Polishing composition and method of use thereof

The polishing composition effectively addresses the challenge of ruthenium and copper removal in semiconductor manufacturing by using anionic silica abrasive and pH adjusters, achieving high ruthenium removal rates with minimal copper corrosion and improved selectivity.

JP2024541266APending Publication Date: 2024-11-08FUJIFILM ELECTRONIC MATERIALS U S A INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024525729
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-28
Filing Date
2022-10-21
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Current CMP slurries struggle to effectively remove ruthenium and copper while minimizing copper corrosion and maintaining selectivity in advanced semiconductor manufacturing, particularly in back-end applications where ruthenium is used as a liner material due to its conductivity and resistance to Cu diffusion.

Method used

A polishing composition comprising anionic silica abrasive, pH adjuster, low-k removal rate inhibitor, ruthenium removal rate enhancer, and water, optionally including additional components like barrier film removal rate enhancers, azole-containing rust inhibitors, chelating agents, and oxidizing agents, formulated to maintain a pH of 7 to 14, which enhances ruthenium removal while minimizing copper corrosion.

Benefits of technology

The composition achieves high ruthenium removal rates with minimal copper corrosion and improved selectivity, reducing defects and maintaining substrate quality in semiconductor processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541266000001_ABST
    Figure 2024541266000001_ABST
Patent Text Reader

Abstract

The polishing composition comprises an anionic abrasive, a pH adjuster, a low-k removal rate inhibitor, a ruthenium removal rate enhancer, and water. A method of polishing a substrate comprises applying a polishing composition described herein to a surface of a substrate, the surface comprising ruthenium or a hard mask material; and contacting the surface of the substrate with a pad and moving the pad relative to the substrate.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to polishing compositions and methods of use thereof. [Background technology]

[0002] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority from U.S. Provisional Application No. 63 / 272,719, filed October 28, 2021, the contents of which are incorporated by reference in their entirety into this disclosure.

[0003] The semiconductor industry is constantly driven to improve chip performance by further miniaturization of devices through process, material, and integration innovations. Previous material innovations include the introduction of copper to replace aluminum as the conductive material in interconnect structures and the use of tantalum (Ta) / tantalum nitride (TaN) as a diffusion barrier to separate Cu conductive material from non-conductive / insulating dielectric materials. Copper (Cu) was chosen as the interconnect material due to its low resistivity and excellent resistance to electromigration.

[0004] However, as newer chip features shrink, multi-layer Cu / barrier / dielectric stacks must become thinner and more conformal to maintain effective interconnect resistivity in the back-end (BEOL). Thinner Cu and Ta / TaN barrier film schemes present issues with resistivity and flexibility in deposition. For example, with smaller dimensions and advanced manufacturing nodes, resistivity is exponentially worsening, and improvements in transistor circuit speed (in the front-end (FEOL)) are halved by delays from conductive Cu / barrier interconnects (BEOL). Ruthenium (Ru) has emerged as a leading candidate for use as a liner material, barrier layer, and conductive layer. Ruthenium has excellent Cu diffusion resistance to dielectric layers, but also promotes copper electrofill directly into small dimension trenches without the use of a copper seed layer. Additionally, ruthenium is also being investigated as a material for vias to replace traditional tungsten (W) metal. Summary of the Invention

[0005] This summary is provided to introduce a selection of concepts that are described below in the more detailed description. This summary is not intended to identify key or essential features of the claimed subject matter, nor is it intended to be used as an aid in limiting the scope of the claimed subject matter.

[0006] As used in this disclosure, unless otherwise specified, all recited percentages should be understood to be weight percentages based on the total weight of the polishing composition.

[0007] In one aspect, the present disclosure provides a method for producing a medicament for use in a method for treating a vascular endotheli (1) An anionic silica abrasive comprising an end group of formula (I): -O m -Si-(CH2) n -CH3(I) In the formula, m is an integer of 1 to 3, n is an integer of 0 to 10, and -(CH2) n an anionic silica abrasive, in which the -CH3 group is replaced with at least one carboxylic acid group; (2) pH adjuster; (3) low-k removal rate inhibitors; (4) a ruthenium removal rate enhancer; and (5)Water The subject matter relates to a polishing composition comprising a polishing composition comprising: a polishing composition having a pH of about 7 to about 14.

[0008] In another aspect, the present disclosure is directed to a method of polishing a substrate, comprising the steps of: applying a polishing composition described herein to a surface of a substrate, the surface comprising ruthenium or a hard mask material; and contacting the surface of the substrate with a pad and moving the pad relative to the substrate.

[0009] Other aspects and advantages of the claimed subject matter will become apparent from the following description and the appended claims. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a plot showing the change in zeta potential with changing pH for aqueous dispersions containing three different silica abrasives. [Diagram 2] FIG. 2 is a plot showing the change in mean particle size (MPS) over time for aqueous dispersions containing unmodified silica, cationically modified silica, sulfonic acid modified silica, and carboxylic acid modified silica. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Detailed Description

[0012] The disclosed embodiments generally relate to compositions and methods of using the compositions to polish substrates that include at least a ruthenium portion and / or a hardmask portion (e.g., tungsten, carbide, nitride ceramics (e.g., TiN), and doped derivatives thereof). The substrate may more specifically include at least a ruthenium portion, a hardmask portion, and a copper portion. The compositions described herein can effectively remove ruthenium, copper, and / or hardmask materials while minimizing copper corrosion (e.g., minimizing surface roughness). For example, the compositions described herein can effectively remove copper, ruthenium liners, hardmask materials (e.g., titanium and doped derivatives thereof, tungsten and doped derivatives thereof (e.g., WB), carbides (e.g., BC, B4C, TiC, SiC, and WC), boron-containing materials (e.g., BO, BCN, and AlMgB 14 ), as well as advanced node films including nitride ceramic materials (e.g., SiN, TiN, BN), barrier materials (e.g., Ta, TaN), and dielectric materials (e.g., TEOS, low-k, ultra low-k, etc.). In some embodiments, the compositions described herein can remove copper at relatively high removal rates while minimizing copper corrosion (e.g., minimizing surface roughness).

