Lithium secondary battery
A non-aqueous electrolyte with specific additives stabilizes the SEI film in lithium secondary batteries with high nickel content, addressing thermal instability and degradation issues, enhancing performance under high temperatures and rapid charging conditions.
Patent Information
- Application Number
- JP2024526703
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-11
- Filing Date
- 2022-11-02
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-11-02
AI Technical Summary
Lithium secondary batteries with high nickel content face issues of poor thermal stability, high cost, and rapid degradation due to intense electrolyte decomposition and unstable solid electrolyte interphase (SEI) films, particularly with silicon-based negative electrodes.
Incorporation of a non-aqueous electrolyte containing specific additives, such as LiSO3R and a heterocyclic group, forms a stable organic/inorganic composite SEI film, preventing electrolyte decomposition and enhancing the stability of both positive and negative electrodes.
The solution improves high-temperature life characteristics and rapid charging performance by stabilizing the SEI film, reducing resistance and volume changes, and maintaining capacity retention.
Smart Images

Figure 2024540733000001 
Figure 2024540733000002 
Figure 2024540733000003
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0154694, filed with the Korean Intellectual Property Office on November 11, 2021, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a lithium secondary battery that includes an electrolyte containing a particular combination of additives and a high nickel positive electrode material. [Background technology]
[0003] Lithium secondary batteries are generally manufactured by forming an electrode assembly by interposing a separator between a positive electrode including a positive electrode active material made of a lithium-containing transition metal oxide and a negative electrode including a negative electrode active material capable of storing lithium ions, inserting the electrode assembly into a battery case, injecting a non-aqueous electrolyte solution that serves as a medium for transmitting lithium ions, and then sealing the battery case.
[0004] Lithium secondary batteries can be miniaturized and have high energy density and operating voltage, so they are used in a variety of fields such as mobile devices, electronic products, and electric vehicles. In particular, low-cost, high-energy positive electrode materials are essential for use in medium- to large-sized devices such as electric vehicles and power storage systems, but LiCoO2, which has a high operating voltage and excellent capacity characteristics, has the disadvantages of poor thermal stability and high cost.
[0005] Therefore, nickel-cobalt-manganese-based lithium transition metal composite oxides (hereinafter simply referred to as "NCM-based lithium transition metal composite oxides") are mainly used as a positive electrode material that can replace LiCoO2, and NCM-based lithium transition metal composite oxides have the advantages of being relatively inexpensive and having high reversible capacity. However, when the nickel content in NCM-based lithium transition metal composite oxides is increased to achieve high capacity, the surface stability decreases and the electrolyte decomposition reaction becomes more intense, which causes problems such as an increase in battery resistance and a decrease in life characteristics.
[0006] Therefore, there is a need to develop a method that can improve such problems. Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention is intended to solve the above problems, and aims to improve the high-temperature life characteristics of lithium secondary batteries containing NCM-based positive electrode active materials by introducing a nonaqueous electrolyte containing a combination of two specific additives.
[0008] Another object of the present invention is to provide a lithium secondary battery with improved rapid charging performance by using the nonaqueous electrolyte to effectively solve the problem of decomposition of the SEI film of a lithium secondary battery containing a silicon-based negative electrode material. [Means for solving the problem]
[0009] According to one embodiment, the present invention comprises: A non-aqueous electrolyte solution including a lithium salt, an organic solvent, a first additive represented by the following chemical formula 1, and a second additive represented by the following chemical formula 2; A positive electrode including a positive electrode active material including a lithium composite transition metal oxide including nickel, cobalt, and manganese; a negative electrode including a negative electrode active material; and a separator interposed between the positive electrode and the negative electrode.
[0010] [Chemical formula 1] LiSO3R
[0011] In the above Chemical Formula 1, R is an alkyl group having 1 to 10 carbon atoms which may or may not be substituted with fluorine; [ka] In the above Chemical Formula 2, A is a heterocyclic group having 3 to 5 carbon atoms or a heteroaryl group having 3 to 5 carbon atoms, R1 is an alkylene group having 1 to 3 carbon atoms. Effect of the Invention
[0012] The lithium secondary battery according to the present invention contains a nonaqueous electrolyte solution including a specific combination of additives, and thus can improve the life characteristics and rapid charging performance of a lithium secondary battery including an NCM-based positive electrode active material and / or a Si-based negative electrode active material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present invention will now be described in more detail.
[0014] In general, anions contained in lithium salts such as LiPF6, which are widely used in electrolytes for lithium secondary batteries, form decomposition products such as hydrogen fluoride (HF) and PF5 due to thermal decomposition or moisture. Such decomposition products have acid properties and deteriorate the coating or electrode surface in the battery.
[0015] Due to the decomposition products of the electrolyte and the structural changes of the positive electrode caused by repeated charging and discharging, the transition metals in the positive electrode are easily dissolved into the electrolyte, and the dissolved transition metals are further redeposited on the positive electrode, increasing the resistance of the positive electrode. Furthermore, if the dissolved transition metals move to the negative electrode through the electrolyte, they are electrodeposited on the negative electrode, causing destruction of the solid electrolyte interphase (SEI) film and further electrolyte decomposition reactions, which causes problems such as increased consumption of lithium ions and resistance.
