Flame retardant multilayer material, its manufacturing method and use
A multilayer polymer foam structure with specific density and thickness ratios addresses the challenge of achieving flame retardancy and cushioning in thin compressible foams, enhancing performance in electronic devices.
Patent Information
- Application Number
- JP2024521851
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-27
- Filing Date
- 2022-10-21
- Publication Date
- 2024-11-08
AI Technical Summary
Existing technologies face challenges in producing compressible polymer foams with thicknesses of 3.0 mm or less that maintain good cushioning properties and achieve high flame retardancy, particularly in electronic devices where space is limited and heat generation is increased.
A multilayer material comprising a lower density first polymer foam layer and a higher density second polymer foam layer, each infused with a flame retardant composition, achieving a thickness of 3.5 mm or less with a UL-94 rating of V1 or V0, HF1, by adjusting the density and thickness ratios of the layers.
The multilayer material provides improved flame retardancy and cushioning properties, maintaining compressive force deflection and compression set within desired ranges, suitable for thin electronic devices.
Smart Images

Figure 2024541193000001_ABST
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to and the benefit of U.S. Provisional Application No. 63 / 272,286, filed October 27, 2021, the entire contents of which are incorporated herein by reference.
[0002] The present application relates to a flame retardant multi-layer material, in particular a flame retardant multi-layer material comprising multiple polymer foam layers, a method for preparing the flame retardant multi-layer material, and uses thereof. [Background technology]
[0003] Polymer foams have a variety of uses in the art. Compressible (as opposed to rigid) foams are particularly useful for cushioning and shock protection, especially in electronic devices. As the demand for smaller, thinner and more compact devices increases, thinner, lower density polymer foams, e.g., 200 kilograms per cubic meter (kg / m 3 There is a demand for foams having a density of less than 3.5 millimeters (mm), less than 3 mm, or even less than 2 mm. However, it has been difficult to produce foams of this thickness while meeting the stringent requirements for good cushioning properties, such as good compression set, and good flame retardancy. These properties are important in electronic devices such as handheld electronic devices, as well as televisions, radios, computers, medical devices, business machines, and communication devices. The increased performance of such devices has made flame retardancy more difficult to achieve due to the increased heat generated in ever smaller spaces. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] U.S. Patent No. 7,338,983 [Non-patent literature]
[0005] [Non-Patent Document 1] "Tests for Flammability of Plastic Materials, UL94", Underwriter's Laboratory Bulletin 94 Summary of the Invention [Problem to be solved by the invention]
[0006] Thus, there remains a need in the art for lightweight materials that are thin, provide good cushioning to minimize shock or vibration, and can provide good flame retardancy, for example UL-94 ratings of V0, HF1, or a combination thereof, at thicknesses of 3.0 mm or less. [Means for solving the problem]
[0007] Disclosed herein is a multi-layer material having a strength of 481 kg / m 3 (30 lb / ft 3 a first polymeric foam layer having a density of less than 240 kg / m2, a compression force deflection of 5 to 1,035 kPa at 25% deflection determined in accordance with ASTM D3574-17, and a thickness of less than 3.5 millimeters (130 mils); and a second polymeric foam layer disposed on a first surface of the first polymeric foam layer, the second polymeric foam layer having a density of less than 240 kg / m2. 3 (15 lb / ft 3 and a second polymer foam layer having a density greater than 0.3 millimeters (11.8 mils) and a thickness less than 0.3 millimeters (11.8 mils) and the thickness of the first polymer foam layer is at least twice the thickness of the second polymer foam layer; each of the first polymer foam layer and the second polymer foam layer comprises a flame retardant composition, and the multi-layer material has a thickness of 3.5 millimeters (130 mils) or less and a UL-94 rating of V1, preferably V0, HF1, or a combination thereof.
[0008] Methods for preparing the multi-layer materials are also disclosed, as well as electronic devices that include the multi-layer materials.
[0009] These and other features are illustrated by the following figures, detailed description, and claims.
[0010] The following figures are exemplary embodiments provided to illustrate the present disclosure. The figures illustrating examples are not intended to limit the products produced according to the present disclosure to the materials, conditions, or process parameters explicitly set forth therein. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a cross-sectional schematic diagram of an embodiment of a flame retardant multi-layer material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The inventors have discovered that a very thin, flame retardant multi-layer material with good cushioning and flame retardant properties can be produced using a lower density compressible foam layer and a thinner, higher density second polymer foam layer. The flame retardant properties achieved with this combination allow for the production of a very thin compressible material with low overall density, good compression properties, and excellent flame retardant properties.
[0013] While reduced thickness flame retardant materials are desirable, the flame retardancy of compressible foam layers decreases with decreasing thickness. For example, the flame retardancy of compressible foam layers is reduced to 12 pounds per cubic foot (lb / ft 3 or PCF) ((192 kilograms per cubic meter (kg / m 3A compressible foam layer having a density of 1000 .mu.m or less and a thickness of 3 millimeters (mm) or less may not provide a desired level of flame retardancy. The inventors have surprisingly discovered that by combining a compressible foam layer having a thickness that does not provide a desired level of flame retardancy with a thinner, higher density second polymer foam layer, improved flame retardancy can be achieved while maintaining other desirable properties of the compressible foam layer, such as compression force deflection, compression set, or combinations thereof. In one aspect, the lower density compressible foam layer (which may be referred to herein for convenience as the first polymer foam layer) is at least twice as thick, e.g., at least three times as thick, at least five times as thick, or at least 50 times as thick, or more, as the thinner, higher density second polymer foam layer (which may be referred to herein for convenience as the second polymer foam layer).
[0014] A polymer foam layer of a second, thinner, denser polymer is in contact with the first polymer foam layer to improve flame retardancy. The multi-layer material has desirable structural features such as constant compression force and shock and vibration protection in addition to improved flame retardancy. In one embodiment, the multi-layer material can achieve a UL-94 rating of V1, or even V0, HF1, or combinations thereof. The flame retardant multi-layer material can be used in a variety of applications and is particularly suitable for use as a low density, flame retardant compressible layer in electronic devices.
[0015] An exemplary flame retardant multi-layer material (which may be referred to herein for convenience as a "multi-layer material") is shown in FIG. 1, where the multi-layer material 10 includes a first polymer foam layer 12 having a first surface 14. As used herein, "polymer foam" refers to any polymer material having a porous or cellular structure. The pores may be open, closed, or a combination thereof. At least a portion of the pores may be open and extend through the first polymer foam layer. In one embodiment, the lower first polymer foam layer includes a combination of open and closed pore cells.
[0016] The second polymer foam layer 16 is disposed on the first surface 14 of the first polymer foam layer 12. In a preferred embodiment, the second polymer foam layer 16 is disposed directly on a surface of the first polymer foam layer. Each layer 12, 16 can be independently continuous or discontinuous. For example, there can be vias through one or both layers. In one embodiment, both the first polymer foam layer 12 and the second polymer foam layer 16 are continuous. The respective ends of the layers 14, 16 can be co-terminous, or the ends of the first polymer foam layer or the second polymer foam layer may extend through the other layer.
[0017] To achieve the desired combination of cushioning and flame retardant properties, the first polymer foam layer is preferably 481 kg / m 3 (30 lb / ft 3 ) less than, for example, 400 kg / m 3 (25 lb / ft 3 ) or less than 320kg / m 3 (20 lb / ft 3 ), as further details are provided below. As used herein, the phrase "higher density" refers to the relative density of the second polymer foam layer 16 compared to the density of the first polymer foam layer 12, and the phrase "lower density" refers to the relative density of the first polymer foam layer 12 compared to the density of the second polymer foam layer 16. That is, the density of the second polymer foam layer is higher than the density of the first polymer foam layer. In one embodiment, the density of the second polymer foam layer is significantly higher than the first polymer foam layer, e.g., at least two times, at least three times, or at least five times the density of the first polymer foam layer, as further details are also provided below.
[0018] The thickness of each of the first and second polymer foam layers is adjusted to provide the desired properties and minimize the total thickness of the multi-layer material, the thickness being shown in the Z direction in Figure 1. As mentioned above, the multi-layer material may be, for example, 200 kg / m 3In one embodiment, the multi-layer material may have a thickness of 0.1 to 3.5 mm, or 0.1 to 3 mm, or 0.5 to 3.0 mm, or 0.5 to 2.5 mm. Without being bound by theory, it is believed that the combination of a thicker first polymer foam layer and a thinner second polymer foam layer compared to the first polymer foam layer allows the multi-layer material to have a desired combination of cushioning and flame retardancy. Thus, the first polymer foam layer may have a thickness of less than 1 to 3.5 mm, preferably 0.1 to 3 mm, 0.45 to 2.95 mm, or 0.45 to 2.45 mm. The second polymer foam layer may have a thickness of 10 to 300 micrometers (μm) (0.01 to 0.3 mm), or 25 to 250 μm (0.025 to 0.25 mm).
[0019] The specific properties and compositions of each of the first and second polymeric foam layers are described below.