[0013] Many of the currently available CMP slurries are specifically designed to remove materials more common in legacy chip designs, such as the aforementioned copper and tungsten. However, in back-end (BEOL) applications in the semiconductor industry, ruthenium is finding use as a liner material due to its good electrical conductivity, deposition properties, and resistance to Cu diffusion. Unlike some other materials, such as cobalt and copper, ruthenium is relatively stable chemically and therefore does not degrade, and can be difficult to remove during polishing. Furthermore, ruthenium is often used in combination with copper, which is a conductive layer. As mentioned above, copper is a relatively soft material and therefore easy to remove. Copper is essential to the function of many semiconductor devices, and thus the use of a CMP slurry that too easily strips or damages the copper layer or copper inlay can adversely affect the performance of the finished device. Legacy CMP slurries may not be able to effectively remove ruthenium without causing harmful and unacceptable defects in the copper, which is more susceptible to chemical attack. As a result, less advanced slurries may exhibit unacceptable erosion, wafer topology, and / or removal rate selectivity for one or more components of the multi-component substrate being polished. Additionally, more complex integration schemes may employ a hard mask as an etch mask in combination with a Ru liner and a Cu conductive layer, which presents yet another material that must be effectively removable by the polishing slurry.

[0014] With the increased use and decreasing size of multi-component integration schemes in semiconductor fabrication, there is a market need for CMP slurries that can effectively polish substrates containing ruthenium, copper, and hardmask materials with minimal copper corrosion, but with good removal rates and selectivity for all other components.

[0015] In one or more embodiments, the polishing composition described herein comprises an anionic silica abrasive, a pH adjuster, a low-k removal rate inhibitor, a ruthenium removal rate enhancer, and water. In one or more embodiments, the polishing composition may optionally comprise a barrier film removal rate enhancer, an azole-containing rust inhibitor, a chelating agent, and / or an oxidizing agent. In one or more embodiments, the polishing composition described herein may comprise about 0.1 wt % to about 50 wt % abrasive, about 0.0001 wt % to about 30 wt % pH adjuster, about 0.0005 wt % to about 5 wt % low-k removal rate inhibitor, about 0.0001 wt % to about 5 wt % ruthenium removal rate enhancer, and the remaining wt % (e.g., about 20 wt % to about 99 wt %) of a solvent (e.g., deionized water). In one or more embodiments, the polishing composition may further comprise about 0.002 wt % to about 4 wt % of a barrier film removal rate enhancing agent, about 0.0001 wt % to about 1 wt % of an azole-containing rust inhibitor, about 0.001 wt % to about 1 wt % of a chelating agent, and / or about 0.001 wt % to about 5 wt % of an oxidizing agent.

[0016] In one or more embodiments, the present disclosure provides concentrated polishing compositions that can be diluted with water up to a factor of two, or up to a factor of four, or up to a factor of six, or up to a factor of eight, or up to a factor of ten prior to use. In other embodiments, the present disclosure provides point-of-use (POU) polishing compositions for use on ruthenium-containing substrates, the POU polishing composition comprising the polishing composition described above, water, and optionally an oxidizing agent.

[0017] In one or more embodiments, the polishing composition described herein may comprise at least one (e.g., two or three) anionic silica abrasives. In one or more embodiments, the at least one anionic silica abrasive may comprise one or more (e.g., two or three) end groups of formula (I). -O m -Si-(CH2) n -CH3(I) In the formula, m is an integer of 1 to 3, n is an integer of 0 to 10, and -(CH2) n The -CH group is substituted with at least one (e.g., two, three, or four) carboxylic acid group. In some embodiments, the substitution with a carboxyl group is -(CH) n The -CH3 group may be at the central carbon and / or at the terminal carbon. In some embodiments, the terminal group may be a terminal group of formula (II). -O m -Si-(CH2) n -CH (3-p) Y p (II) In the formula, m is an integer of 1 to 3, n is an integer of 0 to 10, p is an integer of 1 to 3, and Y is a carboxylic acid group.

[0018] In some embodiments, the at least one anionic silica abrasive may be of high purity and have less than about 100 ppm alcohol, less than about 100 ppm ammonia, and about 100 parts per billion (ppb) alkali cations (e.g., sodium cations).Without wishing to be bound by theory, it is believed that the anionic silica abrasive containing carboxylic acid groups can significantly reduce defects formed on a semiconductor substrate polished by the polishing composition.

[0019] In one or more embodiments, the abrasives described herein may have an average particle size of about 1 nm or more (e.g., about 5 nm or more, about 10 nm or more, about 20 nm or more, about 40 nm or more, about 50 nm or more, about 60 nm or more, about 80 nm or more, or about 100 nm or more) to about 1000 nm or less (e.g., about 800 nm or less, about 600 nm or less, about 500 nm or less, about 400 nm or less, about 200 nm or less, or about 150 nm or less). As used in this disclosure, average particle size (MPS) is determined by dynamic light scattering techniques. In one or more embodiments, the abrasives may be particles of a single chemical species (e.g., silica particles), and the polishing composition may not include an abrasive that is a composite of two or more materials (e.g., silica particles embedded in a ceramic matrix).

