Thermally Conductive Plastic
A thermally conductive plastic composition with rounded silicon particles addresses the limitations of traditional fillers by achieving high thermal conductivity and low flammability, suitable for electric vehicles and electronics.
Patent Information
- Application Number
- JP2024529859
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2022-07-21
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2042-07-21
AI Technical Summary
Existing thermally conductive plastics face challenges such as high weight, cost, electrical conductivity, flammability, and limited thermal conductivity due to the use of ceramic, metal, and silicon fillers, which are either dense, expensive, or pose safety risks.
A thermally conductive plastic composition containing predominantly rounded silicon particles with a specific size range (30-200 μm) and broad particle size distribution, combined with a low volume fraction of smaller particles, achieves high thermal conductivity (≥0.6 W/mK) while minimizing flammability and weight.
The composition provides enhanced thermal conductivity, reduced flammability, and lower weight, making it suitable for applications in electric vehicles and electronics without the drawbacks of traditional fillers.
Smart Images

Figure 2024540596000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to thermally conductive plastics, their manufacture and their uses. [Background technology]
[0002] Thermally conductive plastics are widely used for thermal management in the automotive and electronics industries. Important applications include thermally conductive adhesives, thermally conductive pads, gap fillers, potting compounds and pastes.
[0003] Plastics generally exhibit low thermal conductivity. The typical thermal conductivity of plastics is in the range of about 0.2 to 0.3 W / mK.
[0004] The prior art discloses various thermally conductive fillers that are added to plastics to increase their thermal conductivity. However, these have significant drawbacks. Ceramic fillers, such as aluminum oxide, are very dense and therefore add significantly to the weight of the part. They are also relatively expensive. Metal fillers, such as aluminum powder and silver powder, are electrically conductive and therefore unacceptable for many applications. Many metals and alloys are also relatively expensive.
[0005] Furthermore, many highly thermally conductive fillers, such as carbon nanotubes, boron nitride, and aluminum nitride, are relatively expensive and may only be employed to a limited extent, in small quantities, or in specific applications.
[0006] Prior art discloses various thermally conductive plastic compositions containing silicon particles as thermally conductive fillers. These are relatively lightweight and cost-effective. Also, silicon is a semiconductor, so it has very low electrical conductivity. However, the silicon particles of the prior art are not suitable for use in electric vehicles and electronic components.
[0007] Si particles are usually obtained by a grinding process. The disadvantage is that such particles have a large surface area and bind large amounts of polymer. This increases the viscosity of the plastic composition very significantly. Only mixtures with a relatively low filler content and low thermal conductivity can be produced. At higher filler contents, the composition becomes very hard and can no longer be dispensed by classical processes, for example with a dispenser. Plastic compositions containing ground silicon particles have also proven to be relatively flammable.
[0008] The use of silicon particles smaller than 30 μm is disadvantageous because such small particles have a relatively low minimum ignition energy, which poses a risk of dust explosion and requires complex and costly safety measures during industrial processing.
[0009] JP 2019-131669 A2 teaches the use of metallic Si particles of 0.1-200 μm with an electrically insulating coating as a thermally conductive filler in silicone-free organic resins. The particles can be produced by a pyrolysis, melting, grinding process or a grinding, grinding process. The particles are provided with an electrically insulating coating in a separate process step. In the example of JP 2019-131669 A2, an organic resin is disclosed that contains up to 65% by volume of ground Si particles with an average particle size of 32 μm and a thermal conductivity of up to 7 W / mK. The use of relatively flammable ground particles is a disadvantage. The disclosed vulcanizates are not elastic and therefore not suitable for use as gap fillers in lithium-ion batteries.
[0010] CN106753140A claims an epoxy resin containing two kinds of spherical silicon particles with particle sizes of 20 μm and 27 μm.
[0011] JP 2013-221124 A2 claims a polyarylene sulfide resin containing silicon particles larger than 1 μm and of any shape and manufacturing method, in this example using irregularly shaped silicon particles of 6 μm and 17 μm.
[0012] US2015307764A (=EP2935432A1) claims a plastic composition that may contain metal silicon particles. The preferred size range is 1-50 μm. The shape is not further specified. In this example, 2.5 μm silicon particles are used. [Prior art documents] [Patent documents]
[0013] [Patent Document 1] JP 2019-131669A2 A [Patent Document 2] Publication No. CN106753140A [Patent Document 3] JP 2013-221124A2 A [Patent Document 4] US2015307764A publication [Patent Document 5] EP2935432A1 publication Summary of the Invention [Problem to be solved by the invention]
[0014] Silicones are not preferred in many applications because they release volatile polydimethylsiloxanes that can reduce the adhesion of parts and coatings.
[0015] It is therefore an object of the present invention to provide a non-silicone-based, and therefore polydimethylsiloxane-free, plastic composition which does not exhibit the above-mentioned drawbacks of the prior art and which combines the properties of low density, low cost and high thermal conductivity. [Means for solving the problem]
[0016] This object is achieved by a thermally conductive plastic composition (Y) according to the invention, which contains relatively large Si particles with an average particle size of 30-200 μm, which are mainly of rounded shape and at the same time show a particularly large / wide particle size distribution. It has now been found by experiments, very surprisingly, that these thermally conductive plastic compositions (Y) according to the invention show a significantly reduced flammability.
