Nonwoven fabric, method for producing the nonwoven fabric, and article made from the nonwoven fabric
The core-sheath composite fiber nonwoven fabric addresses the challenge of maintaining strength and bonding properties by employing specific melting indices and manufacturing processes, resulting in a tough and stable spunbond fabric with enhanced bonding and strength.
Patent Information
- Application Number
- JP2024529821
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-09-13
- Filing Date
- 2022-10-25
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2042-10-25
AI Technical Summary
Existing nonwoven fabrics face challenges in maintaining strength and bonding properties while reducing weight due to process and equipment limitations, making it difficult to enhance their physical properties.
A nonwoven fabric composed of core-sheath composite fibers with specific melting indices and viscosity ranges, produced using separate extruders and a spinneret, followed by cooling, stretching, and mechanical property enhancement, results in a spunbond fabric with improved toughness and bonding.
The fabric achieves excellent bonding properties and strength with a toughness range of 100 to 300, maintaining stability in the manufacturing process and enhancing individual fiber strength and bonding forces.
Smart Images

Figure 2024540589000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a nonwoven fabric, a manufacturing method for the nonwoven fabric, and an article made from the nonwoven fabric, and more specifically, to a nonwoven fabric having excellent bondability and strength, a manufacturing method for the nonwoven fabric, and an article made from the nonwoven fabric. [Background technology]
[0002] Nonwoven fabrics are used in a variety of applications, such as in medical applications, in industrial applications such as for protective clothing and masks, and in sanitary products such as diapers and sanitary napkins.
[0003] In addition, nonwoven fabrics are generally manufactured and used in a multi-layer structure in which two or more layers are bonded together, and since excellent strength is required for most applications, many researchers are currently devoting themselves to the development of multi-layer nonwoven fabrics with excellent strength.
[0004] In addition, in accordance with the recent trend to reduce the weight of existing nonwoven fabrics, there are process and equipment limitations in maintaining the physical properties of the existing nonwoven fabrics as they are or even in further improving the physical properties of the nonwoven fabrics. Summary of the Invention [Problem to be solved by the invention]
[0005] An embodiment of the present invention provides a nonwoven fabric having excellent bondability and strength. Another embodiment of the present invention provides a method for producing the nonwoven fabric. Yet another embodiment of the present invention provides an article comprising the nonwoven fabric. [Means for solving the problem]
[0006] One aspect of the present invention is ASTM D4440-08, 100sec -1 The nonwoven fabric has a melt viscosity of 500 to 740 poise, measured at a shear rate of 1000 rpm and a temperature of 230°C.
[0007] The nonwoven fabric comprises a core-sheath type composite fiber, and the core-sheath type composite fiber includes a core having a melt index (MFR (measurement temperature: 230°C, load: 2.16 kg)) of 20 to 50 g / 10 min as measured according to ASTM D1238, and a sheath having a melt index (MFR (measurement temperature: 230°C, load: 2.16 kg)) of 40 to 120 g / 10 min as measured according to ASTM D1238.
[0008] The sheath may have a melt index greater than that of the core by about 10 to 100 g / 10 min.
[0009] The weight ratio of the sheath to the core is also 1-5:9-5.
[0010] The core also includes a first polypropylene and the sheath also includes a second polypropylene.
[0011] The nonwoven fabric also has a toughness represented by the following formula 1 of 100 to 300:
number
[0012] The nonwoven fabric may also be a spunbond nonwoven fabric.
[0013] The nonwoven fabric may be made up of two or more layers.
[0014] Another aspect of the present invention is A step (S10) of melting a polymer for forming a core portion and a polymer for forming a shell portion in separate extruders to form a melt for forming a core portion and a melt for forming a shell portion; (S20) discharging the molten materials through a spinneret having a composite spinning nozzle to release composite long fibers; (S30) cooling and stretching the released composite filaments; (S40) collecting the cooled and drawn composite filaments on a collecting belt and depositing them to a predetermined thickness to form a nonwoven fabric; In the step (S20), the temperature of the spinneret is maintained at 230 to 250°C.
