Conductive dispersions containing ultrathin graphene
A conductive ink with graphene, binder, and stabilizer components addresses the limitations of current inks by ensuring uniformity and flexibility, enabling efficient production of durable and cost-effective printed electronics.
Patent Information
- Application Number
- JP2024526771
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-04
- Filing Date
- 2022-11-03
- Publication Date
- 2024-10-31
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Current conductive inks used in printed electronics are limited by high cost, poor adhesion to substrates, non-uniformity, and inability to tailor viscosity and surface tension for specific printing methods, making large-scale production of durable and flexible electronic devices challenging.
A conductive ink comprising graphene, a binder, a stabilizer, and a solvent, with specific compositions and properties that allow for single-layer printing, improved adhesion, and tunable viscosity, enabling uniform coating and high conductivity.
The conductive ink provides excellent stability, uniform coverage, and flexibility, allowing for the production of low-cost, durable, and highly conductive printed electronics with tunable electrochemical properties, suitable for a wide range of printing techniques.
Smart Images

Figure 2024540341000001_ABST
Abstract
Description
[Technical Field]
[0001] cross reference This application claims the benefit of U.S. Provisional Patent Application No. 63 / 275,804, filed November 4, 2021, which is incorporated herein by reference in its entirety. [Background technology]
[0002] Printing conductive patterns onto flexible substrates enables the fabrication of microscale, low-cost flexible electronics. Improvements in printing inks are needed to keep pace with the increasing demand for such devices. Printed electronics are used in devices such as touchscreens, solar cells, sensors, flexible displays, foldable displays, e-paper, sensors, radio frequency identification (RFID) tags, batteries, and supercapacitors. Summary of the Invention
[0003] The conductive ink can be a high viscosity ink that is particularly suitable for applications such as screen printing, flexographic printing, slot-die printing, knife-over-edge coating, screen printing, gravure printing, spraying, dipping, or any combination thereof. Another conductive ink can be a low viscosity ink that is particularly suitable for applications such as gravure coating, spray coating, and dip coating.
[0004] In one aspect herein, there is provided a conductive ink comprising graphene sheets that are at least about 90% monolayer, have an oxygen content of up to about 6%, or both, a binder, a stabilizer, and a solvent.
[0005] In some embodiments, the graphene comprises reduced graphene oxide or activated reduced graphene oxide. In some embodiments, the binder is a polymeric binder. In some embodiments, the polymeric binder is a thermoplastic copolymer. In some embodiments, the binder comprises polyvinylpyrrolidone, ethyl methacrylate, butyl methacrylate, or any combination thereof. In some embodiments, the stabilizer comprises polytetrahydrofuran, fluorinated triethylene glycol monomethyl ether, wax, ethyl cellulose, diethylene glycol, or any combination thereof. In some embodiments, the stabilizer comprises polytetrahydrofuran and diethylene glycol, wherein the ratio of polytetrahydrofuran to diethylene glycol is about 8:1 to about 11:1. In some embodiments, the solvent includes propylene glycol n-propyl ether, 2-ethyl-1-hexanol, diethylene glycol monobutyl ether, 2-ethyl-1-butanol, 2-methyl-1-pentanol, propylene glycol monomethyl ether acetate, hexamine, cycloheptylamine, isoamylamine, 3-methoxypropylamine, parachlorobenzotrifluoride, ethylene glycol, isopropanol, ethyl acetate, chloroform, dimethylformamide, n-methyl-2-pyrrolidone, tetrahydrofuran, and dichlorobenzene, or any combination thereof. In some embodiments, the conductive ink has a graphene weight percentage concentration of about 0.1% to about 10%. In some embodiments, the conductive ink has a binder weight percentage concentration of about 5% to about 60%. In some embodiments, the conductive ink has a stabilizer weight percentage concentration of about 1% to about 80%. In some embodiments, the conductive ink has a solvent weight percentage concentration of about 20% to about 90%. In some embodiments, the solids content of the conductive ink is from about 5% to about 80%. In some embodiments, the viscosity of the conductive ink is from about 25 cP to about 4,000 cP. In some embodiments, the shear rate of the conductive ink is from about 100 s to about 400 s. In some embodiments, the ratio of the wet thickness of the conductive ink dispersed on a substrate to the dry thickness of the conductive ink dried on the substrate is from about 2:1 to about 6:1.In some embodiments, the conductive ink has a dry resistance of about 300 ohm / sq to about 80,000 ohm / sq. In some embodiments, the conductive ink has a dry resistance of about 300 ohm / sq or less. In some embodiments, the conductive ink has a particle size of about 1 um to about 40 um. In some embodiments, the conductive ink further comprises a conductive additive. In some embodiments, the conductive additive comprises nanocarbon. In some embodiments, the nanocarbon comprises carbon nanoparticles, carbon nanodots, carbon nanotubes, graphene nanoribbons, carbon nanofibers, nanographite, carbon onions, carbon nanocones, or any combination thereof. In some embodiments, the conductive ink has a weight percentage concentration of the conductive additive of about 1% to about 40%. In some embodiments, the conductive ink further comprises graphite. In some embodiments, the conductive ink has a weight percentage concentration of graphite of about 5% to about 80%.
[0006] Another aspect herein provides a method for printing a conductive ink, the method comprising depositing up to two layers of the ink of claim 1 onto a substrate and drying the ink on the substrate. In some embodiments, the depositing step is performed by screen printing, flexography, slot-die printing, knife-over-edge coating, screen printing, gravure printing, spraying, dipping, or any combination thereof. In some embodiments, the ink is dried at a temperature of about 100°C to about 180°C. In some embodiments, the ink is dried for a period of about 10 minutes to about 60 minutes. In some embodiments, the ink is deposited on the substrate with a line width of about 150 μm to about 3,000 μm. In some embodiments, the substrate comprises mica, glass, silicon, glass, metal, plastic, woven fabric, graphite sheet, gold, or any combination thereof. In some embodiments, the average roughness of the dried ink is about 1 μm to about 2 μm. In some embodiments, the texture aspect ratio of the dried ink is about 0.25° to about 1.5°. In some embodiments, the resistance of the printed conductive ink is from about 1,000 to about 40,000 ohm / sq. In some embodiments, the method further comprises firing the ink on the substrate.
[0007] 1. A method of forming a conductive ink, comprising: mixing graphene sheets, the graphene sheets being at least about 90% monolayer, or having an oxygen content of up to about 6%, or both, with a solution comprising a binder, a stabilizer, and a solvent.
[0008] In some embodiments, the graphene comprises reduced graphene oxide or activated reduced graphene oxide. In some embodiments, the binder is a polymeric binder. The method of claim 38, wherein the polymeric binder is a thermoplastic copolymer. In some embodiments, the binder comprises polyvinylpyrrolidone, ethyl methacrylate, butyl methacrylate, or any combination thereof. In some embodiments, the stabilizer comprises polytetrahydrofuran, fluorinated triethylene glycol monomethyl ether, wax, ethyl cellulose, diethylene glycol, or any combination thereof. In some embodiments, the solvent comprises propylene glycol n-propyl ether, 2-ethyl-1-hexanol, diethylene glycol monobutyl ether, 2-ethyl-1-butanol, 2-methyl-1-pentanol, propylene glycol monomethyl ether acetate, hexamine, cycloheptylamine, isoamylamine, 3-methoxypropylamine, parachlorobenzotrifluoride, ethylene glycol, isopropanol, ethyl acetate, chloroform, dimethylformamide, n-methyl-2-pyrrolidone, tetrahydrofuran, and dichlorobenzene, or any combination thereof. In some embodiments, the solution has a graphene concentration of about 0.1% to about 10% by weight. In some embodiments, the solution has a binder concentration of about 5% to about 60% by weight. In some embodiments, the solution has a stabilizer concentration of about 1% to about 80% by weight. In some embodiments, the solution has a solvent concentration of about 20% to about 90% by weight. In some embodiments, the solids content of the solution is about 5% to about 80%. In some embodiments, the solution is mixed for a period of about 1 hour to about 4 hours. In some embodiments, the viscosity of the conductive ink is about 25 cP to about 4,000 cP. In some embodiments, the shear rate of the conductive ink is about 100 s-1 to about 400 s-1. In some embodiments, the ratio of the wet thickness of the conductive ink dispersed on the substrate to the dry thickness of the conductive ink dried on the substrate is about 2:1 to about 6:1. In some embodiments, the conductive ink has a dry resistivity of about 300 ohm / sq to about 80,000 ohm / sq. In some embodiments, the conductive ink has a particle size of about 3 um to about 40 um.In some embodiments, the solution further comprises a conductive additive. In some embodiments, the conductive additive comprises nanocarbon. In some embodiments, the nanocarbon comprises carbon nanoparticles, carbon nanodots, carbon nanotubes, graphene nanoribbons, carbon nanofibers, nanographite, carbon anions, carbon nanocones, or any combination thereof. In some embodiments, the solution has a weight percentage concentration of the conductive additive of about 1% to about 40%. In some embodiments, the solution further comprises graphene. In some embodiments, the solution has a weight percentage concentration of graphene of about 5% to about 80%. [Brief explanation of the drawings]
[0009] The novel features of the present disclosure are set forth with particularity in the appended claims. The features and advantages of the present disclosure will be better understood by reference to the following detailed description that sets forth illustrative embodiments, in which the principles of the disclosure are utilized, and the accompanying drawings.
[0010] [Figure 1] FIG. 1 is a diagram of a conductive ink according to one or more embodiments herein. [Figure 2A] 1 is a first optical microscope image of an exemplary first conductive ink according to one or more embodiments herein. [Figure 2B] 1 is a second optical microscope image of an exemplary first conductive ink according to one or more embodiments herein. [Figure 3A] FIG. 2 is a diagram of particle size distribution of an exemplary first conductive ink according to one or more embodiments herein. [Figure 3B] 1 is an image of an exemplary first conductive ink on a Hegman gauge, according to one or more embodiments herein. [Figure 4A] 1 is an X-ray diffraction graph of an exemplary first conductive ink according to one or more embodiments herein. [Figure 4B]1 is a Raman spectroscopy graph of an exemplary first conductive ink according to one or more embodiments herein. [Figure 5] 1 is a graph of shear rate versus viscosity of an exemplary first conductive ink according to one or more embodiments herein. [Figure 6A] 1 is an exemplary first graph of a thermal analysis for an exemplary first conductive ink according to one or more embodiments herein. [Figure 6B] 10 is a second exemplary graph of a thermal analysis for the first exemplary conductive ink according to one or more embodiments herein. [Figure 7] 10 is an exemplary third graph of a thermal analysis for the exemplary first conductive ink according to one or more embodiments herein. [Figure 8A] 1 is a first SEM image of an exemplary second conductive ink according to one or more embodiments herein. [Figure 8B] 1 is a second SEM image of an exemplary second conductive ink according to one or more embodiments herein. [Figure 9A] FIG. 2 is a diagram of particle size distribution of an exemplary second conductive ink according to one or more embodiments herein. [Figure 9B] 1 is an image of an exemplary second conductive ink on a Hegman gauge, according to one or more embodiments herein. [Figure 10] 1 is a Raman spectroscopy graph of an exemplary second conductive ink according to one or more embodiments herein. [Figure 11A] 10 is a graph of shear rate versus viscosity of an exemplary second conductive ink according to one or more embodiments herein. [Figure 11B] 1 is an X-ray diffraction graph of exemplary first and second conductive inks according to one or more embodiments herein. [Figure 12A] 1 is an exemplary first graph of a thermal analysis for an exemplary second conductive ink according to one or more embodiments herein. [Figure 12B] 10 is a second exemplary graph of a thermal analysis for a second exemplary conductive ink according to one or more embodiments herein. [Figure 13] 10 is an exemplary third graph of a thermal analysis for an exemplary second conductive ink according to one or more embodiments herein. [Figure 14A] 1 is a photograph of an exemplary conductive ink screen printed on a silicon wafer according to one or more embodiments herein. [Figure 14B] FIG. 1 shows photographs of exemplary conductive ink screen traces of various widths printed on a silicon wafer, as well as higher magnification photographs of the traces, according to one or more embodiments herein. [Figure 15A] FIG. 14B is an optical profilometry image of the trace of FIG. 14A according to one or more embodiments herein. [Figure 15B] 15B is a three-dimensional rendering of the optical profilometry image of FIG. 15A according to one or more embodiments herein. [Figure 16A] FIG. 15B is a graph of the height of the optical profilometry image along the first axis of the trace of FIG. 15A according to one or more embodiments herein. [Figure 16B] FIG. 15B is a graph of the height of the optical profilometry image along the second axis of the trace of FIG. 15A according to one or more embodiments herein. [Figure 17] 1 is a graph of conductivity versus width of traces formed with exemplary conductive inks, according to one or more embodiments herein. [Figure 18A] 1 is a graph of dry thickness versus sheet resistance of traces formed with exemplary conductive inks, according to one or more embodiments herein. [Figure 18B] 1 is a graph of wet versus dry thickness of traces formed with an exemplary conductive ink, according to one or more embodiments herein. [Figure 19A]10 is a graph of wavelength transmittance of an exemplary trace formed with an exemplary conductive ink, according to one or more embodiments herein. [Figure 19B] 1 is a graph of wavelength transmittance of an exemplary conductive ink according to one or more embodiments herein. [Figure 20A] 1 is a first scanning electron microscope (SEM) image of an exemplary reduced graphene oxide sheet according to one or more embodiments herein. [Figure 20B] 1 is a second SEM image of an exemplary reduced graphene oxide sheet, according to one or more embodiments herein. [Figure 21A] 1 is a first atomic force microscope (AFM) image of an exemplary reduced graphene oxide sheet, according to one or more embodiments herein. [Figure 21B] 10 is a second AFM image of an exemplary reduced graphene oxide sheet, according to one or more embodiments herein. [Figure 22A] 10 is a graph of shear rate versus viscosity of an exemplary third conductive ink according to one or more embodiments herein. [Figure 22B] 10 is a graph of torque versus speed for an exemplary third conductive ink according to one or more embodiments herein. [Figure 23A] 10 is a graph of heat flow versus time for an exemplary third conductive ink according to one or more embodiments herein. [Figure 23B] 10 is a graph of weight versus time for an exemplary third conductive ink according to one or more embodiments herein. [Figure 24A] 10 is an XRD pattern of a substrate coated with an exemplary third conductive ink according to one or more embodiments herein. [Figure 24B] 10 is a Raman spectrum of a substrate coated with an exemplary third conductive ink according to one or more embodiments herein. [Figure 25A]10 is a graph of dry film thickness versus sheet resistance for a substrate coated with an exemplary third conductive ink according to one or more embodiments herein. [Figure 25B] 10 is a graph of wet film thickness versus dry film thickness for a substrate coated with an exemplary third conductive ink according to one or more embodiments herein. [Figure 26A] 10 is a graph of particle distribution of an exemplary third conductive ink according to one or more embodiments herein. [Figure 26B] FIG. 10 illustrates trace width versus resistance for an exemplary third conductive ink coated substrate according to one or more embodiments herein. [Figure 27A] 10 is a graph of shear rate versus viscosity of an exemplary fourth conductive ink according to one or more embodiments herein. [Figure 27B] 10 is a graph of torque versus speed for an exemplary fourth conductive ink according to one or more embodiments herein. [Figure 28A] 10 is a graph of heat flow versus