[0017] In the context of the present invention, "predominantly rounded" Si particles are to be understood as having a spherical to elliptical shape with a smooth surface. They can also be described as potato-like. FIG. 1 shows, by way of example, the predominantly rounded shape of these Si particles according to the invention. The Si particles of the present invention have a width / length ratio (aspect ratio w / l) of at least 0.76. Non-inventive Si particle shapes with a width / length ratio (aspect ratio w / l) smaller than 0.76 are shown in FIG. 2 as "sputter-like particles", in FIG. 3 as "nodular" particles, and in FIG. 4 as "acute-angled" and "pointed" particles. The skilled person will recognize that there is a wide overlap between the different particle shapes. The metallic Si particles of the present invention have a width / length ratio (aspect ratio w / l) of at least 0.76 and are preferably substantially neither acute nor pointed, preferably neither sputter-like, nodular, acute nor pointed. However, it should be understood that this means that the particles of the present invention described above may contain such particles in the context of impurities without interfering with the effect of the invention.
[0018] The properties of the Si particles according to Figures 1-4 are further shown in the table below. [Table 1]
[0019] The present invention relates to a thermally conductive plastic composition (Y), - 5 to 50% by volume of a plastic composition (S), and - 50 to 95% by volume of at least one thermally conductive filler (Z) having a thermal conductivity of at least 5 W / mK Contains, however, The thermally conductive plastic composition (Y) has a thermal conductivity of at least 0.6 W / mK, and Thermally conductive filler (Z) has the following characteristics: a) the average diameter x50 is within the range of 30 to 200 μm; b) be predominantly rounded, with a width / length ratio (aspect ratio w / l) of at least 0.76; c) The distribution width SPAN ((x90-x10) / x50) is at least 0.28 A thermally conductive plastic composition (Y) is provided in which the metallic silicon particles are present in an amount of at least 20% by volume.
[0020] The plastic composition according to the invention preferably has the following characteristics: d) Contains 1.5% by mass or less of silicon particles smaller than 2 μm Also satisfies.
[0021] In the context of the present invention, the terms "heat-conducting", "thermoconductive" or "thermally conductive" are synonymous.
[0022] In the context of the present invention, the term "thermally conductive filler (Z)" is understood to mean a filler having a thermal conductivity of at least 5 W / mK.
[0023] In the context of the present invention, the term "thermally conductive plastic composition (Y)" is understood to mean a plastic composition having a thermal conductivity significantly higher than that of plastics containing no fillers or additives, generally about 0.2 to 0.3 W / mK, and is characterized in that it has a thermal conductivity of at least 0.6 W / mK.
[0024] In the context of the present invention, all parameters describing particle size (parameter: mean diameter x50), particle size distribution (parameters: standard deviation Sigma and distribution width SPAN) or particle shape (parameters: aspect ratio w / l and sphericity SPHT) relate to a volumetric distribution. The mentioned indices can be measured, for example, by dynamic image analysis according to ISO 13322-2 and ISO 9276-6, for example with the Camsizer X2 device from Retsch Technology.
[0025] Those skilled in the art recognize that standard deviation is not normalized and is a useful characteristic for evaluating the particle size distribution of different samples only when the average particle size of the comparative samples is approximately equal. Therefore, in the context of the present invention, the relative width of the particle size distribution is described using the average particle size x 50 weighted width of the particle size distribution, the dimensionless distribution width SPAN defined as: SPAN = (x90 - x10) / x50. The aspect ratio is used as an index to describe the particle shape. In older prior art, the aspect ratio is often expressed as the ratio of length to width (l / w), which gives a value greater than or equal to 1. In newer literature, e.g. ISO 9276-6, the aspect ratio is calculated as the inverse ratio of width to length (w / l), which gives a value less than or equal to 1. The two indices can be interconverted by forming their reciprocals. In the context of the present invention, the aspect ratio is defined as the ratio of the particle's width to its length (w / l). The particle width is the minimum of all the largest measured chords of the particle projections, x c min The particle length is defined as x, which is the longest Feret diameter of all measured Feret diameters of the particle. Fe max More detailed information can be found, for example, in "Operating Instructions / Manual Particle Size Analysis System CAMSIZER(R)", Retsch Technology GmbH, 42781 Haan; Doc. No. CAMSIZER V0115. The aspect ratio is then calculated according to the following formula: b / l=x c min / xFe max . The sphericity SPHT is calculated from the projected area A of the analyzed particle relative to the area of a circle having the same circumference P as the projected particle according to the following formula (more detailed information can be found, for example, in "Operating Instructions / Manual Particle Size Analysis System CAMSIZER(R)", Retsch Technology GmbH, 42781 Haan; Doc. CAMSIZER V0115): SPHT=4πA / P 2 . The parameter SPHT corresponds to the square of the circularity C according to ISO 9276-6.
[0026] In order to avoid excessive page count in the description of the invention, only preferred embodiments of individual features are specified below. However, the professional reader should expressly understand that such disclosure means that all combinations of different preferred levels are also expressly disclosed and expressly desired. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] (Plastic composition (S)) Suitable plastics include all known classical non-silicone based elastomers, thermoplastic or thermosetting polymers and copolymers, as described in the prior art, for example in Ullmann, Vol. 15, p. 457 ff., Verlag VCH.
[0028] Suitable thermoplastic polymers are, for example, polyolefins, such as polyethylene, polypropylene and polystyrene, polyamides, polyimides, polyesters, polyetheresters, polyphenylene ethers, polyacetals, polybutylene terephthalate (PBT), polyethylene terephthalate (PET), polymethyl methacrylate, polyvinyl acetals, polycarbonates, polyacrylates, acrylonitrile-butadiene-styrene (ABS), acrylonitrile-styrene-acrylic acid esters (ASA), styrene-acrylonitrile (SAN), polycarbonates, polyureas, silane-modified polymers (SMPs), polyurethanes, polyethersulfones and polyetherketones as well as copolymers, mixtures and / or polymer blends thereof, such as, for example, PC / ABS, MABS. Suitable thermosetting polymers are, for example, phenolic resins, thermosetting polyurethanes, melamine resins, polyesters and epoxy resins, acrylic resins.
