Perovskite-Crystalline Silicon Stacked Cell with Nanostructured Carrier Transport Layer for Resistance Enhancement

The nanostructured carrier transport layer in perovskite-crystalline silicon stacked solar cells addresses the issue of uneven perovskite thin films by using resistance-enhancing nanostructures, enhancing carrier transport and light confinement, thus improving energy conversion efficiency.

JP2024541143AInactive Publication Date: 2024-11-07LONGI GREEN ENERGY TECH CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024529743
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-18
Filing Date
2022-05-23
Publication Date
2024-11-07
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The challenge in manufacturing perovskite-crystalline silicon stacked solar cells is the difficulty in achieving a uniformly thick and controllable perovskite thin film on textured crystalline silicon surfaces, leading to inefficiencies due to discontinuous films or excessive thickness, which causes short-circuiting and carrier recombination, limiting the energy conversion efficiency.

Method used

A perovskite-crystalline silicon stacked battery with a nanostructured carrier transport layer that includes a first carrier transport layer with integrally formed resistance-enhancing nanostructures, allowing for uniform perovskite thin film coverage and enhanced carrier transport, using methods like vapor phase or electroplating to fabricate the nanostructures.

Benefits of technology

This design results in improved energy conversion efficiency by ensuring uniform perovskite thickness and preserving the textured light-trapping structure, allowing for flexible bandgap adjustment and enhanced carrier collection and conduction, thereby increasing the overall efficiency of the solar cell.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541143000001_ABST
    Figure 2024541143000001_ABST
Patent Text Reader

Abstract

The present application provides a perovskite-crystalline silicon stacked cell including a crystalline silicon cell, a serial structure layer, a first carrier transport layer, a perovskite light absorbing layer, a second carrier transport layer, and an upper transparent electrode layer, which are sequentially stacked, wherein the first carrier transport layer includes a base layer of the carrier transport layer and a resistance enhancing nanostructure integrally formed with the base layer of the carrier transport layer, which is discretely distributed on the base layer of the carrier transport layer, and the resistance enhancing nanostructure extends from the base layer of the carrier transport layer into the perovskite light absorbing layer. The perovskite-crystalline silicon stacked cell of the present application can enhance the carrier collection and conduction capabilities of the carrier transport material and greatly improve the energy conversion efficiency of the perovskite-crystalline silicon stacked cell. In addition, the light trapping effect of the perovskite-crystalline silicon stacked solar cell can be enhanced, and the cell conversion efficiency can be further improved. The perovskite components can be flexibly adjusted, and the energy conversion efficiency can be greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to the technical field of solar cells, and in particular to perovskite-crystalline silicon stacked cells having a nanostructured carrier transport layer for enhanced resistance.

[0002] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims priority to a Chinese patent application, application number 202111370294.3, entitled "Perovskite-Crystalline Silicon Stacked Battery with Nanostructured Carrier Transport Layer for Resistance Enhancement," filed with the China Patent Office on November 18, 2021, all of which are incorporated herein by reference. [Background technology]

[0003] The maximum energy conversion efficiency of single-junction crystalline silicon cells is currently 26.7%, approaching the theoretical upper limit of 29.4%, with very limited room for efficiency improvement. Perovskite cells, as the new solar cells that have attracted the most attention in recent decades, have improved in efficiency from the initial 3.8% to the current 25.5%, and have great potential for future applications. The theoretical upper limit of perovskite cells is also around 30%, with very limited room for efficiency improvement.

[0004] However, by utilizing the band gap difference between perovskite (~1.4-1.8eV) and crystalline silicon (1.14eV) materials to construct a perovskite-crystalline silicon stacked solar cell, a more efficient solar cell can be obtained. According to theoretical calculations, the efficiency of a perovskite-crystalline silicon stacked cell can reach 40% or more, but the conversion efficiency currently achieved in the laboratory is only 29.5%, leaving much room for improvement.

[0005] At present, perovskite batteries are mainly manufactured using solution methods. The solution method has many advantages, such as low cost, simple manufacturing, and easy adjustment of perovskite components and band gap, and has become a manufacturing method for various high-efficiency perovskite batteries. However, when manufacturing perovskite-crystalline silicon stacked batteries, the surface of the high-efficiency crystalline silicon battery has a textured light trapping structure, but it is difficult to obtain a high-quality perovskite absorption layer with uniform thickness on the crystalline silicon texture using the solution method.

[0006] As shown in Figure 1, in the figure, 1 is a crystalline silicon cell, and 4 is a perovskite thin film produced by solution method. When using solution method to produce perovskite thin film on textured crystalline silicon, if the amount of solution added is small, as shown in Figure 1a), the thin film will be too thin, and the tops of some textured pyramids cannot be covered by the perovskite thin film, so the thin film will be discontinuous and the upper layer of the cell will be prone to short circuit. If the amount of solution applied is increased so that the tips of the pyramids are covered by the thin film, the perovskite thin film in the pyramid bottom region will be too thick, as shown in Figure 1b). If the absorption layer is too thick, the transition distance of the photogenerated carriers will be too long, which will affect the cell efficiency.

[0007] In addition, the size of the textured pyramids in currently commercially available crystalline silicon cells is usually 1 to 5 microns, and the thickness of the absorber layer in high-efficiency perovskite cells is usually less than 1 micron. If the absorber layer is too thick, the recombination of photogenerated carriers becomes intense, resulting in a decrease in cell efficiency. Therefore, even in the case of Figure 1a), where the tips of some pyramids are not covered with the absorber layer, the thickness of the absorber layer in most of the pyramid bottom regions exceeds 1 micron, which causes intense carrier recombination, and this is also one of the important causes that limit the efficiency improvement of perovskite-crystalline silicon stacked cells.