time for an exemplary fourth conductive ink according to one or more embodiments herein. [Figure 28B] 10 is a graph of weight versus time for an exemplary fourth conductive ink according to one or more embodiments herein. [Figure 29A] 10 is an XRD graph of an exemplary fourth conductive ink according to one or more embodiments herein. [Figure 29B] 10 is a Raman spectrum of an exemplary fourth conductive ink according to one or more embodiments herein. [Figure 30A] 10 is a graph of dry film thickness versus sheet resistance for a substrate coated with an exemplary fourth conductive ink, according to one or more embodiments herein. [Figure 30B] 10 is a graph of wet film thickness versus dry film thickness for a substrate coated with an exemplary fourth conductive ink according to one or more embodiments herein. [Figure 31]10 is a graph of particle distribution of an exemplary fourth conductive ink according to one or more embodiments herein. [Figure 32A] 10 is a graph of shear rate versus viscosity of an exemplary fifth conductive ink according to one or more embodiments herein. [Figure 32B] 10 is a graph of torque versus speed for an exemplary fifth conductive ink according to one or more embodiments herein. [Figure 33A] 10 is a graph of heat flow versus time for an exemplary fifth conductive ink according to one or more embodiments herein. [Figure 33B] 10 is a graph of weight versus time for an exemplary fifth conductive ink according to one or more embodiments herein. [Figure 34A] 10 is an XRD graph of an exemplary fifth conductive ink according to one or more embodiments herein. [Figure 34B] 10 is a Raman spectrum of an exemplary fifth conductive ink according to one or more embodiments herein. [Figure 35A] 10 is a graph of particle distribution of an exemplary fifth conductive ink according to one or more embodiments herein. [Figure 35B] FIG. 10 illustrates trace width versus resistance for an exemplary fifth conductive ink coated substrate according to one or more embodiments herein. [Figure 36A] FIG. 10 shows a first optical profilometry image of an exemplary fifth conductive ink coated substrate according to one or more embodiments herein. [Figure 36B] FIG. 36B shows a graph of the dried thickness of the exemplary fifth conductive ink along the length of the sample in FIG. 36A according to one or more embodiments herein. [Figure 36C] FIG. 36B shows a graph of the dried thickness of the exemplary fifth conductive ink along the width of the sample in FIG. 36A according to one or more embodiments herein. [Figure 37A]FIG. 10 shows a second optical profilometry image of an exemplary fifth conductive ink coated substrate according to one or more embodiments herein. [Figure 37B] FIG. 10 shows a third optical profilometry image of a fifth exemplary conductive ink coated substrate according to one or more embodiments herein. [Figure 38A] 10 is a graph of dry film thickness versus sheet resistance for a substrate coated with an exemplary fifth conductive ink according to one or more embodiments herein. [Figure 38B] 10 is a graph of wet film thickness versus dry film thickness for a substrate coated with an exemplary fifth conductive ink according to one or more embodiments herein. [Figure 39A] 10 is a low magnification SEM image of an exemplary fifth conductive ink coated substrate according to one or more embodiments herein. [Figure 39B] 10 is a high magnification SEM image of an exemplary fifth conductive ink coated substrate according to one or more embodiments herein. [Figure 40A] 10 is a graph of shear rate versus viscosity of an exemplary sixth conductive ink according to one or more embodiments herein. [Figure 40B] 10 is a graph of torque versus speed for an exemplary sixth conductive ink according to one or more embodiments herein. [Figure 41A] 10 is a graph of heat flow versus time for an exemplary sixth conductive ink according to one or more embodiments herein. [Figure 41B] 10 is a graph of weight versus time for an exemplary sixth conductive ink according to one or more embodiments herein. [Figure 42A] 10 is an XRD pattern of a substrate coated with an exemplary sixth conductive ink according to one or more embodiments herein. [Figure 42B] 10 is a Raman spectrum of a substrate coated with an exemplary sixth conductive ink according to one or more embodiments herein. [Figure 43A]10 is a graph of particle distribution of an exemplary sixth conductive ink according to one or more embodiments herein. [Figure 43B] 10 is a graph of dry film thickness versus sheet resistance for a substrate coated with an exemplary sixth conductive ink according to one or more embodiments herein. [Figure 44A] 10 is a graph of wet thickness versus dry thickness of a trace formed with an exemplary sixth conductive ink, according to one or more embodiments herein. [Figure 44B] FIG. 10 illustrates trace width versus resistance for an exemplary sixth conductive ink coated substrate. DETAILED DESCRIPTION OF THE INVENTION
[0011] Currently, available methods for producing printed electronics are limited by the limited range of conductive inks available. Current silver- and copper-based inks are often too expensive for large-scale device production. Furthermore, such inks often aggregate during printing, resulting in inhomogeneous and inconsistent components, and have viscosities and surface tensions that cannot be tailored to specific printing methods, resulting in poor adhesion to substrates and low flexibility. Therefore, economically producing durable, highly conductive printed parts using such inks is often difficult or ineffective.
[0012] Improved inks are needed to improve the performance of such printed electronics and enable their more widespread manufacturing. Provided herein are conductive inks and methods for their formulation whose electrical and mechanical properties (e.g., viscosity and surface tension) enable their use in a wide range of printing techniques. The remarkable electrical conductivity, thermal stability, chemical stability, and flexibility of graphene in the inks of the present invention enable the production of low-cost electronics with tunable electrochemical properties. Finally, while many current conductive inks require multiple layers for adequate adhesion and conductivity, the inks herein can reduce the number of layers to form electronic circuits with sufficient thickness, even in a single print.
[0013] conductive ink FIG. 1 is a diagram of a conductive ink (1000). In some embodiments, the conductive ink (1000) comprises graphene (110), a binder (120), a stabilizer (130), and a solvent (140). In some embodiments, the conductive ink (1000) consists of graphene (110), a binder (120), a stabilizer (130), and a solvent (140). In some embodiments, the conductive ink (1000) consists essentially of graphene (110), a binder (120), a stabilizer (130), and a solvent (140). In some embodiments, the conductive ink (1000) does not include a surfactant. In some embodiments, the conductive ink (1000) does not include an antifoaming agent.
[0014] The specific components of the conductive ink (1000) herein allow for unexpected improvements in its elasticity, adhesion, thermal stability, coating uniformity, chemical stability, and tunable viscosity. The ink exhibits excellent stability, uniform coating without leaving voids, and a smooth surface.
[0015] In some embodiments, the graphene (110) comprises reduced graphene oxide. In some embodiments, the graphene (110) comprises activated reduced graphene oxide. In some embodiments, at least about 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, or more of the graphene (110) sheets consist of monolayers of graphene (111). In some embodiments, a high content of monolayer graphene sheets (111) in the conductive ink (1000) improves the conductivity of the conductive ink (1000) upon drying. In some embodiments, the percentage of monolayer reduced graphene oxide is determined by atomic force microscopy (AFM). In some embodiments, the oxygen content of the graphene sheets (110) is up to about 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, or 10%, including increments therein. In some embodiments, the low oxygen content of the graphene sheets (110) in the conductive ink (1000) improves the conductivity of the conductive ink (1000) when dried.
[0016] In some embodiments, the binder (120) is a polymeric binder (120). In some embodiments, the polymeric binder (120) is a thermoplastic copolymer. In some embodiments, the binder (120) comprises polyvinylpyrrolidone, ethyl methacrylate, butyl methacrylate, or any combination thereof. The particular binders (120) herein enable unexpected improvements in elasticity, adhesion, thermal stability, chemical stability, and tunable viscosity of the conductive inks (1000) herein and electronics formed therefrom.
[0017] In some embodiments, the stabilizer (130) comprises a polymer. In some embodiments, the stabilizer (130) is solid at room temperature. In some embodiments, the stabilizer (130) comprises polytetrahydrofuran, fluorinated triethylene glycol monomethyl ether, ethyl cellulose, diethylene glycol, or any combination thereof. The specific stabilizer (130) herein provides the ink (1000) herein with uniform substrate coverage, slow drying to prevent cracking and island formation, and stabilizes the graphene (110) within the ink (1000), preventing agglomeration and providing an unexpected improvement in its ability to elastically bend without damage. In some embodiments, the stabilizer (130) comprises polytetrahydrofuran, which increases the viscosity, flexibility, and elasticity of the conductive ink (1000), stabilizes the graphene (110) within the conductive ink (1000), and slows the drying process at room temperature to prevent cracking and island formation. In some embodiments, the stabilizer (130) comprises diethylene glycol, which improves the flexibility and strength of the dried conductive ink (1000).
[0018] In some embodiments, the solvent (140) includes propylene glycol n-propyl ether, 2-ethyl-1-hexanol, diethylene glycol monobutyl ether, 2-ethyl-1-butanol, 2-methyl-1-pentanol, propylene glycol monomethyl ether acetate, hexamine, cycloheptylamine, isoamylamine, 3-methoxypropylamine, parachlorobenzotrifluoride, ethylene glycol, isopropanol, ethyl acetate, chloroform, dimethylformamide, n-methyl-2-pyrrolidone, tetrahydrofuran, and dichlorobenzene, or any combination thereof. In some embodiments, the wax is an animal wax, a plant wax, a mineral wax, a petroleum wax, or any combination thereof. In some embodiments, the solvent (140) increases the stability of the graphene (110) in the ink (1000) herein. In some embodiments, the solvent (140) is volatile. In some embodiments, the vapor pressure of the solvent (140) is about 20 Pa to about 250 Pa at 20° C. In some embodiments, the boiling point of the solvent (140) is between about 110°C and about 200°C. In some embodiments, the vapor pressure and boiling point of the solvent allow the ink (1000) herein to dry slowly, thereby preventing cracking. In some embodiments, a high boiling point solvent may increase the drying time of the conductive ink, increasing the time to coat a substrate with the conductive ink and allowing for uniform drying of the conductive ink across the surface of the ink applied to the substrate. In some embodiments, uniform drying of the ink across the surface of the ink applied to the substrate may prevent the edges from drying before the bulk of the conductive ink, prevent outward capillary flow of suspended reduced graphene oxide particles from the bulk of the conductive ink to the edges of the conductive ink when applied to the substrate, and allow for uniform coverage of the conductive ink on the substrate with uniform or nearly uniform distribution of graphene oxide particles throughout the conductive ink applied to the substrate. In some embodiments, the slow and uniform drying of the ink across the surface of the ink applied to the substrate may allow for highly uniform coverage of the conductive ink applied to the substrate, improving the conductivity of the final product produced with the conductive ink applied to the substrate.
[0019] In some embodiments, the particle size of the conductive ink is from about 3 um to about 20 um, including increments therein, such as from about 3 um to about 4 um, from about 3 um to about 6 um, from about 3 um to about 8 um, from about 3 um to about 10 um, from about 3 um to about 12 um, from about 3 um to about 14 um, from about 3 um to about 16 um, from about 3 um to about 18 um, from about 3 um to about 20 um, from about 4 um to about 6 um, from about 4 um to about 8 um, from about 4 um to about 10 um, from about 4 um to about 12 um, from about 4 um to about 14 um, from about 4 um to about 16 um, from about 4 um to about 18 um, from about 4 um to about 20 um, from about 6 um to about 8 um, from about 6 um to about 10 um, from about 6 um to about 12 um, from about 6 um to about 14 um, from about 6 um to about 16 um, and from about 6 um to about 6 um. m ~ about 18um, about 6um - about 20um, about 8um - about 10um, about 8um - about 12um, about 8um - about 14um, about 8um - about 16um, about 8um - about 18um, about 8um - about 20um, about 10um - about 12um, about 10um - about 14um, about 10um - about 16um, about 10um - about 18um, about 1 0um to about 20um, about 12um to about 14um, about 12um to about 16um, about 12um to about 18um, about 12um to about 20um, about 14um to about 16um, about 14um to about 18um, about 14um to about 20um, about 16um to about 18um, about 16um to about 20um, or about 18um to about 20um. In some embodiments, the particle size of the conductive ink is about 3 um, about 4 um, about 6 um, about 8 um, about 10 um, about 12 um, about 14 um, about 16 um, about 18 um, or about 20 um. In some embodiments, the particle size of the conductive ink is at least about 3 um, about 4 um, about 6 um, about 8 um, about 10 um, about 12 um, about 14 um, about 16 um, or about 18 um. In some embodiments, the particle size of the conductive ink is at most about 4 um, about 6 um, about 8 um, about 10 um, about 12 um, about 14 um, about 16 um, about 18 um, or about 20 um. In some embodiments, the specific particle size of the inks herein results in tunable viscosity and surface tension that allows printing by a variety of methods and machines to produce a wide variety of electronic components. In some embodiments, the particle size referred to above refers to the mean or average particle size.In some embodiments, the particle sizes stated above refer to at least 80%, at least 90%, or at least 95% of the ink having the recited particle size.
[0020] The viscosity of the conductive ink can be adjusted by adjusting the shear mixing time, with longer shear times resulting in lower viscosity. In some embodiments, the viscosity of the conductive ink is from about 25 cP to about 3,000 cP. In some embodiments, the viscosity of the conductive ink is from about 25 cP to about 50 cP, from about 25 cP to about 100 cP, from about 25 cP to about 250 cP, from about 25 cP to about 500 cP, from about 25 cP to about 750 cP, from about 25 cP to about 1,000 cP, from about 25 cP to about 2,000 cP, from about 25 cP to about 3,000 cP, from about 25 cP to about 400 cP, from about 50 cP to about 100 cP, from about 50 cP to about 25, including increments therein. 0cP, approximately 50cP to approximately 500cP, approximately 50cP to approximately 750cP, approximately 50cP to approximately 1,000cP, approximately 50cP to approximately 2,000cP, approximately 50cP to approximately 3,000cP, approximately 50cP to approximately 400cP, Approximately 100cP to approximately 250cP, approximately 100cP to approximately 500cP, approximately 100cP to approximately 750cP, approximately 100cP to approximately 1,000cP, approximately 100cP to approximately 2,000cP, approximately 100cP to approximately 3,000c P, about 100cP to about 400cP, about 250cP to about 500cP, about 250cP to about 750cP, about 250cP to about 1,000cP, about 250cP to about 2,000cP, about 250cP to about 3,00 0cP, approximately 250cP to approximately 400cP, approximately 500cP to approximately 750cP, approximately 500cP to approximately 1,000cP, approximately 500cP to approximately 2,000cP, approximately 500cP to approximately 3,000cP, approximately 500cP to approximately 400 cP, about 750 cP to about 1,000 cP, about 750 cP to about 2,000 cP, about 750 cP to about 3,000 cP, about 750 cP to about 400 cP, about 1,000 cP to about 2,000 cP, about 1,000 cP to about 3,000 cP, about 1,000 cP to about 400 cP, about 2,000 cP to about 3,000 cP, about 2,000 cP to about 400 cP, or about 3,000 cP to about 400 cP. In some embodiments, the viscosity of the conductive ink is about 25 cP, about 50 cP, about 100 cP, about 250 cP, about 500 cP, about 750 cP, about 1,000 cP, about 2,000 cP, about 3,000 cP, or about 400 cP. In some embodiments, the viscosity of the conductive ink is at least about 25 cP, about 50 cP, about 100 cP, about 250 cP, about 500 cP, about 750 cP, about 1,000 cP, about 2,000 cP, or about 3,000 cP.In some embodiments, the viscosity of the conductive ink is at most about 50 cP, about 100 cP, about 250 cP, about 500 cP, about 750 cP, about 1,000 cP, about 2,000 cP, about 3,000 cP, or about 400 cP. In some embodiments, the viscosity of the inks herein allows for printing by a variety of methods and machines to produce a wide variety of electronic components.