[0029] Suitable elastomers are, for example, styrene butadiene rubber (SBR), nitrile rubber (NBR), chloroprene rubber (CR), fluororubber (FKM), butadiene rubber (BR), ethylene-propylene-diene rubber (EPDM), silane-modified polymers (SMPs), polyacrylate elastomers, polyurethanes.
[0030] Mixtures and copolymers of different polymers are also suitable. The term copolymer includes variants in which prepolymers or monomers of different chemical structure are polymerized together. Suitable examples include ethylene-vinyl acetate copolymers (EVA, VAE). Mixtures of two or more substances, also called terpolymers, are also suitable.
[0031] Preferred plastics are selected from polyurethanes, polyacrylates, epoxy resins, acrylic resins, polyureas, ethylene-vinyl acetate copolymers (EVA, VAE), silane-modified polymers (SMPs), polyethylene, polypropylene and polystyrene. Particularly preferred plastics are polyurethanes, polyacrylates, epoxy resins, acrylic resins, silane-modified polymers (SMPs).
[0032] The plastic composition (S) of the invention may also contain further additives and additives, which are known to the skilled person and described in the prior art. Examples of further additives are processing aids, stabilizers, flame retardants, fungicides, fragrances, active or inactive fillers, plasticizers, flame retardant agents, agents for influencing electrical properties, dispersants, solvents, pigments, impact modifiers, heat stabilizers, dyes, nesosilicates, adhesion promoters.
[0033] The addition-crosslinkable plastic composition (S) of the invention may contain alkyltrialkoxysiloxanes (F) as further additives to reduce its viscosity. If they are present, they are preferably present in an amount of 0.1 to 8% by weight, more preferably 0.2 to 6% by weight, based on the total weight of the plastic composition (S), where the alkyl groups are saturated or unsaturated, linear or branched, alkyl groups having 2 to 20 carbon atoms, preferably 8 to 18 carbon atoms, and the alkoxy groups may contain 1 to 5 carbon atoms. Examples of alkoxy groups include methoxy, ethoxy, propoxy and butoxy groups, with methoxy and ethoxy groups being particularly preferred. Particularly preferred alkyltrialkoxysiloxanes (F) are n-octyltrimethoxysilane, n-dodecyltrimethoxysilane, n-hexadecyltrimethoxysilane and n-octadecyltrimethoxysilane.
[0034] (Thermal conductive filler (Z)) The thermally conductive plastic composition (Y) of the present invention contains at least one thermally conductive filler (Z) having a thermal conductivity of at least 5 W / mK, provided that the thermally conductive plastic composition (Y) of the present invention contains at least 20 vol. % of metal silicon particles as the thermally conductive filler (Z) that also satisfies at least the further specific characteristics a) to c), and the total amount of the thermally conductive filler (Z) is at least 50 vol. %.
[0035] a) The average diameter x50 of these metal silicon particles (Z) of the present invention is in the range of 30 to 200 μm, preferably in the range of 35 to 180 μm, and more preferably in the range of 40 to 160 μm.
[0036] b) The metallurgical silicon particles (Z) of the present invention are mainly rounded and are preferably produced by a melting process. The mainly rounded shape of the particles according to the present invention is characterized by a width / length ratio (aspect ratio w / l) of at least 0.76, preferably at least 0.77, more preferably at least 0.78, in particular at least 0.79.
[0037] The silicon particles (Z) of the invention have a sphericity SPHT of at least 0.77, preferably at least 0.78, particularly preferably at least 0.79. In a particularly preferred embodiment, the silicon particles (Z) of the invention have an aspect ratio of at least 0.76 and at the same time a sphericity SPHT of at least 0.77, preferably at least 0.78, particularly preferably at least 0.79.
[0038] c) The particle size distribution width (SPAN) is defined as SPAN=(x90-x10) / x50. The SPAN of the metal silicon particles (Z) of the present invention is at least 0.28, preferably at least 0.30, particularly preferably at least 0.35, and particularly preferably at least 0.38. In a preferred embodiment, the SPAN is between 0.40 and 2.5, preferably between 0.41 and 2.2, and particularly preferably between 0.5 and 2.0. It is not important whether a single fraction of silicon particles (Z) whose SPAN is within the range of the present invention is used, or whether two or more fractions of silicon particles are mixed to achieve the particle size distribution width of the present invention according to characteristic c) of the silicon particles (Z) of the present invention. When two or more fractions of silicon particles are mixed, they may be mixed before mixing with one or more components of the composition of the present invention, or the fractions of silicon particles may be mixed separately with one or more components of the composition of the present invention. The order of addition is not important. It is preferred that up to four fractions of silicon particles are mixed to achieve the distribution width of the present invention, it is preferred that up to three fractions of silicon particles are mixed to achieve the distribution width of the present invention, it is particularly preferred that up to two fractions of silicon particles of the present invention are used to achieve the distribution width of the present invention, and it is particularly preferred that only a single silicon powder of the present invention is used.
[0039] In a preferred embodiment, the silicon particles (Z) also satisfy the following characteristic d): d) The silicon particles (Z) of the present invention preferably contain 1.5% by mass or less, preferably 1% by mass or less, particularly preferably 0.5% by mass or less of silicon particles smaller than 2 μm, in each case based on the total amount of the silicon particles (Z). Particularly preferred silicon particles (Z) are substantially free of particle fractions smaller than 2 μm. The term "substantially free" should be understood to mean that the presence of such particles is acceptable in the context of "impurities" of the particles (Z) of the present invention and does not interfere with the effect of the invention.
[0040] The silicon particles (Z) of the present invention preferably comprise a particle fraction having a diameter of less than 20 μm, in each case based on the total amount of silicon particles, of less than 20% by weight, preferably less than 15% by weight, particularly preferably less than 10% by weight.