[0015] The method for producing a nonwoven fabric may further include a step (S50) of imparting mechanical properties to the nonwoven fabric formed in the step (S40).
[0016] Yet another aspect of the invention provides an article comprising the nonwoven fabric described above. Effect of the Invention
[0017] The nonwoven fabric according to an embodiment of the present invention and an article including the same have the advantages of excellent bondability and strength. [Brief description of the drawings]
[0018] [Figure 1] 1 is a cross-sectional view of a core-sheath type composite fiber constituting a nonwoven fabric according to an embodiment of the present invention. [Diagram 2] FIG. 13 is a cross-sectional view of a side-by-side type conjugate fiber constituting a nonwoven fabric according to Comparative Example 11. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, a nonwoven fabric according to an embodiment of the present invention will be described in detail.
[0020] The nonwoven fabric according to one embodiment of the present invention has a 100 sec. -1 The melt viscosity measured at a shear rate of 1000 to 740 poise at a temperature of 230° C.
[0021] If the melt viscosity of the nonwoven fabric is within the above range, the nonwoven fabric can have excellent bondability and strength.
[0022] If the melt viscosity of the nonwoven fabric is less than 500 poise, the strength of the individual fibers constituting the nonwoven fabric will decrease, resulting in a decrease in the strength of the nonwoven fabric itself, whereas if the melt viscosity of the nonwoven fabric is more than 740 poise, the bonding property of the individual fibers constituting the nonwoven fabric will decrease, weakening the bonding strength between the individual fibers, resulting in a decrease in the strength of the nonwoven fabric produced by laminating the individual fibers.
[0023] The melt viscosity of the nonwoven fabric can be determined by the structure of the fibers constituting the nonwoven fabric, the types of raw materials constituting the fibers, the ratio and physical properties of the raw materials, the manufacturing conditions and method of the fibers, and the manufacturing conditions and method of the nonwoven fabric using the fibers.
[0024] The nonwoven fabric also contains core-sheath type composite fibers.
[0025] The core-sheath type composite fiber also includes a core having a melt index (MFR (measurement temperature 230°C, load 2.16 kg)) of 20 to 50 g / 10 min as measured by ASTM D1238, and a sheath having a melt index (MFR (measurement temperature 230°C, load 2.16 kg)) of 40 to 120 g / 10 min as measured by ASTM D1238. If the melt index (MFR) of the core and the melt index (MFR) of the sheath are each within the above range, the core-sheath type composite fiber can be used for 100 sec. / min ... -1 At a shear rate of 100 to 400 and a melt viscosity of 500 to 740 poise measured at a temperature of 230° C., a nonwoven fabric having a toughness of 100 to 300 can be obtained.
[0026] In addition, the sheath may have a melt flow rate (MFR) of about 10 to 100 g / 10 min higher than that of the core. If the melt flow rate (MFR) of the sheath relative to that of the core is within the above range, the sheath may be melted at 100 sec according to ASTM D4440-08. -1At a shear rate of 100 to 400 and a melt viscosity of 500 to 740 poise measured at a temperature of 230° C., a nonwoven fabric having a toughness of 100 to 300 can be obtained.
[0027] The weight ratio of the sheath to the core is also 1-5:9-5. If the weight ratio of the sheath to the core is within the above range, the 100 sec. -1 At a shear rate of 100 to 400 and a melt viscosity of 500 to 740 poise measured at a temperature of 230° C., a nonwoven fabric having a toughness of 100 to 300 can be obtained.
[0028] The core portion includes a first polypropylene, and the sheath portion includes a second polypropylene.
[0029] The first propylene-based polymer and the second propylene-based polymer are also produced using a highly stereoregular polymerization catalyst.