[0020] The first polymer foam layer provides the cushioning properties of the multi-layer material. The first polymer foam layer may have an average cell size of 10 to 500, or 50 to 250 μm, for example, as may be measured according to ASTM D 3574-95. The cell size and distribution is preferably substantially uniform throughout the layer to provide the desired compressive properties. The first polymer foam layer may have a compressive strength of up to 481 kg / m 3 (30 lb / ft 3 ) less than, for example, 400 kg / m 3 (25 lb / ft 3 ) or less than 320kg / m 3 (20 lb / ft 3 For example, the first polymer foam layer may have a density of 80 to 481 kg / m 3 (5~30 lb / ft 3 ), or 128-400kg / m 3 (8~25 lb / ft 3 ), or 160-288kg / m 3 (10-18 lb / ft 3 ), or 192-288kg / m 3(12-18 lb / ft 3 The first polymer foam layer may have a density of 5 to 1,035 kilopascals (kPa), or 5 to 500 kPa, e.g., 10 to 500 kPa, compression deflection at 25% deflection, determined in accordance with ASTM D3574-17. The first polymer foam layer may further have a compression deflection at 75% deflection, determined in accordance with ASTM D3574-17, of 100 to 500 kPa. The first polymer foam layer may have a compression set of less than 15%. The first polymer foam layer may have a SAG factor (defined as the compression deflection at 65% divided by the compression deflection at 25%, 3 or less). In one embodiment, the first polymer foam layer has a combination of at least two, and preferably all, of the aforementioned properties.
[0021] The first polymer foam layer comprises a polymeric material that can be foamed to form a compressible material and can be thermoplastic, thermoset, or a combination thereof. For example, the first polymer foam layer can be made of polyacetal, poly(C 1~6 alkyl)acrylate, polyacrylic, polyamide, polyamideimide, polyanhydride, polyarylate, polyarylene ether, polyarylene sulfide, polybenzoxazole, polycarbonate, polyester (alkyd, etc.), polyetheretherketone, polyetherimide, polyetherketoneketone, polyetherketone, polyethersulfone, polyisocyanurate, polyimide, poly(C 1~6The polymer may comprise a poly(alkyl)methacrylate, poly((meth)acrylic acid), polyphthalide, polyolefin (such as fluorinated polyolefin), polysilazane, polystyrene, polysulfide, polysulfonamide, polysulfonate, polythioester, polytriazine, polyurea, polyvinyl alcohol, polyvinyl ether, polyvinyl halide, polyvinyl ketone, polyvinylidene fluoride, polyvinyl ester, crosslinked poly(ester), epoxy resin, melamine, phenolic polymer, polyurethane, urea-formaldehyde, silicone, natural rubber, polychloroprene, ethylene-propylene-diene monomer (EPDM) rubber, or a combination thereof. The polymer may be a homopolymer, such as, for example, polyethylene, or a copolymer, such as, for example, polyethylene-polypropylene. Preferred polymers are thermosets, particularly epoxy resins, polyurethanes, or a combination thereof.
[0022] Polyurethanes that can be used include aliphatic, cycloaliphatic, aromatic, and polycyclic polyurethanes. The polyurethane foam is formed from a reactive composition that includes an organic polyisocyanate component, an active hydrogen-containing component that is reactive with the polyisocyanate component, a surfactant, and a catalyst. The process of forming the foam can use a chemical or physical blowing agent, or the foam can be mechanically foamed. For example, one process of forming the foam includes substantially and uniformly dispersing an inert gas throughout a mixture of the reactive composition by vigorous mechanical agitation of the mixture to form a substantially structurally and chemically stable, yet heat-curable foam that is workable at room conditions; and curing the foam to form a cured foam. In one embodiment, a physical blowing agent is introduced into the foam during the crosslinking process to further reduce the foam density. In another embodiment, the polyurethane foam is formed from the reactive composition using only a physical or chemical blowing agent without the use of mechanical foaming. Preferably, the foam is formed by mechanical foaming, which allows for greater control over the thickness of the foam and improved cell structure.
[0023] Exemplary organic polyisocyanates include those having the general formula Q(NCO): I where i is an integer equal to or greater than 2 and Q is an organic group having valence i, where i has an average value greater than 2. Q is a substituted or unsubstituted hydrocarbon group that may or may not contain aromatic functionality, or isocyanates having the formula Q 1 -ZQ 1 [In the formula, Q 1 is C 1~36 Alkylene or C 6~36 An arylene group, Z is -O-, -OQ 2 -O, -CO-, -S-, -SQ 2 -S-, -SO-, -SO 2 -, C 1~24 Alkylene or C 6~24
[0033] Examples of such polyisocyanates include hexamethylene diisocyanate, 1,8-diisocyanato-p-methane, xylyl diisocyanate, diisocyanatocyclohexane, phenylene diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, and tolylene diisocyanates, including crude tolylene diisocyanate, bis(4-isocyanatophenyl)methane, chlorophenylene diisocyanate, diphenylmethane-4,4'-diisocyanate (also known as 4,4'-diphenylmethane diisocyanate, or MDI) and its adducts, naphthalene-1,5-diisocyanate, triphenylmethane-4,4',4"-triisocyanate, isopropylbenzene-alpha-4-diisocyanate, and polymeric isocyanates such as polymethylene polyphenylisocyanate.
[0024] Q can also represent a polyurethane group having a valence of i, in which case Q(NCO) iis a composition known as a prepolymer. Such prepolymers are formed by reacting a stoichiometric excess of the polyisocyanates described above with an active hydrogen-containing component, particularly a polyhydroxy-containing material or polyol disclosed herein. In one embodiment, the polyisocyanate is used in a stoichiometric excess in a ratio of 30 percent to 200 percent, the stoichiometry being based on the equivalents of isocyanate groups per equivalent of hydroxyl in the polyol. The amount of polyisocyanate used will vary slightly depending on the nature of the polyurethane being prepared.
[0025] The active hydrogen-containing component may include a polyol (e.g., a polyether polyol, a polyester polyol, or a combination thereof). Exemplary polyester polyols include polycondensation products of polyols with dicarboxylic acids or their ester-forming derivatives (such as anhydrides, esters, and halides), polylactone polyols obtained by ring-opening polymerization of lactones in the presence of polyols, polycarbonate polyols obtained by reaction of carbonate diesters with polyols, or castor oil polyols. Exemplary dicarboxylic acids and derivatives of dicarboxylic acids useful in producing polycondensed polyester polyols are aliphatic or cycloaliphatic dicarboxylic acids such as glutaric acid, adipic acid, sebacic acid, fumaric acid, or maleic acid; dimer acids; aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, or terephthalic acid; tribasic acids or higher functional polycarboxylic acids such as pyromellitic acid; as well as anhydrides or secondary alkyl esters such as maleic anhydride, phthalic anhydride, or dimethyl terephthalate.
[0026] The additional active hydrogen-containing component is a polymer of cyclic ester. Suitable cyclic ester monomers include, but are not limited to, δ-valerolactone, ε-caprolactone, zeta-enantholactone, monoalkyl-valerolactone, such as monomethyl-, monoethyl- and monohexyl-valerolactone. Suitable polyester polyols include caprolactone-based polyester polyols, aromatic polyester polyols, ethylene glycol adipate-based polyols, and mixtures containing any one of the aforementioned polyester polyols. Exemplary polyester polyols are polyester polyols made from ε-caprolactone, adipic acid, phthalic anhydride, terephthalic acid, or the dimethyl ester of terephthalic acid.
[0027] Polyether polyols are prepared by dissolving alkylene oxides, such as ethylene oxide, propylene oxide, and mixtures thereof, in water or in the presence of ethylene glycol, propylene glycol, trimethylene glycol, 1,2-butylene glycol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,2-hexylene glycol, 1,10-decanediol, 1,2-cyclohexanediol, 2-butene-1,4-diol, 3-cyclohexene-1,1-dimethanol, 4-methyl-3-cyclohexene, or the like. -1,1-dimethanol, 3-methylene-1,5-pentanediol, diethylene glycol, (2-hydroxyethoxy)-1-propanol, 4-(2-hydroxyethoxy)-1-butanol, 5-(2-hydroxypropoxy)-1-pentanol, 1-(2-hydroxymethoxy)-2-hexanol, 1-(2-hydroxypropoxy)-2-octanol, 3-allyloxy-1,5-pentanediol, 2-allyloxymethyl-2-methyl-1,3-propanediol, [4,4-pentyloxy]-methyl [2-hydroxyethoxy]-1,2-propanediol, 3-(o-propenylphenoxy)-1,2-propanediol, 2,2'-diisopropylidenebis(p-phenyleneoxy)diethanol, glycerol, 1,2,6-hexanetriol, 1,1,1-trimethylolethane, 1,1,1-trimethylolpropane, 3-(2-hydroxyethoxy)-1,2-propanediol, 3-(2-hydroxypropoxy)-1,2-propanediol, 2,4-dimethyl-2-(2-hydroxyethoxy)-methylpentanediol They are obtained by chemical addition to polyvalent organic components such as 1,5;1,1,1-tris[2-hydroxyethoxy)methyl]-ethane, 1,1,1-tris[2-hydroxypropoxy)-methyl]propane, diethylene glycol, dipropylene glycol, pentaerythritol, sorbitol, sucrose, lactose, alpha-methyl glucoside, alpha-hydroxyalkyl glucoside, novolak resins, phosphoric acid, benzene phosphoric acid, polyphosphoric acids such as tripolyphosphoric acid and tetrapolyphosphoric acid, ternary condensation products, etc. The alkylene oxides utilized in the production of polyoxyalkylene polyols usually have 2 to 4 carbon atoms.Exemplary alkylene oxides are propylene oxide and mixtures of propylene oxide and ethylene oxide.The polyols listed above can be used by themselves as the active hydrogen component.