[0016] In addition, during initial activation of the battery, a protective coating is formed on the positive and negative electrodes due to electrolyte reaction. If the coating becomes unstable for the reasons described above, further decomposition of the electrolyte will occur during charging / discharging or exposure to high temperatures, accelerating battery degradation and generating gas.
[0017] In particular, a battery including a positive electrode active material with a high nickel content has improved initial capacity characteristics, but when repeatedly charged and discharged, side reactions can increase the amount of lithium by-products and gas generated, and the decomposition reaction of the electrolyte can become more severe.
[0018] In order to solve this problem, the present inventors have found that a first additive represented by the following Chemical Formula 1 and a second additive represented by the following Chemical Formula 2 are added to a non-aqueous electrolyte solution, which has the effect of forming an organic / inorganic composite SEI coating on the electrode, thereby maintaining the film in a more stable form and preventing the decomposition reaction of the electrolyte solution from becoming violent.
[0019] Each component of the present invention will be described in more detail below.
[0020] non-aqueous electrolyte The lithium secondary battery according to the present invention includes a non-aqueous electrolyte solution including a lithium salt, an organic solvent, a first additive represented by the following Chemical Formula 1, and a second additive represented by the following Chemical Formula 2.
[0021] Each component of the nonaqueous electrolyte will be specifically described below.
[0022] (1) First additive and second additive The non-aqueous electrolyte of the present invention contains a first additive represented by the following chemical formula 1.
[0023] [Chemical formula 1] LiSO3R
[0024] In the above Chemical Formula 1, R is an alkyl group having 1 to 10 carbon atoms which may or may not be substituted with fluorine.
[0025] In one embodiment of the present invention, R in Formula 1 is C n F 2n+1and n may be any one of integers from 1 to 5, and may be preferably 1 or 4. That is, the first additive may be LiSO3CF3 or LiSO3C4F9.
[0026] The first additive contains lithium ions, SO3 and C in its structure. n F 2n+1 Since SO3 contains C, it has the effect of forming a stable SEI film that is favorable for the transfer of lithium ions. Specifically, SO3 has a low bond energy with lithium ions, so lithium ions are easily decoupled, and C n F 2n+1 contributes to the formation of a coating of the LiF component.
[0027] In one embodiment of the present invention, the content of the first additive may be 0.1 wt% to 5 wt%, preferably 0.5 wt% to 3 wt%, based on the total weight of the nonaqueous electrolyte. Considering the solubility of the solvent and the viscosity of the electrolyte after the additive is added, the content of the first additive is preferably 5 wt% or less.
[0028] Specifically, the first additive is LiSO3C n F 2n+1 When n is an integer of 3 or less, the content of the first additive is preferably 2 wt % to 4 wt % based on the total weight of the non-aqueous electrolyte, and when n is an integer of 4 or more, the content of the first additive is preferably 0.1 wt % to 1 wt % based on the total weight of the non-aqueous electrolyte. Since the solubility differs depending on n, the optimal content range differs.
[0029] The non-aqueous electrolyte of the present invention further contains a second additive represented by the following chemical formula 2.
[0030] [ka]
[0031] In the above Chemical Formula 2, A is a heterocyclic group having 3 to 5 carbon atoms or a heteroaryl group having 3 to 5 carbon atoms, R1 is an alkylene group having 1 to 3 carbon atoms.
[0032] Since the second additive represented by the formula 2 contains a propargyl functional group, the functional group is reduced and decomposed to form an SEI film with high passivity on the surface of the negative electrode, thereby improving the high-temperature durability of the negative electrode itself and preventing electrodeposition of transition metals on the surface of the negative electrode. In addition, the propargyl group is adsorbed on the surface of metallic impurities contained in the positive electrode, making it difficult for the impurities to be dissolved, thereby preventing internal short circuits that may occur when dissolved metal ions are deposited on the negative electrode. In addition, the first additive binds to PF5, a decomposition product of the electrolyte, and suppresses the generation of HF, thereby preventing the destruction of the CEI (cathode electrolyte interphase) film formed on the surface of the positive electrode by the first additive and suppressing further decomposition of the electrolyte.
[0033] That is, when the nonaqueous electrolyte of the present invention is used, the first additive forms a coating of inorganic LiF, LiSO3F components, and the propargyl functional group in the second additive forms a stable organic component coating that can entirely cover the surface of the negative electrode active material. In particular, when a silicon-based negative electrode material is used, the phenomenon of an unstable SEI coating being formed is intensified, but when the electrolyte of the present invention is applied, a more stable organic / inorganic composite coating is formed, so that the decomposition reaction of the electrolyte that becomes intensified when a positive electrode material with a high nickel content is used can be suppressed, and thus the deterioration of the negative electrode can be effectively prevented.
[0034] In one embodiment of the present invention, A in the above chemical formula 2 may be a nitrogen-containing heteroaryl group having 3 to 5 carbon atoms, and may be preferably represented by the following chemical formula 2-1.
[0035] [ka]
[0036] In the above Chemical Formula 2-1, R1 is as defined in Chemical Formula 2 above.