[0030] The highly stereoregular polymerization catalyst may include a diester component catalyst, a succinate component catalyst, a metallocene catalyst, or a combination thereof.
[0031] FIG. 1 is a cross-sectional view of a core-sheath type composite fiber 100 constituting a nonwoven fabric according to an embodiment of the present invention.
[0032] Referring to FIG. 1, the core-sheath type composite fiber 100 includes a core portion 110 and a sheath portion 120 configured to surround the core portion 110.
[0033] The nonwoven fabric also has a toughness represented by the following formula 1 of 100 to 300:
number
[0034] The nonwoven fabric may also be a spunbond nonwoven fabric.
[0035] The nonwoven fabric may also be made of two or more layers, for example, the nonwoven fabric may be a nonwoven fabric laminate.
[0036] The fineness and basis weight of the nonwoven fabric may be appropriately selected depending on the application. Generally, the fineness is 1.0 to 2.5 denier, for example, 0.7 to 2.0 denier, and the basis weight is 15 to 100 g / m 2 , for example, 7 to 30 g / m 2 It is also.
[0037] The core-sheath type composite fiber further contains additives, if necessary, in addition to the first propylene polymer and the second propylene polymer, within the scope of the object of the present invention. The additives include known heat stabilizers, weather stabilizers, various stabilizers, antistatic agents, antiblocking agents, anticlouding agents, fillers, dyes, pigments, natural oils, synthetic oils, waxes, or combinations thereof.
[0038] The stabilizer may include an anti-aging agent such as 2,6-di-t-butyl-4-methylphenol (BHT); a phenolic antioxidant such as tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane, β-(3,5-di-t-butyl-4-hydroxyphenyl)propionic acid alkyl ester, or 2,2′-oxamidobis[ethyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate; a fatty acid metal salt such as zinc stearate, calcium stearate, or calcium 1,2-hydroxystearate; a polyhydric alcohol fatty acid ester such as glycerin monostearate, glycerin distearate, pentaerythritol monostearate, pentaerythritol distearate, or pentaerythritol tristearate; or a combination thereof.
[0039] The filler may also include silica, diatomaceous earth, alumina, titanium dioxide, magnesium oxide, pumice powder, pumice balloons, aluminum hydroxide, magnesium hydroxide, basic magnesium carbonate, dolomite, calcium sulfate, potassium titanate, barium sulfate, calcium sulfite, talc, clay, mica, asbestos, calcium silicate, montmorillonite, bentonite, graphite, aluminum powder, molybdenum sulfide, or combinations thereof.
[0040] The propylene-based polymer and the additives used as necessary can be mixed using a known method.
[0041] Hereinafter, a method for producing a nonwoven fabric according to an embodiment of the present invention will be described in detail.
[0042] A method for producing a nonwoven fabric according to an embodiment of the present invention includes the steps of: melting a polymer for forming a core portion and a polymer for forming a sheath portion in separate extruders to form a melt for forming a core portion and a melt for forming a sheath portion (S10); discharging the melts through a spinneret having a composite spinning nozzle configured to form and discharge a desired fiber structure to discharge composite long fibers (S20); cooling and stretching the discharged composite long fibers (S30); and collecting the cooled and stretched composite long fibers on a collecting belt and depositing them to a predetermined thickness to form a nonwoven fabric (S40).
[0043] In the step (S20), the temperature of the spinneret may be maintained at 230 to 250° C. If the temperature of the spinneret is within the above range in the step (S20), the spinneret may be heated for 100 seconds according to ASTM D4440-08. - When the melt viscosity measured at a shear rate of 1 and a temperature of 230°C is 500 to 740 poise, a nonwoven fabric having a toughness of 100 to 300 can be obtained, and good process stability (spinnability) can be obtained in the nonwoven fabric production process.