[0021] In some embodiments, the shear rate of the conductive ink is from about 100 s to about 400 s, inclusive of increments therein. In some embodiments, the shear rate of the conductive ink is from about 100 s to about 150 s, from about 100 s to about 200 s, from about 100 s to about 250 s, from about 100 s to about 300 s, from about 100 s to about 350 s, from about 100 s to about 400 s, from about 150 s to about 200 s, from about 150 s to about 250 s, from about 150 s to about 300 s, from about 150 s to about 3 50 s-1, about 150 s-1 to about 400 s-1, about 200 s-1 to about 250 s-1, about 200 s-1 to about 300 s-1, about 200 s-1 to about 350 s-1, about 200 s-1 to about 400 s-1, about 250 s-1 to about 300 s-1, about 250 s-1 to about 350 s-1, about 250 s-1 to about 400 s-1, about 300 s-1 to about 350 s-1, about 300 s-1 to about 400 s-1, or about 350 s-1 to about 400 s-1. In some embodiments, the shear rate of the conductive ink is about 100 s, about 150 s, about 200 s, about 250 s, about 300 s, about 350 s, or about 400 s. In some embodiments, the shear rate of the conductive ink is at least about 100 s, about 150 s, about 200 s, about 250 s, about 300 s, or about 350 s. In some embodiments, the shear rate of the conductive ink is at most about 150 s, about 200 s, about 250 s, about 300 s, about 350 s, or about 400 s. In some embodiments, the shear rates of the inks herein enable printing by a variety of methods and machines to produce a wide variety of electronic components.
[0022] In some embodiments, the conductive ink has a weight percent concentration of graphene, when wet, of about 0.1% to about 10%. In some embodiments, the conductive ink has a weight percent concentration of graphene, when wet, of about 0.1% to about 0.5%, about 0.1% to about 1%, about 0.1% to about 2%, about 0.1% to about 3%, about 0.1% to about 4%, about 0.1% to about 5%, about 0.1% to about 6%, about 0.1% to about 7%, about 0.1% to about 8%, about 0.1% to about 9%, about 0.1% to about 10%, about 0.5% to about 1%, and about 0. 5% to about 2%, about 0.5% to about 3%, about 0.5% to about 4%, about 0.5% to about 5%, about 0.5% to about 6%, about 0.5% to about 7%, about 0.5% to about 8%, about 0.5% to about 9%, about 0.5% to about 10%, about 1% to about 2%, about 1% to about 3%, about 1% to about 4%, about 1% to about 5%, about 1% to about 6%, about 1% to about 7%, about 1% to about 8%, about 1% to about 9%, about 1% to about 10 %, about 2% to about 3%, about 2% to about 4%, about 2% to about 5%, about 2% to about 6%, about 2% to about 7%, about 2% to about 8%, about 2% to about 9%, about 2% to about 10%, about 3% to about 4%, about 3% to about 5%, about 3% to about 6%, about 3% to about 7%, about 3% to about 8%, about 3% to about 9%, about 3% to about 10%, about 4% to about 5%, about 4% to about 6%, about 4% to about 7%, about 4% to about 8%, about 4% In some embodiments, the conductive ink has a weight percent concentration of graphene of about 0.1%, about 0.5%, about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, about 9%, about 10%, about 10% to ... In some embodiments, the conductive ink has a graphene weight percentage concentration of at least about 0.1%, about 0.5%, about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, or about 9% when wet. In some embodiments, the conductive ink has a graphene weight percentage concentration of at most about 0.5%, about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, about 9%, or about 10% when wet.In some embodiments, the low concentrations of graphene oxide herein, in addition to the additional components of the conductive ink, reduce the cost of the conductive ink herein while maintaining high conductivity and low resistance.
[0023] In some embodiments, the conductive ink has a binder weight percentage concentration, when wet, of about 10% to about 60%. In some embodiments, the conductive ink has a binder weight percentage concentration, when wet, of about 10% to about 15%, about 10% to about 20%, about 10% to about 25%, about 10% to about 30%, about 10% to about 35%, about 10% to about 40%, about 10% to about 45%, about 10% to about 50%, about 10% to about 55%, about 10% to about 60%, about 15% to about 20%, about 15% to about 25%, about 15% to about 30%, about 15% to about 35%, about 15% to about 40%, about 15% to about 45%, and about 15% to about 50%, including increments therein. Approximately 15% to approximately 55%, approximately 15% to approximately 60%, approximately 20% to approximately 25%, approximately 20% to approximately 30%, approximately 20% to approximately 35%, approximately 20% to approximately 40%, approximately 20% to approximately 45%, approximately 20% to approximately 50%, approximately 20% to approximately 55%, approximately 20% to approximately 60%. Approximately 25% to approximately 30%, approximately 25% to approximately 35%, approximately 25% to approximately 40%, approximately 25% to approximately 45%, approximately 25% to approximately 50%, approximately 25% to approximately 55%, approximately 25% to approximately 60%, approximately 30% to approximately 35%, approximately 30% to approximately 40%, approximately 30% to approximately 45%, approximately 30% to approximately 50%, approximately 30% to approximately 55%, approximately 30% to approximately 60%, approximately 35% to approximately 40%, approximately 35% to approximately 45% , about 35% to about 50%, about 35% to about 55%, about 35% to about 60%, about 40% to about 45%, about 40% to about 50%, about 40% to about 55%, about 40% to about 60%, about 45% to about 50%, about 45% to about 55%, about 45% to about 60%, about 50% to about 55%, about 50% to about 60%, or about 55% to about 60% by weight of binder. In some embodiments, the conductive ink, when wet, has a binder concentration of about 10%, about 15%, about 20%, about 25%, about 30%, about 35%, about 40%, about 45%, about 50%, about 55%, or about 60% by weight. In some embodiments, the conductive ink has a binder weight percentage concentration of at least about 10%, about 15%, about 20%, about 25%, about 30%, about 35%, about 40%, about 45%, about 50%, or about 55% when wet, hi some embodiments, the conductive ink has a binder weight percentage concentration of at most about 15%, about 20%, about 25%, about 30%, about 35%, about 40%, about 45%, about 50%, about 55%, or about 60% when wet.The binders herein at specific weight percentage concentrations improve the elasticity, adhesion, thermal stability, and chemical stability of the inks herein while maintaining tunable viscosity and surface tension.
[0024] In some embodiments, the conductive ink has a weight percent concentration of stabilizer, when wet, of about 1% to about 80%. In some embodiments, the conductive ink has a weight percent concentration of stabilizer, when wet, of about 1% to about 5%, about 1% to about 10%, about 1% to about 15%, about 1% to about 20%, about 1% to about 25%, about 1% to about 30%, about 1% to about 40%, about 1% to about 50%, about 1% to about 60%, about 1% to about 70%, about 1% to about 80%, about 5% to about 10%, about 5% to about 15%, about 5% to about 20%, about 5% to about 25%, about 5% to about 30%, about 5% to about 40%, about 5% to about 50%, about 5% to about 60%, about 5% to about 70%, about 5% to about 80%, about 10% to about 15%, about 10% to about 20%, about 10% to about 25%, about 10% to about 30%, about 10% to about 40%, about 10% to about 50%, about 10% to about 60%, about 10% to about 70%, about 10% to about 80%, about 15% to about 20%, about 15% to about 25%, about 15% to about 30%, about 15% ~ about 40%, about 15% to about 50%, about 15% to about 60%, about 15% to about 70%, about 15% to about 80%, about 20% to about 25%, about 20% to about 30%, about 20% to about 40%, about 20% to about 50%, about 20% to about 60%, about 20% to about 70%, about 20% to about 80%, about 25% to about 30%, about 25% to about 40%, about 25% to about 50%, about 25% to about 60%, about 25% to about 70%, about 25% to about The stabilizer may be present at a weight percent concentration of about 80%, about 30% to about 40%, about 30% to about 50%, about 30% to about 60%, about 30% to about 70%, about 30% to about 80%, about 40% to about 50%, about 40% to about 60%, about 40% to about 70%, about 40% to about 80%, about 50% to about 60%, about 50% to about 70%, about 50% to about 80%, about 60% to about 70%, about 60% to about 80%, or about 70% to about 80%. In some embodiments, the conductive ink, when wet, has a weight percent concentration of the stabilizer of about 1%, about 5%, about 10%, about 15%, about 20%, about 25%, about 30%, about 40%, about 50%, about 60%, about 70%, or about 80%. In some embodiments, the conductive ink has a weight percentage concentration of stabilizer, when wet, of at least about 1%, about 5%, about 10%, about 15%, about 20%, about 25%, about 30%, about 40%, about 50%, about 60%, or about 70%.In some embodiments, the conductive ink has a stabilizer weight percentage concentration of up to about 5%, about 10%, about 15%, about 20%, about 25%, about 30%, about 40%, about 50%, about 60%, about 70%, or about 80% when wet. The stabilizer weight percentage concentrations disclosed herein can improve the ink's ability to uniformly coat a substrate while preventing cracking and island formation, and stabilize the graphene in the ink to prevent agglomeration while maintaining tunable viscosity and surface tension. In some embodiments, the stabilizer weight percentage concentrations herein can increase the drying time of the conductive ink, increasing the time to coat a substrate with the conductive ink and enabling uniform drying of the conductive ink across the entire surface of the ink applied to the substrate. In some embodiments, uniform drying of the ink across the surface of the ink applied to the substrate may prevent the edges from drying before the bulk of the conductive ink, prevent the suspended reduced graphene oxide particles from undergoing outward capillary flow from the bulk of the conductive ink to the edges of the conductive ink when applied to the substrate, and enable a uniform coverage of the conductive ink on the substrate with uniform or near-uniform distribution of graphene oxide particles throughout the conductive ink applied to the substrate. In some embodiments, slow and uniform drying of the ink across the surface of the ink applied to the substrate may enable a highly uniform coverage of the conductive ink applied to the substrate, improving the conductivity of final products produced with the conductive ink applied to the substrate.
[0025] In some embodiments, the ratio of polytetrahydrofuran to diethylene glycol is from about 8:1 to about 11:1. In some embodiments, the ratio of polytetrahydrofuran to diethylene glycol is from about 8:1 to about 8.5:1, from about 8:1 to about 9:1, from about 8:1 to about 9.5:1, from about 8:1 to about 10:1, from about 8:1 to about 10.5:1, from about 8:1 to about 11:1, from about 8.5:1 to about 9:1, from about 8.5:1 to about 9.5:1, from about 8.5:1 to about 10:1, and about 8:1 to about 11:1, including increments therein. The ratio is 5:1 to about 10.5:1, about 8.5:1 to about 11:1, about 9:1 to about 9.5:1, about 9:1 to about 10:1, about 9:1 to about 10.5:1, about 9:1 to about 11:1, about 9.5:1 to about 10:1, about 9.5:1 to about 10.5:1, about 9.5:1 to about 11:1, about 10:1 to about 10.5:1, about 10:1 to about 11:1, or about 10.5:1 to about 11:1. In some embodiments, the ratio of polytetrahydrofuran to diethylene glycol is about 8:1, about 8.5:1, about 9:1, about 9.5:1, about 10:1, about 10.5:1, or about 11:1. In some embodiments, the ratio of polytetrahydrofuran to diethylene glycol is at least about 8:1, about 8.5:1, about 9:1, about 9.5:1, about 10:1, or about 10.5:1. In some embodiments, the ratio of polytetrahydrofuran to diethylene glycol is at most about 8.5:1, about 9:1, about 9.5:1, about 10:1, about 10.5:1, or about 11:1.
[0026] In some embodiments, the conductive ink has a weight percent concentration of solvent when wet of about 20% to about 90%. In some embodiments, the conductive ink has a weight percent concentration of solvent when wet of about 20% to about 30%, about 20% to about 40%, about 20% to about 50%, about 20% to about 60%, about 20% to about 70%, about 20% to about 80%, about 20% to about 90%, about 30% to about 40%, about 30% to about 50%, about 30% to about 60%, about 30% to about 70%, about 30% to about 80%, about 30% to about 90%, about 40%, including increments therein. The solvent may be present at a weight percent concentration of 0% to about 50%, about 40% to about 60%, about 40% to about 70%, about 40% to about 80%, about 40% to about 90%, about 50% to about 60%, about 50% to about 70%, about 50% to about 80%, about 50% to about 90%, about 60% to about 70%, about 60% to about 80%, about 60% to about 90%, about 70% to about 80%, about 70% to about 90%, or about 80% to about 90%. In some embodiments, the conductive ink has a weight percent concentration of solvent, when wet, of about 20%, about 30%, about 40%, about 50%, about 60%, about 70%, about 80%, or about 90%. In some embodiments, the conductive ink has a weight percentage concentration of solvent when wet of at least about 20%, about 30%, about 40%, about 50%, about 60%, about 70%, or about 80%. In some embodiments, the conductive ink has a weight percentage concentration of solvent when wet of at most about 30%, about 40%, about 50%, about 60%, about 70%, about 80%, or about 90%. The particular weight percentage concentrations of solvent herein unexpectedly improve the stability of graphene within the ink while maintaining tunable viscosity and surface tension.
[0027] In some embodiments, the conductive ink (1000) further comprises a conductive additive (150). In some embodiments, the conductive additive (150) comprises nanocarbon. In some embodiments, the nanocarbon comprises carbon nanoparticles, carbon nanodots, carbon nanotubes, graphene nanoribbons, carbon nanofibers, nanographite, carbon onions, carbon nanocones, or any combination thereof. In some embodiments, the conductive additive (150) herein improves the conductivity of the ink (2000) herein while maintaining its rheological properties, allowing for the formation of a wide range of electronic components by printing via various means. In some embodiments, the conductive additive (150) herein improves the conductivity of the ink and reduces the overall viscosity to meet the requirements of microgravure printing. In some embodiments, the carbon nanoparticles comprise carbon black.