[0037] In one embodiment of the present invention, R1 in Chemical Formula 2 may be a linear or branched alkylene group having 1 to 3 carbon atoms, preferably a linear alkylene group having 1 to 3 carbon atoms, and more preferably a methylene group.
[0038] In one embodiment of the present invention, the second additive may be represented by the following formula 2A:
[0039] [ka]
[0040] In one embodiment of the present invention, the content of the second additive may be 0.01 wt% to 2 wt%, preferably 0.05 wt% to 1 wt%, more preferably 0.1 wt% to 0.5 wt%, based on the total weight of the nonaqueous electrolyte. It is preferable that the content of the second additive is 2 wt% or less in terms of reducing the initial resistance.
[0041] (2) The third and fourth additives In one embodiment of the present invention, the non-aqueous electrolyte may further include one or more third additives selected from vinylene carbonate (VC) and vinyl ethylene carbonate (VEC). In this case, when the second additive is reductively decomposed at the negative electrode, a propargyl radical attacks the VC or VEC double bond, which makes it easy for a polymerization reaction to occur, so that when an organic coating is formed on the negative electrode, the surface of the active material can be covered more quickly and effectively.
[0042] In one embodiment of the present invention, the content of the third additive may be 0.01 wt% to 3 wt%, preferably 0.05 wt% to 2 wt%, more preferably 0.1 wt% to 1 wt%, based on the total weight of the nonaqueous electrolyte. It is preferable that the content of the second additive is 3 wt% or less in terms of reducing the initial resistance.
[0043] In addition, the nonaqueous electrolyte of the present invention may further include the following additive as a fourth additive, if necessary, in order to prevent the electrolyte from being decomposed in a high voltage environment, causing the collapse of the electrodes, or to further improve the effects of low-temperature high-rate discharge characteristics, high-temperature stability, overcharge prevention, and suppression of battery expansion at high temperatures.
[0044] The fourth additive may be at least one selected from halogen-substituted carbonate compounds, sultone compounds, sulfate compounds, phosphate or phosphite compounds, nitrile compounds, amine compounds, silane compounds, benzene compounds, and lithium salt compounds.
[0045] The halogen-substituted carbonate compound may be fluoroethylene carbonate (FEC).
[0046] The sultone-based compound is a material capable of forming a stable SEI film on the surface of the negative electrode through a reduction reaction, and may be one or more compounds selected from 1,3-propane sultone (PS), 1,4-butane sultone, ethene sultone, 1,3-propene sultone (PRS), 1,4-butene sultone, and 1-methyl-1,3-propene sultone, and specifically, may be 1,3-propane sultone (PS).
[0047] The sulfate-based compound is a material that can be electrically decomposed on the surface of the negative electrode to form a stable SEI film that does not crack even when stored at high temperatures, and may be at least one selected from ethylene sulfate (Esa), trimethylene sulfate (TMS), and methyl trimethylene sulfate (MTMS).
[0048] The phosphate or phosphite compound may be one or more selected from lithium difluoro(bisoxalato)phosphate, lithium difluorophosphate, tris(trimethylsilyl)phosphate, tris(trimethylsilyl)phosphite, tris(2,2,2-trifluoroethyl)phosphate, and tris(trifluoroethyl)phosphite.
[0049] The nitrile compound may be one or more selected from succinonitrile (SN), adiponitrile (ADN), acetonitrile, propionitrile, butyronitrile, valeronitrile, caprylonitrile, heptanenitrile, cyclopentanecarbonitrile, cyclohexanecarbonitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, phenylacetonitrile, 2-fluorophenylacetonitrile, 4-fluorophenylacetonitrile, ethylene glycol bis(2-cyanoethyl)ether (ASA3), 1,3,6-hexanetricarbonitrile (HTCN), 1,4-dicyano-2-butene (DCB), and 1,2,3-tris(2-cyanoethyl)propane (TCEP).
[0050] The amine compound may be one or more selected from triethanolamine and ethylenediamine, and the silane compound may be tetravinylsilane.
[0051] The benzene-based compound may be one or more selected from monofluorobenzene, difluorobenzene, trifluorobenzene, and tetrafluorobenzene.
[0052] The lithium salt-based compound is a compound different from the lithium salt contained in the nonaqueous electrolyte, and may be one or more compounds selected from lithium difluorophosphate (LiDFP; LiPO2F2), lithium bis(oxalato)borate (LiBOB; LiB(C2O4)2), lithium tetrafluoroborate (LiBF4), lithium tetraphenylborate, and lithium difluoro(bis(oxalato)phosphate)phosphate (LiDFOP).
[0053] Meanwhile, the content of the fourth additive may be 0.1 wt % to 5 wt % based on the total weight of the non-aqueous electrolyte solution. When the content of the additive is within the above range, a side reaction suppressing effect due to the formation of a coating on the positive electrode and the negative electrode can be obtained.
[0054] (3) Organic Solvent The nonaqueous electrolyte of the present invention contains an organic solvent.
[0055] As the organic solvent, various organic solvents that are generally used in lithium electrolytes can be used without limitation.For example, the organic solvent may be a cyclic carbonate solvent, a linear carbonate solvent, a linear ester solvent, a cyclic ester solvent, a nitrile solvent, or a mixture thereof, and preferably may include a mixture of a cyclic carbonate solvent and a linear carbonate solvent.