[0008] Therefore, the fabrication of a complete coverage, uniform and controllable thickness perovskite thin film on textured crystalline silicon cells by solution coating method, thereby significantly improving the energy conversion efficiency of perovskite-crystalline silicon stacked solar cells, is currently an important technical problem that needs to be urgently solved. Summary of the Invention

[0009] Regarding the problems existing in the prior art, the present application provides a perovskite-crystalline silicon stacked battery having a nanostructured carrier transport layer for enhanced resistance. Specifically, the present application relates to the following aspects:

[0010] A perovskite-crystalline silicon stacked cell, the perovskite-crystalline silicon stacked cell including a crystalline silicon cell, a series structure layer, a first carrier transport layer, a perovskite light absorbing layer, a second carrier transport layer, and an upper transparent electrode layer, which are sequentially stacked, the first carrier transport layer including a base layer of the carrier transport layer and a resistance enhancing nanostructure formed integrally with the base layer of the carrier transport layer and discretely distributed on the base layer of the carrier transport layer, the resistance enhancing nanostructure extending from the base layer of the carrier transport layer into the perovskite light absorbing layer.

[0011] Optionally, a surface of the first carrier transport layer facing the perovskite light absorbing layer has a textured structure.

[0012] Optionally, each of said resistance-enhancing nanostructures is a fibrous structure, a rod-like structure, or a nanotube structure.

[0013] Optionally, the resistance-enhancing nanostructures have a length of between 50 and 1500 nm.

[0014] Optionally, the resistance-enhancing nanostructures have a diameter of between 100 and 1000 nm.

[0015] Optionally, the coverage of the resistance enhancing nanostructures on the surface of the base layer of the carrier transport layer is 5-70%, preferably 10-60%.

[0016] Optionally, the base layer of the carrier transport layer has a thickness of 10 to 200 nm.

[0017] Optionally, the first carrier transport layer is one selected from TiO2, SnO2, ZnO, or one selected from PEDOT, PEDOT:PSS, P3HT, P3OHT, P3ODDT, PTAA, NiO.

[0018] Optionally, the perovskite light-absorbing layer covers the first carrier transport layer and fills within voids of the resistance-enhancing nanostructures of the first carrier transport layer.

[0019] Optionally, the series structure layer is a conductive material layer or a tunnel junction layer.

[0020] The present application further provides a method for producing the above-mentioned perovskite-crystalline silicon stacked battery, the method comprising: forming a series structure layer on one surface of a crystalline silicon cell; fabricating a first carrier transport layer on a surface of the series structure layer opposite the crystalline silicon cell; applying a perovskite light absorbing layer to a surface of the first carrier transport layer opposite to the series structure layer; forming a second carrier transport layer on a surface of the perovskite light absorbing layer opposite the first carrier transport layer; forming an upper transparent electrode layer on a surface of the second carrier transport layer opposite the perovskite light absorbing layer; The step of manufacturing a first carrier transport layer includes manufacturing a base layer of a carrier transport layer, and manufacturing discretely distributed resistance enhancing nanostructures on the base layer of the carrier transport layer, the nanostructures being integrally formed with the base layer of the carrier transport layer.

[0021] Optionally, said first carrier transport layer is achieved by a one-step conformal manufacturing process or a two-step conformal manufacturing process.

[0022] Optionally, the first carrier transport layer is fabricated by a vapor phase method or an electroplating method.

[0023] The present application provides a perovskite-crystalline silicon stacked battery having a nanostructured carrier transport layer for enhancing resistance, which is used in the upper layer of the perovskite-crystalline silicon stacked battery, and can enhance the carrier collection and conduction ability of the carrier transport material as the carrier transport layer, and can allow the perovskite precursor solution to form a thin film with a uniform thickness and completely covering the textured pyramid structure of the crystalline silicon battery (based on the capillary effect of the nanostructure), so that the perovskite thickness at the top and bottom of the pyramid is almost the same, avoiding the problem that the absorption layer at the bottom of the pyramid is too thick and the top of the pyramid is difficult to completely cover, and thus greatly improving the energy conversion efficiency of the perovskite-crystalline silicon stacked battery. In addition, the light trapping effect of the perovskite-crystalline silicon stacked solar cell can be enhanced, and the cell conversion efficiency can be further improved. The perovskite components can be flexibly adjusted, and the energy conversion efficiency can be greatly improved.

[0024] The above has outlined the technical solutions of the present application. In order to make the technical solutions of the present disclosure more clearly understood and implemented based on the contents of the specification, and to make the above and other objectives, features and advantages of the present disclosure more comprehensible, specific embodiments of the present disclosure are given below. [Brief description of the drawings]

[0025] In order to more clearly describe the technical solutions in the embodiments of the present disclosure or related technologies, the following briefly describes the drawings used in the description of the embodiments or related technologies. Of course, the drawings described below are part of the embodiments of the present disclosure, and those skilled in the art may come up with other drawings based on these drawings without any creative effort. The drawings are provided to facilitate a better understanding of the present application and are not intended to unduly limit the present application. [Figure 1] FIG. 1 is a structural schematic diagram of a perovskite-crystalline silicon stacked battery in the prior art. [Diagram 2] FIG. 1 is a structural schematic diagram of the perovskite-crystalline silicon stacked battery of the present application. [Diagram 3] 3A and 3B are schematic diagrams showing the application of a perovskite thin film by a solution method to the surface of a carrier transport layer having (FIG. 3A) / not having (FIG. 3B) a nanostructure for enhancing resistance. [Figure 4] FIG. 2 is a schematic diagram of the resistance enhancing nanostructure of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] In order to make the objectives, technical solutions and advantages of the embodiments of the present disclosure clearer, the following will clearly and completely describe the technical solutions in the embodiments of the present disclosure with reference to the drawings in the embodiments of the present disclosure, and it should be understood that the described embodiments are only a part of the embodiments of the present disclosure, and are not all of the embodiments. Based on the embodiments in the present disclosure, all other embodiments obtained by those skilled in the art without requiring creative efforts all belong to the scope of protection of the present disclosure.