[0020] In one or more embodiments, the at least one anionic silica abrasive is present in an amount of about 0.1 wt.% or more (e.g., about 0.5 wt.% or more, about 1 wt.% or more, about 2 wt.% or more, about 4 wt.% or more, about 5 wt.% or more, about 10 wt.% or more, about 12 wt.% or more, about 15 wt.% or more, or about 20 wt.% or more) to about 50 wt.% or less (e.g., about 45 wt.% or less, about 40 wt.% or less, about 35 wt.% or less, about 30 wt.% or less, about 25 wt.% or less, about 20 wt.% or less, about 15 wt.% or less, about 12 wt.% or less, about 10 wt.% or less, or about 5 wt.% or less) of the polishing composition described herein.

[0021] In one or more embodiments, the polishing composition described herein may include at least one (eg, two or three) pH adjuster or pH adjusting agent. In some embodiments, the at least one pH adjuster is selected from the group consisting of formic acid, acetic acid, malonic acid, citric acid, propionic acid, malic acid, adipic acid, succinic acid, lactic acid, oxalic acid, peracetic acid, potassium acetate, phenoxyacetic acid, benzoic acid, nitric acid, sulfuric acid, sulfurous acid, phosphoric acid, phosphonic acid, hydrochloric acid, periodic acid, lithium hydroxide, potassium hydroxide, sodium hydroxide, cesium hydroxide, ammonium hydroxide, triethanolamine, diethanolamine, monoethanolamine, methylethanolamine, methyldiethanolamine, tetrabutylammonium hydroxide, tetrapropylammonium hydroxide, tetraethylammonium hydroxide, tetramethylammonium hydroxide, ethyltrimethylammonium hydroxide, diethyldimethylammonium hydroxide, dimethyldipropylammonium hydroxide, benzyltrimethylammonium hydroxide, tris(2-hydroxyethyl)methylammonium hydroxide, choline hydroxide, and mixtures thereof. In one or more embodiments, the pH adjuster is a monocarboxylic acid, a dicarboxylic acid, or a tricarboxylic acid.

[0022] In one or more embodiments, the at least one pH adjuster comprises about 0.0001 wt % or more (e.g., about 0.0005 wt % or more, about 0.001 wt % or more, about 0.005 wt % or more, about 0.01 wt % or more, about 0.05 wt % or more, about 0.1 wt % or more, about 0.5 wt % or more, about 1 wt % or more, about 2 wt % or more, about 4 wt % or more, about 5 wt % or more, about 6% or more, or about 8% or more) to about 30% or less (e.g., about 25% or less, about 20% or less, about 15% or less, about 10% or less, about 9% or less, about 8% or less, about 7% or less, about 6% or less, about 5% or less, about 4% or less, about 3% or less, about 2% or less, about 1% or less, about 0.5% or less, about 0.2% or less, or about 0.1% or less).

[0023] In one or more embodiments, the pH value of the polishing composition may be about 7 or more (e.g., about 7.5 or more, about 8 or more, about 8.5 or more, about 9 or more, about 9.5 or more, about 10 or more, about 10.5 or more, about 11 or more, about 11.5 or more, or about 12 or more) to about 14 or less (e.g., about 13.5 or less, about 13 or less, about 12.5 or less, about 12 or less, about 11.5 or less, about 11 or less, about 10.5 or less, about 10 or less, about 9.5 or less, or about 9 or less). Without wishing to be bound by theory, it is believed that a polishing composition having a pH lower than 7 significantly increases the copper removal rate and corrosion, and a polishing composition having a pH higher than 14 affects the stability of the suspended abrasive and significantly increases the roughness and reduces the overall quality of the film polished by the composition.

[0024] In one or more embodiments, the polishing composition described herein may include at least one (e.g., two or three) low-k removal rate inhibitor. In some embodiments, the at least one low-k removal rate inhibitor is a nonionic surfactant. In one or more embodiments, the nonionic surfactant is selected from the group consisting of alcohol alkoxylates, alkylphenol alkoxylates, tristyrylphenol alkoxylates, sorbitan ester alkoxylates, polyalkoxylates, polyalkylene oxide block copolymers, alkoxylated diamines, and mixtures thereof. In one or more embodiments, the nonionic surfactant does not include an alkylphenol alkoxylate. In one or more embodiments, the nonionic surfactant is a polymer having a number average molecular weight of about 500 g / mol or more, or about 1,000 g / mol or more, or about 2,500 g / mol or more, or about 5,000 g / mol or more, or about 7,500 g / mol or more, or about 10,000 g / mol or more. In one or more embodiments, the nonionic surfactant is a polymer having a number average molecular weight of about 1,000,000 g / mol or less, or about 750,000 g / mol or less, or about 500,000 g / mol or less, or about 250,000 g / mol or less, or about 100,000 g / mol or less. In one or more embodiments, the alkoxylate group of the alkoxylated nonionic surfactant is an ethoxylate, a propoxylate, or a combination of an ethoxylate group and a propoxylate group. Without wishing to be bound by theory, it is surprising that the nonionic surfactant (such as the one described above) can be used as a low-k removal rate inhibitor in the polishing composition described in the present disclosure, thereby reducing or minimizing the removal rate of low-k films (e.g., carbon-doped silicon oxide films) in semiconductor substrates.

[0025] In one or more embodiments, the low-k removal rate inhibitor is present in an amount of about 0.0005 wt.% or more (e.g., about 0.001 wt.% or more, about 0.005 wt.% or more, about 0.01 wt.% or more, about 0.05 wt.% or more, about 0.1 wt.% or more, about 0.5 wt.% or more, about 1 wt.% or more, about 1.5 wt.% or more, about 2 wt.% or more, or about 3 wt.% or more) to about 5 wt.% or less (e.g., about 4.5 wt.% or less, about 4 wt.% or less, about 3.5 wt.% or less, about 3 wt.% or less, about 2.5 wt.% or less, about 2 wt.% or less, about 1.5 wt.% or less, about 1 wt.% or less, about 0.5 wt.% or less, or about 0.1 wt.% or less) relative to the polishing composition described herein.