[0056] The cyclic carbonate solvent is a high-viscosity organic solvent that has a high dielectric constant and therefore easily dissociates the lithium salt in the electrolyte. The cyclic carbonate solvent may be one or more selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, and vinylene carbonate, and may preferably contain ethylene carbonate (EC).
[0057] The linear carbonate solvent is an organic solvent having low viscosity and low dielectric constant, and may be one or more selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methyl propyl carbonate, and ethyl propyl carbonate, and may preferably contain ethyl methyl carbonate (EMC).
[0058] In order to produce an electrolyte solution having high ionic conductivity, it is preferable to use a mixture of a cyclic carbonate solvent and a linear carbonate solvent as the organic solvent.
[0059] The linear ester solvent may be one or more selected from methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, and butyl propionate, and may be preferably methyl propionate, ethyl propionate, or propyl propionate.
[0060] The cyclic ester solvent may be one or more selected from γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone.
[0061] The nitrile solvent may be one or more selected from succinonitrile, acetonitrile, propionitrile, butyronitrile, valeronitrile, caprylonitrile, heptanenitrile, cyclopentanecarbonitrile, cyclohexanecarbonitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, phenylacetonitrile, 2-fluorophenylacetonitrile, and 4-fluorophenylacetonitrile, and may be preferably succinonitrile.
[0062] In the total weight of the nonaqueous electrolyte, the remainder excluding the organic solvent, such as the compound represented by Formula 1, the additive, and the lithium salt, is the organic solvent unless otherwise specified.
[0063] (4) Lithium salt The non-aqueous electrolyte of the present invention contains a lithium salt.
[0064] The lithium salt may be any one that is commonly used in electrolytes for lithium secondary batteries, and may be used without limitation. Specifically, the lithium salt may have a cation of Li + and as an anion, F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , B 10 Cl 10 - , AlCl4 - , AlO4 - , PF6 - , CF3SO3 - , CH3CO2 - , CF3CO2 - , AsF6 - , SbF6 - , CH3SO3 - , (CF3CF2SO2)2N - , (CF3SO2)2N - , (FSO2)2N- , BF2C2O4 - , BC4O8 - , BF2C2O4CHF - , PF4C2O4 - , PF2C4O8 - , PO2F2 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , C4F9SO3 - , CF3CF2SO3 - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , CF3(CF2)7SO3 - , and SCN - may include any one or more selected from the following:
[0065] Specifically, the lithium salt may be LiPF6, LiClO4, LiBF4, LiN(FSO2)2 (LiFSI), LiTFSI, lithium bis(pentafluoroethanesulfonyl)imide (LiBETI), LiSO3CF3, LiPO2F2, lithium bis(oxalate)borate (LiBOB), lithium difluoro(oxalate)borate (LiFOB), lithium difluoro(bisoxalato)phosphate (LiDFOP), lithium tetrafluoro(oxalate)phosphate (LiTFOP), and lithium fluoromalonato(difluoro)borate (LiTFOP). borate, LiFMDFB), and preferably LiPF6.
[0066] In one embodiment of the present invention, the concentration of the lithium salt in the non-aqueous organic solution containing the lithium salt and the organic solvent may be 0.5 M to 4.0 M, specifically 0.5 M to 3.0 M, more specifically 0.8 M to 2.0 M. When the concentration of the lithium salt is within the above range, the effects of improving low-temperature output and cycle characteristics are sufficiently ensured, while the viscosity and surface tension are prevented from becoming excessively high, and appropriate electrolyte impregnation is obtained.
[0067] positive electrode The lithium secondary battery according to the present invention includes a positive electrode that includes a positive electrode active material that includes a lithium composite transition metal oxide that includes nickel, cobalt, and manganese.
[0068] Specifically, the lithium transition metal composite oxide may contain nickel in an amount of 70 mol % or more, preferably 80 mol % or more, and more preferably 85 mol % or more, based on the total number of moles of transition metals.
[0069] Lithium composite transition metal oxides containing nickel, cobalt, and manganese have an unstable structure that causes accelerated chemical / electrochemical reactions at the interface between the electrode and electrolyte, so the components of the electrolyte are important in improving this.
[0070] In particular, high-nickel (High-Ni) positive electrode active materials are prone to structural collapse at high voltages, and in the process, reactive oxygen species are generated along with cracks in the active material particles. This reactive oxygen species reacts with the electrolyte, causing the electrolyte to decompose intensified.
[0071] As described above, the lithium secondary battery according to the present invention can improve this by controlling the decomposition reaction of the electrolyte solution occurring at the interface with the electrode by using a nonaqueous electrolyte solution containing the first additive and the second additive.
[0072] In one embodiment of the present invention, the lithium composite transition metal oxide may be represented by the following Chemical Formula 3.
[0073] [Chemical Formula 3] Li 1+x (Ni a Co b Mn c M d )O2
[0074] In Chemical Formula 3, M is one or more selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo, x, a, b, c, and d are respectively -0.2 ≦ x ≦ 0.2, 0.70 ≦ a < 1, 0 < b ≦ 0.25, 0 < c ≦ 0.25, 0 ≦ d ≦ 0.1, and a + b + c + d = 1.