[0041] The silicon particles (Z) of the invention preferably comprise a particle fraction having a diameter of less than 10 μm, in each case based on the total amount of silicon particles, of less than 15% by weight, preferably less than 10% by weight, particularly preferably less than 5% by weight.
[0042] In a particularly preferred embodiment, no silicon particles having an average diameter of 10 μm or less are intentionally added. It is also preferred that no silicon particles having a particle size of 15 μm or less are added. It is particularly preferred that no silicon particles having an average diameter of 20 μm or less are intentionally added.
[0043] Very fine or crushed silicon particles as employed in the prior art also have the disadvantage that such particles have a relatively large surface area and bind a lot of polymer. This increases the viscosity of the plastic composition very significantly, so that only mixtures with a relatively low filler content and therefore a low thermal conductivity are obtained. At higher filler contents, the composition becomes very hard and can no longer be dispensed by classical processes, for example with a dispenser. Plastic compositions containing crushed silicon particles have also proven to be relatively flammable. The relatively large, substantially rounded silicon particles of the present invention, which simultaneously meet the characteristics a) to c), have the advantage that it makes it possible to obtain plastic compositions of the present invention with a high filler content and high thermal conductivity, which exhibit good processability and relatively low flammability.
[0044] Metallic silicon has some very advantageous properties for use as a thermally conductive filler (Z). For example, the very high thermal conductivity of silicon particles (Z) improves the thermal conductivity of the thermally conductive plastic composition (Y) produced therefrom. The low density of silicon particles (Z) reduces the weight of the composition and the parts produced therefrom, which helps to reduce costs. The low electrical conductivity allows the production of electrically insulating parts and improves the dielectric strength. The low Mohs hardness of silicon particles (Z) reduces wear during processing. Those skilled in the art are aware that if the purity of silicon is reduced, all or part of the aforementioned advantages are lost. The purity of silicon particles (Z) of the present invention, and therefore the silicon content, is at least 80%, preferably at least 90%, particularly preferably at least 95%.
[0045] Those skilled in the art further recognize that under certain conditions, metal silicon particles are flammable, and the dust poses an explosion hazard. Those skilled in the art also recognize that the risk of dust formation, flammability and explosion hazard of metal powders increases significantly with decreasing particle size. This is why very small silicon particles below 30 μm are not suitable for many applications. Due to the low minimum ignition energy, such particles are dangerous to handle and require complex and expensive safety measures during industrial processing. Furthermore, compositions containing very small silicon particles below 30 μm have been found to be relatively flammable.
[0046] Larger silicon particles having an average particle size of more than 30 μm exhibit a relatively high minimum ignition energy and are therefore simpler and safer to handle in industrial processes. Nevertheless, compositions containing non-inventive crushed sharp-edged silicon particles larger than 30 μm have proven to be relatively flammable.
[0047] Silicon particles having an average particle size of more than 200 μm are not suitable for many applications of thermally conductive plastic compositions because such large silicon particles often do not fit into the small gaps that the gap filler is intended to fill, for example. Moreover, even such large silicon particles have been found to be relatively flammable.
[0048] The use of spherical fillers to improve the flowability and processability of filled polymers is well known in the prior art.However, there are only a few documents in the prior art that use spherical silicone particles in thermally conductive plastics.The compositions disclosed only contain very small spherical silicone particles with an average particle size of less than 30 μm, and their shortcomings are as described above.
[0049] It has now been found, quite surprisingly, that the thermally conductive plastic composition (Y) of the present invention has thermal conductivity and at the same time exhibits low flammability when it contains the metal silicon particles of the present invention in a minimum necessary amount so as to simultaneously satisfy characteristics a) to c).
[0050] The plastic composition (Y) of the present invention contains at least 20% by volume, preferably at least 25% by volume, more preferably at least 30% by volume, particularly preferably at least 35% by volume of such metal silicon particles (Z). If the plastic composition (Y) contains a smaller amount of metal silicon particles (Z), the desired beneficial effects of metal silicon, such as low density and high thermal conductivity, are no longer fully evident.
[0051] The prior art discloses various methods for producing finely divided metal particles with a rounded shape. The silicon particles (Z) of the present invention are preferably produced from a molten state, so that they show a relatively smooth surface and are substantially free of breaks, sharp edges and sharp corners. This differs from conventional crushed particles, which are brought to their final shape, for example, by crushing, grinding or milling. It is not important whether the particles are crushed in a cold state in a first step, for example by grinding, and then brought to a molten form by heating above the melting point, for example by heat treatment in a hot zone using plasma, or whether a silicon melt is first produced and then crushed, for example by atomization. It is preferred if the silicon particles of the present invention are brought to the solid particle shape of the present invention by spraying or atomizing a silicon melt and then cooling.
[0052] Suitable methods for producing the silicon particles (Z) of the present invention are known to those skilled in the art and are described, for example, in Chapter 2, 2 of "Pulvermetallurgie: Technologien und Werkstoffe, Schatt, Werner, Wieters, Klaus-Peter, Kieback, Bernd, S. 5-48, ISBN 978-3-540-681112-0, E-Book: https: / / doi.org / 10.1007 / 978-3-540-68112-0_2". Preferred methods for producing the silicon particles (Z) of the present invention are inert gas atomization, also known as gas atomization, pressurized water atomization, also known as liquid atomization or water atomization process, or centrifugal atomization, also known as rotary atomization, melt spinning process. The described method makes it possible to produce silicon metal particles with very different particle size ranges, in particular with average particle sizes ranging from a few micrometers to a few millimeters. Furthermore, the silicon metal particles can be produced with very different particle shapes, for example "sputtered", i.e. very irregular, ellipsoidal, spherical, and with very different particle size distribution widths. It has now been found, quite surprisingly, that exclusively silicon particles which are predominantly rounded and at the same time satisfy characteristics a) to c) of the invention exhibit the advantageous properties of the invention, in particular the relatively low flammability.