[0028] In some embodiments, the conductive ink has a weight percent concentration of the conductive additive when wet of about 1% to about 40%. In some embodiments, the conductive ink has a weight percent concentration of the conductive additive when wet of about 1% to about 5%, about 1% to about 10%, about 1% to about 15%, about 1% to about 20%, about 1% to about 25%, about 1% to about 30%, about 1% to about 35%, about 1% to about 40%, about 5% to about 10%, about 5% to about 15%, about 5% to about 20%, about 5% to about 25%, about 5% to about 30%, about 5% to about 35%, about 5% to about 40%, and about 10% to about 15%, including increments therein. The conductive additive has a weight percentage concentration of about 10% to about 20%, about 10% to about 25%, about 10% to about 30%, about 10% to about 35%, about 10% to about 40%, about 15% to about 20%, about 15% to about 25%, about 15% to about 30%, about 15% to about 35%, about 15% to about 40%, about 20% to about 25%, about 20% to about 30%, about 20% to about 35%, about 20% to about 40%, about 25% to about 30%, about 25% to about 35%, about 25% to about 40%, about 30% to about 35%, about 30% to about 40%, or about 35% to about 40%. In some embodiments, the conductive ink has a weight percentage concentration of the conductive additive when wet of about 1%, about 5%, about 10%, about 15%, about 20%, about 25%, about 30%, about 35%, or about 40%. In some embodiments, the conductive ink has a weight percentage concentration of the conductive additive when wet of at least about 1%, about 5%, about 10%, about 15%, about 20%, about 25%, about 30%, or about 35%. In some embodiments, the conductive ink has a weight percentage concentration of the conductive additive when wet of at most about 5%, about 10%, about 15%, about 20%, about 25%, about 30%, about 35%, or about 40%.
[0029] Conductive ink characterization The conductive inks herein exhibit Level 5B adhesion (ideal adhesion), enabling them to be used on a wide range of substrates, including polyimide, glass, aluminum, and polyethylene terephthalate. Furthermore, while components in many current conductive inks separate and form indispersible clumps, the conductive inks herein exhibit a shelf life of over one year, and the ink components remain in solution. Furthermore, unlike many current conductive inks, the conductive inks herein can be produced and supplied in large quantities. Additionally, the conductive inks herein can be cured at any temperature, and in short cure times of 10 minutes or less at temperatures below 110°C, improving the efficiency and speed of forming printed conductive materials. Finally, the conductive inks herein are water-soluble and dry to produce a consistent, continuous coating.
[0030] In some embodiments, the solids content of the conductive ink is from about 5% to about 80%. In some embodiments, the solids content of the conductive ink is from about 5% to about 10%, from about 5% to about 20%, from about 5% to about 30%, from about 5% to about 40%, from about 5% to about 50%, from about 5% to about 60%, from about 5% to about 70%, from about 5% to about 80%, from about 10% to about 20%, from about 10% to about 30%, from about 10% to about 40%, from about 10% to about 50%, from about 10% to about 60%, from about 10% to about 70%, from about 10% to about 80%, from about 20% to about 30%, or from about 20% to about 40%, including increments therein. , about 20% to about 50%, about 20% to about 60%, about 20% to about 70%, about 20% to about 80%, about 30% to about 40%, about 30% to about 50%, about 30% to about 60%, about 30% to about 70%, about 30% to about 80%, about 40% to about 50%, about 40% to about 60%, about 40% to about 70%, about 40% to about 80%, about 50% to about 60%, about 50% to about 70%, about 50% to about 80%, about 60% to about 70%, about 60% to about 80%, or about 70% to about 80%. In some embodiments, the solids content of the conductive ink is about 5%, about 10%, about 20%, about 30%, about 40%, about 50%, about 60%, about 70%, or about 80%. In some embodiments, the solids content of the conductive ink is at least about 5%, about 10%, about 20%, about 30%, about 40%, about 50%, about 60%, or about 70%. In some embodiments, the solids content of the conductive ink is at most about 10%, about 20%, about 30%, about 40%, about 50%, about 60%, about 70%, or about 80%.
[0031] In some embodiments, the ratio of the wet thickness of the conductive ink dispersed on the substrate to the dry thickness of the conductive ink dried on the substrate is from about 2:1 to about 6:1. In some embodiments, the ratio of the wet thickness of the conductive ink dispersed on a substrate to the dry thickness of the conductive ink dried on the substrate is from about 2:1 to about 2.5:1, from about 2:1 to about 3:1, from about 2:1 to about 3.5:1, from about 2:1 to about 4:1, from about 2:1 to about 4.5:1, from about 2:1 to about 5:1, from about 2:1 to about 5.5:1, from about 2:1 to about 6:1, from about 2.5:1 to about 3:1, from about 2.5:1 to about 3.5:1, from about 2.5:1 to about 4:1, from about 2.5:1 to about 4.5:1, from about 2.5:1 to about 5:1, from about 2.5:1 to about 5.5:1, from about 2.5:1 to about 6:1, from about 3:1 to about 4:1, from about 3:1 to about 5:1, from about 3:1 to about 5:1, from about 3:1 to about 5.5:1, from about 3:1 to about ... about 3.5:1, about 3:1 to about 4:1, about 3:1 to about 4.5:1, about 3:1 to about 5:1, about 3:1 to about 5.5:1, about 3:1 to about 6:1, about 3.5:1 to about 4:1, about 3.5:1 to about 4.5:1, about 3.5:1 to about 5:1, about 3.5:1 to about 5.5:1, about 3.5:1 to about 6:1, about 4:1 to about 4.5:1, about 4:1 to about 5:1, about 4:1 to about 5.5:1, about 4:1 to about 6:1, about 4.5:1 to about 5:1, about 4.5:1 to about 5.5:1, about 4.5:1 to about 6:1, about 5:1 to about 5.5:1, about 5:1 to about 6:1, or about 5.5:1 to about 6:1. In some embodiments, the ratio of the wet thickness of the conductive ink dispersed on the substrate to the dry thickness of the conductive ink dried on the substrate is about 2:1, about 2.5:1, about 3:1, about 3.5:1, about 4:1, about 4.5:1, about 5:1, about 5.5:1, or about 6:1. In some embodiments, the ratio of the wet thickness of the conductive ink dispersed on the substrate to the dry thickness of the conductive ink dried on the substrate is at least about 2:1, about 2.5:1, about 3:1, about 3.5:1, about 4:1, about 4.5:1, about 5:1, or about 5.5:1. In some embodiments, the ratio of the wet thickness of the conductive ink dispersed on the substrate to the dry thickness of the conductive ink dried on the substrate is at most about 2.5:1, about 3:1, about 3.5:1, about 4:1, about 4.5:1, about 5:1, about 5.5:1, or about 6:1.
[0032] In some embodiments, the dry resistance of the conductive ink is from about 300 ohm / sq to about 80,000 ohm / sq, inclusive of increments therein, from about 300 ohm / sq to about 500 ohm / sq, from about 300 ohm / sq to about 750 ohm / sq, from about 300 ohm / sq to about 1,000 ohm / sq, from about 300 ohm / sq to about 2,500 ohm / sq, from about 300 ohm / sq to about 5,000 ohm / sq, from about 300 ohm / sq to about 7,500 ohm / sq, from about 300 ohm / sq to about 10,000 ohm / sq, from about 300 ohm / sq to about 25,0 ...5,000 ohm / sq, from about 300 ohm / sq to about 7,500 ohm / sq, from about 300 ohm / sq to about 10,000 ohm / sq, from about 300 ohm / sq to about 25,000 ohm / sq, from Approximately 50,000ohm / sq, approximately 300ohm / sq to approximately 80,000ohm / sq, approximately 500ohm / sq to approximately 750ohm / sq, approximately 500ohm / sq to approximately 1,000ohm / sq, approximately 500ohm / sq to approximately 2,500ohm / sq, approximately 500ohm / sq to approximately 5,000ohm / sq, approximately 500ohm / sq to approximately 7,500ohm / sq, approximately 500ohm / sq to approximately 10,000ohm / sq, approximately 500ohm / sq to approximately 25,000ohm / sq, approximately 500ohm / sq to approximately 50,000ohm / sq, approximately 500 ohm / sq to approximately 80,000ohm / sq, approximately 750ohm / sq to approximately 1,000ohm / sq, approximately 750ohm / sq to approximately 2,500ohm / sq, approximately 750ohm / sq to approximately 5,000ohm / sq, approximately 750ohm / sq to approximately 7,500ohm / sq, approximately 750ohm / sq to approximately 10,000ohm / sq, approximately 750ohm / sq to approximately 25,000ohm / sq, approximately 750ohm / sq to approximately 50,000ohm / sq, approximately 750ohm / sq to approximately 80,000ohm / sq, approximately 1,000ohm / sq to approximately 2,500 ohm / sq, approximately 1,000ohm / sq to approximately 5,000ohm / sq, approximately 1,000ohm / sq to approximately 7,500ohm / sq, approximately 1,000ohm / sq to approximately 10,000ohm / sq, approximately 1,000ohm / sq to approximately 25,000ohm / sq, approximately 1,000ohm / sq to approximately 50,000ohm / sq, approximately 1,000ohm / sq to approximately 80,000ohm / sq, approximately 2,500ohm / sq to approximately 5,000ohm / sq, approximately 2,500ohm / sq to approximately 7,500ohm / sq, approximately 2,500ohm / sq to approximately 10,000ohm / sq, about 2,500ohm / sq to about 25,000ohm / sq, about 2,500ohm / sq to about 50,000ohm / sq, about 2,500ohm / sq to about 80,000ohm / sq, about 5,000ohm / sq to about 7,500ohm / sq, about 5,000ohm / sq to about 10,000ohm / sq, about 5,000ohm / sq to about 25,000ohm / sq, about 5,000ohm / sq to about 50,000ohm / sq, about 5,000ohm / sq to about 80,000ohm / sq, about 7,500ohm / sq to about 10,000ohm / sq, about 7,500 ohm / sq to about 25,000 ohm / sq, about 7,500 ohm / sq to about 50,000 ohm / sq, about 7,500 ohm / sq to about 80,000 ohm / sq, about 10,000 ohm / sq to about 25,000 ohm / sq, about 10,000 ohm / sq to about 50,000 ohm / sq, about 10,000 ohm / sq to about 80,000 ohm / sq, about 25,000 ohm / sq to about 50,000 ohm / sq, about 25,000 ohm / sq to about 80,000 ohm / sq, or about 50,000 ohm / sq to about 80,000 ohm / sq. In some embodiments, the conductive ink has a dry resistance of about 300 ohm / sq, about 500 ohm / sq, about 750 ohm / sq, about 1,000 ohm / sq, about 2,500 ohm / sq, about 5,000 ohm / sq, about 7,500 ohm / sq, about 10,000 ohm / sq, about 25,000 ohm / sq, about 50,000 ohm / sq, or about 80,000 ohm / sq. In some embodiments, the conductive ink has a dry resistivity of at least about 300 ohm / sq, about 500 ohm / sq, about 750 ohm / sq, about 1,000 ohm / sq, about 2,500 ohm / sq, about 5,000 ohm / sq, about 7,500 ohm / sq, about 10,000 ohm / sq, about 25,000 ohm / sq, or about 50,000 ohm / sq. In some embodiments, the conductive ink has a dry resistance of at most about 500 ohm / sq, about 750 ohm / sq, about 1,000 ohm / sq, about 2,500 ohm / sq, about 5,000 ohm / sq, about 7,500 ohm / sq, about 10,000 ohm / sq, about 25,000 ohm / sq, about 50,000 ohm / sq, or about 80,000ohm / sq.
[0033] In some embodiments, the conductive ink printed on a substrate is thermally stable up to about 400°C. In some embodiments, the conductive ink is flexible when dried and applied to a substrate. In some embodiments, the flexibility of the conductive ink is measured by measuring the sheet resistance of the conductive ink when applied to a substrate after bending. In some embodiments, the sheet resistance of the conductive ink does not decrease after bending, folding, or creasing the substrate. In some embodiments, the sheet resistance of the conductive ink decreases by 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, 1%, 0.5%, 0.1% or less after bending, folding, or creasing the substrate.
[0034] In some embodiments, the conductive ink is adhesive and crack-resistant. Cracking of the conductive ink can be measured by scoring a coating on the surface of the conductive ink and applying an adhesive surface to the scored surface of the conductive ink. In some embodiments, the conductive ink is crack-resistant, and none of the conductive ink is removed from the scored surface after applying the adhesive surface to the scored surface of the conductive ink. In some embodiments, the conductive ink is crack-resistant, and less than 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, 1%, 0.5%, or 0.1% of the conductive ink is removed from the scored surface after applying the adhesive surface to the scored surface of the conductive ink.
[0035] Method for forming conductive ink 1. A method of forming a conductive ink, the method comprising: mixing a solution comprising graphene, a binder, a stabilizer, and a solvent; heating the solution to a first temperature; maintaining the solution at the first temperature for a holding time; and heating the solution to a second temperature.
[0036] In some embodiments, the graphene comprises reduced graphene oxide or activated reduced graphene oxide. In some embodiments, the binder is a polymeric binder. In some embodiments, the polymeric binder is a thermoplastic copolymer. In some embodiments, the binder comprises polyvinylpyrrolidone, ethyl methacrylate, butyl methacrylate, or any combination thereof. In some embodiments, the stabilizer comprises polytetrahydrofuran, fluorinated triethylene glycol monomethyl ether, wax, ethyl cellulose, or any combination thereof. In some embodiments, the stabilizer comprises polytetrahydrofuran and diethylene glycol. In some embodiments, the ratio of polytetrahydrofuran to diethylene glycol in the stabilizer is about 8:1 to about 11:1.
[0037] In some embodiments, the solvent comprises propylene glycol n-propyl ether, 2-ethyl-1-hexanol, diethylene glycol monobutyl ether, 2-ethyl-1-butanol, 2-methyl-1-pentanol, propylene glycol monomethyl ether acetate, hexamine, cycloheptylamine, isoamylamine, 3-methoxypropylamine, parachlorobenzotrifluoride, ethylene glycol, isopropanol, ethyl acetate, chloroform, dimethylformamide, n-methyl-2-pyrrolidone, tetrahydrofuran, and dichlorobenzene, or any combination thereof.
[0038] In some embodiments, the solution has a graphene concentration of about 0.1% to about 10% by weight. In some embodiments, the solution has a binder concentration of about 5% to about 60% by weight. In some embodiments, the solution has a stabilizer concentration of about 1% to about 80% by weight. In some embodiments, the solution has a solvent concentration of about 20% to about 90% by weight. In some embodiments, the solids content of the solution is about 5% to about 80%. In some embodiments, the solution is mixed for a period of about 1 hour to about 4 hours. In some embodiments, the first temperature is about 100°C to about 200°C. In some embodiments, the solution is heated to the first temperature at a rate of about 1°C / min to about 10°C / min. In some embodiments, the holding time is about 2 hours to about 5 hours. In some embodiments, the second temperature is about 800°C to 1,000°C. In some embodiments, the solution is heated to the second temperature at a rate of about 1°C / min to about 10°C / min. In some embodiments, the viscosity of the conductive ink is about 25 cP to about 4,000 cP. In some embodiments, the shear rate of the conductive ink is about 100 s-1 to about 400 s-1. In some embodiments, the ratio of the wet thickness of the conductive ink dispersed on the substrate to the dry thickness of the conductive ink dried on the substrate is about 21 to about 61. In some embodiments, the dry resistivity of the conductive ink is about 300 ohm / sq to about 80,000 ohm / sq. In some embodiments, the particle size of the conductive ink is about 3 um to about 40 um.