[0028] Exemplary polyether polyols generally have the formula R[(OC n H 2n ) z OH] a where R is hydrogen or a polyvalent hydrocarbon group; a is an integer equal to the valence of R (i.e., 1 or 2 through 6-8), n in each occurrence is an integer from 2 to 4, including (especially 3), and z in each occurrence is an integer having a value from 2 to 200, especially 15 to 100. In one embodiment, the polyether polyol comprises one or more of dipropylene glycol, 1,4-butanediol, 2-methyl-1,3-propanediol, and the like, or a mixture of combinations thereof.
[0029] Other examples of active hydrogen-containing materials include polymer polyol compositions obtained by polymerizing ethylenically unsaturated monomers in a polyol. Exemplary monomers for producing such compositions include acrylonitrile, vinyl chloride, styrene, butadiene, vinylidene chloride, and other ethylenically unsaturated monomers. The polymer polyol composition comprises 1 weight percent or more, specifically 5 weight percent or more, and more specifically 10 weight percent or more (wt%) of monomer polymerized in the polyol, the weight percent being based on the total amount of polyol. In one embodiment, the polymer polyol composition comprises 70 wt% or less, specifically 50 wt% or less, and more specifically 40 wt% or less of monomer polymerized in the polyol. Such compositions are conveniently prepared by polymerizing the monomers in the selected polyol at a temperature between 40 and 150° C. in the presence of a free radical polymerization catalyst, such as a peroxide, persulfate, percarbonate, perborate, azo compound, and the like.
[0030] The active hydrogen-containing component may also include polyhydroxy-containing compounds, such as hydroxy-terminated polyhydrocarbons, hydroxy-terminated polyformals, fatty acid triglycerides, hydroxy-terminated polyesters, hydroxymethyl-terminated perfluoromethylenes, hydroxy-terminated polyalkylene ether glycols, hydroxy-terminated polyalkylenearylene ether glycols, and hydroxy-terminated polyalkylene ether triols.
[0031] The polyols may have hydroxyl values that vary widely. For example, the hydroxyl value of a polyol, including other crosslinking additives, if used, may be from 28 to 1,000, or from 100 to 800. The hydroxyl value is defined as the number of milligrams of potassium hydroxide required to complete the neutralization of the hydrolysis product of the fully acetylated derivatives prepared from one gram of polyol or mixture of polyols, with or without other crosslinking additives.
[0032] Various blowing agents or mixtures of blowing agents are suitable, and when a blowing agent is used, water is particularly suitable. Water reacts with the isocyanate component to produce CO 2 The curing reaction is controlled by selectively using a catalyst when water is used as the blowing agent. In one embodiment, compounds that decompose to liberate a gas (e.g., azo compounds) can also be used.
[0033] Exemplary blowing agents are physical blowing agents that include hydrogen atom-containing components, which can be used alone or in mixtures with each other or with another type of blowing agent, such as water or azo compounds. These blowing agents can be selected from a wide range of materials, including hydrocarbons, ethers, esters, and partially halogenated hydrocarbons, ethers, and esters. Exemplary physical blowing agents have boiling points of -50 to 100°C, or -50 to 50°C. Among the hydrogen-containing blowing agents are HCFCs (halochlorofluorocarbons) such as 1,1-dichloro-1-fluoroethane, 1,1-dichloro-2,2,2-trifluoroethane, monochlorodifluoromethane, and 1-chloro-1,1-difluoroethane; 1,1,1,3,3,3-hexafluoropropane, 2,2,4,4-tetrafluorobutane, 1,1,1,3,3,3-hexafluoro-2-methylpropane, 1,1,1,3,3-pentafluoropropane, 1,1,1,2,2-pentafluoropropane, 1,1,1,2,3-pentafluoropropane, 1,1,2,3,3-pentafluoropropane, 1,1,2,2,3-pentafluoropropane, 1,1,1,3,3,4-hexafluorobutane, HFCs (halofluorocarbons) such as ethane, 1,1,1,3,3-pentafluorobutane, 1,1,1,4,4,4-hexafluorobutane, 1,1,1,4,4-pentafluorobutane, 1,1,2,2,3,3-hexafluoropropane, 1,1,1,2,3,3-hexafluoropropane, 1,1,1,2,3,3-hexafluoropropane, 1,1-difluoroethane, 1,1,1,2-tetrafluoroethane, (Z)-1,1,1,4,4,4-hexafluoro-2-butene, and pentafluoroethane; HFEs (halofluoroethers) such as methyl-1,1,1-trifluoroethyl ether and difluoromethyl-1,1,1-trifluoroethyl ether; and hydrocarbons such as n-pentane, isopentane, and cyclopentane. Typically, the physical blowing agent can be used in an amount of from 0.5 to 50 wt%, or from 3 to 30 wt%, based on the total weight of the reactive composition.
[0034] Exemplary chemical blowing agents include water, azo compounds such as azoisobutyronitrile, azodicarbonamide (i.e., azo-bis-formamide), barium azodicarboxylate, etc.; substituted hydrazines such as diphenylsulfone-3,3'-disulfohydrazide, 4,4'-hydroxy-bis-(benzenesulfohydrazide), trihydrazinotriazine, aryl-bis-(sulfohydrazide), etc.; semicarbazides such as p-tolylenesulfonylsemicarbazide, 4,4'-hydroxy-bis-(benzenesulfonylsemicarbazide), etc.; triazoles such as 5-morpholyl-1,2,3,4-thiatriazole, etc.; N-nitroso compounds such as N,N'-dinitrosopentamethylenetetraamine, N,N-dimethyl-N,N'-dinitrosophthalamide, etc.; benzoxazines such as isatoic anhydride, etc.; or mixtures (e.g., sodium carbonate / citric acid mixtures). Chemical blowing agents can include water. For example, the blowing agent may include ammonium salts, phosphates, polyphosphates, borates, polyborates, sulfates, urea, urea-formaldehyde resins, dicyandiamide, or melamine.
[0035] The amount of chemical foaming agent varies depending on the agent and the desired foam density, and can be easily determined by one skilled in the art. For example, the chemical foaming agent can be used in an amount of 0.1-10 wt %, based on the total weight of the reactive composition. The decomposition products formed during the decomposition process can be physiologically safe and do not significantly adversely affect the thermal stability or mechanical properties of the polymer foam.
[0036] Many catalysts can be used to catalyze the reaction between the isocyanate component and the active hydrogen-containing component, including organic and inorganic acid salts or organometallic derivatives of bismuth, lead, tin, iron, antimony, uranium, cadmium, cobalt, thorium, aluminum, mercury, zinc, nickel, cerium, molybdenum, vanadium, copper, manganese, or zirconium, as well as phosphines or tertiary organic amines. Exemplary catalysts include dibutyltin dilaurate, dibutyltin diacetate, stannous octoate, lead octoate, cobalt naphthenate, triethylamine, triethylenediamine, N,N,N',N'-tetramethylethylenediamine, 1,1,3,3-tetramethylguanidine, N,N,N'N'-tetramethyl-1,3-butanediamine, N,N-dimethylethanolamine, N,N-diethylethanolamine, 1,3,5-tris(N,N-dimethylaminopropyl)-s-hexahydrotri ... azines, o- and p-(dimethylaminomethyl)phenol, 2,4,6-tris(dimethylaminomethyl)phenol, N,N-dimethylcyclohexylamine, pentamethyldiethylenetriamine, 1,4-diazobicyclo[2.2.2]octane, N-hydroxyl-alkyl quaternary ammonium carboxylates, tetramethylammonium formate, tetramethylammonium acetate, tetramethylammonium 2-ethylhexanoate, and the like, or combinations thereof.
[0037] For example, the catalyst can be a metal acetylacetonate containing metals such as aluminum, barium, cadmium, calcium, cerium (III), chromium (III), cobalt (II), cobalt (III), copper (II), indium, iron (II), lanthanum, lead (II), manganese (II), manganese (III), neodymium, nickel (II), palladium (II), potassium, samarium, sodium, terbium, titanium, vanadium, yttrium, zinc, zirconium, or combinations thereof. Exemplary catalysts can include bis(2,4-pentanedionato)nickel(II) (also known as nickel acetylacetonate or nickel diacetylacetonate) or derivatives thereof, such as nickel diacetonitrile acetylacetonate, nickel diphenylnitrile acetylacetonate, or nickel bis(triphenylphosphine) diacetyl acetylacetonate. Ferric acetylacetonate (FeAA) is also a suitable catalyst due to its relative stability, good catalytic activity, and lack of toxicity. In one embodiment, the metal acetylacetonate is conveniently added by pre-dissolving it in a suitable solvent, such as dipropylene glycol or other hydroxyl-containing component, and then participates in the reaction and becomes part of the final product. The amount of catalyst present in the reactive composition can be 0.03 to 3 wt %, based on the total weight of the active hydrogen-containing components. In one embodiment, the foam is formed using the delayed action catalyst and process described in U.S. Pat. No. 7,338,983.
[0038] The reactive composition may include a surfactant that may stabilize the reactive composition prior to curing. The surfactant may include an organosilicon surfactant. The organosilicon may be SiO 2 (Silicate) units and (CH3) 3 SiO 0.5The organosilicon may be a copolymer comprising or consisting essentially of (trimethylsiloxy) units, with the molar ratio of silicate to trimethylsiloxy units being 0.8:1 to 2.2:1, or 1:1 to 2.0:1. The organosilicon may comprise a partially crosslinked siloxane-polyoxyalkylene block copolymer, with the siloxane blocks and polyoxyalkylene blocks linked by silicon-carbon bonds or by silicon-oxygen-carbon bonds. The surfactant may be present in an amount of 0.5 to 10 wt%, or 1 to 6 wt%, based on the total weight of the active hydrogen component.