[0026] In one or more embodiments, the polishing composition described herein may include at least one (e.g., two or three) ruthenium removal rate enhancing agent. In some embodiments, the at least one ruthenium removal rate enhancing agent may include ammonium hydroxide or a salt thereof, a thiocyanate, a nitric acid or a salt thereof, and / or a halide salt. In some embodiments, the at least one ruthenium removal rate enhancing agent is selected from the group consisting of ammonium hydroxide, ammonium chloride, ammonium fluoride, ammonium bromide, ammonium sulfate, ammonium carbonate, ammonium bicarbonate, ammonium nitrate, ammonium phosphate, ammonium acetate, ammonium thiocyanate, potassium thiocyanate, sodium thiocyanate, sulfuric acid, sulfurous acid, phosphoric acid, phosphonic acid, hydrochloric acid, periodic acid, nitric acid, sodium nitrate, potassium nitrate, rubidium nitrate, cesium nitrate, sodium fluoride, potassium fluoride, rubidium fluoride, cesium fluoride, sodium chloride, potassium chloride, rubidium chloride, cesium chloride, and mixtures thereof.

[0027] In one or more embodiments, the ruthenium removal rate enhancing agent is in an amount of about 0.0001 wt % to about 5 wt % of the composition. In one or more embodiments, the ruthenium removal rate enhancing agent is in an amount of about 0.0001 wt % or more (e.g., about 0.0002 wt % or more, about 0.0005 wt % or more, about 0.001 wt % or more, about 0.002 wt % or more, about 0.005 wt % or more, about 0.01 wt % or more, about 0.02 wt % or more, about 0.05 wt % or more, about 0.1 wt % or more, about 0. 2% by weight or more, or about 0.5% by weight or more) to about 5% by weight or less (e.g., 4% by weight or less, about 3% by weight or less, about 2% by weight or less, about 1% by weight or less, about 0.8% by weight or less, about 0.6% by weight or less, about 0.5% by weight or less, about 0.4% by weight or less, about 0.2% by weight or less, about 0.1% by weight or less, about 0.05% by weight or less, about 0.02% by weight or less, about 0.01% by weight or less, or about 0.005% by weight or less).

[0028] In one or more embodiments, the polishing composition described herein may optionally include at least one (e.g., two or three) barrier film removal rate enhancing agent. In some embodiments, the at least one barrier film removal rate enhancing agent is an organic acid (such as a carboxylic acid, an amino acid, a sulfonic acid, or a phosphonic acid) or a salt thereof. In some embodiments, the barrier film removal rate enhancing agent may be an organic acid or a salt thereof selected from the group consisting of gluconic acid, lactic acid, citric acid, tartaric acid, malic acid, glycolic acid, malonic acid, formic acid, oxalic acid, acetic acid, propionic acid, peracetic acid, succinic acid, lactic acid, aminoacetic acid, phenoxyacetic acid, bicine, diglycolic acid, glyceric acid, tricine, alanine, histidine, valine, phenylalanine, proline, glutamine, aspartic acid, glutamic acid, arginine, lysine, tyrosine, benzoic acid, salts thereof, and mixtures thereof. In some embodiments, if the polishing composition described herein includes both a barrier film removal rate enhancing agent and a pH adjuster (or other acidic material, such as a chelating agent or an amino acid), the barrier film removal rate enhancing agent is different from the pH adjuster (or other acidic material). Without wishing to be bound by theory, it is believed that an organic acid or a salt thereof (e.g., those described above) can be used as an effective barrier film removal rate enhancing agent in the polishing composition described herein, thereby improving the removal rate of a barrier film (e.g., a Ta film or a TaN film) in a semiconductor substrate.

[0029] In one or more embodiments, the barrier film removal rate increasing agent is present in an amount of about 0.002 wt % or more (e.g., about 0.005 wt % or more, about 0.01 wt % or more, about 0.05 wt % or more, about 0.1 wt % or more, about 0.15 wt % or more, about 0.2 wt % or more, about 0.5 wt % or more, about 1 wt % or more, about 1.5 wt % or more, or about 2 wt % or more) to about 4 wt % or less (e.g., about 3.5 wt % or less, about 3 wt % or less, about 2.5 wt % or less, about 2 wt % or less, about 1.5 wt % or less, or about 1 wt % or less) relative to the polishing composition described herein.