[0053] The method for producing the metal silicon particles (Z) of the present invention is preferably carried out so that the particles are obtained in a mainly rounded shape according to the present invention, thus satisfying the characteristics a) to c), and are substantially free of sharp-edged or pointed particles. The method for producing the metal silicon particles (Z) of the present invention is preferably carried out so that the particles are obtained in a mainly rounded shape according to the present invention, thus satisfying the characteristics a) to c), and are substantially free of sputtered, nodular, sharp-edged or pointed particles. The solidified particles can be separated by size by methods commonly used in subsequent steps, such as, for example, classification, sieving, or sifting. These methods make it possible to separate agglomerated or bonded particles, without substantially destroying the particles. The term "substantially rounded / substantially free" should be understood to mean that the presence of such particles is permitted in the context of the "impurities" of the particles (Z) of the present invention and does not interfere with the effect of the invention.
[0054] In addition to these metal silicon particles (Z), the plastic composition (Y) of the present invention may contain further thermally conductive fillers (Z) having a thermal conductivity of more than 5 W / mK. Examples of such further thermally conductive fillers (Z) are magnesium oxide, metallic aluminum powder, metallic silver powder, zinc oxide, boron nitride, silicon carbide, aluminum nitride, aluminum hydroxide, aluminum oxide, graphite, etc. Preferred further fillers are aluminum powder, magnesium oxide, aluminum hydroxide, zinc oxide and aluminum oxide. Particularly preferred further thermally conductive fillers (Z) are zinc oxide, aluminum hydroxide and aluminum oxide. The shape of said further fillers is not limited in principle. The particles may be, for example, spherical, ellipsoidal, needle-like, tubular, flaky, fibrous or irregularly shaped. They are preferably spherical, ellipsoidal or irregularly shaped. The average diameter of said further thermally conductive filler (Z) is preferably in the range of 0.01 to 200 μm, preferably in the range of 0.1 to 150 μm, particularly preferably in the range of 0.2 to 120 μm, in particular in the range of 0.4 to 80 μm.
[0055] Fillers with very high densities are disadvantageous for use in, for example, aircraft or electric vehicles, since they increase the weight of the component very significantly. The further thermally conductive filler (Z) preferably has a density of 6.0 g / cm 3 Less than 4.5 g / cm 3 More preferably, it is 3.0 g / cm or less. 3 It has the following density:
[0056] The plastic composition (Y) of the present invention has a viscosity of 5.0 g / cm 3 It is preferred that the further thermally conductive filler (Z) having a higher density is contained in an amount of up to 24% by weight, preferably up to 20% by weight, particularly preferably up to 16% by weight, particularly preferably up to 12% by weight.
[0057] In many applications, electrical conductivity of the thermally conductive composition is undesirable as it may lead to, for example, short circuits. The plastic composition (Y) of the present invention preferably has a resistivity of at least 1 Ω mm 2 / m.
[0058] A preferred inventive thermally conductive plastic composition (Y) contains the inventive metal silicon particles as the only thermally conductive filler (Z) or in combination with up to three further thermally conductive fillers (Z). Impurities up to 5% are not considered to constitute further fillers (Z).
[0059] The total amount of the thermally conductive filler (Z) in the thermally conductive plastic composition (Y) of the present invention is 50 to 95% by volume, preferably 60 to 90% by volume, and more preferably 65 to 88% by volume. If the amount of the thermally conductive filler (Z) contained in the plastic composition (Y) is small, the thermal conductivity is insufficient, and if the amount of the thermally conductive filler (Z) contained in the plastic composition (Y) is large, the composition (Y) becomes highly viscous or brittle, making it difficult to process.
[0060] The thermally conductive plastics composition (Y) of the present invention exhibits a thermal conductivity of at least 0.6 W / mK, preferably at least 0.8 W / mK, preferably at least 1.2 W / mK, in particular at least 1.5 W / mK.
[0061] The viscosity of the thermally conductive plastic composition (Y) of the invention may vary over a very wide range and can be adapted to the requirements of its application. The adjustment of the viscosity of the thermally conductive plastic composition (Y) of the invention is preferably carried out via the content of the thermally conductive filler (Z) and / or the composition of the plastic composition (S) according to conventional methods from the prior art, which are known to the person skilled in the art. The adjustment of the viscosity is preferably carried out by the selection of the combination of components (S) and (Z) and the optional addition of additives.
[0062] The density of the thermally conductive plastic composition (Y) of the present invention is 4.5 g / cm 3 and preferably less than 4.0 g / cm 3 less than 3.5 g / cm 3 Less than 3.3 g / cm 3 is less than.
[0063] [Production method of thermally conductive plastic composition (Y)] The present invention further provides a method for producing the thermally conductive plastic composition (Y) of the present invention by mixing the individual components. The inventive thermally conductive filler (Z) can be compounded, for example, by compounding through a masterbatch, through a paste, or through direct addition. The inventive composition (S) may optionally be mixed with further additives during compounding of the inventive thermally conductive filler (Z). The aforementioned components may in principle be added in any desired order. The components can be mixed by conventional continuous and batch methods of the prior art. Suitable mixing equipment includes all known equipment. Examples thereof include single or double screw continuous mixers, double rollers, Ross mixers, Hobart mixers, dental mixers, extruders, planetary mixers, kneaders, and Henschel mixers or similar mixers. The preferred processing methods generally depend on the polymeric raw materials used.