[0027] Unless otherwise defined, technical and scientific terms in this specification have the same meaning as commonly understood by those skilled in the art. Methods and materials similar or equivalent to those described herein can be used in experimental or practical applications, but the methods and materials are described below. In case of conflict, the present specification, including definitions, will prevail. In addition, the materials, methods, and examples are merely illustrative and are not intended to be limiting. The present application will be further described below with specific examples, but the scope of the present application is not limited thereto.

[0028] Regarding the problems existing in the prior art, the present application provides a perovskite-crystalline silicon stacked battery having a nano-structured carrier transport layer for enhancing resistance. Specifically, the structure of the perovskite-crystalline silicon stacked battery is as shown in Figure 2, which includes a crystalline silicon cell 1, a serial structure layer 2, a first carrier transport layer 31, a perovskite light absorbing layer 32, a second carrier transport layer 33, and an upper transparent electrode layer 34, which are stacked in sequence. Among them, the crystalline silicon cell 1 is the lower cell, and the first carrier transport layer 31, the perovskite light absorbing layer 32, the second carrier transport layer 33, and the upper transparent electrode layer 34 together constitute the upper cell.

[0029] The type of the crystalline silicon cell 1 can be a monocrystalline silicon, polycrystalline silicon solar cell, the doping type of its substrate silicon material is not limited, it can be a front PN junction or back PN junction structure, and it can be a single-sided or double-sided structure. The crystalline silicon cell 1 can be manufactured by methods known in the art, or it can be a commercialized crystalline silicon cell, such as a P-PERC monocrystalline silicon cell, a HIT cell, a Topcon cell, etc.

[0030] In a specific embodiment, the surface of the crystalline silicon cell 1 facing the serially structured layer 2 has a pyramidal texture, i.e., the crystalline silicon cell 1 has the structure shown in Fig. 1, and the surface facing the serially structured layer 2 has pyramidal structures arranged in series.

[0031] The series structure layer 2 is located between the crystalline silicon cell 1 and the first carrier transport layer 31, and is used to connect the upper cell and the lower cell in series. The series structure layer 2 can be a conductive material layer, a tunnel junction layer, or other series structure layer. Here, the conductive material can be a transparent conductive semiconductor material such as indium tin oxide (ITO) or aluminum doped zinc oxide (AZO), or can be a metal material, a mixed material of multiple metals, etc. The conductive material can be a complete layer, or a structure with openings or grooves filled with conductive material.

[0032] 2 and 4, the structure of the first carrier transport layer 31 includes a base layer 311 of the carrier transport layer and a resistance enhancing nanostructure 312 formed integrally with the base layer of the carrier transport layer, which is discretely distributed on the base layer 311 of the carrier transport layer, and the resistance enhancing nanostructure 312 extends from the base layer 311 of the carrier transport layer into the perovskite light absorbing layer 32. The integral formation means that the base layer 311 of the carrier transport layer and the resistance enhancing nanostructure 312 are formed integrally and seamlessly connected, and the resistance enhancing nanostructure 312 is an end structure of the base layer 311 of the carrier transport layer.

[0033] The integrated structure of the resistance enhancing nanostructure and the base layer of the carrier transport layer can reduce unnecessary interface resistance, and the resistance enhancing nanostructure can fix the perovskite light absorbing layer and penetrate deep into the perovskite light absorbing layer as a terminal structure for carrier transport, thereby further enhancing carrier transport. The resistance enhancing nanostructure can also produce a light trapping effect. Furthermore, when the surface of the first carrier transport layer facing the perovskite light absorbing layer has a textured structure, the light trapping effect can be further enhanced.

[0034] Here, the first carrier transport layer 31 may be an organic polymer material or a metal oxide material. If it is an organic polymer, it can be manufactured using a one-step conformal manufacturing method, and if it is a metal oxide material, it can be manufactured using a two-step conformal manufacturing method.

[0035] The first carrier transport layer 31 may be made of an electron transport material or a hole transport material. Here, the electron transport material may be TiO2, SnO2, ZnO, BBL:PEI (poly(benzoimidazobenzophenanthroline)-polyethyleneimine), etc. The hole transport material may be PEDOT, PEDOT:PSS, P3HT, P3OHT, P3ODDT, PTAA, NiO, etc. The first carrier transport layer 31 with the resistance enhancing nanostructure 312 can also be used in the upper layer cell of the perovskite-crystalline silicon stacked cell, and used as the carrier transport layer, so that the perovskite precursor solution forms a thin film with a uniform thickness and completely covers the texture pyramid structure of the crystalline silicon cell. The specific working principle of the resistance-enhancing nanostructure 312 is as shown in Figure 3, in which Figure 3a is a schematic diagram of applying a perovskite thin film by solution method to the surface of a carrier transport layer having a resistance-enhancing nanostructure, and Figure 3b is a schematic diagram of applying a perovskite thin film by solution method to the surface of a carrier transport layer not having a resistance-enhancing nanostructure.