[0030] In one or more embodiments, the polishing composition described herein may optionally include at least one (e.g., two or three) azole-containing rust inhibitor. In some embodiments, the at least one azole-containing rust inhibitor is selected from the group consisting of substituted or unsubstituted triazole, substituted or unsubstituted tetrazole, substituted or unsubstituted benzotriazole, substituted or unsubstituted pyrazole, and substituted or unsubstituted imidazole. In some embodiments, suitable substituents include halo (e.g., F, Cl, Br, or I), amino, aryl, or C1-C6 alkyl optionally substituted with aryl. In one or more embodiments, the azole-containing rust inhibitor is selected from the group consisting of 1,2,4-triazole, 1,2,3-triazole, tetrazole, benzotriazole, tolyltriazole, methylbenzotriazole (e.g., 1-methylbenzotriazole, 4-methylbenzotriazole, and 5-methylbenzotriazole), ethylbenzotriazole (e.g., 1-ethylbenzotriazole), propylbenzotriazole (e.g., 1-propylbenzotriazole), butylbenzotriazole (e.g., 1-butylbenzotriazole and 5-butylbenzotriazole), pentylbenzotriazole (e.g., 1-pentylbenzotriazole), hexylbenzotriazole, ... The benzotriazole may be selected from the group consisting of triazoles (e.g., 1-hexylbenzotriazole and 5-hexylbenzotriazole), dimethylbenzotriazoles (e.g., 5,6-dimethylbenzotriazole), chlorobenzotriazoles (e.g., 5-chlorobenzotriazole), dichlorobenzotriazoles (e.g., 5,6-dichlorobenzotriazole), chloromethylbenzotriazoles (e.g., 1-(chloromethyl)-1-H-benzotriazole), chloroethylbenzotriazole, phenylbenzotriazole, benzylbenzotriazole, aminotriazole, aminobenzimidazole, aminotetrazole, isothiazole, and mixtures thereof.In one or more embodiments, the polishing composition may include both benzotriazole and a benzotriazole derivative (e.g., a substituted benzotriazole). Without wishing to be bound by theory, it is believed that azole-containing corrosion inhibitors (such as those described above) can significantly reduce or minimize the removal rate of copper in semiconductor substrates.

[0031] In one or more embodiments, the azole-containing rust inhibitor is present in an amount of 0.0001 wt.% or more (e.g., about 0.0002 wt.% or more, about 0.0005 wt.% or more, about 0.001 wt.% or more, about 0.002 wt.% or more, about 0.005 wt.% or more, about 0.01 wt.% or more, about 0.02 wt.% or more, about 0.05 wt.% or more, about 0.1 wt.% or more, about 0.2 wt.% or more, or about 0.5 wt.% or more) to about 1 wt.% or less (e.g., about 0.8 wt.% or less, about 0.6 wt.% or less, about 0.5 wt.% or less, about 0.4 wt.% or less, about 0.2 wt.% or less, about 0.1 wt.% or less, about 0.05 wt.% or less, about 0.02 wt.% or less, about 0.01 wt.% or less, about 0.005 wt.% or less).

[0032] In one or more embodiments, the polishing composition described herein may optionally include at least one (e.g., two or three) chelating agent. In some embodiments, the at least one optional chelating agent may be an amino-containing carboxylic acid (e.g., a polyaminopolycarboxylic acid) or a phosphonic acid. In some embodiments, the chelating agent is selected from the group consisting of ethylenediaminetetraacetic acid, iminodiacetic acid, N-hydroxyethyl-ethylenediaminetriacetic acid, nitrilotriacetic acid, diethylenetriaminepentaacetic acid, hydroxyethylethylenediaminetriacetic acid, triethylenetetraaminehexaacetic acid, diaminocyclohexanetetraacetic acid, nitrilotrimethylphosphonic acid, ethylenediaminetetra(methylenephosphonic acid), 1-hydroxyethylidene-1,1-diphosphonic acid, diethylenetriaminepenta(methylenephosphonic acid), hydroxyethylidenediphosphonic acid, 2-phosphono-1,2,4-butanetricarboxylic acid, aminotrimethylenephosphonic acid, hexamethylenediaminetetra(methylenephosphonic acid), bis(hexamethylene)triaminephosphonic acid, aminoacetic acid, and combinations thereof. In some embodiments, if the polishing composition described herein includes both a chelating agent and a pH adjuster (or other acidic material, such as a barrier film removal rate enhancing agent or an amino acid), the chelating agent is different from the pH adjuster (or other acidic material). Without wishing to be bound by theory, it is believed that including a chelating agent (such as those described above) in the polishing composition described herein can significantly reduce or minimize defects observed on semiconductor substrates (such as defects on the surface of a copper wafer).

[0033] In one or more embodiments, the chelating agent is present in an amount of 0.001 wt.% or more (e.g., about 0.002 wt.% or more, about 0.005 wt.% or more, about 0.01 wt.% or more, about 0.02 wt.% or more, about 0.05 wt.% or more, about 0.1 wt.% or more, about 0.2 wt.% or more, or about 0.5 wt.% or more) to about 1 wt.% or less (e.g., about 0.8 wt.% or less, about 0.6 wt.% or less, about 0.5 wt.% or less, about 0.4 wt.% or less, about 0.2 wt.% or less, about 0.1 wt.% or less, about 0.05 wt.% or less, about 0.02 wt.% or less, about 0.01 wt.% or less, or about 0.005 wt.% or less).

[0034] An optional oxidizer (or oxidizing agent) may be added when diluting the concentrated slurry to form the POU slurry. The oxidizer may be selected from the group consisting of hydrogen peroxide, orthoperiodic acid, metaperiodic acid, dimesoperiodic acid, diorthoperiodic acid, ammonium periodate, potassium periodate, sodium periodate, ammonium persulfate, iodic acid, iodate salts, perchloric acid, perchlorate salts, hydroxylamine and hydroxylamine salts, and any combination thereof. In one or more embodiments, the oxidizer may be hydrogen peroxide.

[0035] In one or more embodiments, the oxidizing agent is present in an amount of about 0.001 wt% or more (e.g., about 0.002 wt% or more, about 0.004 wt% or more, about 0.005 wt% or more, about 0.01 wt% or more, about 0.025 wt% or more, about 0.05 wt% or more, about 0.075 wt% or more, about 0.1 wt% or more, about 0.5 wt% or more, about 1 wt% or more, or about 2 wt% or more) to about 5 wt% or less (e.g., about 4.5 wt% or less, about 4 wt% or less, about 3.5 wt% or less, about 3 wt% or less, about 2.5 wt% or less, about 2 wt% or less, about 1.5 wt% or less, about 1 wt% or less, about 0.5 wt% or less, or about 0.1 wt% or less) relative to the polishing composition described herein. In some embodiments, without wishing to be bound by theory, it is believed that the oxidizing agent can aid in removing hardmask material in a substrate that includes a hardmask.