[0064] The present invention further provides the use of a thermally conductive filler (Z) for improving the thermal conductivity of a plastic composition (S) selected from non-silicone based elastomeric, thermoplastic, and thermosetting polymers and copolymers.
[0065] The present invention further provides a plastic product obtained by filling or spreading and subsequent crosslinking or curing, said cured plastic product (e.g. a thermally conductive element) exhibiting excellent thermal conductivity and precise film thickness. The hardness of the thermally conductive plastic composition (Y) of the present invention may vary over a very wide range and can be adapted to the requirements of its application. Thus, for example, a relatively soft and flexible product is preferred for use in gap filler applications, whereas a relatively hard and rigid product is preferred for use in thermally conductive adhesive applications. The adjustment of the hardness of the thermally conductive plastic composition (Y) of the present invention generally depends on the polymer raw material used and is carried out according to conventional methods from the prior art. These are known to the person skilled in the art. The plastic article according to the invention exhibits a thermal conductivity of at least 0.6 W / mK, preferably at least 0.8 W / mK, preferably at least 1.2 W / mK, in particular at least 1.5 W / mK.
[0066] The present invention further provides the use of the thermally conductive plastic composition (Y) as a thermally conductive paste, gap filler (=thermally conductive element), thermally conductive pad, thermally conductive adhesive and potting compound for dissipating heat from a heat generating body or a heat sink in an electronic device. The thermally conductive plastic composition (Y) is applied to a heat generating element or a heat sink, or the heat generating element or the heat sink is coated therewith, or the already crosslinked or cured thermally conductive plastic composition (Y) is introduced between the heat generating element or the heat sink, for example in the form of a thermally conductive pad. Suitable heating elements are found, for example, in electronic equipment and electronic devices of electrical power supplies, such as supply transistors, power modules, transistors, thermocouples, temperature sensors; heat-generating electronic components, such as integrated circuit components, such as CPUs, and batteries. In the automotive industry, heating elements are found especially in the vicinity of lithium-ion batteries, charging infrastructure, control devices, and sensors. Suitable heat dissipators consist of heat dissipation components, such as heat distributors, heat sinks, and cooling fins. When the thermally conductive plastic composition (Y) is introduced between the heating element and the heat dissipation element, heat is efficiently conducted from the heating element to the heat dissipation element. This allows the heating element to be effectively cooled. The thermally conductive plastic composition (Y) of the present invention is particularly suitable for use, for example, as a gap filler in the lithium-ion batteries of electric vehicles, and as a potting compound for electronic components of electric vehicles.
[0067] <Measurement method> <Measurement of thermal conductivity lambda> Thermal conductivity is measured according to ASTM D5470-12 using a TIM Tester (Steinbeis Transferzentrum Waermemanagement in der Elektronik, Lindenstr. 13 / 1, 72141 Wadorf-Heslach, Germany). The thermal resistance of a sample placed between two test cylinders is measured by constant heat flow. The film thickness of the sample is used to calculate the effective thermal conductivity of the sample. For the measurement, the sample is applied using a stencil and the measuring cylinder is manually brought to a thickness of 1.9-2.0 mm and excess material is removed. The thermal conductivity measurements are made with a constant gap of 1.8-1.6-1.4-1.2-1.0 mm. The evaluation is made by an integrated reporting unit. After validity tests (linear coefficient of determination >0.998), the thermal conductivity lambda is reported as effective thermal conductivity W / (m*K).
[0068] <Analysis of particle size and shape> The particle size (mean diameter x50), particle size distribution (parameters: standard deviation sigma and distribution width SPAN) and particle shape (parameters: aspect ratio w / l and sphericity SPHT) were analyzed using a Camsize X2 (measurement principle: dynamic image analysis) from Retsch Technology in accordance with ISO 13322-2 and ISO 9276-6 (analysis type: dry measurement of powders and granules; measurement range: 0.8 μm to 30 mm; compressed air dispersion with X-Jet, dispersion pressure = 0.3 bar). The evaluation was performed using the following formula: c min This was done on a volumetric basis based on the model. EXAMPLES
[0069] The following examples are intended to illustrate in principle how the invention can be put into practice, but are not intended to limit the above-described invention to the disclosure therein.
[0070] In the following examples, all amounts reported in parts and percentages are by weight unless otherwise indicated. Unless otherwise indicated, the following examples are carried out at normal pressure, i.e., about 1000 hPa, at room temperature, i.e., about 20° C., or at a temperature established by combining the reactants at room temperature without further heating or cooling.
[0071] <Summary of the silicon powders and silicon powder mixtures used according to the present invention and non-invention> Table 1 summarizes the properties of the inventive and non-inventive silicon powders used in this example. Inventive Example 1 uses silicon powder according to the invention, which is obtained by inert gas atomization and therefore has a predominantly rounded and relatively broad particle size distribution according to the invention. The non-inventive comparative example C1 uses a non-inventive silicon powder obtained by inert gas atomization and therefore has a mainly rounded, but relatively narrow, non-inventive particle size distribution and does not satisfy feature c) of the invention. The non-inventive comparative example C2 uses a non-inventive silicon powder which has a relatively broad, inventive particle size distribution, but which is obtained by a milling process and is therefore substantially sharp and angular, not satisfying feature b) of the invention.