[0075] Preferably, a, b, c, and d in Chemical Formula 3 may be respectively 0.80 ≦ a < 1, 0 < b ≦ 0.15, 0 < c ≦ 0.15, and 0 ≦ d ≦ 0.05, and more preferably 0.85 ≦ a ≦ 0.95, 0.025 ≦ b ≦ 0.1, 0.025 ≦ c ≦ 0.1, and 0 ≦ d ≦ 0.05.
[0076] In one embodiment of the present invention, M in Chemical Formula 3 may be Al, which is advantageous in terms of stability in this case.
[0077] The positive electrode according to the present invention can be manufactured by coating a positive electrode slurry containing a positive electrode active material, a binder, a conductive material, a solvent, etc. on a positive electrode current collector and then drying and rolling.
[0078] The positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity. For example, stainless steel; aluminum; nickel; titanium; baked carbon; or aluminum or stainless steel whose surface has been surface-treated with carbon, nickel, titanium, silver, or the like may be used.
[0079] The positive electrode active material may be included in an amount of 80% by weight to 99% by weight, specifically 90% by weight to 99% by weight, based on the total weight of the solid content in the positive electrode slurry. In this case, if the content of the positive electrode active material is 80% by weight or less, the energy density may be reduced, and the capacity may be reduced.
[0080] The binder is a component that assists in binding the active material and conductive material, etc., and binding to the current collector, and may be added in an amount of 1% by weight to 30% by weight based on the total weight of the solid content in the positive electrode slurry. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber, fluororubber, or various copolymers thereof.
[0081] The conductive material is a substance that imparts conductivity to the battery without causing any chemical change, and may be added in an amount of 0.5% by weight to 20% by weight based on the total weight of the solid content in the positive electrode slurry.
[0082] Examples of the conductive material include carbon blacks such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; graphite powders such as natural graphite, artificial graphite, carbon nanotubes, and graphite; conductive fibers such as carbon fibers and metal fibers; conductive powders such as carbon fluoride powder, aluminum powder, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives; or combinations thereof.
[0083] The solvent for the positive electrode slurry may contain an organic solvent such as NMP (N-methyl-2-pyrrolidone), and may be used in an amount that provides a suitable viscosity when containing the positive electrode active material, binder, conductive material, etc. For example, the positive electrode slurry containing the positive electrode active material, binder, and conductive material may be contained so that the solid content concentration is 40% by weight to 90% by weight, preferably 50% by weight to 80% by weight.
[0084] negative electrode The lithium secondary battery according to the present invention includes a negative electrode including a negative electrode active material, and the negative electrode can be manufactured by coating a negative electrode current collector with a negative electrode slurry including a negative electrode active material, a binder, a conductive material, a solvent, and the like, followed by drying and rolling.
[0085] The negative electrode current collector generally has a thickness of 3 μm to 500 μm. Such a negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has high conductivity. For example, copper; stainless steel; aluminum; nickel; titanium; fired carbon; a surface-treated product with carbon, nickel, titanium, silver, etc. on the surface of copper or stainless steel; or an aluminum-cadmium alloy, etc. may be used. Also, similar to the positive electrode current collector, the binding force of the negative electrode active material may be strengthened by forming fine irregularities on the surface, and it may be used in various forms such as a film, sheet, foil, net, porous body, foam, non-woven fabric body, etc.
[0086] In one embodiment of the present invention, the negative electrode active material may contain a silicon-based material.
[0087] The silicon-based material is one or more selected from Si, SiO x (0 < x < 2), and Si-Y alloys (wherein Y is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements, and combinations thereof, and is not Si), preferably Si. The element Y may be selected from the group consisting of Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db (dubnium), Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof. Si has the advantage of having a higher theoretical capacity compared to SiO x There is an advantage of having a higher theoretical capacity compared to.
[0088] The silicon-based negative electrode active material has a capacity nearly about 10 times higher than that of graphite, so the mass loading (mg·cm -2) and improve the rapid charging performance of the battery. However, there is a problem that the lithium ion loss rate due to irreversible reactions is high and the volume change is large, which may adversely affect the lifespan, but by applying the above-mentioned nonaqueous electrolyte, such problems can be solved. Specifically, a negative electrode containing a silicon-based negative electrode active material, particularly a negative electrode containing 100% Si, has a problem that the SEI film is easily cracked due to a large volume change during charging and discharging compared to a negative electrode containing a carbon-based negative electrode active material, and further, a regeneration reaction occurs continuously. However, when the nonaqueous electrolyte according to the present invention is applied, the SEI film can be strengthened as described above, and such problems can be effectively solved.
[0089] In one embodiment of the present invention, the silicon-based material may be contained in an amount of 70% by weight to 100% by weight, preferably 80% by weight to 100% by weight, based on the total weight of the negative electrode active material, and more preferably, the negative electrode active material may be made of a silicon-based material. When the silicon-based material is contained in the above range, the effects of increasing the negative electrode capacity and improving the quick charging performance can be obtained.
[0090] In a preferred embodiment, the negative electrode active material may be composed only of Si, that is, pure silicon (Pure Si).