[0036] In one or more embodiments, the polishing compositions described herein may include a solvent (e.g., a primary solvent) such as water. In some embodiments, the solvent (e.g., water) is present in an amount of about 20% by weight or more (e.g., about 25% by weight or more, about 30% by weight or more, about 35% by weight or more, about 40% by weight or more, about 45% by weight or more, about 50% by weight or more, about 55% by weight or more, about 60% by weight or more, about 65% by weight or more, about 70% by weight or more, about 75% by weight or more, about 80% by weight or more, about 85% by weight or more, about 90% by weight or more, about 92% by weight or more, about 94% by weight or more, about 95% by weight or more, or about 97% by weight or more) to about 99% by weight or less (e.g., about 98% by weight or less, about 96% by weight or less, about 94% by weight or less, about 92% by weight or less, about 90% by weight or less, about 85% by weight or less, about 80% by weight or less, about 75% by weight or less, about 70% by weight or less, or about 65% by weight or less).

[0037] In one or more embodiments, an optional secondary solvent (e.g., an organic solvent) may be used in the polishing composition (e.g., POU polishing composition or concentrated polishing composition) of the present disclosure, which may aid in dissolving components such as an azole-containing rust inhibitor. In one or more embodiments, the secondary solvent may include one or more types of alcohol, alkylene glycol, or alkylene glycol ether. In one or more embodiments, the secondary solvent includes one or more types of solvent selected from the group consisting of ethanol, 1-propanol, 2-propanol, n-butanol, propylene glycol, 2-methoxyethanol, 2-ethoxyethanol, propylene glycol propyl ether, dimethyl sulfoxide, and ethylene glycol.

[0038] In one or more embodiments, the second solvent is present in an amount of about 0.0025 wt % or more (e.g., about 0.005 wt % or more, about 0.01 wt % or more, about 0.02 wt % or more, about 0.05 wt % or more, about 0.1 wt % or more, about 0.2 wt % or more, about 0.4 wt % or more, about 0.5 wt % or more, about 0.6 wt % or more, about 0.8 wt % or more, or about 1 wt % or more) to about 5 wt % or less (e.g., about 4 wt % or less, about 3 wt % or less, about 2 wt % or less, about 1 wt % or less, about 0.8 wt % or less, about 0.6 wt % or less, about 0.5 wt % or less, or about 0.1 wt % or less) relative to the polishing composition described herein.

[0039] In one or more embodiments, the polishing composition described herein can comprise any of a number of additives, such as an organic solvent, a pH adjusting agent or pH adjusters, a quaternary ammonium compound (e.g., a salt or hydroxide), an amine, an alkali base (such as an alkali hydroxide), a fluorine-containing compound (e.g., a fluoride compound or a fluorinated compound (e.g., a polymer / surfactant)), a silicon-containing compound such as a silane (e.g., an alkoxysilane or an inorganic silicate), an imine (e.g., an amidine such as 1,8-diazabicyclo[5.4.0]-7-undecene (DBU) and 1,5-diazabicyclo[4.3.0]non-5-ene (DBN)), a salt (e.g., a halide salt or a metal salt), a polymer (e.g., a tertiary ammonium salt), a tertiary ammonium salt, ... The polishing composition may be substantially free of one or more specific components, such as a polymer (e.g., cationic or anionic polymer), a surfactant (e.g., a cationic surfactant, an anionic surfactant, or a nonionic surfactant), a plasticizer, an oxidizer (e.g., H2O2 or periodic acid), a rust inhibitor (e.g., an azole rust inhibitor or a non-azole rust inhibitor), an electrolyte (e.g., a polyelectrolyte), and / or a certain abrasive (e.g., a polymeric abrasive, a ceria abrasive, a nonionic abrasive, a surface-modified abrasive, a ceramic abrasive composite, or a negatively / positively charged abrasive). Halide salts that may be absent from the polishing composition include alkali metal halides (e.g., sodium halide or potassium halide) or ammonium halides (e.g., ammonium chloride), and may be fluorides, chlorides, bromides, or iodides. As used in this disclosure, a component that is "substantially free" from the polishing composition refers to a component that is not intentionally added to the polishing composition. In some embodiments, the polishing composition described herein may have about 1000 ppm or less (e.g., about 500 ppm or less, about 250 ppm or less, about 100 ppm or less, about 50 ppm or less, about 10 ppm or less, or about 1 ppm or less) of one or more of the above components that are substantially absent from the polishing composition. In some embodiments, the polishing composition described herein may be completely free of one or more of the above components.

[0040] The present disclosure also contemplates methods of using any of the above polishing compositions (e.g., concentrates or POU slurries). For concentrates, the methods may include diluting the concentrate (e.g., by 2x or more) to form a POU slurry, and then contacting a surface at least partially comprising ruthenium and / or a hardmask material with the POU slurry. In some embodiments, an oxidizer may be added to the slurry before, after, or during the dilution. For POU slurries, the methods may include contacting a surface at least partially comprising ruthenium and / or a hardmask material with the slurry.