[0039] Other optional additives can be added to the reactive composition, for example, additives can include fillers (e.g., alumina trihydrate, silica, talc, calcium carbonate, or clay), dyes, pigments (e.g., titanium dioxide or iron oxide), antioxidants, antiozonants, ultraviolet (UV) or other light stabilizers, and the like, or combinations thereof.
[0040] In the process of producing polyurethane foam, the components for producing the foam, i.e., isocyanate component, active hydrogen-containing component, surfactant, catalyst, optional blowing agent, and other additives, are first mixed and then subjected to mechanical frothing with air. Alternatively, the components may be added sequentially to the liquid phase during the mechanical frothing process. The gas phase of the foam is particularly air, due to its low cost and ready availability. However, other gases that are gaseous at room conditions and are substantially inert or non-reactive with any of the components of the liquid phase may be used if desired. Such other gases include, for example, nitrogen, carbon dioxide, and fluorocarbons, which are normally gases at room temperature. Inert gases may be incorporated into the liquid phase by vigorous mechanical agitation of the liquid phase in a high shear device such as a Hobart mixer or Oakes mixer. The gas may be introduced under pressure in the normal operation of an Oakes mixer, or may be drawn from the surrounding atmosphere by vigorous agitation or stirring action, as in a Hobart mixer. The mechanical stirring operation is carried out at a rate of 7 to 14 kilograms per square centimeter (kg / cm 2 The mixing is carried out at pressures of 100-200 pounds per square inch (psi) or less. Readily available mixing equipment can be used and special equipment is generally not required. The amount of inert gas entering the liquid phase during agitation is controlled by a gas flow metering device to produce a foam of the desired density. Mechanical agitation is carried out for a few seconds in an Oakes mixer, or for 3-30 minutes in a Hobart mixer, or for as long as the mixing equipment used requires to obtain the desired foam density. The foam resulting from the mechanical agitation operation is substantially chemically stable and structurally chemically stable, yet easily workable at room temperature, e.g., 10-40°C.
[0041] In one embodiment, the first polymer foam layer has an average cell size of 50 to 250 μm as measured according to ASTM D 3574-95; 3 , more preferably 128 to 400 kg / m 3and a compression deflection at 25% deflection of 5 to 1,035 kPa, preferably 5 to 500 kPa, as determined in accordance with ASTM D3574-17. In one embodiment, the polyurethane foam may further have a compression deflection at 75% deflection of 100 to 500 kPa, as determined in accordance with ASTM D3574-17; a compression set of less than 15%; a SAG factor, defined as the compression deflection at 65% divided by the compression deflection at 25%, of 3 or less; or a combination thereof. Such materials are sold under the name PORON by Rogers Corporation, Chandler, AZ. PORON foams have been formulated to provide excellent properties, including compression set resistance. Foams with good compression set resistance provide cushioning and maintain their original shape or thickness under load for extended periods of time.
[0042] In one embodiment, the compressible polymer foam layer can be a thermosetting silicone foam. Silicone foams can be produced by reaction between water and hydride groups in the reactive polysiloxane composition with the resultant liberation of hydrogen gas. In one embodiment, the polysiloxane polymer has a viscosity of 100 to 1,000,000 poise at 25° C. and has chain substituents such as hydride, methyl, ethyl, propyl, vinyl, phenyl, and trifluoropropyl. The end groups of the polysiloxane polymer can be hydride, hydroxyl, vinyl, vinyldiorganosiloxy, alkoxy, acyloxy, allyl, oxime, aminoxy, isopropenoxy, epoxy, mercapto, or other known reactive end groups. Suitable silicone foams can also be produced by using several polysiloxane polymers each having a different molecular weight (e.g., bimodal or trimodal molecular weight distribution), provided that the viscosity of the combination falls within the above specified range. It is also possible to have several polysiloxane base polymers with different functional or reactive groups to produce the desired foam. In one embodiment, the polysiloxane contains 0.2 moles of hydride (Si-H) groups per mole of water.
[0043] Physical or chemical blowing agents, including the physical and chemical blowing agents described herein, can be used to produce silicone foam.Other examples of chemical blowing agents include benzyl alcohol, methanol, ethanol, isopropyl alcohol, butanediol, and silanol.In one embodiment, a combination of blowing methods is used to obtain a foam with desired characteristics.For example, a physical blowing agent such as chlorofluorocarbons can be added to the reactive mixture as a second blowing agent, and the first mode of foaming is hydrogen released as a result of the reaction of water with hydride substituents on the polysiloxane.
[0044] A suitable reactive silicone composition is a 1:1 liquid silicone rubber (LSR) or liquid injection molding (LIM) composition. The use of a low durometer LSR or LIM results in the formation of a soft foam. In one embodiment, the LSR or LIM system is provided as a two-part formulation suitable for mixing in a 1:1 volume ratio. Part "A" of the formulation comprises one or more polysiloxanes having two or more alkenyl groups and has an extrusion rate of less than 500 grams per minute (g / min). Suitable alkenyl groups are exemplified by vinyl, allyl, butenyl, pentenyl, hexenyl, and heptenyl, with vinyl being particularly preferred. The alkenyl groups may be attached at the chain ends, at pendant positions on the chain, or both. Other silicon-bonded organic groups in polysiloxanes having two or more alkenyl groups are exemplified by substituted and unsubstituted monovalent hydrocarbon groups, for example, alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, and hexyl; aryl groups such as phenyl, tolyl, and xylyl; aralkyl groups such as benzyl and phenethyl; and halogenated alkyl groups such as 3-chloropropyl and 3,3,3-trifluoropropyl. Exemplary substituents are methyl and phenyl groups.
[0045] The alkenyl-containing polysiloxane can have a linear, partially branched linear, branched, or network molecular structure, or can be a mixture of two or more selected from polysiloxanes having the exemplified molecular structures. The alkenyl-containing polysiloxanes include trimethylsiloxy endblocked dimethylsiloxane-methylvinylsiloxane copolymers, trimethylsiloxy endblocked methylvinylsiloxane-methylphenylsiloxane copolymers, trimethylsiloxy endblocked dimethylsiloxane-methylvinylsiloxane-methylphenylsiloxane copolymers, dimethylvinylsiloxy endblocked dimethylpolysiloxanes, dimethylvinylsiloxy endblocked methylvinylpolysiloxanes, dimethylvinylsiloxy endblocked methylvinylphenylsiloxanes, dimethylvinylsiloxy endblocked dimethylvinylsiloxane-methylvinylsiloxane copolymers, dimethylvinylsiloxy endblocked dimethylsiloxane-methylphenylsiloxane copolymers, dimethylvinylsiloxy endblocked dimethylsiloxane-diphenylsiloxane copolymers, R 3 SiO 1 / 2 and SiO 4 / 2 Polysiloxanes containing the unit RSiO 3 / 2 Polysiloxanes containing units, R 2 SiO 2 / 2 and RSiO 3 / 2 Polysiloxanes containing units, R 2 SiO 2 / 2 , RSiO 3 / 2 and SiO 4 / 2 units, as well as mixtures of two or more of the foregoing polysiloxanes. R represents substituted and unsubstituted monovalent hydrocarbon groups, such as alkyl groups, such as methyl, ethyl, propyl, butyl, pentyl, and hexyl; aryl groups, such as phenyl, tolyl, and xylyl; aralkyl groups, such as benzyl and phenethyl; and halogenated alkyl groups, such as 3-chloropropyl and 3,3,3-trifluoropropyl, with the proviso that at least two R groups per molecule are alkenyl.
[0046] The "B" component of the LSR or LIM system comprises one or more polysiloxanes containing at least two silicon-bonded hydrogen atoms per molecule and has an extrusion rate of less than 500 g / min. The hydrogen can be attached to the chain ends, pendant positions on the chain, or both. Other silicon-bonded groups are organic groups exemplified by non-alkenyl, substituted and unsubstituted monovalent hydrocarbon groups, such as alkyl groups, such as methyl, ethyl, propyl, butyl, pentyl, and hexyl; aryl groups, such as phenyl, tolyl, and xylyl; aralkyl groups, such as benzyl and phenethyl; and halogenated alkyl groups, such as 3-chloropropyl and 3,3,3-trifluoropropyl. Exemplary substituents are methyl and phenyl groups.
[0047] The hydrogen-containing polysiloxane component may have a linear, partially branched linear, branched, cyclic, network molecular structure, or may be a mixture of two or more polysiloxanes selected from the exemplified molecular structures. Hydrogen-containing polysiloxanes are exemplified by trimethylsiloxy endblocked methylhydrogenpolysiloxanes, trimethylsiloxy endblocked dimethylsiloxane-methylhydrogensiloxane copolymers, trimethylsiloxy endblocked methylhydrogensiloxane-methylphenylsiloxane copolymers, trimethylsiloxy endblocked dimethylsiloxane-methylhydrogensiloxane-methylphenylsiloxane copolymers, dimethylhydrogensiloxy endblocked dimethylpolysiloxanes, dimethylhydrogensiloxy endblocked methylhydrogenpolysiloxanes, dimethylhydrogensiloxy endblocked dimethylsiloxane-methylhydrogensiloxane copolymers, dimethylhydrogensiloxy endblocked dimethylsiloxane-methylphenylsiloxane copolymers, and dimethylhydrogensiloxy endblocked methylphenylpolysiloxanes.