[0044] The step (S30) is a step of cooling the composite continuous fibers discharged in the step (S20) with cooling air and applying tension with drawing air to the composite continuous fibers so that the composite continuous fibers have a predetermined fineness.
[0045] The method for producing a nonwoven fabric may further include a step (S50) of imparting mechanical properties to the nonwoven fabric formed in the step (S40).
[0046] The step (S50) may be performed by a method using means such as needle punch, water jet, ultrasonic wave, etc., an embossing process using a heated embossing roll, or a method of heat fusing by high temperature ventilation.
[0047] Hereinafter, an article according to an embodiment of the present invention will be described in detail.
[0048] An article according to one embodiment of the present invention includes the nonwoven fabric described above.
[0049] The article may also be a diaper, an absorbent product, a toilet product, a support layer, a top sheet, a medical garment, a protective garment or a mask.
[0050] The present invention will be described in more detail below with reference to examples. These examples are provided to more specifically explain the present invention, but the scope of the present invention is not limited to these examples. EXAMPLES
[0051] Examples 1 to 11 and Comparative Examples 1 to 10: Production of nonwoven fabrics A nonwoven fabric made of a core-sheath type composite fiber 100 having the structure of FIG. 1 was manufactured by the following method. Specifically, a first polypropylene for forming the core and a second polypropylene for forming the sheath were melted in separate extruders to form a melt for forming the core and a melt for forming the sheath. Then, each of the melts was discharged through a spinneret having a composite spinning nozzle. Then, each of the discharged melts was cooled by cooling air, and tension was applied by stretching air to give a predetermined fineness. Then, the cooled and stretched composite long fibers were collected on a collecting belt and piled up to a predetermined thickness to form a nonwoven fabric. Then, mechanical properties were imparted to the formed nonwoven fabric by embossing processing using a heated embossing roll.
[0052] The melt index (MFR) of the first polypropylene for forming the core, the melt index (MFR) of the second propylene for forming the sheath, the melt index (MFR) difference between the second propylene and the first propylene, and the weight ratio of the sheath to the core are shown in Table 1. In Table 1, "production temperature of the nonwoven fabric" means the temperature of the spinneret.
[0053] Comparative Example 11: Production of nonwoven fabric A nonwoven fabric made of side-by-side type composite fiber (1) having the structure of FIG. 2 was produced by the following method. Specifically, a first polypropylene for forming side A and a second polypropylene for forming side B were melted in separate extruders to form a melt for forming side A and a melt for forming side B. Then, each of the melts was discharged through a spinneret having a composite spinning nozzle. Then, each of the discharged melts was cooled by cooling air, and tension was applied by stretching air to give a predetermined fineness. Then, the cooled and stretched composite long fibers were collected on a collecting belt and accumulated to a predetermined thickness to form a nonwoven fabric. Then, mechanical properties were imparted to the formed nonwoven fabric by embossing processing using a heated embossing roll.
[0054] The melt index (MFR) of the first polypropylene for forming Side A, the melt index (MFR) of the second polypropylene for forming Side B, the melt index (MFR) difference between the second propylene and the first propylene, and the weight ratio of Side A to Side B are shown in Table 1. In Table 1, "production temperature of nonwoven fabric" means the temperature of the spinneret.
[0055] [Table 1]
[0056] Evaluation example: Evaluation of the physical properties of nonwoven fabric The physical properties of each of the nonwoven fabrics produced in Examples 1 to 11 and Comparative Examples 1 to 11 were evaluated by the following methods, and the results are shown in Table 2 below. (1) Melt viscosity: ASTM D4440-08, 100 sec -1 The melt viscosity of the nonwoven fabric was measured at a shear rate of 100 rpm and a temperature of 230° C. (2) Tensile strength: Using an Instron measuring device, a tensile test was performed according to the KSK 0520 method with a test piece width of 5 cm, spacing of 10 cm, and a tensile speed of 500 mm / min to determine the maximum tensile load. (3) Tensile elongation: The elongation at the maximum elongation measured by the method in (3) above was determined. (4) Basic weight (weight: g / m 2 ):Measured according to ASTM D3776-1985. (5) Toughness: Using the tensile strength (N / 5 cm) obtained in (2) above and the tensile elongation (%) obtained in (3) above, toughness was calculated according to the following formula 1.