[0036] In FIG. 3a, a resistance enhancing nanostructure 312 is provided on the base layer 311 of the carrier transport layer, and after the perovskite solution is applied on the pyramid texture, i.e., the crystalline silicon cell 1, the perovskite precursor solution can be adsorbed and fixed in the gaps between the nanostructures by the capillary action of the nanostructures, and a uniform coating layer can be formed on the surface of the nanostructures (the tension action of the liquid surface). After the solution is applied, before the heat treatment is performed to obtain the perovskite light absorbing layer thin film, certain measures are taken to remove the excess solution in the valley region of the pyramid texture, and then the wet film is heat treated, so that the perovskite light absorbing layer 32 that uniformly covers the carrier transport layer having the resistance enhancing nanostructure 312 shown in FIG. 3a can be obtained, and the perovskite light absorbing layer 32 can be fully filled in the gaps between the multiple resistance enhancing nanostructures 312 that are discretely distributed, thereby further enhancing the carrier collection and conduction ability of the carrier transport material.

[0037] On the other hand, as shown in FIG. 3b, when the perovskite light-absorbing layer is manufactured using a solution method without the resistance-enhancing nanostructures 312, the situation shown in the figure is likely to occur, that is, a large amount of solution is deposited in the valley region of the pyramid texture, so the perovskite light-absorbing layer is too thick, while the solution is difficult to adhere to the tip region of the pyramid, so the absorption layer is too thin, and even the tip is exposed.

[0038] Therefore, by using the resistance-enhancing nanostructure 312 of the present application, the perovskite thickness at the top and bottom of the pyramid is almost the same, avoiding the problem that the absorption layer at the bottom of the pyramid is too thick and the top of the pyramid is difficult to completely cover, thereby greatly improving the energy conversion efficiency of the perovskite-crystalline silicon stacked battery.

[0039] The base layer 311 of the carrier transport layer is provided on the upper surface of the crystalline silicon cell 1, and may have a thickness of 10 to 200 nm, for example, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 110 nm, 120 nm, 130 nm, 140 nm, 150 nm, 160 nm, 170 nm, 180 nm, 190 nm, 200 nm. The base layer 311 of the carrier transport layer mainly plays the role of lateral collection and transport of carriers, that is, transporting the carriers generated by the absorption layer in the lateral direction and collecting them in the series structure layer. Therefore, the thickness of the base layer should not be too thick or too thin. If the base layer is too thick, the vertical transport distance to the series structure is too long, and the transport resistance is too large. If the base layer is too thin, the cross-sectional area of ​​the thin film is too small and the lateral transport resistance is too large, which is unfavorable to the lateral collection and transport of carriers in the absorbing layer.

[0040] As shown in FIGS. 2 to 4, the resistance enhancing nanostructure 312 may be a fibrous structure, a rod-like structure, or a nanotube structure, and is formed in a roughly sawtooth or comb-like structure on the base layer 311 of the carrier transport layer.

[0041] The resistance-enhancing nanostructure 312 should not be too short or too long. If it is too short, the capillary action is too weak and the effect of resistance enhancement is not obvious. If it is too long, the absorption layer will be too thick, which is unfavorable to the improvement of the battery efficiency of the upper layer, and it will be difficult to fill the perovskite precursor solution at the base of the nanostructure, and some voids will occur at the base, affecting the battery efficiency. Usually, in a perovskite-crystalline silicon stacked battery, the thickness of the absorption layer of the upper perovskite battery is not more than 1600 nm. The specific thickness of the absorption layer of the upper perovskite battery should be determined according to the current of the lower crystalline silicon battery based on the principle of current matching. Therefore, it is desirable that the upper limit of the resistance-enhancing nanostructure does not exceed the thickness of the absorption layer. If the resistance-enhancing nanostructure exceeds the thickness of the absorption layer of the upper perovskite battery, a short circuit phenomenon will occur due to contact with the opposing carrier transport layer, and the battery efficiency will be reduced. Therefore, taking into account the variation in thickness of the portion of the absorbing layer beyond the resistance-enhancing nanostructures, the length of the resistance-enhancing nanostructures of this application is ≦1500 nm.

[0042] In addition, if the upper perovskite cell absorption layer is composed of quantum dots, the resistance-enhancing nanostructures must be larger than the size of the quantum dots, otherwise the resistance-enhancing nanostructures are insignificant. Generally, the size of quantum dots is <50 nm, so the length of the resistance-enhancing nanostructures in this application is ≧50 nm.

[0043] In a specific embodiment, the length of the resistance enhancing nanostructure 312 is 50 to 1500 nm, and may be, for example, 50 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, 1000 nm, 1100 nm, 1200 nm, 1300 nm, 1400 nm, or 1500 nm. Here, the length of the resistance enhancing nanostructure means the distance from the end of the resistance enhancing nanostructure to the surface facing the perovskite light absorbing layer of the base layer of the carrier transport layer.

[0044] The diameter of the resistance-enhancing nanostructure 312 needs to take into consideration the resistance-enhancing effect, the filling effect in the nanostructure, and the strength of the nanostructure itself. The diameter of the resistance-enhancing nanostructure also needs to take into consideration the special size of the crystalline silicon texture pyramid structure. Generally, the pyramid structure of the existing commercial textured crystalline silicon surface is 1000 nm or more. Therefore, the diameter of the resistance-enhancing nanostructure is generally 1000 nm or less. If the diameter is too large, the resistance-enhancing nanostructure itself will fill the texture structure, making it impossible to achieve "conformity" and maintaining the light trapping effect of the texture. In addition, if the diameter of the nanostructure is too small, the strength of the nanostructure itself will be insufficient, making it easy to collapse or break, and the resistance-enhancing effect will not be achieved. In the field of nanomaterials, it is generally believed that nanostructures of 100 nm or more have excellent performance in terms of strength and long-term stability.

[0045] In a specific embodiment, the diameter of the resistance enhancing nanostructure 312 is 100-1000 nm, for example, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, 1000 nm, etc. Here, the diameter of the resistance enhancing nanostructure refers to the average diameter of the cross section of the resistance enhancing nanostructure.