[0048] The hydrogen-containing polysiloxane component is added in an amount sufficient to cure the composition, specifically, in an amount of from 0.5 to 10 silicon-bonded hydrogen atoms per alkenyl group in the alkenyl-containing polysiloxane.
[0049] Silicone compositions generally further include, as part of component "A", a catalyst such as platinum to promote curing. Platinum and platinum compounds known as hydrosilylation catalysts may be used, such as platinum black, platinum on alumina powder, platinum on silica powder, platinum on carbon powder, chloroplatinic acid, alcoholic solutions of chloroplatinic acid, platinum-olefin complexes, platinum-alkenylsiloxane complexes, and catalysts obtained by micronizing dispersions of platinum addition catalysts in thermoplastic resins such as methyl methacrylate, polycarbonate, polystyrene, silicone, and the like. Mixtures of catalysts may also be used. The amount of catalyst effective to cure the present composition is generally 0.1 to 1,000 parts per million (by weight) of platinum metal relative to the combined amounts of alkenyl and hydrogen components.
[0050] Various platinum catalyst inhibitors can also be used to control the kinetics of the foaming and curing reaction to control the porosity and density of the silicone foam. Examples of such inhibitors include polymethylvinylsiloxane cyclic compounds and acetylenic alcohols. These inhibitors must not interfere with the foaming and curing in such a way that it destroys the foam. The inhibitors can be present as part of component "A".
[0051] The silicone of the compressible polymer foam layer is 80 to 481 kg / m 3 , more preferably 160 to 240 kg / m 3The silicone may further have an average cell size of 10 to 500, or 50 to 250 μm, as may be measured, for example, according to ASTM D 3574-95; a compression deflection of 5 to 1,035 kilopascals (kPa) at 25% deflection, or 5 to 500 kPa, as determined according to ASTM D3574-17; or a combination thereof. The silicone for the compressible polymer foam layer may further have a compression deflection of 100 to 500 kPa at 75% deflection, as determined according to ASTM D3574-17; a compression set of less than 15%; a SAG factor of 3 or less (defined as the compression deflection at 65% divided by the compression deflection at 25%); or a combination thereof. In one embodiment, the compressible polymer foam layer has a combination of at least two, and preferably all, of the aforementioned properties.
[0052] As mentioned above, the second polymer foam layer has a higher density than the first polymer foam layer. The second polymer foam layer has a density of 240 kg / m 3 Higher density, preferably 350-950 kg / m 3 In addition, the second polymer foam layer can be selected to provide the multi-layer material with a flame retardant rating of V0, HF1, or a combination thereof, and not significantly affect the cushioning properties of the multi-layer material.
[0053] A variety of polymers can be used for the second polymer foam layer to provide the desired properties, including the thermoplastic or thermoset polymers mentioned above. Preferred polymers are flexible at the thicknesses used. Specific polymers that may be used include polyamides, polyamideimides, polyanhydrides, polyarylates, polyarylene ethers, polyarylene sulfides, polybenzoxazoles, polycarbonates, polyesters (such as alkyds), polyetheretherketones, polyetherimides, polyetherketoneketones, polyetherketones, polyethersulfones, polyisocyanurates, polyimides, poly(C 1~6alkyl)methacrylates, poly((meth)acrylic acid), polyphthalides, polyolefins (such as fluorinated polyolefins), polysilazanes, polystyrenes, polysulfides, polysulfonamides, polysulfonates, polythioesters, polytriazines, polyureas, polyvinyl alcohols, polyvinyl ethers, polyvinyl halides, polyvinyl ketones, polyvinylidene fluoride, polyvinyl esters, crosslinked poly(esters), epoxy resins, melamine, phenolic polymers, polyurethanes, urea-formaldehyde, silicones, natural rubber, polychloroprene, ethylene-propylene-diene monomer (EPDM) rubber, or combinations thereof.
[0054] In one embodiment, the second polymer foam layer comprises a polyurethane or silicone foam as described above, provided, of course, that the second polymer foam layer has a higher density than the first polymer foam layer. Methods for adjusting compositions to obtain different foam densities are known in the art.
[0055] Optional additives may be present in the second polymer foam layer. For example, the additives may include fillers (e.g., alumina trihydrate, silica, talc, calcium carbonate, or clay), dyes, pigments (e.g., titanium dioxide or iron oxide), antioxidants, antiozonants, ultraviolet (UV) or other light stabilizers, and the like, or combinations thereof.
[0056] Each of the first polymeric foam layer and the second polymeric foam layer includes a flame retardant additive composition.
[0057] These flame retardant additive compositions may include any compound or particulate additive that increases the flame resistance, particularly the flame spread, of a multi-layer material, as tested by UL94. Some useful flame retardants include those that act by forming a charred layer over the surface of the test specimen when exposed to a flame. Other flame retardants include those that act by releasing water upon thermal decomposition of the flame retardant compound. Flame retardant synergists, such as antimony oxide, may be present in the composition.
[0058] In one aspect, the flame retardant additive composition in each of the first and second polymeric foam layers independently includes a metal hydroxide, a metal oxide, a metal borate, a metal carbonate, a melamine (e.g., melamine cyanurate, melamine phosphate, melamine polyphosphate, etc.), a halogenated aromatic compound (e.g., a brominated compound), a guanidine, a carbon black, an expandable graphite, a nanoclay, an organic phosphorus-containing compound (e.g., an aromatic phosphine oxide, an aromatic phosphate, a phosphinic acid, a phosphinate, a phosphazene, a phosphenathrene oxide such as 10-dihydro-9-oxa-10-phosphenanthrene-10-oxide (DOPO) and 10-(2,5-dihydroxyphenyl)-10-H-9-oxa-10-phosphaphenanthrene-10-oxide (ODOPB)), a silazane, a Rimar salt, or a combination thereof.
[0059] Exemplary metal hydroxide flame retardants include aluminum, magnesium, zinc, boron, calcium, nickel, cobalt, tin, molybdenum, copper, iron, titanium, or combinations thereof, such as aluminum trihydroxide, magnesium hydroxide, calcium hydroxide, iron hydroxide, etc. Exemplary metal oxide flame retardants include antimony oxide, antimony trioxide, antimony pentoxide, iron oxide, titanium oxide, manganese oxide, magnesium oxide, zirconium oxide, zinc oxide, molybdenum oxide, cobalt oxide, bismuth oxide, chromium oxide, tin oxide, nickel oxide, copper oxide, tungsten oxide, etc. Exemplary metal borate flame retardants include zinc borate, zinc metaborate, barium metaborate, etc. Exemplary metal carbonate flame retardants include zinc carbonate, magnesium carbonate, calcium carbonate, barium carbonate, etc.
[0060] Exemplary halogen-containing flame retardants include aromatic brominated or chlorinated flame retardants such as tribromoneopentyl alcohol, tris(2-chloroisopropyl)phosphate, tris(dichloropropyl)phosphate, chlorinated alkyl phosphate esters, halogenated aryl ester / aromatic phosphate blends, pentabromobenzyl alkyl ethers, brominated epoxies, alkylated triphenyl phosphate esters, or combinations thereof. However, in one aspect, the flame retardant composition does not include a halogenated flame retardant.
[0061] Exemplary aromatic phosphorus-containing flame retardants include diphenyl pentaerythritol diphosphate, phenyl bis(dodecyl)phosphate, phenyl bis(neopentyl)phosphate, phenyl bis(3,5,5'-trimethylhexyl)phosphate, ethyl diphenyl phosphate, 2-ethylhexyl di(p-tolyl)phosphate, bis(2-ethylhexyl)p-tolyl phosphate, tritolyl phosphate, bis(2-ethylhexyl)phenyl phosphate, tri(nonylphenyl)phosphate, bis(dodecyl)p-tolyl phosphate, dibutylphenyl phosphate, 2-chloroethyl diphenyl phosphate, p-tolyl phosphate, ethyl diphenyl phosphate, 2-ethylhexyl di(p-tolyl)phosphate, bis(2-ethylhexyl)p-tolyl phosphate, triitolyl phosphate, bis(2-ethylhexyl)phenyl phosphate, tri(nonylphenyl)phosphate, bis(dodecyl)p-tolyl phosphate, dibutylphenyl phosphate, 2-chloroethyl diphenyl phosphate, p-tolyl phosphate, ethyl diphenyl ...ethyl diphenyl phosphate, ethyl diphenyl phosphate, ethyl diphenyl phosphate, ethyl diphenyl phosphate, ethyl diphenyl phosphate, ethyl diphenyl phosphate, ethyl diphenyl phosphate, ethyl diphenyl phosphate, ethyl diphenyl phosphate, ethyl diphenyl phosphate, ethyl diphenyl phosphate, ethyl diphenyl phosphate, ethyl diphenyl phosphate, ethyl diphenyl phosphate, ethyl diphenyl phosphate, aromatic phosphates such as aryl bis(2,5,5'-trimethylhexyl)phosphate, 2-ethylhexyl diphenyl phosphate; phosphinic acids, phosphinates, or zinc or aluminum metal salts thereof, such as diphosphinic acid, dimethylphosphinic acid, ethylmethylphosphinic acid, diethylphosphinic acid, and the like; aromatic phosphine oxides are isobutylbis(hydroxyalkyl)phosphine oxide and 1,4-diisobutylene-2,3,5,6-tetrahydroxy-1,4-diphosphine oxide or 1,4-diisobutylene-1,4-diphosphoryl-2,3,5,6-tetrahydroxycyclohexane. Such compounds are known in the art, and examples of commercially available phosphorus-containing compounds include those available under the trade names NH1197 (Chemtura Corporation), NH1511 (Chemtura Corporation), NCENDX P-30 (Albemarle), HOSTAFLAM OP5500 (Clariant), HOSTAFLAM OP910 (Clariant), EXOLIT 935 (Clariant), and CYAGUARD RF 1204, CYAGUARD RF 1241, and CYAGUARD RF 1243R (Cytec Industries). In one aspect, ammonium polyphosphate can be used, which can be melamine coated, silane coated, or uncoated.