[0039] In some embodiments, the solution further comprises a conductive additive. In some embodiments, the conductive additive comprises nanocarbon. In some embodiments, the nanocarbon comprises carbon nanoparticles, carbon nanodots, carbon nanotubes, graphene nanoribbons, carbon nanofibers, nanographite, carbon onions, carbon nanocones, or any combination thereof. In some embodiments, the solution has a weight percentage concentration of the conductive additive of about 1% to about 40%. In some embodiments, the solution further comprises graphene. In some embodiments, the solution has a weight percentage concentration of graphene of about 5% to about 80%.
[0040] Conductive ink printing method Provided herein are methods of printing the conductive inks herein. In some embodiments, the methods include depositing up to two layers of the conductive inks herein onto a substrate and drying the ink on the substrate. In some embodiments, the methods further include baking the ink on the substrate. In some embodiments, the methods include depositing up to 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 layers of the conductive inks herein onto a substrate.
[0041] In some embodiments, the depositing step is performed by screen printing, flexography, slot die printing, knife-over-edge coating, roll-to-roll coating, screen printing, gravure printing, spraying, dipping, or any combination thereof. The viscosity and surface tension of the inks herein allow for deposition by a variety of such methods to produce a wide range of electronic components. Furthermore, the composition and rheological properties of the inks herein allow for the formation of durable, thermally stable, and chemically stable electronic components using any one or more of the methods described herein.
[0042] In some embodiments, the conductive ink is printed onto the substrate by a Meyer rod, a metal rod covered with wire that is used to apply a controlled and consistent thickness of ink to a surface. Hereinafter, the size of the Meyer rod determines the wet thickness.
[0043] [Table 1]
[0044] In some embodiments, the conductive inks herein are printed onto a substrate having a wet thickness, where the wet thickness is the maximum, minimum, or average thickness of the ink applied to the substrate. In some embodiments, the substrate comprises mica, glass, silicon, glass, metal, plastic, woven fabric, graphite sheet, gold, or any combination thereof. In some embodiments, the plastic comprises PET, HDPE, LDPE, PTFE, Kapton, or any combination thereof. In some embodiments, the metal comprises copper, aluminum, steel, platinum, or any combination thereof. In some embodiments, the printed conductive ink has a resistance of about 300 ohm / sq to about 80,000 ohm / sq. In some embodiments, the ink is deposited on the substrate with a line width of about 150 um to about 3,000 um.
[0045] In some embodiments, the ink is dried at a temperature of about 100° C. to about 180° C. In some embodiments, the ink is dried at a temperature of about 100° C. to about 110° C., about 100° C. to about 120° C., about 100° C. to about 130° C., about 100° C. to about 140° C., about 100° C. to about 150° C., about 100° C. to about 160° C., about 100° C. to about 170° C., about 100° C. to about 180° C., about 110° C. to about 120° C., about 110° C. to about 130° C., about 110° C. to about 140° C., about 110° C. to about 150° C., about 110° C. to about 160° C., about 110° C. to about 170° C., about 110° C. to about 180° C., about 120° C. to about 130° C., about 120° C. to about 140° C., about 120° C. The drying temperature is about 150°C, about 120°C to about 160°C, about 120°C to about 170°C, about 120°C to about 180°C, about 130°C to about 140°C, about 130°C to about 150°C, about 130°C to about 160°C, about 130°C to about 170°C, about 130°C to about 180°C, about 140°C to about 150°C, about 140°C to about 160°C, about 140°C to about 170°C, about 140°C to about 180°C, about 150°C to about 160°C, about 150°C to about 170°C, about 150°C to about 180°C, about 160°C to about 170°C, about 160°C to about 180°C, or about 170°C to about 180°C. In some embodiments, the ink is dried at a temperature of about 100° C., about 110° C., about 120° C., about 130° C., about 140° C., about 150° C., about 160° C., about 170° C., or about 180° C. In some embodiments, the ink is dried at a temperature of at least about 100° C., about 110° C., about 120° C., about 130° C., about 140° C., about 150° C., about 160° C., or about 170° C. In some embodiments, the ink is dried at a temperature of at most about 110° C., about 120° C., about 130° C., about 140° C., about 150° C., about 160° C., about 170° C., or about 180° C.
[0046] In some embodiments, the ink is dried over a period of about 10 minutes to about 60 minutes, including increments therein, such as about 10 minutes to about 15 minutes, about 10 minutes to about 20 minutes, about 10 minutes to about 25 minutes, about 10 minutes to about 30 minutes, about 10 minutes to about 35 minutes, about 10 minutes to about 40 minutes, about 10 minutes to about 45 minutes, about 10 minutes to about 50 minutes, about 10 minutes to about 55 minutes, about 10 minutes to about 60 minutes, about 15 minutes to about 2 ...35 minutes, about 10 minutes to about 40 minutes, about 10 minutes to about 45 minutes, about 10 minutes to about 50 minutes, about 10 minutes to about 55 minutes, about 10 minutes to about 60 minutes, about 15 minutes to about 20 minutes, about 15 minutes to about 25 5 minutes to about 30 minutes, about 15 minutes to about 35 minutes, about 15 minutes to about 40 minutes, about 15 minutes to about 45 minutes, about 15 minutes to about 50 minutes, about 15 minutes to about 55 minutes, about 15 minutes to about 60 minutes, about 20 minutes to about 25 minutes, about 20 minutes to about 30 minutes, about 20 minutes to about 35 minutes, about 20 minutes to about 40 minutes, about 20 minutes to about 45 minutes, about 20 minutes to about 50 minutes, about 20 minutes to about 55 minutes, about 20 minutes to about 60 minutes, Approximately 25 minutes to approximately 30 minutes, approximately 25 minutes to approximately 35 minutes, approximately 25 minutes to approximately 40 minutes, approximately 25 minutes to approximately 45 minutes, approximately 25 minutes to approximately 50 minutes, approximately 25 minutes to approximately 55 minutes, approximately 25 minutes to approximately 60 minutes, approximately 30 minutes to approximately 35 minutes, approximately 30 minutes to approximately 40 minutes, approximately 30 minutes to approximately 45 minutes, approximately 30 minutes to approximately 50 minutes, approximately 30 minutes to approximately 55 minutes, approximately 30 minutes to approximately 60 minutes, approximately 35 minutes to approximately 40 minutes, approximately 35 minutes to approximately 4 The ink is dried for a period of about 5 minutes, about 35 minutes to about 50 minutes, about 35 minutes to about 55 minutes, about 35 minutes to about 60 minutes, about 40 minutes to about 45 minutes, about 40 minutes to about 50 minutes, about 40 minutes to about 55 minutes, about 40 minutes to about 60 minutes, about 45 minutes to about 50 minutes, about 45 minutes to about 55 minutes, about 45 minutes to about 60 minutes, about 50 minutes to about 55 minutes, about 50 minutes to about 60 minutes, or about 55 minutes to about 60 minutes. In some embodiments, the ink is dried for a period of about 10 minutes, about 15 minutes, about 20 minutes, about 25 minutes, about 30 minutes, about 35 minutes, about 40 minutes, about 45 minutes, about 50 minutes, about 55 minutes, or about 60 minutes. In some embodiments, the ink is dried for a minimum of about 10 minutes, about 15 minutes, about 20 minutes, about 25 minutes, about 30 minutes, about 35 minutes, about 40 minutes, about 45 minutes, about 50 minutes, or about 55 minutes, hi some embodiments, the ink is dried for a maximum of about 15 minutes, about 20 minutes, about 25 minutes, about 30 minutes, about 35 minutes, about 40 minutes, about 45 minutes, about 50 minutes, about 55 minutes, or about 60 minutes.
[0047] In some embodiments, the conductive inks described herein are printed using only a single pass to produce a monolayer of reduced graphene oxide on the surface of a conductive-ink-coated substrate. In some embodiments, the single-pass printing produces a conductive-ink-coated substrate, and the conductive surface resulting from the single-pass printing process is characterized by at least about 90% graphene sheets consisting of a single layer, a graphene weight percentage concentration of about 0.25% to about 5%, an oxygen content of the graphene sheets of up to about 6%, and a dry resistivity of about 1,000 ohm / sq to about 5,000 ohm / sq. In some embodiments, single-pass printing produces a substrate coated with a conductive ink, and the conductive surface resulting from the single-pass printing process is characterized by a single layer of graphene sheets, a graphene weight percentage concentration of about 0.25% to about 5%, an oxygen content of the graphene sheets of up to about 6%, and a dry resistivity of about 1,000 ohm / sq to about 5,000 ohm / sq.
[0048] In some embodiments, the substrate onto which the conductive ink is printed includes silicon wafer, glass, Kapton tape, polyamide, PET, mica, silicon wafer, ITO glass, polyethylene sheet, Teflon, acrylic, polymer, plastic, graphite sheet, gold coated Kapton, aluminum, copper, metal, current collector, metallic current collector, non-metallic current collector, paper, although the present disclosure is not limited to these materials and may include any other suitable material.
[0049] Reduced graphene oxide The reduced graphene oxide (rGO) used to form the conductive inks herein can be easily dispersed and processed from a wide range of solvents, enabling conductive inks with tunable electronic and mechanical properties for a wide range of applications.
[0050] Figure 20A is a first scanning electron microscope (SEM) image of an exemplary rGO sheet. Figure 20B is a second SEM image of an exemplary rGO sheet. Figure 21A is a first atomic force microscope (AFM) image of an exemplary rGO sheet. Figure 21B is a second AFM image of an exemplary rGO sheet.
[0051] In some embodiments, the rGO sheets exhibit a dendritic shape with a large perimeter. In some embodiments, the rGO exhibits a shape comprising nanoplates, nanosheets, nanoparticles, nanoflakes, nanoplatelets, or any combination thereof.
[0052] In some embodiments, the rGO is monolayer rGO. In some embodiments, the rGO sheets are flakes with a wrinkled monolayer. In some embodiments, the large wrinkles and ridges in the basal plane of the graphene nanosheets prevent the graphene sheets from collapsing and re-stacking due to van der Waals interactions.
[0053] In some embodiments, the rGO comprises 2, 3, 4, 5, 6, 7, 8, 9, 10, or more layers. In some embodiments, the rGO comprises multiple layers that form interlayer pores between them. In some embodiments, the interlayer pores form a continuous network. In some embodiments, one or more of the interlayer pores are closed. In some embodiments, one or more of the interlayer pores are defined by 2, 3, 4, 5, 6, 7, 8, 9, 10, or more layers. In some embodiments, the layers are interconnected. In some embodiments, one or more of the layers are corrugated. In some embodiments, one or more of the layers have wrinkles. In some embodiments, one or more of the layers have folds. In some embodiments, the multiple layers form a bellows-like structure. In some embodiments, the multiple layers form a foam-like structure. In some embodiments, the multiple layers in the rGO are generally parallel. In some embodiments, the layers are not stacked. The large size of the interlayer spaces demonstrated herein allows for the creation of high surface areas and ion diffusion rates within the dried ink.
[0054] In some embodiments, the rGO sheets have a size ranging from about 1 μm to about 5 μm. In some embodiments, the rGO sheets have a size ranging from about 0.1 μm to about 1 μm, with a median of about 0.5 μm. In some embodiments, the rGO sheets have a size minimum of about 0.1 μm, 0.25 μm, 0.5 μm, 0.75 μm, 1 μm, 1.25 μm, 1.5 μm, 2 μm, 2.5 μm, or about 3 μm, including increments therein. In some embodiments, the rGO sheets have a size maximum of about 0.25 μm, 0.5 μm, 0.75 μm, 1 μm, 1.25 μm, 1.5 μm, 2 μm, 2.5 μm, about 3 μm, or 3.5 μm, including increments therein. In some embodiments, the size of the rGO sheets is measured as an average or median particle size. In some embodiments, the size of the rGO sheets is measured as a length, width, or diagonal. In some embodiments, the size (e.g., length, width, or diagonal) is measured as an average. For example, multiple measurements may be taken and averaged to determine the average size.
[0055] In some embodiments, the rGO sheet has a maximum, minimum, or average thickness of from about 0.5 nm to about 20 nm. In some embodiments, the rGO sheet has a maximum, minimum, or average thickness of from about 0.5 nm to about 0.75 nm, from about 0.5 nm to about 1 nm, from about 0.5 nm to about 1.25 nm, from about 0.5 nm to about 1.5 nm, from about 0.5 nm to about 1.75 nm, from about 0.5 nm to about 2 nm, from about 0.5 nm to about 3 nm, from about 0.5 nm to about 4 nm, from about 0.5 nm to about 5 nm, from about 0.5 nm to about 10 nm, from about 0.5 nm to about 20 nm, from about 0.75 nm to about 1 nm, from about 0.75 nm to about 1.25 nm, from about 0.75 nm to about 1.5 nm, from about 0.75 nm to about 1.75 nm, from about 0.75 nm to about 2 nm, from about 0.75 nm to about 3 nm, from about 0.75 nm to about 4 nm, from about 0.75 nm to about 5 nm, from about 0.75 nm to about 10 nm, from about 0.75 nm to about 20 nm, from about 1 nm to about 1.25 nm, from about 1 nm to about 1.5 nm, from about 1 nm to about 1.75 nm, from about 1 nm to about 2 nm, from about 1 nm to about 3 nm, from about 1 nm to about 4 nm, from about 1 nm to about 5 nm, from about 1 nm to about 10 nm, from about 1 nm to about 20 nm, from about 1.25 nm to about 1.5 nm, from about 1.25 nm to about 1.75 nm, from about 1.25 nm to about 2 nm, from about 1.25 nm to about 3 nm, from about 1.25 nm to about 4 nm, from about 1.25 nm to about 5 nm, from about 1.25 nm to about 10 nm, from about 1.25 nm to about 20 nm, from about 1.5 nm to about 1.75 nm, from about 1.5 nm to about 2 nm, from about 1.5 nm to about 3 nm, from about 1.5 nm to about 4 nm, from about 1.5 nm to about 5 nm, from about 1.5 nm to about 10 nm, from about 1.5 nm to about 20 nm, from about 1.75 nm to about 2 nm, from about 1.75 nm to about 3 nm, from about 1.75 nm to about 4 nm, from about 1.75 nm to about 5 nm, from about 1.75 nm to about 10 nm, from about 1.75 nm to about 20 nm, from about 2 nm to about 3 nm, from about 2 nm to about 4 nm, from about 2 nm to about 5 nm, from about 2 nm to about 10 nm, from about 2 nm to about 20 nm, from about 3 nm to about 4 nm, from about 3 nm to about 5 nm, from about 3 nm to about 10 nm, from about 3 nm to about 20 nm, from about 4 nm to about 5 nm, from about 4 nm to about 10 nm, from about 4 nm to about 20 nm, from about 5 nm to about 10 nm, from about 5 nm to about 20 nm, or from about 10 nm to about 20 nm.In some embodiments, the rGO sheets have a maximum, minimum, or average thickness of about 0.5 nm, about 0.75 nm, about 1 nm, about 1.25 nm, about 1.5 nm, about 1.75 nm, about 2 nm, about 3 nm, about 4 nm, about 5 nm, about 10 nm, or about 20 nm. In some embodiments, the rGO sheets have a maximum, minimum, or average thickness of about 0.75 nm, about 1 nm, about 1.25 nm, about 1.5 nm, about 1.75 nm, about 2 nm, about 3 nm, about 4 nm, about 5 nm, about 10 nm, or about 20 nm.
