selected so as to satisfy the above.
2. The monomer mixture may comprise the following: - at least partially neutralized acrylic acid: 10% to 70% by weight -Water: 30% to 80% by weight Crosslinking agent: 0.05% to 5% by weight Initiator: 0.1% to 1% by weight Comonomer: 0% by weight - Water-soluble polymer: 0% by weight - Foaming agent precursor: 0% to 1% by weight -Additional ingredients: 0% to 20% by weight Prepared according to the recipe of The percentages given add up to 100% by weight, The method of claim 1 , wherein the given percentage is based on the total weight of the monomer mixture.
3. 3. The method of claim 2, wherein the monomer mix includes a blowing agent precursor, the amount of the precursor being in the range of 1000 ppm to 1500 ppm by weight of the monomer mix, and the precursor is at least one member selected from the group consisting of sodium carbonate, potassium carbonate, ammonium carbonate, ammonium carbamate, magnesium carbonate, calcium carbonate, barium carbonate, lithium carbonate, sodium bicarbonate, potassium bicarbonate, ammonium bicarbonate, magnesium bicarbonate, calcium bicarbonate, barium bicarbonate, 3-oxopentanedioic acid, and urea.
4. 4. The method of claim 2 or claim 3, wherein the total amount of crosslinker in the monomer mixture is greater than 10 millimoles and less than 50 millimoles, based on one mole of the monomer.
5. The surface crosslinking step comprises: adding at least one surface cross-linking agent and, optionally, at least one additional ingredient to said sized fraction of said polymer powder or its daughter products to obtain a mixture; subjecting the mixture to a heat treatment to increase the crosslink density in the surface area of the polymer powder; The method according to any one of claims 1 to 4, comprising:
6. The method according to any one of claims 1 to 5, wherein the reactor and the extruder are structurally separate.
7. A water-absorbing polymer having a yield stress (YS) in the range of 180 Pa to 254 Pa measured according to the gel bed rheology method defined herein, and obtainable by the method according to at least one of claims 1 to 6.
8. below: (A) a free swell rate (FSR) greater than 0.48 seconds and less than 0.88 seconds, as measured according to the FSR Method defined herein; (B) an absorption at 20 g / g (T20) greater than 62 seconds and less than 125 seconds, as measured according to the k(t) method defined herein; The water-absorbing polymer according to claim 7, which cumulatively satisfies all of the performance parameters of
9. The water-absorbing polymer according to claim 8, having a storage modulus (G') measured according to the gel bed rheology method defined herein, and the product of the storage modulus and the free swelling rate (G' x FSR) is greater than 2666 Pa.s and less than 5106 Pa.s.
10. below: (A) Centrifuge retention capacity (CRC) of 25.8 g / g to 29.9 g / g as measured in accordance with EDANA standard test WSP241.2(5) (B) an absorbance at a pressure of 4.83 kPa (AUP) of 23.0 g / g to 25.6 g / g, as measured in accordance with EDANA WSP 242.2(5); The water-absorbing polymer according to claim 8 or claim 9, which cumulatively satisfies the performance parameters of
11. By screening, the following: - 600μm to 710μm: More than 0% by weight and less than 10% by weight, the target is 5% by weight - 500μm to 600μm: More than 20% by weight but less than 40% by weight, with a target of 30% by weight - 300μm to 500μm: More than 40% by weight but less than 60% by weight, with a target of 50% by weight - 150μm to 300μm: more than 5% by weight and less than 25% by weight, the target is 15% by weight The particle size distribution is adjusted to 11. The water-absorbing polymer according to at least one of claims 7, 8, 9 or 10, wherein the percentages given add up to 100% by weight.
12. At least one of claims 7 to 11, wherein the water content according to EDANA standard NWSP 230.
0. R2 (19) is at most 10% by weight, or at most 7% by weight, or at most 5% by weight, or at most 3% by weight.
13. The water-absorbing polymer according to at least one of claims 7 to 12, comprising monolith particles and agglomerated particles, wherein the ratio r of the number of monolith particles to the number of agglomerated particles is greater than 20, or greater than 32, or greater than 50, or greater than 80, or greater than 126, or greater than 200, or greater than 500, said ratio being measured as defined in the specification.
14. The water-absorbing polymer according to at least one of claims 7 to 13, wherein the shear stress (σ) and the shear strain (ε) are linearly related, and said linear relationship is valid when the shear stress value (σ) is lower than the yield stress (YS), and the shear stress (σ) and the shear strain (ε) are measured as defined in the specification.
15. The water-absorbing polymer according to at least one of claims 7 to 14, having a storage modulus (G') and a loss modulus (G''), both measured according to the gel bed rheology method defined in the specification, the storage modulus (G') being greater than the loss modulus (G'') as long as the water-absorbing polymer is strained in the range of 0.1% to 1000% or 1% to 100%, and the shear strain (ε) being measured as defined in the specification.
Citation Information
Patent Citations
Absorbent structure
EP0443627A2
Method for determining properties of superabsorbent polymer particles and of absorbent structures containing such particles
EP2535697A1
Method for producing water absorbent polyacrylic acid (SALT) resin powder, and water absorbent polyacrylic acid (SALT) resin powder
EP2557095A1
Polyacrylic acid (SALT), polyacrylic acid (SALT)-based water-absorbing resin, and process for producing same
EP2565211A1
Agglomerated superabsorbent polymer particles
EP2944376A1