[0062] In one aspect, both the first and second polymer foam layers can include a plurality of expandable graphite particles. In one embodiment, only the second polymer foam layer includes a plurality of expandable graphite particles (also known as expandable flaky graphite, swollen flaky graphite, or expandable flaky). The expandable graphite particles can be intercalated with intercalants such as halogens, alkali metals, sulfates, nitrates, various organic acids, aluminum chloride, ferric chloride, other metal halides, arsenic sulfide, thallium sulfide, and the like, or combinations thereof. In one embodiment, the expandable graphite does not include a halogenated intercalant. The plurality of expandable graphite particles can be present in the second polymer foam layer in an amount of 10-50 wt % based on the total weight of the second polymer foam layer.
[0063] The expandable graphite may have an average size, for example a diameter of 30 μm to 1.5 mm, preferably 50 μm to 1.0 mm, more preferably 180 to 850 μm. For example, the expandable graphite may have an average size, for example a diameter of at least 30 μm, preferably at least 180 μm, more preferably at least 300 μm. The expandable graphite may have a carbon content of 75 to 99 wt%, based on the mass of the expandable graphite. The expandable graphite may have a sulfur content of up to 8 wt%, or 2.6 to 5.0 wt%, preferably 3.0 to 3.5 wt%, based on the total mass of the expandable graphite. The expandable graphite may have an expansion ratio (mL / g) of 10:1 to 500:1. For example, the expansion ratio (mL / g) may be 20:1 to 450:1, preferably 30:1 to 400:1, more preferably 50:1 to 350:1. The temperature at which the expandable graphite begins to expand (also known as the onset temperature or expansion temperature) can be from 100 to 250° C. For example, the onset temperature can be from 160 to 225° C., preferably from 180 to 200° C.
[0064] The first and second polymer foam layers can be prepared using any suitable method in the art, such as by casting, molding, calendaring, etc. The flame retardant composition can be dispersed in the polymer of the first or second polymer foam layer and disposed as a separate layer on the first or second polymer foam layer, or both. For example, the flame retardant composition can be incorporated into the composition used to form the first or second polymer foam layer, or coated onto the first or second polymer foam layer (before or after curing, in the case of thermosetting polymers) to form a film. In the case of a separate film, the flame retardant composition can be disposed on the side of the second polymer foam layer facing the first polymer foam layer, disposed on the side of the first polymer foam layer facing the second polymer foam layer, disposed between the first and second polymer foam layers, or a combination thereof.
[0065] In one aspect, the flame retardant composition does not exist as a separate film that increases the thickness of the first or second polymer foam layer. For example, the flame retardant composition can be impregnated into the first or second polymer foam layer, forming a film inside and coating the inner surface of the pores, so that the film does not significantly increase the film thickness. For example, the foam can be saturated with a liquid composition that includes the flame retardant composition and then dried to remove the solvent. If the flame retardant composition is deposited on the foam by an immersion method such as dip coating, then there may be an increase in the amount not only on the surface but also inside the foam.
[0066] Methods for preparing the multi-layer material include those known in the art. For example, in one embodiment, the multi-layer material can be prepared by separately manufacturing the first and second polymer foam layers, followed by bonding the layers by lamination under conditions effective to bond the layers, such as by using heat and pressure. An adhesive may be used between the layers. Preferably, no adhesive is present, so that the thickness of the multi-layer material is not significantly increased. If a thermosetting material is used for one or both of the first and second polymer foam layers, each layer may be manufactured separately, and one or both may be partially cured (B-stage). The layers can then be brought into contact and fully cured (e.g., by heat or by heat and pressure) to provide adhesion between the layers of the multi-layer material.
[0067] In another embodiment, one of the first and second polymer foam layers can be prefabricated and then used as a substrate for the fabrication of the other layer. For example, the reactive composition for forming the first polymer foam layer can be cast onto the surface of the prefabricated second polymer foam layer and subsequently cured to provide a multi-layer material. Conversely, the first polymer foam layer can be fabricated and then the composition for forming the second polymer foam layer can be cast or coated onto the first polymer foam layer to provide a multi-layer material. The polymer foam layer can be cast to a thickness of 4 mils (0.1 mm) or greater. Coating can be performed, for example, by spray coating, dip coating, flow coating, roll coating, and the like.
[0068] In yet another aspect, the first and second polymer foam layers can be produced simultaneously. For example, the reactive compositions for forming each layer can be cast or co-extruded simultaneously to form multiple layers and then cured to provide a multi-layer material. Some mixing can occur between the foams before curing, forming a mixed region between each layer after curing. Alternatively, no mixed region is formed between the first and second polymer foam layers, i.e., the first and second polymer foam layers are separate layers. For example, a flexible gauze layer can be inserted between the layers during casting or co-extrusion to provide a higher separation between the multi-layer material layers.
[0069] In one aspect, a film including the flame retardant composition can be formed on the multi-layer material after manufacture as described above, for example by impregnation of a foam layer.
[0070] Multi-layer materials have a strength of 50 to 1,000 kilograms per cubic meter (kg / m 3 ), preferably 50 to 500 kg / m 3 , more preferably 100 to 250 kg / m 3 The density may be determined in accordance with ASTM D3574-95, Test A.
[0071] The multilayer material may have a compressive force deflection at 25% deflection determined according to ASTM D3574-17 of 5 to 1,035 kPa, preferably 5 to 500 kPa, or 25 to 250 kPa, or 25 to 80 kPa. "Compressive force deflection at 25%" refers to the load required to physically compress the multilayer material by 25%.
[0072] The multi-layer material may have a compressive force deflection at 75% deflection of 100 to 500 kPa, or 200 to 300 kPa.
[0073] The multi-layer material may have a SAG factor of 3 or less, where SAG factor is defined as the compressive force deflection at 65% divided by the compressive force deflection at 25%.
[0074] The multi-layer material may have a compression set at 50% deflection at 23° C. or 70° C. of 0 to 15%, or 0 to 5%, determined according to ASTM D3574-95, Test D.
[0075] In one aspect, the multilayer material can include a compressible polyurethane foam layer having a compression force deflection of 5 to 1,035 kPa at 25% deflection determined in accordance with ASTM D3574-17; and a second polymer foam layer disposed on a first surface of the first polymer foam layer, each optionally including a plurality of expandable graphite particles, the multilayer material having a UL-94 rating of V0, HF1, or a combination thereof. The multilayer material can have a thickness of 3.5 mm or less. The compression force deflection can be 5 to 500 kPa, or 5 to 80 kPa, at 25% deflection. The first polymer foam layer, e.g., polyurethane foam layer, can have a compression force deflection of 100 to 500 kPa, or 200 to 300 kPa, at 75% deflection determined in accordance with ASTM D3574-17.
[0076] The multilayer material is thin and lightweight, yet provides a good combination of cushioning and flame retardant properties. The multilayer material is therefore useful in electronic devices. Electronic devices that may include the multilayer foam include televisions, radios, computers, medical devices, business machines, communication devices, and the like. The multilayer material is particularly useful in handheld electronic devices such as mobile phones, personal digital assistants, and the like. The multilayer material may be used in other applications such as antennas or batteries (such as Li-ion batteries).
[0077] The following examples are merely illustrative and are not intended to limit the disclosure with respect to the equipment, materials, conditions, or process parameters explicitly stated herein. EXAMPLES
[0078] The following examples demonstrate the flame retardant properties of the flame retardant multi-layer material.
[0079] Polyurethane foams for multi-layer materials were produced using the formulations and methods described in U.S. Pat. No. 7,338,983, specifically, the formulations according to Examples 1 and 2 of this patent, and the method according to Example 3 of this patent.
[0080] Flammability was determined in accordance with the procedures of Underwriter's Laboratory Bulletin 94, entitled "Tests for Flammability of Plastic Materials, UL94." In accordance with this procedure, materials may be classified as V1, or V0, HF1, or combinations thereof, based on test results obtained on five specimens at a specified specimen thickness. Each of these flammability classifications is described below.
[0081] The criteria for obtaining V1 and V2 ratings are as follows: for samples placed with their major axis at 180 degrees to the flame, the average period of flaming and / or smoldering after removal of the ignition flame does not exceed 25 seconds, and for the V1 rating, none of the samples placed vertically produce drips of burning particles that ignite the cotton wool. The V2 standard is the same as V1, except that drips are permitted.