[0056] In some embodiments, the low height of the rGO sheets significantly increases their surface area and minimizes restacking. In some embodiments, the oxygen-containing functionality of the rGO sheets herein enables the formation of inks using polar solvents.
[0057] Method for forming reduced graphene oxide In some embodiments, the graphene comprises reduced graphene oxide (rGO) or activated reduced graphene oxide (ArGO). In some embodiments, the rGO, ArGO, or both are thermally reduced. In some embodiments, the rGO, ArGO, or both are not chemically reduced. In some embodiments, the thermal reduction reduces the oxygen content of the rGO, ArGO, or both.
[0058] In some embodiments, graphene oxide is activated to form activated graphene oxide (AGO) by a method comprising: (a) heating a first solution containing an etchant and a graphene oxide solution; (b) cooling the first solution; (c) filtering and washing the first solution; and (d) spray-drying the first solution. Activation of graphene oxide can be used to create in-plane defects within individual graphene oxide sheets. The number and / or size of these defects in the sheets can be controlled throughout this activation process, for example, by adjusting the reaction temperature and / or weight percentage concentration of the etchant. Alternative mechanisms to spray drying, such as air drying, heating, freeze-drying, and vacuum drying, can be used to dry the first solution to obtain graphene oxide sheets.
[0059] In some embodiments, the first solution has a graphene oxide weight percentage concentration of about 1 mg / ml to about 20 mg / ml. In some embodiments, the first solution has a graphene oxide weight percentage concentration of at least about 1 mg / ml, 2 mg / ml, 3 mg / ml, 4 mg / ml, 6 mg / ml, 8 mg / ml, 10 mg / ml, 12 mg / ml, 14 mg / ml, 16 mg / ml, 18 mg / ml, or more, including increments therein. In some embodiments, the first solution has a graphene oxide weight percentage concentration of at most 2 mg / ml, 3 mg / ml, 4 mg / ml, 6 mg / ml, 8 mg / ml, 10 mg / ml, 12 mg / ml, 14 mg / ml, 16 mg / ml, 18 mg / ml, 20 mg / ml, or more, including increments therein. In some embodiments, the first solution has a weight percentage concentration of the etchant of about 60% to about 98% by volume. In some embodiments, the first solution has a weight percentage concentration of the etchant of at least about 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, or more by volume, including increments therein. In some embodiments, the first solution has a weight percentage concentration of the etchant of at most about 65%, 70%, 75%, 80%, 85%, 90%, 95%, 98%, or more by volume, including increments therein. In some embodiments, the weight percentage concentration of the etchant in the first solution by volume determines the size and / or density of defects in the graphene sheets. In some embodiments, the weight percentage concentrations of the graphene oxide, the etchant, or both affect the oxygen content of the AGO.
[0060] In some embodiments, the first solution is heated to a temperature of about 60°C to about 120°C. In some embodiments, the first solution is heated to a temperature of at least about 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, or higher, including increments therein. In some embodiments, the first solution is heated to a temperature of at most about 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, or higher, including increments therein. In some embodiments, the first solution is cooled after the heating step. In some embodiments, the first solution is cooled to a temperature of about 70°C to about 90°C. In some embodiments, the first solution is cooled to a temperature of at least about 70°C, 75°C, 80°C, 85°C, or higher, including increments therein. In some embodiments, the first solution is cooled to a temperature of up to about 75° C., 80° C., 85° C., 90° C., or higher, including increments therein. In some embodiments, the temperature of heating and / or cooling affects the water content, and therefore the oxygen content, of the AGO.
[0061] In some embodiments, the first solution is filtered using a filter with a mesh size of about 0.5 μm to about 3 μm. In some embodiments, the first solution is filtered using a filter with a mesh size of at least about 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, or more, including increments therein. In some embodiments, the first solution is filtered using a filter with a mesh size of at most about 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, or more, including increments therein. In some embodiments, the filter comprises two or more filtration layers. In some embodiments, the filter comprises at least 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 filter layers. In some embodiments, at least one mesh filter layer is metal. In some embodiments, the filter comprises a vacuum filter. In some embodiments, the vacuum filter comprises at least one spray bar assembly positioned to dispense at least one of the first solution and the cleaning solution onto the filter. In some embodiments, the vacuum filter comprises a vacuum source configured to apply negative pressure to the filter to improve filtration. In some embodiments, the vacuum filter comprises a pH sensor for measuring the pH of the first solution. In some embodiments, the filtered and washed first solution has a pH of about 1 to about 5. In some embodiments, the filtered and washed first solution has a pH of at least about 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, or more, including increments therein. In some embodiments, the filtered and washed first solution has a pH of at most about 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, or more, including increments therein. In some embodiments, the pH of the first solution, the filtration method, or both, determine the size and / or density of defects in the graphene sheets.
[0062] In some embodiments, spray drying is performed by passing the first solution through a spray drying nozzle. In some embodiments, the spray drying nozzle is an ultrasonic nozzle, and the first solution passes through the nozzle at a velocity faster than the speed of sound in the first solution. In some embodiments, the spray drying nozzle is a subsonic nozzle, and the first solution passes through the nozzle at a velocity less than the speed of sound in the first solution. In some embodiments, the spray drying nozzle is a plain-orifice nozzle that atomizes the first solution. In some embodiments, the spray drying nozzle has a pressure swirl spray to reduce the particle size of the first solution. In some embodiments, the spray drying nozzle is a single-effect nozzle. In some embodiments, the spray drying nozzle is a multiple-effect nozzle. In some embodiments, the spray drying nozzle comprises an atomizer.
[0063] In some embodiments, spray drying is carried out at a flow rate of about 1 ml / hr to about 6,000 ml / hr. In some embodiments, spray drying is carried out at a flow rate of at least about 1 ml / hr, 5 ml / hr, 10 ml / hr, 50 ml / hr, 100 ml / hr, 500 ml / hr, 1,000 ml / hr, 2,000 ml / hr, 4,000 ml / hr, or more, including increments therein. In some embodiments, spray drying is carried out at a flow rate of at most about 5 ml / hr, 10 ml / hr, 50 ml / hr, 100 ml / hr, 500 ml / hr, 1,000 ml / hr, 2,000 ml / hr, 4,000 ml / hr, 6,000 ml / hr, or more, including increments therein. In some embodiments, spray drying is carried out at a pressure of about 10 psi to about 50 psi. In some embodiments, spray drying is carried out at a pressure of at least about 10 psi, 15 psi, 20 psi, 25 psi, 30 psi, 35 psi, 40 psi, 45 psi, or more, including increments therein. In some embodiments, spray drying is carried out at a pressure of at most about 15 psi, 20 psi, 25 psi, 30 psi, 35 psi, 40 psi, 45 psi, 50 psi, or more, including increments therein. In some embodiments, spray drying is carried out at an inlet temperature of about 120° C. to about 200° C. In some embodiments, spray drying is carried out at an inlet temperature of at least about 120° C., 130° C., 140° C., 150° C., 160° C., 170° C., 180° C., 190° C., or more, including increments therein. In some embodiments, spray drying is carried out at an inlet temperature of up to about 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, or more, including increments therein. In some embodiments, the spray drying outlet temperature is from about 30°C to about 80°C. In some embodiments, the spray drying outlet temperature is at least about 30°C, 40°C, 50°C, 60°C, 70°C, or more, including increments therein. In some embodiments, the spray drying outlet temperature is up to about 40°C, 50°C, 60°C, 70°C, 80°C, or more, including increments therein.
[0064] In some embodiments, heating the first solution comprises stirring the first solution. In some embodiments, the baking is performed in air, nitrogen, argon, or any combination thereof. In some embodiments, the first solution is cooled by adding ice to the first solution. In some embodiments, the etching solution comprises hydrogen peroxide, bromine, iodine, potassium permanganate, potassium chlorate, potassium dichromate, manganese oxide, iron(III) chloride, sodium peroxide, potassium persulfate, hypochlorous acid, or any combination thereof.
[0065] While graphene can be difficult to disperse in solvent media, the oxygen-containing functional groups of the AGO herein allow for dispersion in polar solvents. In some embodiments, the AGO herein is dispersed in organic or aqueous solvents (e.g., n-methyl-2-pyrrolidone (NMP), dimethylformamide (DMF), tetrahydrofuran (THF), chloroform, and dichlorobenzene) by adding a surfactant and applying mechanical force, for example, by shear mixing, ultrasonic agitation, ball milling, or any combination thereof.
[0066] In some embodiments, graphene oxide can be reduced to yield rGO. In some embodiments, activated graphene oxide can be reduced to yield ArGO. For example, activated graphene oxide resulting from an activation process can be subjected to a chemical reduction process to yield ArGO.
[0067] In some embodiments, the chemical reduction to form rGO includes heating a second solution containing AGO, a strong base, and a reducing agent to a second solution, and optionally filtering and washing the reducing agent and second solution. In some embodiments, the strong base includes sodium hydroxide, ammonium hydroxide, potassium hydroxide, urea, melamine, sodium carbonate, or any combination thereof. In some embodiments, the reducing agent includes ascorbic acid, hydrazine, sodium borohydride, pyrogallol, lithium aluminum hydride, ammonia borane, thiourea dioxide, hydroiodic acid, hydrogen bromide, ethanethiol-aluminum chloride, Lawesson's reagent, sodium bisulfite, sodium dithionite, aluminum, iron, zinc, magnesium, or any combination thereof.
[0068] In some embodiments, reducing the AGO comprises calcining the spray-dried first solution. In some embodiments, the calcination is carried out by a flame torch, a heating strip, a heating coil, or any combination thereof. In some embodiments, the calcination is carried out in air, nitrogen, argon, or any combination thereof. In some embodiments, the calcination is carried out at a temperature less than about 30,000°C, 2,500°C, or 2,000°C, including increments therein. In some embodiments, reducing the AGO does not comprise calcining the spray-dried first solution. In some embodiments, the calcination is carried out at a temperature between about 100°C and about 1,500°C. In some embodiments, the calcination is carried out at a temperature of at least about 100°C, 110°C, 150°C, 250°C, 500°C, 750°C, 1,000°C, or 1,250°C, including increments therein. In some embodiments, calcination is performed at temperatures up to 250°C, 500°C, 750°C, 1,000°C, 1,250°C, or 1,500°C, including increments therein. In some embodiments, calcination is performed for a period of about 1 minute to about 1,500 minutes. In some embodiments, the calcination temperature, method, time, or any combination thereof, affects the ignition, explosion, and expansion of AGO, and therefore its morphology. In some embodiments, reducing AGO involves initial thermal expansion followed by calcination. The calcination process can improve AGO properties, such as surface area and electrical conductivity. In some embodiments, calcining activated graphene oxide removes oxygen functional groups therein. In some embodiments, calcining activated graphene oxide removes about 25% to about 75% of the oxygen functional groups therein. In some embodiments, removing oxygen functional groups from activated graphene oxide increases its electrical conductivity. In some embodiments, removing oxygen functional groups from activated graphene oxide increases its electrical conductivity by about 75% to about 125%. In some embodiments, calcining the activated graphene oxide increases its surface area. In some embodiments, calcining the activated graphene oxide increases its surface area by about 75% to about 125%. In one example, calcining the activated graphene oxide increases its surface area by about 350 m 2 / g to 700m 2 / g, the oxygen content decreases from about 30% to about 16%, and the conductivity increases from about 50 S / m to about 100 S / m.
[0069] In some embodiments, drying occurs over a period of about 3 minutes to about 60 minutes. In some embodiments, drying occurs over a period of at least about 3 minutes, 5 minutes, 10 minutes, 20 minutes, 30 minutes, 40 minutes, 50 minutes, or more, including increments therein. In some embodiments, drying occurs over a period of at most about 5 minutes, 10 minutes, 20 minutes, 30 minutes, 40 minutes, 50 minutes, 60 minutes, or more, including increments therein. In some embodiments, the second solution is heated to a temperature of about 60°C to about 120°C. In some embodiments, the second solution is heated to a temperature of at least about 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, or higher, including increments therein. In some embodiments, the second solution is heated to a temperature of at most about 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, or higher, including increments therein. In some embodiments, the filtering and washing of the second solution is performed within about 0.5 hours to 10 hours after adding the reducing agent to the second solution, and in some embodiments, the filtering and washing of the second solution is performed when the pH of the second solution is about 8 to about 11.
[0070] In some embodiments, reducing the AGO comprises a thermal reduction method as described above to produce a first ARGO and microwave irradiation of the first ARGO to produce a second ARGO. In some embodiments, the second ARGO has reduced oxygen content compared to the first ARGO. In some embodiments, microwave irradiation is carried out for a period of about 10 seconds to about 60 seconds. In some embodiments, microwave irradiation is carried out at a power of about 500 W to about 2,000 W. In some embodiments, microwave irradiation is carried out at a power of at least about 500 W, 750 W, 1,000 W, 1,250 W, 1,500 W, 1,750 W, or more, including increments therein. In some embodiments, the duration, wattage, or both of microwave irradiation affect the ignition, explosion, and expansion of the AGO, and therefore its morphology.
[0071] Characterization of printed conductive ink 14A and 14B show photographs of exemplary conductive ink screens printed on silicon wafers using a Meyer rod. In some embodiments, as shown, ink traces with thicknesses of 150 μm, 300 μm, 500 μm, 1,000 μm, 2,000 μm, and 3,000 μm can be printed in a single pass without gaps or separation. As shown, the ink traces are approximately 4 cm long. While current conductive inks have poor dispersibility, resulting in clumps that clog printers and dry inconsistently, the conductive inks herein enable consistent printing of conductive traces and other shapes, even at small scales.