[0072] <abbreviation> Example C Comparative example PS particle shape r Mainly rounded a. Angular I. The present invention NI Non-invention nd Not measured
[0073] Table 1: Overview of silicon powders used [Table 2]
[0074] <General manufacturing procedure 1 (GP1) of one-component curing type thermally conductive silicon powder-containing plastic moldings (invention example 2 and non-invention examples C3 to C5)> [Step 1: Preparation of one-component curable thermally conductive silicone powder-containing plastic composition] The one-component curable heat-conductive plastic composition and silicon powder were mixed for 25 seconds at 2350 rpm using a SpeedMixer DAC 400 FVZ (Hauschild & Co KG, Waterkamp 1, 59075 Hamm, Germany). The silicon particle-containing plastic composition was stirred with a spatula to mix in the remaining silicon powder from the edge of the container. The mixture was then homogenized for another 25 seconds at 2350 rpm using the SpeedMixer and cooled to room temperature. The raw materials and amounts charged are shown in Table 2. A pasty mass was obtained. [Step 2: Manufacturing of plastic molded products containing hardened thermally conductive silicon powder] The curing of the silicon powder-containing plastic composition from step 1 was carried out according to the manufacturer's specifications and according to the specific curing conditions of the plastic composition used, as shown in Table 2.
[0075] <General manufacturing procedure 2 (GP2) of two-component plastic composition containing thermally conductive silicon powder (inventive example 3 and non-inventive examples C6 to C8)> [Step 1: Production of two-component thermally conductive silicon powder-containing plastic composition] The A and B components of the two-component plastic composition were mixed separately with the silicon powder using a SpeedMixer DAC 400 FVZ (Hauschild & Co KG, Waterkamp 1, 59075 Hamm, Germany) at a speed of 2350 rpm for 25 seconds. The plastic compositions containing silicon particles were each stirred with a spatula so that the remaining silicon powder from the edge of the container was mixed in. The mixtures were then homogenized using the SpeedMixer at 2350 rpm for another 25 seconds and cooled to room temperature. The raw materials and amounts charged are shown in Table 3. A paste-like mass of each was obtained. [Step 2: Production of cross-linked thermally conductive silicon powder-containing plastic molded products] The silicon powder-containing A and B components prepared in step 1 were mixed and homogenized using a SpeedMixer at 2350 rpm for 25 seconds. The two-component silicon powder-containing plastic composition was cured according to the specific curing conditions of the plastic composition used according to the manufacturer's specifications. The conditions used are shown in Table 3.
[0076] <Example 4: Flammability test> Flammability testing is performed using a simplified test based on UL 94 HB. The inventive plastic compositions according to examples 2 and 3, as well as the non-inventive plastic compositions according to comparative examples C3 to C6, are applied in a 2 mm thick layer to an aluminium plate 150 mm long, 10 mm wide and 2 mm thick and cured according to the details in Tables 2 and 3. The plate is fixed with the right long side vertical, with the aluminium substrate facing downwards and the knife-coated sample facing upwards. The burner is adjusted so that a blue flame is formed with a length of 325 mm. The flame is directed horizontally to the specimen, with the tip of the blue flame pointing towards the front of the specimen 20 mm away from the left edge of the specimen. The flame is removed after 30 seconds of irradiation. Flammability Test and Evaluation: During the flame application, the flame pattern and glowing flame height are measured. The afterflame time (total time consisting of afterburn and afterglow) of the test specimen is recorded.
[0077] Table 2: Composition and flammability of one-component plastic compositions containing silicon powder [Table 3]
[0078] The non-inventive comparative test C3 contained 64.6 vol.-% of non-inventive crushed silicon particles according to comparative test C2, which in particular did not satisfy characteristic b), resulting in a plastic composition with a very high viscosity which could not be applied in a uniform layer and therefore could not be tested.
[0079] Table 3: Composition and flammability of two-component plastic compositions containing silicon powder [Table 4]
[0080] The non-inventive comparative test C6 contained 73.4 vol.-% of non-inventive crushed silicon particles according to comparative example C2, which in particular did not satisfy characteristic b), resulting in a plastic composition with a very high viscosity which could not be applied in a uniform layer and therefore could not be tested.
[0081] It surprisingly becomes clear that the inventive plastic compositions according to examples 2 and 3, which simultaneously fulfill the characteristics a) to c), exhibit a comparatively low flammability.
[0082] Example 5: Preparation of a thermally conductive plastic composition containing an in-situ mixture of silicon powder (present invention) A thermally conductive plastic composition according to the invention was prepared according to general procedure GP1, where 46.0 g of Soudal "Transpacryl" (transparent acrylic) was used as the plastic composition, and the following silicon powders were added separately and mixed to form the in-situ silicon powder mixture of the invention: 18.4 g of non-inventive silicon powder with x50 of 68.6 μm, SPAN of 0.20, w / l of 0.85, and SPHT of 0.84, 3 g of non-inventive silicon powder from comparative example C2, 1 g of non-inventive silicon powder from comparative example C3, 1 g of non-inventive silicon powder from comparative example C4, 1 g of non-inventive silicon powder from comparative example C5, 1 g of non-inventive silicon powder from comparative example C6, 1 g of non-inventive silicon powder from comparative example C7, 1 g of non-inventive silicon powder from comparative example C8, 1 g of non-inventive silicon powder from comparative example C9, 1 g of non-inventive silicon powder from comparative example C1, 1 g of non-inventive silicon powder from comparative example C1, 1 g of non-inventive silicon powder from comparative example C2, 1 g of non-inventive silicon powder from comparative example C1, 1 g of non-inventive silicon powder from comparative example C2, 1 g of non-inventive silicon powder from comparative example C3, 1 g of non-inventive silicon powder from comparative example C4, 1 g of non-inventive silicon powder from comparative example C5, 1 g of non-inventive silicon powder from comparative example C6, 1 g of non-inventive silicon powder from comparative example C7, 1 g of non-inventive silicon powder from comparative example C8, 1 g of non-inventive silicon powder from comparative example C9, 1 g of non-inventive silicon powder from comparative example C1, 1 g of non-inventive silicon powder from comparative example C1, 1 g of non- 6.8g, 73.6g of non-invention silicon powder having a x50 of 105.4 μm, a SPAN of 0.24, a w / l of 0.83, and a SPHT of 0.92, 36.8g of non-invention silicon powder having a x50 of 133.8 μm, a SPAN of 0.25, a w / l of 0.82, and a SPHT of 0.94, and 18.4g of non-invention silicon powder having a x50 of 162.1 μm, a SPAN of 0.22, a w / l of 0.82, and a SPHT of 0.94. This resulted in a plastic composition according to the invention, containing 64.6% by volume of silicon particles according to the invention. The pasty mass according to the invention has good processability. The flammability test according to Example 4 resulted in a medium flame pattern, with a flame height of 9 cm and an afterflame time of 10 seconds, thus indicating a significantly weaker flammability than the comparative examples C3 to C5, which used the same plastic composition as a reference.