[0091] In addition to the silicon-based material, the negative electrode active material may include at least one selected from the group consisting of a carbon material capable of reversibly intercalating / deintercalating lithium ions; a metal or an alloy of such a metal and lithium; a metal composite oxide; a material capable of doping and dedoping lithium; lithium metal; and a transition metal oxide.
[0092] As the carbon material capable of reversibly intercalating / deintercalating the lithium ions, any carbon-based negative electrode active material generally used in lithium ion secondary batteries can be used without particular limitation. Representative examples thereof include crystalline carbon, amorphous carbon, or a combination of these. Examples of the crystalline carbon include graphite such as amorphous, plate-like, flaky, spherical, or fibrous natural graphite or artificial graphite. Examples of the amorphous carbon include soft carbon (low-temperature calcined carbon), hard carbon, mesophase pitch carbide, calcined coke, and the like.
[0093] As the metal or an alloy of these metals and lithium, a metal selected from the group consisting of Cu, Ni, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn, or an alloy of these metals and lithium can be used.
[0094] Examples of the metal composite oxide include PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, Bi2O5, Li x Fe2O3 (0 ≦ x ≦ 1), Li x WO2 (0 ≦ x ≦ 1), and Sn x Me 1-x Me’ y O z (Me: Mn, Fe, Pb, Ge; Me’: Al, B, P, Si, elements of Group 1, Group 2, Group 3 of the periodic table, halogen; 0 < x ≦ 1; 1 ≦ y ≦ 3; 1 ≦ z ≦ 8), one or more selected from the group can be used.
[0095] The material capable of doping and dedoping lithium includes Sn, SnO2, Sn-Y' (wherein Y is an element selected from the group consisting of alkali metals, alkaline earth metals, group 13 elements, group 14 elements, transition metals, rare earth elements, and combinations thereof, and is not Sn), etc. The element Y' may be selected from the group consisting of Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db (dubnium), Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Si, In, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.
[0096] Examples of the transition metal oxide include lithium-containing titanium oxide (LTO), vanadium oxide, and lithium vanadium oxide.
[0097] The negative electrode active material may be included in an amount of 60% by weight to 99% by weight based on the total weight of solids in the negative electrode slurry.
[0098] The binder is a component that assists in bonding between the conductive material, the active material, and the current collector, and may be added in an amount of 1% by weight to 30% by weight based on the total weight of the solid content in the negative electrode slurry. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber, fluororubber, and various copolymers thereof.
[0099] The conductive material is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 0.5% by weight to 20% by weight based on the total weight of the solid content in the negative electrode slurry. Such a conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and may be, for example, carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, or thermal black; graphite powder such as natural graphite, artificial graphite, carbon nanotube, or graphite with a highly developed crystal structure; conductive fiber such as carbon fiber or metal fiber; conductive powder such as carbon fluoride powder, aluminum powder, or nickel powder; conductive whisker such as zinc oxide or potassium titanate; conductive metal oxide such as titanium oxide; conductive material such as polyphenylene derivative; or a combination thereof.
[0100] The solvent for the negative electrode slurry may include water or an organic solvent such as NMP or alcohol, and may be used in an amount that provides a suitable viscosity when containing the negative electrode active material, binder, conductive material, etc. For example, the solvent may be included so that the concentration of solids in the slurry containing the negative electrode active material, binder, and conductive material is 30% by weight to 80% by weight, preferably 40% by weight to 70% by weight.
[0101] Separator The lithium secondary battery according to the present invention includes a separator between the positive electrode and the negative electrode.
[0102] The separator separates the negative electrode and the positive electrode and provides a path for lithium ion migration. Any separator that is typically used as a separator in a lithium secondary battery can be used without any particular limitation. In particular, a separator that has low resistance to the migration of ions in the electrolyte and has excellent electrolyte impregnation ability and safety is preferred.
[0103] Specifically, the separator may be a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, or an ethylene / methacrylate copolymer; or a laminated structure of two or more layers thereof. In addition, a normal porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, or the like, may be used. In order to ensure heat resistance or mechanical strength, a coated separator containing a ceramic component or a polymeric substance may be used, and may be used as a single layer or a multilayer structure.
[0104] The lithium secondary battery according to the present invention as described above can be usefully used in portable devices such as mobile phones, notebook computers, and digital cameras; and electric vehicles such as hybrid electric vehicles (HEVs).
[0105] According to another embodiment of the present invention, there is provided a battery module including the lithium secondary battery as a unit cell, and a battery pack including the same.
[0106] The battery module or battery pack can be used as a power source for one or more medium- to large-sized devices, including power tools; electric vehicles, including electric vehicles (EVs), hybrid electric vehicles, and plug-in hybrid electric vehicles (PHEVs); and power storage systems.
[0107] The external shape of the lithium secondary battery of the present invention is not particularly limited, and may be a cylindrical shape using a can, a square shape, a pouch shape, a coin shape, or the like.
[0108] The lithium secondary battery according to the present invention can be used not only as a battery cell used as a power source for small devices, but also suitably as a unit battery in a medium- to large-sized battery module containing a large number of battery cells.
[0109] The present invention will now be described in more detail with reference to specific examples.