[0046] Considering the same influencing factors as the length of the resistance enhancing nanostructures 312 and the diameter of the resistance enhancing nanostructures 312, the coverage of the resistance enhancing nanostructures 312 on the surface of the base layer 311 of the carrier transport layer is 5 to 70%, preferably 10 to 60%, and may be, for example, 5%, 10%, 20%, 30%, 40%, 50%, 60%, or 70%. Here, the coverage of the resistance enhancing nanostructures 312 on the surface of the base layer 311 of the carrier transport layer refers to the ratio of the area of ​​the resistance enhancing nanostructures 312 on the surface of the base layer 311 of the carrier transport layer to the area of ​​the base layer 311 of the carrier transport layer.

[0047] The perovskite-crystalline silicon stacked battery having the resistance-enhancing nanostructured carrier transport layer of the present application has the advantage of significantly improving the energy conversion efficiency of the perovskite-crystalline silicon stacked battery described above, and further has the following technical effects.

[0048] (1) Because the perovskite thin film grows almost conformally on the crystalline silicon texture, the textured light trapping structure of the crystalline silicon is preserved in the upper layer of the cell, enhancing the light trapping effect of the perovskite-crystalline silicon stacked solar cell and further improving the cell conversion efficiency.

[0049] (2) Although the deposition method can obtain a perovskite thin film with uniform thickness and conformal morphology, it is difficult to control the perovskite components when producing the perovskite thin film by deposition method, which makes it difficult to control the band gap of the perovskite layer, which is disadvantageous for the absorption layer of the upper cell of the stacked battery. By adopting the technical solution described in this application, the absorption layer of the upper cell of the perovskite-crystalline silicon stacked battery can be grown conformally and the band gap can be flexibly adjusted, which can greatly improve the energy conversion efficiency.

[0050] The present application further provides a method for producing the above-mentioned perovskite-crystalline silicon stacked battery, the method comprising: forming a series structure layer on one surface of a crystalline silicon cell; fabricating a first carrier transport layer on a surface of the series structure layer opposite the crystalline silicon cell; applying a perovskite light absorbing layer to a surface of the first carrier transport layer opposite to the series structure layer; forming a second carrier transport layer on a surface of the perovskite light absorbing layer opposite to the first carrier transport layer; forming an upper transparent electrode layer on a surface of the second carrier transport layer opposite the perovskite light absorbing layer; Here, the step of manufacturing the first carrier transport layer includes manufacturing a base layer of the carrier transport layer, and manufacturing the resistance enhancing nanostructures on the base layer of the carrier transport layer, which are discretely distributed and integrally formed with the base layer of the carrier transport layer. The manufacturing method of the first carrier transport layer 31 cannot use a liquid phase coating method, and when manufacturing by the liquid phase coating method, the problem of coating unevenness in the texture pyramid still exists, and the technical problem of the present application cannot be completely solved.

[0051] Therefore, the manufacturing method of the first carrier transport layer 31 must have the characteristic of conformal growth.

[0052] "Conformal growth" refers to the growth of a coating layer or thin film on a substrate having a specific surface morphology, and the thin film then grows in accordance with the original morphology of the substrate. The "substrate + thin film combination" with the coating layer or thin film has the same "surface morphology" as the original surface of the substrate.

[0053] Specifically, the manufacturing method of 31 can adopt the following two methods.

[0054] (1) One-step conformal manufacturing method Materials that can be used in the one-step conformal manufacturing process are organic polymeric materials and can employ gas phase processes known in the art.

[0055] The vapor phase method can synthesize the first carrier transport layer of an organic polymer having the resistance enhancing nanostructure described in this patent in one step.

[0056] Specifically, a substrate is first prepared, and a catalyst layer necessary for the polymerization reaction of the polymer monomer is deposited on the substrate by physical vapor deposition.Then, the substrate with the catalyst deposited is placed in the polymer monomer vapor, and the monomer vapor comes into contact with the catalyst on the substrate, and the polymerization reaction occurs at the interface between the two phases.

[0057] The principle of morphology control is as follows: a) When the vapor pressure of the monomer in the reaction vessel is large, the monomer vapor condenses into mist droplets, and when the mist droplets come into contact with the catalyst layer, a reaction occurs in the contact area, and in the area where there is no contact with the mist droplets, there is no monomer and no polymerization reaction occurs, in this case, nanostructures are formed; b) When the vapor pressure of the monomer in the reaction vessel is small, the monomer vapor is uniformly distributed in the cavity of the reaction vessel, the monomer comes into uniform contact with the catalyst, and a uniform polymer thin film is formed on the substrate.

[0058] During the above polymerization reaction, the vapor pressure of the monomer is controlled and saturated to form droplets in the early stage, forming the resistance enhancing nanostructures 312, and in the later stage, the vapor pressure is low and the reaction occurs over the entire surface to form the uniform base layer 311. Since 311 and 312 are formed continuously at one time, 311 and 312 are connected together, which is more favorable for carrier transport.

[0059] (2) Two-step conformal manufacturing method Materials that can be used in the two-step conformal manufacturing process are metal oxide materials.

[0060] In the first step, conformal features are required (a necessary condition), and physical vapor deposition, electroplating, etc. can be used. A thin film of a metal element corresponding to the "metal oxide" is deposited or electroplated onto a substrate.

[0061] In the second step, the metal layer is oxidized to a metal oxide by anodic electrochemical oxidation.

[0062] The principle of morphology control is as follows: by controlling parameters such as current, electrolyte solvent type, and solute concentration during anodization, if the oxidation reaction occurs locally, resistance-enhancing nanostructures 312 are formed, and if the oxidation reaction occurs on the surface, a base layer 311 is formed.

[0063] If the metal oxidation process described above is not interrupted, 312 and 311 will be joined together.