Claims
1. A thermally conductive plastic composition (Y), - 5 to 50% by volume of a non-silicone-based plastic composition (S), and - 50 to 95% by volume of at least one thermally conductive filler (Z) having a thermal conductivity of at least 5 W / mK Contains, however, The thermally conductive plastic composition (Y) has a thermal conductivity of at least 0.6 W / mK, and The thermally conductive filler (Z) has the following characteristics: a) average diameter x50 is in the range of 30 to 200 μm; b) being predominantly rounded with a width / length ratio (aspect ratio w / l) of at least 0.76; c) The distribution width SPAN ((x90-x10) / x50) is at least 0.28 A thermally conductive plastic composition (Y) in which at least 20% by volume of metal silicon particles satisfying the above formula are present.
2. 2. The thermally conductive plastic composition (Y) according to claim 1, wherein said plastic composition (S) is selected from non-silicone based elastomers, thermoplastic and thermosetting polymers, and copolymers.
3. The plastic composition (S) the group consisting of thermoplastic polymers: polyethylene, polypropylene and polystyrene, polyamides, polyimides, polyesters, polyetheresters, polyphenylene ethers, polyacetals, polybutylene terephthalate (PBT), polyethylene terephthalate (PET), polymethyl methacrylate, polyvinyl acetals, polycarbonates, polyacrylates, acrylonitrile-butadiene-styrene (ABS), acrylonitrile-styrene-acrylates (ASA), styrene-acrylonitrile (SAN), polycarbonates, polyureas, silane-modified polymers (SMPs), polyurethanes, polyethersulfones and polyetherketones, as well as their copolymers, mixtures and / or polymer blends; - the group consisting of thermosetting polymers: phenolic resins, thermosetting polyurethanes, melamine resins, polyesters, epoxy resins, acrylic resins, from the group consisting of elastomers: styrene-butadiene rubber (SBR), nitrile rubber (NBR), chloroprene rubber (CR), fluororubber (FKM), butadiene rubber (BR), ethylene-propylene-diene rubber (EPDM), silane-modified polymers (SMPs), polyacrylate elastomers, polyurethanes, - mixtures thereof and prepolymers or copolymers of the abovementioned polymers in which the monomers are polymerized with one another; The thermally conductive plastic composition (Y) according to claim 1 or 2, selected from the group consisting of
4. The thermally conductive plastic composition (Y) according to claim 1 or 2, wherein the plastic composition (S) is selected from polyurethanes, polyacrylates, epoxy resins, acrylic resins, polyureas, ethylene-vinyl acetate copolymers (EVA, VAE), silane-modified polymers (SMPs), polyethylene, polypropylene and polystyrene, and mixtures and copolymers thereof.
5. 3. The thermally conductive plastic composition (Y) according to claim 1 or 2, wherein the plastic composition (S) is selected from polyurethanes, polyacrylates, epoxy resins, acrylic resins and silane-modified polymers (SMPs) and mixtures and copolymers thereof.
6. The thermally conductive plastic composition (Y) according to any one of claims 1 to 5, wherein the plastic composition (S) contains at least 25% by volume of metal silicon particles as the thermally conductive filler (Z).
7. The metal silicon particles present as thermally conductive filler (Z) are provided with the following additional conditions: d) Contains 1.5% by mass or less of silicon particles smaller than 2 μm The thermally conductive plastic composition (Y) according to any one of claims 1 to 6, which also satisfies the above requirements.
8. The thermally conductive plastic composition (Y) according to any one of claims 1 to 7, wherein the metallic silicon particles present as thermally conductive filler (Z) are produced from the molten state.
9. The thermally conductive plastic composition (Y) according to any one of claims 1 to 8, wherein the metallic silicon particles present as the thermally conductive filler (Z) are brought into solid particle form from a silicon melt by spraying or atomization.
10. A method for producing the thermally conductive plastic composition (Y) according to any one of claims 1 to 9 by mixing the individual components.
11. 2. Use of said thermally conductive filler (Z) to improve the thermal conductivity of a plastic composition (S) according to claim 1, selected from non-silicone based elastomers, thermoplastic and thermosetting polymers and copolymers.
12. A plastic product obtained by filling or applying the thermally conductive plastic composition (Y) according to any one of claims 1 to 9, and then crosslinking or curing the same.
13. Use of the thermally conductive plastic composition (Y) according to any one of claims 1 to 9 as a thermally conductive paste, gap filler (= thermally conductive element), thermally conductive pad, thermally conductive adhesive and potting compound for heat dissipation from heat generating or heat dissipating bodies in electronic devices.
Citation Information
Patent Citations
Filler for sealing resin and its production
JP1992008757A
Thermally conductive silicone rubber composition and its molded item
JP2000063670A
Housing made of resin
JP2011063707A
Resin composition and insulation heat conductive sheet
JP2019131669A
Epoxy adhesive for motor of electric vehicle and preparation method of epoxy adhesive
CN106753140A
Cited By
Thermal conductive paste containing silicon
JP2025522509A