[0082] The criteria for achieving a V0 rating are as follows: for samples oriented with their major axis at 180 degrees to the flame, the average period of flaming and / or smoldering after removal of the ignition flame does not exceed 5 seconds, none of the vertically oriented samples produces a drip of burning particles that ignites cotton wool, and no test sample burns to the holding clamp after flaming or glowing.
[0083] HF1 and HF2 are classifications applied to low density foam materials. The criteria for achieving an HF1 rating are that burning ceases within 2 seconds; afterglow is less than 30 seconds; no burning drips are observed, while the criteria for achieving an HF2 rating are that burning ceases within 3 seconds; afterglow is less than 30 seconds; no burning drips are observed.
[0084] (Comparative Example 1 to Comparative Example 10) Flexible polyurethane foams of different densities and thicknesses were tested in accordance with the procedures of Underwriter's Laboratory Bulletin 94, entitled "Tests for Flammability of Plastic Materials, UL94," to the V0 standard. The results are seen in Table 1.
[0085] [Table 1]
[0086] (Examples 1 to 3) Multi-layer materials composed of flexible polyurethane foam and flame-retardant polyurethane layers of different densities and thicknesses were tested in accordance with the procedures of Underwriter's Laboratory Bulletin 94, entitled "Tests for Flammability of Plastic Materials, UL94", to the V0 standard. The results can be seen in Table 2. The densities and thicknesses listed in Table 2 refer to the entire multi-layer material.
[0087] [Table 2]
[0088] As can be seen from the data in the above table, the preferred combination of foam layers is the preferred combination of total density and total thickness (e.g., 14.4 PCF (231 kg / m 3 ) and a thickness of 0.077 inches (2.0 mm), as well as resulting desirable flame retardancy.
[0089] Set forth below are various non-limiting aspects of the disclosure.
[0090] Aspect 1: A multi-layer material having a strength of 481 kg / m 3 (30 lb / ft 3a first polymeric foam layer having a density of less than 240 kg / m2, a compression force deflection of 5 to 1,035 kPa at 25% deflection determined in accordance with ASTM D3574-17, and a thickness of less than 3.5 millimeters (130 mils); and a second polymeric foam layer disposed on a first surface of the first polymeric foam layer, the second polymeric foam layer having a density of less than 240 kg / m2. 3 (15 lb / ft 3 and a second polymer foam layer having a density greater than 0.3 millimeters (11.8 mils) and a thickness less than 0.3 millimeters (11.8 mils) and a thickness less than 0.3 millimeters (11.8 mils) and a thickness of the first polymer foam layer that is at least twice the thickness of the second polymer foam layer; each of the first polymer foam layer and the second polymer foam layer comprises a flame retardant composition, the multilayer material having a thickness of 3.5 millimeters (130 mils) or less and a UL-94 rating of V1, preferably V0, HF1, or a combination thereof.
[0091] Aspect 2: The first polymer foam layer has a compressive strength of 80 to 481 kg / m 3 (5~30 lb / ft 3 ), or 128-400kg / m 3 (8~25 lb / ft 3 ), or 160-288kg / m 3 (10-18 lb / ft 3 ), or 192-288kg / m 3 (12-18 lb / ft 3 2. The multi-layer material of embodiment 1, having a density of from 0.1 to 1.0 mm; and a compressive force deflection at 25% deflection determined in accordance with ASTM D3574-17 of from 5 to 500 kPa.
[0092] Aspect 3: The multilayer material of aspect 1 or 2, wherein the first polymer foam layer has a thickness of less than 0.1 to 3.5 millimeters (less than 0.04 to 0.14 inches), or 0.1 to 3.3 millimeters (0.04 to 0.13 inches), or 0.1 to 3 millimeters (0.04 to 0.11 inches).
[0093] Aspect 4: The multilayer material of any one of Aspects 1 to 3, wherein the first polymer foam layer further has a compression force deflection at 25% deflection of 5 to 1,035 kPa, preferably 5 to 500 kPa, determined in accordance with ASTM D3574-17; a compression force deflection at 75% deflection of 100 to 500 kPa, determined in accordance with ASTM D3574-17; a compression set at 50% deflection of 0 to 15% at 23° C. or 70° C., determined in accordance with ASTM D3574-95, Test D; or a combination thereof.
[0094] Aspect 5: Each of the first polymer foam layer and the second polymer foam layer are independently made of polyacetal, poly(C 1~6 alkyl)acrylate, polyacrylic, polyamide, polyamideimide, polyanhydride, polyarylate, polyarylene ether, polyarylene sulfide, polybenzoxazole, polycarbonate, polyester, polyetheretherketone, polyetherimide, polyetherketoneketone, polyetherketone, polyethersulfone, polyisocyanurate, polyimide, poly(C 1~6 2. The multilayer material of embodiment 1, wherein the polymeric foam layer comprises a poly(alkyl)methacrylate, poly((meth)acrylic acid), polyphthalide, polyolefin (such as fluorinated polyolefin), polysilazane, polystyrene, polysulfide, polysulfonamide, polysulfonate, polythioester, polytriazine, polyurea, polyvinyl alcohol, polyvinyl ether, polyvinyl halide, polyvinyl ketone, polyvinylidene fluoride, polyvinyl ester, crosslinked poly(ester), epoxy resin, melamine, phenolic polymer, polyurethane, urea-formaldehyde, silicone, natural rubber, polychloroprene, ethylene-propylene-diene monomer (EPDM) rubber, or combinations thereof, preferably wherein each of the first polymeric foam layer and the second polymeric foam layer independently comprises an epoxy resin, a polyurethane, or combinations thereof.
[0095] Embodiment 6: The multilayer material of any one of embodiments 1 to 5, wherein the first polymer foam layer comprises a polyurethane foam.
[0096] Aspect 7: The second polymer foam has a compressive strength of 240 to 1,000 kg / m 3 (15-62 lb / ft 3 ), or 288-1,000 kg / m 3 (18-62 lb / ft 3 ), or 350-950kg / m 3 (22-59 lb / ft 3 ), or 400~950kg / m 3 (25-59 lb / ft 3 7. The multilayer material of any one of the preceding embodiments, having a density of
[0097] Embodiment 8: The multilayer material of embodiment 7, wherein the second polymer foam layer comprises a polyurethane foam.
[0098] Aspect 9: The multilayer material of any one of aspects 1 to 8, wherein the flame retardant composition of each of the first polymer foam layer and the second polymer foam layer independently comprises a metal hydroxide, a metal oxide, a metal borate, a metal carbonate, melamine, a halogenated aromatic compound, guanidine, carbon black, expandable graphite, nanoclay, an organic phosphorus-containing compound, a silazane, a rimal salt, or a combination thereof.
[0099] Aspect 10: The multilayer material of any one of aspects 1 to 9, wherein the flame retardant composition of each of the compressible foam layer and the flame retardant layer, independently, does not include a halogenated flame retardant or an antimony compound.
[0100] Embodiment 11: The multilayer material of any one of embodiments 1 to 10, having a compression deflection at 25% deflection of 5 to 1,035 kPa, preferably 10 to 500 kPa, or 25 to 250 kPa, or 25 to 80 kPa, determined in accordance with ASTM D3574-17; a compression deflection at 75% deflection of 100 to 500 kPa, or 200 to 300 kPa; a compression set at 50% deflection of 0 to 15%, or 0 to 5%, at 23° C. or 70° C., determined in accordance with ASTM D3574-95, test D; or a combination thereof.
[0101] Embodiment 12: The multilayer material of embodiment 11, wherein the first polymer foam layer comprises polyurethane.
[0102] Example 13: A method for preparing a multilayer material described in any one of Examples 1 to 12, comprising: forming a first polymer foam layer and a second polymer foam layer; and contacting the first polymer foam layer and the second polymer foam layer under conditions effective to adhere the layers to form the multilayer material.
[0103] Example 14: A method for preparing a multilayer material described in any one of Examples 1 to 12, comprising: forming one of a first polymer foam layer and a second polymer foam layer; and forming the other of the first polymer foam layer and the second polymer foam layer on a surface of the formed layer to provide a multilayer material.
[0104] Example 15: A method for preparing a multilayer material according to any one of Examples 1 to 12, comprising simultaneously forming a first polymer foam layer and a second polymer foam layer to provide a multilayer material.
[0105] Aspect 16: The method of aspect 15, wherein the step of simultaneously forming the first polymeric foam layer and the second polymeric foam layer comprises the steps of: mechanically foaming a first reactive polyurethane foam-forming composition; mechanically foaming a second reactive polyurethane foam-forming composition; simultaneously casting the first and second mechanically foamed foams to provide a cast bilayer; and curing the cast bilayer under conditions effective to form a multilayer material.
[0106] Embodiment 17: An electronic device comprising the multilayer material according to any one of embodiments 1 to 12, preferably a handheld electronic device.
[0107] The compositions, methods, and devices can alternatively comprise, consist of, or consist essentially of any suitable materials, steps, or ingredients disclosed herein. The compositions, methods, and devices can additionally or alternatively be designed to be devoid, or substantially free of, any materials (or species), steps, or ingredients that are not otherwise necessary to the function or achievement of the purpose of the compositions, methods, and devices.
[0108] The use of singular terms (such as "a", "an" in the foreign language specification of this application) does not denote a limitation of quantity, but rather denotes the presence of at least one of the referenced items. The term "or" means "and / or" unless the context clearly dictates otherwise. Throughout this specification, references to "an embodiment", "separate embodiments", etc., mean that a particular element (e.g., a feature, structure, step, or characteristic) described in connection with an embodiment is included in at least one embodiment described herein and may or may not be present in other embodiments. In addition, it is to be understood that the described elements may be combined in the various embodiments in any suitable manner.