number
[0057] [Table 2]
[0058] Referring to Table 2, the nonwoven fabrics produced in Examples 1 to 10 have melt viscosities in the range of 500 to 740 poise, toughness in the range of 100 to 300, and excellent MD tensile strength and MD tensile elongation. In addition, the nonwoven fabric production process of Examples 1 to 10 has excellent process stability (spinnability).
[0059] On the other hand, it can be seen that the nonwoven fabrics produced in Comparative Examples 1 to 11 have melt viscosities outside the range of 500 to 740 poise, and toughness outside the range of 100 to 300. It can also be seen that the nonwoven fabric production processes of Comparative Examples 1 to 3 have poor process stability (spinnability).
[0060] Although the present invention has been described with reference to the drawings and embodiments, they are merely illustrative, and a person skilled in the art will understand that various modifications and equivalent embodiments are possible therefrom. Therefore, the true technical scope of the present invention is defined by the technical ideas of the claims.
Claims
1. ASTM D4440-08, 100 sec -1 and a temperature of 230° C., the melt viscosity of which is 500 to 740 poise.
2. The nonwoven fabric contains core-sheath type composite fibers, 2. The nonwoven fabric according to claim 1, wherein the core-sheath type composite fiber comprises a core having a melt index (MFR (measurement temperature: 230° C., load: 2.16 kg)) of 20 to 50 g / 10 min as measured by ASTM D1238, and a sheath having a melt index (MFR (measurement temperature: 230° C., load: 2.16 kg)) of 40 to 120 g / 10 min as measured by ASTM D1238.
3. The nonwoven fabric according to claim 2, wherein the sheath has a melt flow rate (MFR) that is about 10 to 100 g / 10 min higher than that of the core.
4. The nonwoven fabric according to claim 2 , wherein the weight ratio of the sheath portion to the core portion is 1-5:9-5.
5. 3. The nonwoven fabric of claim 2, wherein the core comprises a first polypropylene and the sheath comprises a second polypropylene.
6. The nonwoven fabric according to claim 1, having a toughness represented by the following formula 1 of 100 to 300: [0010]
7. The nonwoven fabric of claim 1 , wherein the nonwoven fabric is a spunbond nonwoven fabric.
8. The nonwoven fabric of claim 1 , wherein the nonwoven fabric is made of two or more layers.
9. A step (S10) of melting a polymer for forming a core portion and a polymer for forming a shell portion in separate extruders to form a melt for forming a core portion and a melt for forming a shell portion; (S20) discharging the molten materials through a spinneret having a composite spinning nozzle to release composite long fibers; (S30) cooling and stretching the released composite filaments; (S40) collecting the cooled and drawn composite filaments on a collecting belt and depositing the composite filaments to a predetermined thickness to form a nonwoven fabric; In the step S20, the temperature of the spinneret is maintained at 230 to 250°C.
10. The method of claim 9, further comprising the step of imparting mechanical properties to the nonwoven fabric formed in the step (S40) (S50).
11. An article comprising the nonwoven fabric of any one of claims 1 to 8.
Citation Information
Patent Citations
Spun-bonded nonwoven fabric
JP2019026955A
Nonwoven fabric capable of being elongated and composite nonwoven fabric comprising said nonwoven fabric laminated
WO2004048661A1
Energy complex
WO2004048861A1
Layered nonwoven fabric
WO2008108238A1
Method for producing spun-bonded nonwoven fabric and spun-bonded nonwoven fabric
WO2012105567A1
Cited By
Composite nonwoven fabric and articles containing the same
JP2026505526A