[0064] The perovskite light absorbing layer 32 may be an organic-hybrid halide perovskite, an all-inorganic halide perovskite, or other light absorbing materials with perovskite structures such as lead-free perovskite, double perovskite, etc.

[0065] The second carrier transport layer 33 may be made of an electron transport material or a hole transport material, but has the opposite conductivity type to the first carrier transport layer 31. That is, if the first carrier transport layer 31 is made of an electron transport material, the second carrier transport layer 33 is made of a hole transport material, and if the first carrier transport layer 31 is made of a hole transport material, the second carrier transport layer 33 is made of an electron transport material.

[0066] The upper transparent electrode layer 34 may be a transparent electrode commonly used in the prior art, such as FTO, ITO, AZO, etc.

[0067] Working Example Example 1 A HJT (heterojunction) solar cell using an N-type silicon wafer was prepared as the lower cell.

[0068] A series structure layer was fabricated on the surface of an N-type silicon wafer HJT (heterojunction) solar cell by magnetron sputtering. ITO was used and the thickness was 200 nm.

[0069] A first carrier transport layer was fabricated on the surface of the serial structure layer, where the first carrier transport layer was a hole transport layer having a resistance enhancing nanostructure, using PEDOT synthesized by a gas phase method, the thickness of the base layer of the carrier transport layer was 50 nm, the resistance enhancing nanostructure was fibrous, had a length of 500 nm and a diameter of 150 nm, and the surface coverage of the resistance enhancing nanostructure on the base layer of the carrier transport layer was 40%, where the shape, length, and diameter of the resistance enhancing nanostructure can be obtained by observation with an electron microscope, and the surface coverage can be obtained by a specific surface area analyzer.

[0070] A perovskite light absorbing layer was applied to the surface of the first carrier transport layer opposite to the serial structure layer, where the perovskite light absorbing layer used MAPbI3 perovskite and had a thickness of 800 nm. The perovskite application method used a dip coating method, and the crystalline silicon cell covered with the first carrier transport layer was immersed in a DMF solution of MAPbI3 perovskite with a concentration of 1.5 M and pulled up at a speed of 20 mm / min. After the pulling was completed, it was dried at 100°C for 10 minutes to obtain a MAPbI3 perovskite light absorbing layer.

[0071] A second carrier transport layer, which is an electron transport layer, was produced on the opposite surface of the perovskite light absorbing layer to the first carrier transport layer by using a vapor deposition method. C60 was used as the material of the electron transport layer, and the thickness of the electron transport layer was 50 nm.

[0072] An upper transparent electrode layer was formed on the opposite surface of the second carrier transport layer to the perovskite light absorbing layer by magnetron sputtering, in which ITO was used as the upper transparent electrode and had a thickness of 300 nm.

[0073] Here, the first carrier transport layer is synthesized by vapor phase method, and the specific steps are as follows: deposit a 20nm iron oxide layer on the substrate using physical vapor deposition method, add 12μL of concentrated hydrochloric acid and 60μL of 1.56M pyrrole chlorobenzene solution into a glass reactor, react for 1.5h at 130℃, and finally obtain a PEDOT thin film containing FeCl2 impurities and a comb-shaped structure, then wash with 6M HCl, and finally obtain a PEDOT hole transport layer with a nanostructure for resistance enhancement.

[0074] The efficiency of the perovskite-PERC crystalline silicon stacked cell of this example was 28.1%.

[0075] Example 2 A HJT (heterojunction) solar cell using an N-type silicon wafer was prepared as the lower cell.

[0076] A series structure layer was fabricated on the surface of an N-type silicon wafer HJT (heterojunction) solar cell using magnetron sputtering, ITO was used, and the thickness was 200 nm. A first carrier transport layer was fabricated on the surface of the series structure layer, where the first carrier transport layer was an electron transport layer with resistance-enhancing nanostructures, a TiO2 array fabricated by anodization, the thickness of the base layer of the carrier transport layer was 20 nm, the resistance-enhancing nanostructures were rod-shaped structures, 400 nm in length and 150 nm in diameter, and the coverage of the resistance-enhancing nanostructures on the base layer of the carrier transport layer was 60%.

[0077] A perovskite light absorbing layer was applied to the surface of the first carrier transport layer opposite to the serial structure layer, where the perovskite light absorbing layer used FAPbI3 perovskite material and had a thickness of 700 nm. The perovskite application method used a dip coating method, and the crystalline silicon cell covered with the first carrier transport layer was immersed in a 1.3M FAPbI3 perovskite solution (solvent was a mixed solvent of DMF:DMSO=4:1) and pulled up at a speed of 25 mm / min. After the pulling was completed, it was dried at 120°C for 15 minutes to obtain a FAPbI3 perovskite light absorbing layer.

[0078] A second carrier transport layer, which is a hole transport layer, was fabricated on the surface of the perovskite light absorbing layer opposite to the first carrier transport layer. Spiro-TTB was used to form the second carrier transport layer, and the second carrier transport layer had a thickness of 100 nm and was fabricated by a deposition method.

[0079] An upper transparent electrode was formed on the surface of the second carrier transport layer opposite the perovskite light absorbing layer, where the upper transparent electrode was made of ITO, had a thickness of 350 nm, and was manufactured using a magnetron sputtering method (prior art).

[0080] Here, the first carrier transport layer is fabricated by anodization, and the specific steps are as follows: a 100 nm metallic Ti thin film is deposited on the substrate by evaporation, and then the substrate coated with Ti film is used as the anode, the Pt sheet is used as the cathode, and the substrate is oxidized in an electrolyte of 0.5 wt% NH4F aqueous solution (pH = 4-5) at a voltage of 18 V for 4 hours to obtain a TiO2 electron transport layer with a nanostructure for enhancing resistance.