[0110] <Example> Example 1. (Production of non-aqueous electrolyte) Ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 30:70, and LiPF6 was dissolved therein to a concentration of 1.0 M to prepare a non-aqueous organic solution. 0.5 wt% LiSO3CF3, 0.3 wt% of the compound represented by Formula 2A, 0.5 wt% vinylene carbonate (VC), and the remaining non-aqueous organic solution were mixed to prepare a 100 wt% non-aqueous electrolyte.
[0111] (Manufacture of lithium secondary batteries) N-methyl-2-pyrrolidone (NMP) with LiNi as the positive electrode active material 0.86 Co 0.05 Mn 0.07 Al 0.02 A positive electrode slurry (solid content: 60 wt%) was prepared by adding O2, a conductive material (carbon black), and a binder (polyvinylidene fluoride) in a weight ratio of 97.6:0.8:1.6. The positive electrode slurry was applied to a 13.5 μm thick aluminum (Al) thin film as a positive electrode current collector, dried, and then roll pressed to prepare a positive electrode.
[0112] Anode active material (Si 100wt%), conductive material (Super-C), and binder (styrene-butadiene rubber) were mixed in a weight ratio of 70:20:10 to water as a solvent to prepare anode slurry (solid content: 60wt%). The anode slurry was applied to a copper (Cu) thin film as an anode current collector with a thickness of 6μm, dried, and then roll pressed to prepare an anode.
[0113] The positive electrode, a polyolefin-based porous separator coated with inorganic particles (Al2O3), and a negative electrode were sequentially stacked to prepare an electrode assembly.
[0114] The electrode assembly thus assembled was placed in a pouch-shaped battery case, and the non-aqueous electrolyte thus prepared was poured into the case to prepare a lithium secondary battery.
[0115] Example 2. A lithium secondary battery was manufactured in the same manner as in Example 1, except that the content of LiSO3CF3 was changed to 3 wt % during the preparation of the non-aqueous electrolyte.
[0116] Example 3. A lithium secondary battery was produced in the same manner as in Example 1, except that LiSO3C4F9 was used instead of LiSO3CF3 when producing the non-aqueous electrolyte.
[0117] Example 4. A lithium secondary battery was produced in the same manner as in Example 2, except that LiSO3C4F9 was used instead of LiSO3CF3 when producing the non-aqueous electrolyte.
[0118] Comparative Example 1 When manufacturing the non-aqueous electrolyte, LiSO3CF3 is not added, and LiNi is used as the positive electrode active material. 0.86 Co 0.05 Mn 0.07 Al 0.02 A lithium secondary battery was produced in the same manner as in Example 1, except that LiCoO2 was used instead of O2.
[0119] Comparative Example 2 A lithium secondary battery was produced in the same manner as in Example 1, except that LiSO3CF3 was not added during the production of the non-aqueous electrolyte.
[0120] Comparative Example 3. A lithium secondary battery was manufactured in the same manner as in Example 1, except that the compound represented by Formula 2A was not added during the preparation of the non-aqueous electrolyte solution.
[0121] Comparative Example 4. A lithium secondary battery was manufactured in the same manner as in Example 3, except that the compound represented by Formula 2A was not added during the preparation of the non-aqueous electrolyte.
[0122] <Experimental Example> Experimental example 1: Evaluation of life characteristics at high temperature (45℃) Each of the lithium secondary batteries manufactured in the examples and comparative examples was activated at 0.1 C CC and then degassed.
[0123] After that, the battery was charged at 0.33C CC to 3.6V under constant current-constant voltage (CC-CV) charging conditions at 25°C, then a 0.05C current cut was performed, and the battery was discharged at 0.33C CC to 2.5V under CC conditions. Next, the battery was charged at 0.33C CC to 3.6V under constant current-constant voltage (CC-CV) charging conditions at 45°C, then a 0.05C current cut was performed, and the battery was discharged at 0.33C CC to 2.5V.
[0124] The above charge / discharge cycle was counted as one cycle. While charging / discharging was performed at a high temperature (45° C.), the discharge capacity and resistance were measured after one cycle and after 300 cycles using a charger / discharger (5 V, 6 A).
[0125] The measured discharge capacity and resistance were substituted into the following formulas 1 and 2, respectively, to calculate the capacity retention and the resistance increase rate. The results are shown in Table 1 below.
[0126] The volume increase rate was calculated by substituting the volumes measured by the buoyancy method after 1 cycle and after 300 cycles into the following formula 3.
[0127] [Formula 1] Capacity retention rate (%) = (discharge capacity after 300 cycles / discharge capacity after 1 cycle) x 100
[0128] [Formula 2] Resistance increase rate (%) = {(resistance after 300 cycles - resistance after 1 cycle) / resistance after 1 cycle} x 100
[0129] [Formula 3] Volume increase rate (%) = {(volume after 300 cycles - volume after 1 cycle) / volume after 1 cycle} x 100
[0130] [Table 1]
[0131] From the results in Table 1, it can be seen that the batteries of Examples 1 to 4 using an electrolyte containing both the first additive represented by Chemical Formula 1 and the second additive represented by Chemical Formula 2 have a capacity retention rate of 95% or more, a resistance increase rate and a volume increase rate of 5% or less at high temperatures, and exhibit very excellent performance, despite containing a high nickel positive electrode active material and a Si negative electrode. In contrast, it can be seen that the batteries of Comparative Examples 1 and 2 using an electrolyte containing no first additive, and the batteries of Comparative Examples 3 and 4 using an electrolyte containing no second additive, all have significantly lower capacity retention rates, resistance increase rates, and volume increase rates than the batteries of Examples 1 to 4.