[0109] When an element, such as a layer, is described as being "on" another element, it may be directly on the other element, or intervening elements may also be present. In contrast, when an element is described as being "directly on" another element, there are no intervening elements present. A layer may be disposed on a portion of a surface of an element, or on the entire surface of an element, or may be disposed directly.
[0110] Unless otherwise specified herein to the contrary, all test standards are the latest standards in effect as of the filing date of this application or, if priority is claimed, as of the filing date of the earliest priority application in which the test standard appears.
[0111] As used herein, the "diameter" of a particle refers to the diameter of a sphere or the equivalent diameter obtained from a particle size analyzer or from two-dimensional images in an electron microscope analysis, e.g., a transmission electron microscope image analyzed using a program such as Image J. In one aspect, "size" refers to the average (e.g., mean or median) size of a single particle or a particle or population of particles.
[0112] End points of all ranges relating to the same component or property are inclusive, independently combinable, and include all intermediate points and ranges. The terms "first," "second," "primary," "secondary," and the like, as used herein, do not denote any order, quantity, or importance, but are used to distinguish one element from another. The terms "combination of" or "at least one of" are open-ended, meaning that the list includes every element individually, as well as combinations of two or more elements of the list, and combinations of at least one element of the list with a similar element not named. The term "combination" also includes blends, mixtures, alloys, reaction products, and the like.
[0113] Unless otherwise defined, technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure belongs.
[0114] Compounds are described using standard nomenclature. For example, any position not substituted by a shown group is understood to have its valency satisfied by the shown bond or hydrogen atom. A dash ("-") that is not between two letters or symbols is used to indicate the point of attachment of a substituent. For example, -CHO is attached through the carbon of a carbonyl group.
[0115] All cited patents, patent applications, and other references are incorporated herein by reference in their entirety. However, if a term in this application contradicts or conflicts with a term in an incorporated reference, the term from this disclosure takes precedence over the conflicting term from the incorporated reference.
[0116] While particular embodiments have been described, alternatives, modifications, variations, improvements, and substantial equivalents may occur to applicant or those skilled in the art that are presently unforeseen or unanticipated, and it is therefore intended that the appended claims, as filed and as they may be amended, shall embrace all such alternatives, modifications, variations, improvements, and substantial equivalents. [Explanation of symbols]
[0117] 10 Multilayer materials 12 First polymer foam layer 14 First Side 16 Second polymer foam layer
Claims
1. 1. A multi-layer material comprising: 481 kg / m 3 (30 lb / ft 3 ) density less than Compressive deflection from 5 to 1,035 kPa at 25% deflection determined in accordance with ASTM D3574-17, and Less than 3.5 mm (130 mils) thick a first polymer foam layer having a second polymeric foam layer disposed on the first surface of the first polymeric foam layer, 240 kg / m 3 (15 lb / ft 3 ) greater than 100%, and the density of the second polymer foam layer is at least twice the density of the first polymer foam layer; and a thickness of less than 0.3 millimeters (11.8 mils) and the thickness of the first polymeric foam layer is at least twice the thickness of the second polymeric foam layer; a second polymer foam layer having Including, each of the first polymeric foam layer and the second polymeric foam layer comprises a flame retardant composition; The multilayer material is A thickness of 3.5 millimeters (130 mils) or less, and UL-94 standard of V1, preferably V0, HF1, or a combination thereof A multi-layer material having
2. a first polymer foam layer comprising: 80-481 kg / m 3 (5-30 lb / ft 3 ), or 128 to 400 kg / m 3 (8-25 lb / ft 3 ), or 160 to 288 kg / m 3 (10-18 lb / ft 3 ), or 192-288 kg / m 3 (12-18 lb / ft 3 ) density; and Compressive deflection from 5 to 500 kPa at 25% deflection determined in accordance with ASTM D3574-17 The multilayer material of claim 1 , having
3. 3. The multi-layer material of claim 1 or 2, wherein the first polymer foam layer has a thickness of 0.1 to less than 3.5 millimeters (0.04 to less than 0.14 inches), or 0.1 to 3.3 millimeters (0.04 to 0.13 inches), or 0.1 to 3 millimeters (0.04 to 0.11 inches).
4. a first polymer foam layer comprising: A compressive force deflection at 25% deflection determined in accordance with ASTM D3574-17 of 5 to 1,035 kPa, preferably 5 to 500 kPa; Compressive deflection of 100 to 500 kPa at 75% deflection determined in accordance with ASTM D3574-17; A compression set of 0 to 15% at 50% deflection at 23°C or 70°C, determined in accordance with ASTM D3574-95, Test D; or Combinations of these 4. The multilayer material according to claim 1 , further comprising:
5. Each of the first polymer foam layer and the second polymer foam layer is independently selected from the group consisting of polyacetal, poly(C 1~6 alkyl)acrylate, polyacrylic, polyamide, polyamideimide, polyanhydride, polyarylate, polyarylene ether, polyarylene sulfide, polybenzoxazole, polycarbonate, polyester, polyetheretherketone, polyetherimide, polyetherketoneketone, polyetherketone, polyethersulfone, polyisocyanurate, polyimide, poly(C 1~6 poly(alkyl)methacrylates, poly((meth)acrylic acid), polyphthalides, polyolefins (such as fluorinated polyolefins), polysilazanes, polystyrenes, polysulfides, polysulfonamides, polysulfonates, polythioesters, polytriazines, polyureas, polyvinyl alcohols, polyvinyl ethers, polyvinyl halides, polyvinyl ketones, polyvinylidene fluorides, polyvinyl esters, crosslinked poly(esters), epoxy resins, melamines, phenolic polymers, polyurethanes, urea-formaldehyde, silicones, natural rubber, polychloroprene, ethylene-propylene-diene monomer (EPDM) rubber, or combinations thereof; Preferably, each of the first polymer foam layer and the second polymer foam layer independently comprises an epoxy resin, a polyurethane, or a combination thereof. The multi-layer material of claim 1 .
6. 6. The multilayer material of claim 1, wherein the first polymer foam layer comprises a polyurethane foam.
7. The second polymer foam has a strength of 240 to 1,000 kg / m 3 (15-62 lb / ft 3 ), or 288 to 1,000 kg / m 3 (18-62 lb / ft 3 ), or 350 to 950 kg / m 3 (22-59 lb / ft 3 ), or 400 to 950 kg / m 3 (25-59 lb / ft 3 7. The multilayer material according to claim 1 , having a density of
8. The multi-layer material of claim 7 , wherein the second polymeric foam layer comprises a polyurethane foam.
9. 9. The multilayer material of claim 1, wherein the flame retardant composition of each of the first and second polymeric foam layers independently comprises a metal hydroxide, a metal oxide, a metal borate, a metal carbonate, a melamine, a halogenated aromatic compound, a guanidine, carbon black, expandable graphite, a nanoclay, an organic phosphorus-containing compound, a silazane, a rimal salt, or a combination thereof.
10. 10. The multi-layer material of any one of claims 1 to 9, wherein the flame retardant composition of each of the compressible foam layer and the flame retardant layer is independently free of halogenated flame retardants or antimony compounds.
11. A compression force deflection at 25% deflection determined in accordance with ASTM D3574-17 of 5 to 1,035 kPa, preferably 5 to 500 kPa, or 25 to 250 kPa, or 25 to 80 kPa; Compressive deflection of 100-500 kPa or 200-300 kPa at 75% deflection; A compression set of 0-15%, or 0-5%, at 50% deflection at 23°C or 70°C, as determined in accordance with ASTM D3574-95, Test D; or Combinations of these 11. The multilayer material according to claim 1 , having
12. The multi-layer material of claim 11 , wherein the first polymer foam layer comprises polyurethane.
13. A method for producing a multilayer material according to any one of claims 1 to 12, comprising the steps of: forming a first polymer foam layer and a second polymer foam layer; contacting the first polymeric foam layer with the second polymeric foam layer under conditions effective to adhere the layers together to form a multi-layer material; A method comprising:
14. A method for producing a multilayer material according to any one of claims 1 to 12, comprising the steps of: forming one of a first polymer foam layer and a second polymer foam layer; forming another of the first and second polymer foam layers on a surface of the formed layer to provide a multi-layer material; A method comprising:
15. A method for producing a multilayer material according to any one of claims 1 to 12, comprising the steps of: forming a first polymer foam layer and a second polymer foam layer simultaneously to provide a multi-layer material. A method comprising:
16. Simultaneously forming a first polymer foam layer and a second polymer foam layer, mechanically foaming a first reactive polyurethane foam-forming composition; mechanically foaming the second reactive polyurethane foam-forming composition; simultaneously casting the first and second mechanically foamed foams to provide a cast bilayer; curing the cast bilayer under conditions effective to form a multi-layer material; 16. The method of claim 15, comprising:
17. 13. An electronic device comprising a multilayer material according to any one of claims 1 to 12, preferably a handheld electronic device.
Citation Information
Patent Citations
Composite panel with flame resistant and fireproof performance
JP1989186318A
Polyurethane foam laminate
JP2010221585A
Multilayered structure
JP2012166387A
Double-sided adhesive tape, method of making, method of use, and article assembled therefrom
JP2017506683A
Expanded sheet and adhesive tape
JP2019137795A