[0041] In one or more embodiments, the present disclosure is directed to a polishing method that may include applying a polishing composition according to the present disclosure to a substrate (e.g., a wafer) having at least ruthenium and / or a hard mask material on a surface of the substrate; and contacting the surface of the substrate with a pad and moving the pad relative to the substrate. In some embodiments, when the substrate includes at least one or more of silicon oxide, ruthenium, copper, a hard mask material, and / or a barrier material (e.g., Ta and / or TaN), the above method can effectively polish the substrate without significant corrosion or undesirable removal rate selectivity. In one or more embodiments, the copper removal rate is less than about 500 angstroms / min (e.g., less than about 400 angstroms / min, less than about 300 angstroms / min, less than about 200 angstroms / min, less than about 150 angstroms / min, less than about 125 angstroms / min, less than about 100 angstroms / min, less than about 90 angstroms / min, less than about 80 angstroms / min, or less than about 70 angstroms / min). In one or more embodiments, the static etch rate (SER) of a 2 cm x 2 cm copper coupon incubated with a polishing composition according to the present disclosure at 45°C for 5 minutes is less than about 10 angstroms / min (e.g., less than about 8 angstroms / min, less than about 6 angstroms / min, less than about 5 angstroms / min, less than about 4 angstroms / min, less than about 3.5 angstroms / min, less than about 2 angstroms / min, or less than about 2.5 angstroms / min). In one or more embodiments, the ruthenium removal rate is about 3 angstroms / min or more (e.g., about 5 angstroms / min or more, about 15 angstroms / min or more, about 25 angstroms / min or more, about 35 angstroms / min or more, about 45 angstroms / min or more, or about 55 angstroms / min or more).

[0042] In one or more embodiments, the compositions and / or methods described herein can have a suitable copper / ruthenium removal rate ratio, for example, the ratio of copper removal rate to ruthenium removal rate (Cu:Ru) is about 35:1 or less (e.g., about 30:1 or less, about 25:1 or less, about 20:1 or less, about 15:1 or less, about 10:1 or less, about 5:1 or less, about 4:1 or less, about 3:1 or less, about 2.5:1 or less, about 2:1 or less, about 1.5:1 or less, or about 1:1 or less).

[0043] The term "silicon oxide" described in this disclosure is expressly intended to cover both undoped and doped forms of silicon oxide.For example, in one or more embodiments, the silicon oxide may be doped with at least one dopant selected from carbon, nitrogen (for silicon oxide), oxygen, hydrogen, or any other dopant for silicon oxide.Some examples of types of silicon oxide films include TEOS (tetraethyl orthosilicate), SiOC, SiOCN, SiOCH, SiOH, and SiON.

[0044] In one or more embodiments, the method of using the polishing composition described herein may further include manufacturing a semiconductor device from the substrate treated with the polishing composition through one or more steps. For example, photolithography, ion implantation, dry / wet etching, plasma etching, deposition (e.g., PVD, CVD, ALD, ECD), wafer mounting, die cutting, packaging, and inspection can be performed to manufacture a semiconductor device from the substrate treated with the polishing composition described herein.

[0045] The following specific examples are to be construed as merely illustrative, and not limiting in any way to the remainder of the disclosure, and without further elaboration, it is believed that one skilled in the art can, based on the description herein, utilize the present invention to its fullest extent. EXAMPLES

[0046] Polishing was performed on 200 mm wafers using an AMAT Mirra CMP polisher, a Fujibo soft pad, a downforce pressure of 1.5 psi, and a slurry flow rate of 100-400 mL / min.

[0047] Example 1 FIG. 1 shows a plot of the change in zeta potential with pH for aqueous dispersions of three different types of silica abrasives shown in the figure. Other than water and the abrasives, the aqueous dispersions contained no other components. FIG. 1 shows that in the range of approximately pH 5 to pH 8.5, the carboxylate-modified abrasives have a more negative zeta potential than the unmodified and sulfonic acid-modified abrasives. A more negative zeta potential within this range indicates that the carboxylate-modified abrasive dispersions are more stable than dispersions of unmodified or sulfonic acid-modified abrasives.

[0048] Example 2 Figure 2 shows a plot of the mean particle size (MPS) over time for aqueous dispersions of unmodified silica, cationically modified silica, sulfonic acid modified silica, and carboxylic acid modified silica. Each aqueous dispersion contained the same amount of abrasive, barrier film removal rate enhancer, azole, and ruthenium removal rate enhancer. The aqueous dispersions had a pH of 10 and were aged at 45°C for the times indicated. Table 1 below shows summary data from the plot of Figure 2.

[0049] [Table 1]

[0050] These results show that the carboxylic acid modified abrasive exhibited the most stable MPS over the 35 day test period, indicating very high stability for the dispersed particle solution.

[0051] Example 3 Table 2 below shows the particle stability of three different aqueous abrasive dispersions (i.e., one containing unmodified silica, one containing carboxylic acid modified silica, and one containing sulfonic acid modified silica) with and without the presence of copper ions in the aqueous dispersion. Each of the aqueous dispersions contains the same amount of abrasive, barrier film removal rate enhancer, azole, and ruthenium removal rate enhancer. Particle stability is measured by determining the "Transmission Stability Index" (TSI), which is determined by measuring the light transmission and backscattering of the sample. A higher TSI value indicates that the sample is less stable, has more particle aggregation, and poor dispersion. Measurements were performed at 35°C.

[0052] [Table 2]

[0053] Silica particle stability during metal polishing is very important from the defect point of view. Specifically, silica-metal aggregates can be formed due to the interaction between the abrasive and the metal ions generated during the action of polishing a metal substrate. Once these aggregates are formed, they can cause problems of scratching and / or residue on the polished substrate. Carboxylic acid modified abrasives showed the best stability in the presence of Cu ions, indicating that the carboxylic acid modified abrasives are more stable during the polishing process and have less potential for defect formation.

[0054] Example 4 Table 3 below shows the removal rates of Cu, Co, and CVD-Ru using blanket wafers when polished with polishing compositions containing unmodified silica abrasives, carboxylic acid-modified silica abrasives, or sulfonic acid-modified silica abrasives. All other ingredients in the polishing compositions were the same.