[0081] The efficiency of the perovskite-HJT crystalline silicon stacked cell of this example was 27.6%.

[0082] Example 3 The difference between this embodiment and embodiment 1 is that the length of the resistance enhancing nanostructure in this embodiment is 300 nm. The efficiency of the resulting stacked cell was 26.8%.

[0083] Example 4 The difference between this embodiment and Example 1 is that the coverage of the resistance enhancing nanostructure in this embodiment is 5%. The efficiency of the resulting stacked cell was 25.1%.

[0084] Example 5 The difference between this embodiment and Example 1 is that the coverage of the resistance enhancing nanostructure in this embodiment is 70%. The efficiency of the resulting stacked cell was 24.9%.

[0085] Example 6 The difference between this embodiment and embodiment 1 is that the length of the resistance enhancing nanostructure in this embodiment is 50 nm. The efficiency of the resulting stacked cell was 27.5%.

[0086] Example 7 The difference between this embodiment and embodiment 1 is that the length of the resistance enhancing nanostructure in this embodiment is 1100 nm. The efficiency of the resulting stacked cell was 26.9%.

[0087] Comparative Example 1 The difference between this embodiment and Example 1 is that the first carrier transport layer includes only a base layer and does not include a resistance enhancing nanostructure. The efficiency of the resulting stacked cell was 24.1%.

[0088] Comparative Example 2 A HJT (heterojunction) solar cell using an N-type silicon wafer was prepared as the lower cell.

[0089] A series structure layer was fabricated on the surface of an N-type silicon wafer HJT (heterojunction) solar cell using magnetron sputtering, with ITO and a thickness of 200 nm. A 50 nm thick dense SnO2 thin film was fabricated as the first carrier transport layer on the series structure layer using magnetron sputtering, where the top surface of the lower cell, the series structure layer, and the first carrier transport layer all have an imitation pyramid texture, and a TiO2 resistance enhancing nanomaterial was fabricated on the surface of the first carrier transport layer with the imitation pyramid texture.

[0090] Specifically, the method is as follows: 1) A suspension containing TiO2 nano-suspended particles was prepared, where the size of the TiO2 nanoparticles was 10-150 nm. The ratio of the volume of the TiO2 suspended particles to the total volume of the suspension was 1:1000. 2) A wedge-shaped brush was used to uniformly apply a 2000 nm thick TiO2 suspension onto the surface of the first carrier transport layer having an imitation pyramid texture. 3) The suspension was placed at 200°C for rapid drying to remove moisture, and a TiO2 resistance enhancing nanomaterial with an average spacing of 100 nm was obtained on the first carrier transport layer. Here, the coverage of the TiO2 resistance enhancing nanomaterial on the first carrier transport layer was 40%. 4) The imitation pyramid texture with dispersed nanoparticles was placed at a high temperature of 500°C for 10 min annealing to increase the bonding strength between the TiO2 nanoparticles and the first carrier transport layer, and a first carrier transport layer made of the TiO2 resistance enhancing nanomaterial having nanoscale protrusions on the surface was obtained.

[0091] A perovskite light absorbing layer was applied to the surface of the first carrier transport layer covered with the TiO2 resistance enhancing nano material, where the perovskite light absorbing layer used FAPbI3 perovskite material and had a thickness of 700 nm. The perovskite application method used a dip coating method, and the crystalline silicon cell covered with the first carrier transport layer was immersed in a 1.3M FAPbI3 perovskite solution (solvent was a mixed solvent of DMF:DMSO=4:1) and pulled up at a speed of 25 mm / min. After the pulling was completed, it was dried at 120°C for 15 minutes to obtain a FAPbI3 perovskite light absorbing layer.

[0092] A second carrier transport layer, which is a hole transport layer, was fabricated on the surface of the perovskite light absorbing layer opposite to the first carrier transport layer. Spiro-TTB was used to form the second carrier transport layer, and the second carrier transport layer had a thickness of 100 nm and was fabricated by a deposition method.

[0093] An upper transparent electrode layer was formed on the surface of the second carrier transport layer opposite the perovskite light absorption layer, where the upper transparent electrode layer was made of ITO, had a thickness of 350 nm, and was manufactured using a magnetron sputtering method (prior art).

[0094] Here, 31 was fabricated by anodization, and the specific steps are as follows: a 100 nm metallic Ti thin film was deposited on the substrate by evaporation, and then the substrate coated with Ti film was used as the anode, and the Pt sheet was used as the cathode, and the substrate was oxidized in an electrolyte of 0.5 wt% NH4F aqueous solution (pH = 4-5) under a voltage of 18 V for 4 hours to obtain a TiO2 electron transport layer with a nanostructure for resistance enhancement.

[0095] The efficiency of the perovskite-HJT crystalline silicon stacked cell of this example was 24.8%.

[0096] Table 1 shows the specific conditions for each of the above examples and comparative examples.

[0097] [Table 1]

[0098] By comparing Examples 1, 4, and 5 of the present application, it can be seen that the efficiency increase of the resistance enhancing nanostructure of the present application is lower when the coverage of the first carrier transport layer is 5% than when the coverage is 40%, because the resistance enhancing nanostructure is very sparse, the resistance enhancing effect is limited, and the improvement of carrier absorption and conduction performance is small, so the efficiency improvement is limited; therefore, the coverage of the resistance enhancing nanostructure should not be lower than 5%. When the coverage of the resistance enhancing nanostructure of the first carrier transport layer is 70%, the efficiency increase is lower than when the coverage is 40%, because the coverage is too large, the roughness of the first carrier transport layer is too large, which is unfavorable to the formation of high-quality perovskite absorber layer thin film, but the quality of the absorber layer thin film plays an important role in the battery efficiency. Therefore, the coverage of the resistance enhancing nanostructure should not exceed 70%, because the battery efficiency will decrease rapidly if the coverage continues to increase.