[0072] FIG. 15A is an optical profilometry image of the trace of FIG. 14B. FIG. 15B is a three-dimensional rendering of the optical profilometry image of FIG. 15A. As shown, the trace printed with the exemplary conductive ink has straight, clean edges that exhibit a very uniform cross-sectional profile. FIGS. 16A and 16B are height graphs of the optical profilometry images along a first axis of the trace of FIG. 15A and a second axis of the trace of FIG. 15B, respectively. From the data in FIGS. 15A-16B, the following roughness measurements can be calculated:
[0073] [Table 2]
[0074] Figure 16A shows exemplary measurements of roughness average (Sa) (1601), maximum height (Sp) (1602), maximum valley depth (Sv) (1603), and maximum peak height (Sz) (1604). For a conductive ink printed on a substrate with a thickness T(x) over a set length (1), the roughness variables are:
[0075]
number
[0076] In some embodiments, the printed exemplary conductive ink has a kurtosis of about 3.5 to about 5. Kurtosis is a measure of the sharpness of a roughness profile, with a kurtosis of 3 representing a roughness profile equivalent to a normal distribution curve, with larger kurtosis values correlating with greater sharpness. In some embodiments, deposition is by coated screen printing and the roughness of the dried ink is about 0.02 to about 0.15. In some embodiments, deposition is by coated screen printing and the kurtosis of the dried ink is about 2 to about 8. In some embodiments, deposition is by coated screen printing and the texture aspect ratio of the dried ink is about 0.25° to about 1.5°.
[0077] The texture aspect ratio is a measure of the isotropy or uniformity of a dominant surface pattern or ray. The texture aspect ratio also describes the directionality of an otherwise uniform texture. A surface with a highly patterned texture has a texture aspect ratio of 0, while a highly isotropic surface has a texture aspect ratio of 1.
[0078] The autocorrelation length (Sal) corresponds to the wavelength of the dominant surface pattern or ray. For example, a surface with a high autocorrelation length (Sal) has dominant surface patterns or rays with low frequencies and long wavelengths, and a surface with a low autocorrelation length (Sal) has dominant surface patterns or rays with high frequencies and short wavelengths.
[0079] Figure 17 is a graph of conductivity versus width for traces formed with an exemplary conductive ink. As shown, traces with widths between 300 um and 3,000 um exhibit high conductivities of approximately 2,000 S, and trace widths of at least 150 μm can be successfully printed.
[0080] Figure 18A is a graph of dry thickness versus sheet resistance for traces formed with an exemplary conductive ink, and Figure 18B is a graph of wet thickness versus dry thickness for traces formed with an exemplary conductive ink.
[0081] FIG. 19A is a graph of the wavelength transmittance of an exemplary trace formed with an exemplary conductive ink. FIG. 19B is a graph of the wavelength transmittance of an exemplary conductive ink. As can be seen, the transmittance through the liquid ink and the printed trace is near zero, with maximum transmittances of 0.0092% and 0.0177% for the liquid ink and the printed trace, respectively. In some embodiments, the conductive inks herein have a maximum transmittance of about 0.004% to about 0.015%. In some embodiments, the conductive inks herein have a maximum transmittance of at least about 0.004%. In some embodiments, the conductive inks herein have a maximum transmittance of about 0.01% to about 0.03% as printed and when dry. In some embodiments, the conductive inks herein have a maximum transmittance of at least about 0.01% as printed and when dry.
[0082] Terms and Definitions Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure belongs.
[0083] As used herein, the term "single-layer graphene" refers to graphene or reduced graphene oxide consisting of a single sheet of graphene that is not aggregated into multilayer graphene. The single sheets of graphene are separated from one another such that the two-dimensionally structured sheets are not stacked into a multilayer or graphitic structure but may still exhibit partial physical contact (e.g., interconnected sheets forming a three-dimensional network). For example, single-layer graphene can be formed by high-efficiency exfoliation from graphite by the methods disclosed herein.
[0084] As used herein, the singular forms "a," "an," and "the" include the plural forms unless the context clearly dictates otherwise. All references herein to "or" are intended to include "and / or" unless otherwise specified.
[0085] As used herein, the term "about" refers to an amount that is approximately the stated amount, as the case may be.
[0086] As used herein, the term "about" can refer to an amount to the nearest 10%, 5%, or 1% of the stated amount, including increments therein. Unless specifically stated otherwise, the term "about" refers to an amount where the stated percentage is greater than or less than 10%.
[0087] As used herein, the term "about" in reference to a percentage can refer to an amount that is 10%, 5%, or 1% higher or lower than the stated percentage, including increments therein. Unless specifically stated otherwise, the term "about" in reference to a percentage refers to an amount that is 10% higher or lower than the stated percentage.
[0088] As used herein, the phrases "at least one," "one or more," and "and / or" are open-ended expressions that are both conjunctive and disjunctive in operation. For example, the phrases "at least one of A, B, and C," "at least one of A, B, or C," "one or more of A, B, and C," "one or more of A, B, or C," and "A, B, and / or C" each mean A alone, B alone, C alone, A and B, A and C, B and C, or A, B, and C.
[0089] As used herein, the term "solids content" refers to the percentage of the dispersion or ink that remains after drying, when the volatile solvent has evaporated. [Example]
[0090] The following illustrative examples represent embodiments of the compositions and methods described herein and are not intended to be limiting in any way. Six exemplary inks are provided herein below.
[0091] [Table 3]
[0092] Example 1 - First Conductive Ink 2A and 2B show optical microscope images of an exemplary first conductive ink. As shown, the first conductive ink is highly stable and uniformly coats the substrate, forming a smooth surface without holes or shrinkage. As further shown, the interaction between the 2D graphene sheets and zero-dimensional carbon nanoparticles creates a seamless carbon network with excellent electronic conductivity and low resistance.
[0093] Figure 3A is a particle size distribution of an exemplary first conductive ink. Figure 3B is an image of the exemplary first conductive ink on a Hegman gauge. As shown, the exemplary first conductive ink has a mono-modal particle size distribution with a mean of about 9 μm and a maximum of about 26 μm, with 90% of the particles being less than about 13.5 μm in size.
[0094] Figure 4A is an X-ray diffraction graph of the first conductive ink coated on a substrate. Two broad characteristic peaks at 2θ of 12.3° and 19.4°, corresponding to d values of 7.5° and 4.5° angstroms, respectively, match the XRD chart of the binder. Figure 4B is a Raman spectroscopy graph of the exemplary first conductive ink printed on a substrate. The D band at 1346 cm-1 and the G band at 1603 cm-1 are characteristic of rGO.
[0095] 5 is a graph of shear rate versus viscosity of an exemplary first conductive ink. As shown, the viscosity of the first conductive ink can be adjusted by adjusting the shear mixing time, with longer shear times resulting in lower viscosity.
[0096] FIGS. 6A and 6B are graphs of a thermal analysis for an exemplary first conductive ink. In the thermal analysis, a first conductive ink herein in liquid form was heated to about 140°C at a rate of about 3°C / min, maintained at about 140°C for about 3 hours, and then heated to about 900°C at a rate of about 3°C / min. According to FIGS. 6A and 6B, in some embodiments, the first conductive ink has an endothermic peak (601) at about 129°C, indicating rapid mass loss due to evaporation of a solvent with a high vapor pressure. As further shown, in some embodiments, the first conductive ink has exothermic peaks (611), (612), (613), and (614) at about 415.75°C, 449.98°C, 485.78°C, and 552.40°C, respectively. According to FIG. 6B, the mass of the ink at about 900°C is nearly zero, so all or nearly all of the first conductive ink is consumed during the reaction with oxygen at that temperature.
[0097] FIG. 7 is a graph of a thermal analysis of an exemplary first conductive ink dried on a substrate. As shown, in some embodiments, the first conductive ink has exothermic peaks (701), (702), and (703) at approximately 391.73°C, 469.69°C, and 582.37°C, respectively. The first exothermic peak (701) and second exothermic peak (702) may correspond to the evaporation of the binder, the softener, or both, and the third exothermic peak (703) may correspond to graphene. As shown, at a temperature of approximately 550°C, the mass of the printed first conductive ink decreases by approximately 93.5%. At a temperature of approximately 800°C, nearly all of the first conductive ink is consumed during the reaction with oxygen. This thermal analysis demonstrates that the first conductive ink printed on the substrate is thermally stable up to approximately 400°C.
[0098] Example 2 - Second Conductive Ink 8A and 8B show optical microscope images of an exemplary second conductive ink. As shown, the second conductive ink is highly stable and uniformly coats the substrate, forming a smooth surface without holes or shrinkage. As further shown, the interaction between the 2D graphene sheets and the zero-dimensional carbon nanoparticles creates a seamless carbon network with excellent electronic conductivity. The graphene and carbon nanoparticles are in intimate and seamless contact within the film, thereby reducing the overall resistance of the coated film.
[0099] Figure 9A is a particle size distribution of an exemplary second conductive ink. Figure 9B is an image of the exemplary first conductive ink on a Hegman gauge, with streaks of particle size of approximately 10 μm. As shown, the exemplary second conductive ink has a unimodal particle size distribution with a mean of approximately 9 μm and a maximum of approximately 26 μm, with 90% of the particles being less than approximately 13.5 μm in size.
[0100] FIG. 10 is a Raman spectroscopy graph of an exemplary second conductive ink showing a D peak at about 1,368 cm and a G peak at about 1,624 cm.
[0101] 11A shows the linear relationship between shear rate and viscosity of an exemplary second conductive ink. As shown, the exemplary second conductive ink has a viscosity of about 210 cP at a shear rate of about 100 s-1 and a viscosity of about 185 cP at a shear rate of about 750 s-1. As shown, the viscosity of the second conductive ink can be adjusted by adjusting the shear mixing time, with longer shear times resulting in lower viscosity.
[0102] FIG. 11B is an X-ray diffraction graph of exemplary second and third conductive inks, both showing a peak at about 26°.
[0103] 12A and 12B are graphs of a thermal analysis for an exemplary second conductive ink. In the thermal analysis, a second conductive ink herein in liquid form was heated to about 140°C at a rate of about 3°C / min, maintained at about 140°C for about 3 hours, and then heated to about 900°C at a rate of about 3°C / min. According to FIGS. 12A and 12B, in some embodiments, the second conductive ink has an endothermic peak (1201) at about 29°C, indicating rapid mass loss due to evaporation of a solvent with a high vapor pressure. As further shown, in some embodiments, the second conductive ink has exothermic peaks (1211), (1212), (1213), and (1214) at about 329°C, 422.04°C, 448.37°C, and 654.98°C, respectively. According to FIG. 12B, the mass of the ink at about 900° C. is nearly zero, so all or nearly all of the second conductive ink is consumed during reaction with oxygen at that temperature.
[0104] FIG. 13 is a graph of a thermal analysis of an exemplary second conductive ink dried on a substrate. As shown, in some embodiments, the second conductive ink has exothermic peaks (1301), (1302), (1303), and (1304) at approximately 320.22°C, 413.79°C, 456.48°C, and 663.3°C, respectively. The second exothermic peak (1301) may correspond to the evaporation of the binder, the softener, or both, while the second exothermic peak (1302) and the third exothermic peak (1303) may correspond to graphene. As shown, at a temperature of approximately 680°C, the mass of the printed second conductive ink is reduced by approximately 95%. At a temperature of approximately 800°C, substantially all of the second conductive ink is consumed during the reaction with oxygen. This thermal analysis demonstrates that the second conductive ink printed on the substrate is thermally stable up to approximately 400°C, enabling increased use cases for the second conductive ink herein.
[0105] Example 3 - Third Conductive Ink Figure 22A is a graph of shear rate versus viscosity for an exemplary third conductive ink. While the flow curve appears linear or Newtonian, the exemplary third conductive ink exhibits slight curvature, shear thinning, and / or pseudoplastic orientation. The ink is suitable for screen printing, roll coating with a slot die or reverse comma blade, and even flexographic printing. Figure 22B is a graph of torque versus speed for an exemplary third conductive ink.
[0106] In one experiment, as shown in Figures 23A and 23B, the exemplary third conductive ink was heated to 110°C at a rate of 10°C / min, held at 110°C for 2 hours, and then heated to 800°C at a rate of 10°C / min. As shown, an endothermic peak was detected at 110°C, corresponding to the rapid weight loss of the ink due to the evaporation of the high-vapor-pressure solvent. In some embodiments, optimal conductivity, ideal adhesion, and flexibility are achieved by baking the exemplary third conductive ink at a temperature of approximately 110°C after printing it onto a substrate. As further shown, several exothermic peaks were found at 350°C, 411°C, 537°C, and 637°C, which may correspond to the decomposition of the binder, dispersant, and / or graphene. Since there is almost no residue at 637°C, all ink components are consumed by reacting with oxygen from the airflow at that temperature.
[0107] In FIG. 24A, the XRD pattern of the substrate coated with the exemplary third conductive ink shows two broad characteristic peaks at 12.9° and 20.8° 2θ, corresponding to d-values of 7.5 and 4.5° Angstroms, respectively, which are consistent with values reported for polymeric binders.
[0108] In FIG. 24B, the Raman spectrum of the exemplary third conductive ink printed on a substrate shows a peak at approximately 1400 cm characteristic of rGO. -1 D band and 1600 cm -1 The G band is shown.
[0109] 25A-25B, 1 μm thick polyimide substrates were coated with various thicknesses of the exemplary third conductive ink by Mayer rod, and the coated substrates were cured at 110° C. until dry. As expected, the results show that the sheet resistance increases with decreasing dry thickness, with an average conductivity of about 7.6 S / m and a standard deviation of about 1.8 S / m.
[0110] In FIG. 26A, the exemplary third conductive ink had a median particle size of about 8.8 μm, an average particle size of about 7.9 μm, and a maximum diameter of about 19 μm, with 90% of the particles being less than about 11.5 μm in size.
[0111] FIG. 26B shows the trace width versus resistance for a substrate coated with an exemplary third conductive ink, which can be successfully screen printed into traces with line widths between 150 and 3000 micrometers.
[0112] A polyimide substrate was coated with the exemplary third conductive ink at a wet film thickness of 50 μm, after which the coating was cured at 110°C for 10 minutes and 300°C for 30 minutes, and then sprayed with water. No signs of damage were observed to the coating.
[0113] The results of the liquid immersion test are shown below.
[0114] [Table 4]
[0115] Example 4 - Fourth Conductive Ink 27A and 27B are graphs of shear rate versus viscosity and torque versus speed, respectively, for an exemplary fourth conductive ink. As shown, the flow curve appears linear or Newtonian, and the graphs for the exemplary fourth conductive ink exhibit slight curvature in shear thinning and / or pseudoplastic orientation.
[0116] In the thermal analysis shown in Figures 28A-28B, the liquid of the fourth exemplary conductive ink was heated to 110°C at a rate of 10°C / min, maintained at 110°C for 2 hours, and then heated to 800°C at a rate of 10°C / min. As shown, an endothermic peak was detected at 110°C, corresponding to the rapid weight loss of the ink associated with the evaporation of the high-vapor-pressure solvent. As further shown, optimal conductivity, ideal adhesion, and flexibility were achieved by baking the third exemplary conductive ink at a temperature of approximately 110°C after printing it onto a substrate. Several exothermic peaks were found at 358°C, 466°C, 515.79°C, and 726.24°C, corresponding to the decomposition of the binder, dispersant, carbon, and graphene. At 797.48°C, there was almost no residue, indicating that all ink components were consumed by reacting with oxygen from the airflow.
[0117] The XRD pattern of the substrate coated with the fourth exemplary conductive ink in FIG. 29A shows two broad characteristic peaks at 12.4° and 21.1° 2θ, corresponding to d-values of 7.5 and 4.5° Angstroms, respectively, which are consistent with values reported for polymeric binders.