[0132] That is, when both the first additive and the second additive are contained, it is found that there is a significant effect in improving the high temperature performance of the lithium secondary battery.
[0133] Experimental example 2: Evaluation of quick charging performance For each of the lithium secondary batteries manufactured in the Examples and Comparative Examples, a lithium secondary battery was prepared with a SOC (State Of Charge) of 8%, and then charged at 25° C. while changing the C-rate according to the SOC state as shown in Table 2 below. The voltage value was checked at 1-second intervals for each charging section to measure the voltage profile.
[0134] [Table 2]
[0135] Then, the end condition was set at the voltage value obtained for each section, and the charge amount when charging in CC mode was recorded. Then, further, in CC mode, the battery was discharged at 0.5C to SOC 8%. The above charge and discharge was defined as one cycle, and after 300 cycles were performed, the capacity retention rate, resistance increase rate, and volume increase rate were calculated in the same manner as in Experimental Example 1, and are shown in Table 3 below.
[0136] [Table 3]
[0137] From the results of Table 3, it can be seen that the batteries of Examples 1 to 4 using an electrolyte solution containing both the first additive represented by Chemical Formula 1 and the second additive represented by Chemical Formula 2 have superior performance under rapid charge and discharge conditions compared to the batteries of Comparative Examples 1 to 4, despite containing a high nickel positive electrode active material and a Si negative electrode.
[0138] In contrast, the batteries of Comparative Examples 1 and 2, which used an electrolyte solution not containing the first additive, and the batteries of Comparative Examples 3 and 4, which used an electrolyte solution not containing the second additive, were found to have significantly lower capacity retention rates, resistance increase rates, and volume increase rates than the batteries of Examples 1 to 4.
[0139] From this, it was confirmed that the effect of the present invention can be achieved only when both the first additive and the second additive are contained.
Claims
1. A non-aqueous electrolyte solution including a lithium salt, an organic solvent, a first additive represented by the following chemical formula 1, and a second additive represented by the following chemical formula 2: A positive electrode including a positive electrode active material including a lithium composite transition metal oxide including nickel, cobalt, and manganese; a negative electrode including a negative electrode active material; A lithium secondary battery comprising: [Chemical formula 1] LiSO 3 R (In the above Chemical Formula 1, R is an alkyl group having 1 to 10 carbon atoms which may or may not be substituted with fluorine; 【Chemistry 1】 In the above Chemical Formula 2, A is a heterocyclic group having 3 to 5 carbon atoms or a heteroaryl group having 3 to 5 carbon atoms, R1 is an alkylene group having 1 to 3 carbon atoms.
2. R in Formula 1 is C n F 2n+1 2. The lithium secondary battery according to claim 1, wherein n is an integer of 1 to 5.
3. 2. The lithium secondary battery according to claim 1, wherein A in the formula 2 is a nitrogen-containing heterocyclic group having 3 to 5 carbon atoms or a nitrogen-containing heteroaryl group having 3 to 5 carbon atoms.
4. 2. The lithium secondary battery according to claim 1, wherein the non-aqueous electrolyte further comprises one or more third additives selected from vinylene carbonate and vinyl ethylene carbonate.
5. 2. The lithium secondary battery of claim 1, wherein the content of the first additive is 0.1% by weight to 5% by weight based on the total weight of the non-aqueous electrolyte.
6. 2. The lithium secondary battery of claim 1, wherein the content of the second additive is 0.01% by weight to 2% by weight based on the total weight of the non-aqueous electrolyte.
7. 2. The lithium secondary battery according to claim 1, wherein the organic solvent comprises a mixture of a cyclic carbonate solvent and a linear carbonate solvent.
8. 2. The lithium secondary battery according to claim 1, wherein the lithium composite transition metal oxide contains 70 mol % or more of nickel based on the total number of moles of the transition metals.
9. The lithium secondary battery according to claim 1 , wherein the lithium composite transition metal oxide is represented by the following Chemical Formula 3: [Chemical formula 3] Li 1+x (N a Co b Mn c M d )O 2 (In the above Chemical Formula 3, M is at least one selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; x, a, b, c, and d are -0.2≦x≦0.2, 0.70≦a<1, 0<b≦0.25, 0<c≦0.25, 0≦d≦0.1, and a+b+c+d=1, respectively.
10. 10. The lithium secondary battery according to claim 9, wherein a, b, c, and d in the formula 3 are in the ranges 0.80≦a<1, 0<b≦0.15, 0<c≦0.15, and 0≦d≦0.05, respectively.
11. The lithium secondary battery according to claim 1 , wherein the negative electrode active material comprises a silicon-based material.
Citation Information
Patent Citations
Rechargeable lithium battery
US20160079626A1
Electrolyte for lithium secondary battery, and lithium secondary battery comprising same
WO2020175907A1