[0099] By comparing the efficiency tests of the stacked cells of Examples 1 to 7 of the present application with the efficiency tests of the stacked cells of Comparative Examples 1 and 2, it can be seen that the technical solution of the present application has a significantly improved battery efficiency compared to stacked cells without resistance-enhancing nanomaterials or stacked cells in which resistance-enhancing nanomaterials are formed in a general manner. Here, in Comparative Example 2, a TiO2 resistance-enhancing nanomaterial is used, but the first carrier transport layer and the TiO2 resistance-enhancing nanomaterial are different conductive materials and contact each other only through a physical interface, so a large contact resistance occurs at the contact interface. When the coverage rate of the TiO2 resistance-enhancing nanomaterial on the surface of the first carrier transport layer reaches 40%, not only will the contact resistance cause carrier transport disorders between the first carrier transport layer and the perovskite light absorption layer, but the TiO2 resistance-enhancing nanomaterial itself may be distributed between the first carrier transport layer and the perovskite light absorption layer, forming a small number of carrier recombination centers, which significantly reduces the conversion efficiency of the battery.

[0100] Although the embodiments of the present application have been described above with reference to the drawings, the present application is not limited to the above specific embodiments and application fields, and the above specific embodiments are merely illustrative and instructive, and are not limiting. Based on the teachings of this specification, many forms that a person skilled in the art can make without departing from the scope of protection of the claims of the present application all belong to the scope of protection of the present application. [Explanation of symbols]

[0101] 1. Crystalline silicon battery 2 series structure layers 31 First carrier transport layer 311 Base layer of carrier transport layer 312 Nanostructures for Resistance Enhancement 32 Perovskite light absorbing layer 33 Second carrier transport layer 34 Upper transparent electrode layer 4 Perovskite thin films

Claims

1. A perovskite-crystalline silicon stacked battery comprising a crystalline silicon cell, a series structure layer, a first carrier transport layer, a perovskite light absorbing layer, a second carrier transport layer, and an upper transparent electrode layer, which are stacked in sequence, the first carrier transport layer comprising a base layer of the carrier transport layer and a resistance enhancing nanostructure formed integrally with the base layer of the carrier transport layer which is discretely distributed on the base layer of the carrier transport layer, the resistance enhancing nanostructure extending from the base layer of the carrier transport layer into the perovskite light absorbing layer.

2. 2. The perovskite-crystalline silicon stacked battery according to claim 1, wherein a surface of the first carrier transport layer facing the perovskite light absorbing layer has a textured structure.

3. 2. The perovskite-crystalline silicon stacked battery of claim 1, wherein each of the resistance-enhancing nanostructures is a fibrous structure, a rod-like structure, or a nanotube structure.

4. The perovskite-crystalline silicon stacked battery of claim 3, wherein the length of the resistance-enhancing nanostructure is 50 to 1500 nm.

5. The perovskite-crystalline silicon stacked battery of claim 4, wherein the resistance enhancing nanostructure has a diameter of 100 to 1000 nm.

6. The perovskite-crystalline silicon stacked battery according to any one of claims 1 to 5, wherein the coverage of the resistance enhancing nanostructure on the surface of the base layer of the carrier transport layer is 5 to 70%, preferably 10 to 60%.

7. The perovskite-crystalline silicon stacked battery according to claim 1, wherein the base layer of the carrier transport layer has a thickness of 10 to 200 nm.

8. The first carrier transport layer is made of TiO 2 , SnO 2 , ZnO, or PEDOT, PEDOT:PSS, P 3 H.T., P. 3 OHT, P 3 2. The perovskite-crystalline silicon stacked battery of claim 1, wherein the flux is one selected from ODDT, PTAA, and NiO, and is sprayed on the surface of the conductive boss.

9. 2. The perovskite-crystalline silicon stacked battery according to claim 1, wherein the perovskite light absorbing layer covers the first carrier transport layer and is filled in gaps of the resistance enhancing nanostructures of the first carrier transport layer.

10. The perovskite-crystalline silicon stacked battery according to claim 1, wherein the series structure layer is a conductive material layer or a tunnel junction layer.

11. forming a series structure layer on one surface of a crystalline silicon cell; fabricating a first carrier transport layer on a surface of the series structure layer opposite the crystalline silicon cell; applying a perovskite light absorbing layer to a surface of the first carrier transport layer opposite to the series structure layer; forming a second carrier transport layer on a surface of the perovskite light absorbing layer opposite the first carrier transport layer; forming an upper transparent electrode layer on a surface of the second carrier transport layer opposite the perovskite light absorbing layer; 11. The method for producing a perovskite-crystalline silicon stacked battery according to any one of claims 1 to 10, wherein the step of producing a first carrier transport layer includes producing a base layer of a carrier transport layer, and producing discretely distributed resistance enhancing nanostructures on the base layer of the carrier transport layer and integrally formed with the base layer of the carrier transport layer.

12. The method of claim 11 , wherein the first carrier transport layer is achieved by a one-step conformal manufacturing method or a two-step conformal manufacturing method.

13. The method according to claim 11 , wherein the first carrier transport layer is manufactured by a vapor phase method or an electroplating method.

Citation Information

Patent Citations

  • Heterojunction photovoltaic battery and preparing method thereof

    CN108258124A

  • Perovskite solar cell with array structure electron transport layer and preparation method thereof

    CN110611030A

  • High durability reliable dye-sensitized photoelectric conversion device by dye polymerized on porous semiconductor

    JP2013149504A

  • Solar cell equipped with a light-absorbing structure

    JP2015529982A

  • Composite structure silicon wafer, manufacturing method thereof, and solar cell using same

    JP2016531428A