[0118] In FIG. 29B, the Raman spectrum of the substrate coated with the fourth exemplary conductive ink shows a peak at approximately 1400 cm characteristic of rGO. -1 D band and 1600 cm -1 The G band is shown.
[0119] 30A-30B, 1 μm thick polyimide substrates were coated with various thicknesses of the fourth exemplary conductive ink by Mayer rod, and the coated substrates were cured at 110° C. until dry. As expected, the results show that sheet resistance increases with decreasing dry thickness, with an average conductivity of about 12.7 S / m and a standard deviation of about 3.7 S / m.
[0120] FIG. 31 shows the trace width versus resistance for a substrate coated with the exemplary fourth conductive ink, and the exemplary third conductive ink can be successfully screen printed into traces with line widths between 150 and 3000 micrometers.
[0121] Example 5 - Fifth Conductive Ink 32A and 32B are graphs of shear rate versus viscosity and torque versus speed, respectively, for an exemplary fifth conductive ink. As shown, the flow curve appears linear or Newtonian, and the graphs for the exemplary fifth conductive ink exhibit slight curvature in shear thinning and / or pseudoplastic orientation.
[0122] In the thermal analysis shown in Figures 33A-33B, the liquid of the fourth exemplary conductive ink was heated to 110°C at a rate of 10°C / min, maintained at 110°C for 2 hours, and then heated to 800°C at a rate of 10°C / min. As shown, an endothermic peak was detected at 110°C, corresponding to the rapid weight loss of the ink associated with the evaporation of the high-vapor-pressure solvent. As further shown, optimal conductivity, ideal adhesion, and flexibility were achieved by baking the third exemplary conductive ink at a temperature of approximately 110°C after printing it onto a substrate. Several exothermic peaks were found at 367°C, 474°C, 714°C, and 805°C, corresponding to the decomposition of the binder, dispersant, carbon, and graphene. At 805°C, nearly zero residue was observed, indicating that all ink components were consumed by reacting with oxygen from the airflow.
[0123] The XRD pattern of the substrate coated with exemplary fifth conductive ink in Figure 34A shows a sharp intensity peak at 2θ = 26° characteristic of graphite, with a smaller peak at 2θ = 55°. Another peak near 2θ = 45° correlates to rGO.
[0124] In FIG. 34B, the Raman spectrum of the substrate coated with the exemplary fifth conductive ink shows a peak at approximately 1400 cm characteristic of rGO. -1 D band and 1600 cm-1 The peak at about 2700 cm-1 is characteristic of graphite, which also explains the sharpness of the peak at about 1600 cm-1.
[0125] In FIG. 35A, the exemplary fifth conductive ink had a median particle size of about 11.8 μm and an average particle size of about 11.2 μm, with 90% of the particles being less than about 15.7 μm in size.
[0126] FIG. 35B shows the trace width versus resistance for a substrate coated with an exemplary fifth conductive ink, which can be successfully screen printed into traces with line widths between 150 and 3000 micrometers.
[0127] In Figures 36A-36C and 37A-37B, optical profilometry of the printed lines shows straight, clean edges. The highly uniform cross-sectional profile provides evidence of successful preparation of the ink formulation.
[0128] 38A-38B, 1 μm thick polyimide substrates were coated with various thicknesses of the exemplary fifth conductive ink by Mayer rod, and the coated substrates were cured at 110° C. until dry. As expected, the results show that the sheet resistance increases with decreasing dry thickness, with an average conductivity of about 41.9 S / m and a standard deviation of about 15.8 S / m.
[0129] 39A-39B show low and high magnification SEM images of a substrate coated with an exemplary fifth conductive ink.
[0130] Example 6 - Sixth Conductive Ink Figure 40A is a graph of shear rate versus viscosity for an exemplary third conductive ink. While the flow curve appears linear or Newtonian, the exemplary third conductive ink exhibits slight curvature, shear thinning, and / or pseudoplastic orientation. The ink is suitable for screen printing, roll coating with a slot die or reverse comma blade, and even flexographic printing. Figure 40B is a graph of torque versus speed for an exemplary third conductive ink.
[0131] In one experiment, as shown in Figures 41A and 41B, the exemplary sixth conductive ink was heated to 110°C at a rate of 10°C / min, held at 110°C for 2 hours, and then heated to 800°C at a rate of 10°C / min. As shown, an endothermic peak was detected at 110°C, corresponding to the rapid weight loss of the ink due to the evaporation of the high-vapor-pressure solvent. In some embodiments, optimal conductivity, ideal adhesion, and flexibility are achieved by baking the exemplary sixth conductive ink at a temperature of approximately 110°C after printing it onto a substrate. As further shown, several exothermic peaks were found at 351°C, 462°C, 484°C, and 669°C, which may correspond to the decomposition of the binder, dispersant, and / or graphene. Since there is almost no residue at 669°C, all ink components are consumed by reacting with oxygen from the airflow at that temperature.
[0132] In Figure 42A, the XRD pattern of the substrate coated with the exemplary third conductive ink shows two broad characteristic peaks at 12.3° and 19.4° 2θ, which are consistent with values reported for polymeric binders.
[0133] In FIG. 42B, the Raman spectrum of the exemplary sixth conductive ink printed on a substrate shows a peak at approximately 1400 cm characteristic of rGO. -1 D band and 1600 cm -1 The G band is shown.
[0134] In FIG. 43A, the sixth exemplary conductive ink had a median particle size of about 12.5 μm and an average particle size of about 11.6 μm, with 90% of the particles being less than about 19.6 μm in size.
[0135] In Figure 43B, 1 μm thick polyimide substrates were coated with various thicknesses of exemplary sixth conductive ink by Mayer rod, and the coated substrates were cured at 110°C until dry. As expected, the results show that sheet resistance increases with decreasing dry thickness, with an average conductivity of about 28.4 S / m and a standard deviation of about 14.3 S / m.
[0136] Figure 44A is a graph of wet versus dry thickness of traces formed with an exemplary sixth conductive ink, and Figure 44B shows trace width versus resistance for a substrate coated with an exemplary sixth conductive ink, which can be successfully screen printed into traces with line widths between 150 and 3000 micrometers.
[0137] While preferred embodiments of the present disclosure have been shown and described herein, it will be obvious to those skilled in the art that such embodiments are provided by way of example only. Numerous variations, changes, and substitutions will occur to those skilled in the art without departing from the present disclosure. It is understood that various alternatives to the embodiments of the present disclosure described herein may be employed in practicing the present disclosure.
Claims
1. (a) a graphene sheet, (i) at least about 90% of the graphene sheets consist of a single layer; (ii) the graphene sheets have an oxygen content of at most about 6%, or (iii) graphene sheets, and (b) a binder; and (c) a stabilizer; and (d) a solvent; 13. A conductive ink comprising:
2. 10. The conductive ink of claim 1, wherein the graphene comprises reduced graphene oxide or activated reduced graphene oxide.
3. The conductive ink of claim 1 , wherein the binder is a polymeric binder.
4. The conductive ink of claim 3 , wherein the polymeric binder is a thermoplastic copolymer.
5. The conductive ink of claim 1 , wherein the binder comprises polyvinylpyrrolidone, ethyl methacrylate, butyl methacrylate, or any combination thereof.
6. 10. The conductive ink of claim 1, wherein the stabilizer comprises polytetrahydrofuran, fluorinated triethylene glycol monomethyl ether, a wax, ethyl cellulose, diethylene glycol, or any combination thereof.
7. 7. The conductive ink of claim 6, wherein the stabilizer comprises polytetrahydrofuran and diethylene glycol, the ratio of the polytetrahydrofuran to the diethylene glycol being from about 8:1 to about 11:
1.
8. 2. The conductive ink of claim 1, wherein the solvent comprises propylene glycol n-propyl ether, 2-ethyl-1-hexanol, diethylene glycol monobutyl ether, 2-ethyl-1-butanol, 2-methyl-1-pentanol, propylene glycol monomethyl ether acetate, hexamine, cycloheptylamine, isoamylamine, 3-methoxypropylamine, parachlorobenzotrifluoride, ethylene glycol, isopropanol, ethyl acetate, chloroform, dimethylformamide, n-methyl-2-pyrrolidone, tetrahydrofuran, and dichlorobenzene, or any combination thereof.
9. 10. The conductive ink of claim 1 having a weight percentage concentration of said graphene of about 0.1% to about 10%.
10. The conductive ink of claim 1 having a weight percentage concentration of said binder of about 5% to about 60%.
11. The conductive ink of claim 1 having a weight percentage concentration of said stabilizer of about 1% to about 80%.
12. The conductive ink of claim 1 having a weight percentage concentration of the solvent of about 20% to about 90%.
13. The conductive ink of claim 1 having a solids content of about 5% to about 80%.
14. 10. The conductive ink of claim 1, having a viscosity of about 25 cP to about 4,000 cP.
15. 2. The conductive ink of claim 1, wherein the shear rate is from about 100 s-1 to about 400 s-1.
16. 10. The conductive ink of claim 1, wherein the ratio of the wet thickness of the conductive ink dispersed on a substrate to the dry thickness of the conductive ink dried on the substrate is from about 2:1 to about 6:
1.
17. 10. The conductive ink of claim 1, having a dry resistivity of from about 300 ohm / sq to about 80,000 ohm / sq.
18. 10. The conductive ink of claim 1, having a dry resistivity of about 300 ohms / square or less.
19. 10. The conductive ink of claim 1, wherein the particle size is from about 1 um to about 40 um.
20. The conductive ink of claim 1 further comprising a conductive additive.
21. The conductive ink of claim 20 , wherein the conductive additive comprises nanocarbon.
22. 22. The conductive ink of claim 21, wherein the nanocarbon comprises carbon nanoparticles, carbon nanodots, carbon nanotubes, graphene nanoribbons, carbon nanofibers, nanographite, carbon onions, carbon nanocones, or any combination thereof.
23. The conductive ink of claim 20 having a weight percentage concentration of the conductive additive of about 1% to about 40%.
24. The conductive ink of claim 1 further comprising graphite.
25. 25. The conductive ink of claim 24 having a weight percentage concentration of said graphite of about 5% to about 80%.
26. 1. A method for printing conductive ink, comprising the steps of: (a) depositing up to two layers of the ink of claim 1 onto a substrate; (b) drying the ink on the substrate; The method includes:
27. 27. The method of claim 26, wherein the depositing step is performed by screen printing, flexographic printing, slot-die printing, knife-over edge coating, screen printing, gravure printing, spraying, dipping, or any combination thereof.
28. The method of claim 26, wherein the ink is dried at a temperature of from about 100°C to about 180°C.
29. The method of claim 26, wherein the ink is dried for a period of from about 10 minutes to about 60 minutes.
30. The method of claim 26, wherein the ink is deposited on the substrate in a line width of about 150 um to about 3,000 um.
31. 27. The method of claim 26, wherein the substrate comprises mica, glass, silicon, glass, metal, plastic, woven fabric, graphite sheet, gold, or any combination thereof.
32. 27. The method of claim 26, wherein the average roughness of the dried ink is from about 1 um to about 2 um.
33. 27. The method of claim 26, wherein the dried ink has a texture aspect ratio of from about 0.25° to about 1.5°.
34. 27. The method of claim 26, wherein the printed conductive ink has a resistance of about 1,000 to about 40,000 ohms / sq.
35. 27. The method of claim 26, further comprising the step of baking the ink on the substrate.
36. 1. A method of forming a conductive ink, comprising: (a) a graphene sheet, (i) at least about 90% of the graphene sheets consist of a single layer; (ii) the graphene sheets have an oxygen content of at most about 6%, or (iii) graphene sheets, and (b) a binder; and (c) a stabilizer; and (d) a solvent; The method comprises mixing a solution comprising:
37. 37. The method of claim 36, wherein the graphene comprises reduced graphene oxide or activated reduced graphene oxide.
38. The method of claim 37, wherein the binder is a polymeric binder.
39. 40. The method of claim 38, wherein the polymeric binder is a thermoplastic copolymer.
40. 37. The method of claim 36, wherein the binder comprises polyvinylpyrrolidone, ethyl methacrylate, butyl methacrylate, or any combination thereof.
41. 37. The method of claim 36, wherein the stabilizer comprises polytetrahydrofuran, fluorinated triethylene glycol monomethyl ether, a wax, ethyl cellulose, diethylene glycol, or any combination thereof.
42. 37. The method of claim 36, wherein the solvent comprises propylene glycol n-propyl ether, 2-ethyl-1-hexanol, diethylene glycol monobutyl ether, 2-ethyl-1-butanol, 2-methyl-1-pentanol, propylene glycol monomethyl ether acetate, hexamine, cycloheptylamine, isoamylamine, 3-methoxypropylamine, parachlorobenzotrifluoride, ethylene glycol, isopropanol, ethyl acetate, chloroform, dimethylformamide, n-methyl-2-pyrrolidone, tetrahydrofuran, and dichlorobenzene, or any combination thereof.
43. 37. The method of claim 36, wherein the solution has a weight percentage concentration of graphene from about 0.1% to about 10%.
44. The method of claim 36, wherein the solution has a weight percentage concentration of the binder of about 5% to about 60%.
45. 37. The method of claim 36, wherein the solution has a weight percentage concentration of the stabilizer of about 1% to about 80%.
46. The method of claim 36, wherein the solution has a weight percentage concentration of the solvent of about 20% to about 90%.
47. 37. The method of claim 36, wherein the solids content of the solution is from about 5% to about 80%.
48. 37. The method of claim 36, wherein the solution is mixed for a period of about 1 hour to about 4 hours.
49. The method of claim 36, wherein the conductive ink has a viscosity of about 25 cP to about 4,000 cP.
50. The method of claim 36, wherein the conductive ink has a shear rate of about 100 s-1 to about 400 s-1.
51. 37. The method of claim 36, wherein the ratio of the wet thickness of the conductive ink dispersed on a substrate to the dry thickness of the conductive ink dried on the substrate is from about 2:1 to about 6:
1.
52. 37. The method of claim 36, wherein the conductive ink has a dry resistivity of from about 300 ohm / sq to about 80,000 ohm / sq.
53. 37. The method of claim 36, wherein the conductive ink has a particle size of about 3 um to about 40 um.
54. 37. The method of claim 36, wherein the solution further comprises a conductive additive.
55. 55. The method of claim 54, wherein the conductive additive comprises nanocarbon.
56. 56. The method of claim 55, wherein the nanocarbons comprise carbon nanoparticles, carbon nanodots, carbon nanotubes, graphene nanoribbons, carbon nanofibers, nanographite, carbon anions, carbon nanocones, or any combination thereof.
57. 55. The method of claim 54, wherein the solution has a weight percentage concentration of the conductive additive of about 1% to about 40%.
58. 37. The method of claim 36, wherein the solution further comprises graphene.
59. 60. The method of claim 58, wherein the solution has a weight percentage concentration of the graphene from about 5% to about 80%.