[0055] [Table 3]

[0056] These results show that the carboxylic acid modified silica was able to achieve Cu and Co removal rates as high as unmodified silica, while increasing the CVD-Ru removal rate by approximately 2-fold. In contrast, the sulfonic acid modified silica abrasive only increased the CVD-Ru removal rate compared to the unmodified abrasive, while the Cu and Co removal rates were lower. Furthermore, the carboxylic acid modified silica surprisingly produced more than 35% fewer defects on Cu than either the unmodified or sulfonic acid modified silica.

[0057] Although a few exemplary embodiments have been described in detail above, those skilled in the art will readily recognize that many modifications are possible in the exemplary embodiments without substantially departing from the invention, and all such modifications are intended to be included within the scope of the present disclosure as defined in the following claims.

Claims

1. An anionic silica abrasive comprising an end group of formula (I): -O m -Si-(CH 2 ) n -CH 3 (I) In the formula, m is an integer from 1 to 3, n is an integer from 0 to 10, and -(CH 2 ) n -CH 3 an anionic silica abrasive, wherein the group is substituted with at least one carboxylic acid group; pH adjuster; low-k removal rate inhibitors; A ruthenium removal rate enhancer; and water Including, having a pH of about 7 to about 14 Polishing composition.

2. 2. The polishing composition of claim 1, wherein the anionic silica abrasive is in an amount of about 0.01% to about 50% by weight of the composition.

3. 2. The polishing composition of claim 1, wherein the pH adjuster is selected from the group consisting of formic acid, acetic acid, malonic acid, citric acid, propionic acid, malic acid, adipic acid, succinic acid, lactic acid, oxalic acid, peracetic acid, potassium acetate, phenoxyacetic acid, benzoic acid, nitric acid, sulfuric acid, sulfurous acid, phosphoric acid, phosphonic acid, hydrochloric acid, periodic acid, lithium hydroxide, potassium hydroxide, sodium hydroxide, cesium hydroxide, ammonium hydroxide, triethanolamine, diethanolamine, monoethanolamine, methylethanolamine, methyldiethanolamine, tetrabutylammonium hydroxide, tetrapropylammonium hydroxide, tetraethylammonium hydroxide, tetramethylammonium hydroxide, ethyltrimethylammonium hydroxide, diethyldimethylammonium hydroxide, dimethyldipropylammonium hydroxide, benzyltrimethylammonium hydroxide, tris(2-hydroxyethyl)methylammonium hydroxide, choline hydroxide, and mixtures thereof.

4. 2. The polishing composition of claim 1, wherein the pH adjuster is in an amount of about 0.0001% to about 30% by weight of the composition.

5. The polishing composition of claim 1 , wherein the low-k removal rate inhibitor is a nonionic surfactant.

6. 6. The polishing composition of claim 5, wherein the nonionic surfactant is selected from the group consisting of alcohol alkoxylates, alkylphenol alkoxylates, tristyrylphenol alkoxylates, sorbitan ester alkoxylates, polyalkoxylates, polyalkylene oxide block copolymers, tetrahydroxy oligomers, alkoxylated diamines, and mixtures thereof.

7. 2. The polishing composition of claim 1, wherein the low-k removal rate inhibitor is in an amount of about 0.0005% to about 5% by weight of the composition.

8. 2. The polishing composition of claim 1, wherein the ruthenium removal rate enhancing agent is selected from the group consisting of ammonium hydroxide, ammonium chloride, ammonium fluoride, ammonium bromide, ammonium sulfate, ammonium carbonate, ammonium bicarbonate, ammonium nitrate, ammonium phosphate, ammonium acetate, ammonium thiocyanate, potassium thiocyanate, sodium thiocyanate, nitric acid, sulfuric acid, sulfurous acid, phosphoric acid, phosphonic acid, hydrochloric acid, periodic acid, sodium nitrate, potassium nitrate, rubidium nitrate, cesium nitrate, sodium fluoride, potassium fluoride, rubidium fluoride, cesium fluoride, sodium chloride, potassium chloride, rubidium chloride, cesium chloride, and mixtures thereof.

9. 2. The polishing composition of claim 1, wherein the ruthenium removal rate enhancing agent is in an amount of about 0.0001% to about 5% by weight of the composition.

10. 2. The polishing composition of claim 1, further comprising a chelating agent selected from the group consisting of ethylenediaminetetraacetic acid, iminodiacetic acid, N-hydroxyethyl-ethylenediaminetriacetic acid, nitrilotriacetic acid, diethylenetriaminepentaacetic acid, hydroxyethylethylenediaminetriacetic acid, triethylenetetraaminehexaacetic acid, diaminocyclohexanetetraacetic acid, nitrilotrimethylphosphonic acid, ethylenediaminetetra(methylenephosphonic acid), 1-hydroxylethylidene-1,1-diphosphonic acid, diethylenetriaminepenta(methylenephosphonic acid), hydroxyethylidenediphosphonic acid, 2-phosphono-1,2,4-butanetricarboxylic acid, aminotrimethylenephosphonic acid, hexamethylenediaminetetra(methylenephosphonic acid), bis(hexamethylene)triaminephosphonic acid, aminoacetic acid, and combinations thereof.

11. 11. The polishing composition of claim 10, wherein the chelating agent is in an amount of about 0.001% to about 1% by weight of the composition.

12. 2. The polishing composition of claim 1, further comprising an oxidizing agent selected from the group consisting of hydrogen peroxide, orthoperiodic acid, metaperiodic acid, dimesoperiodic acid, diorthoperiodic acid, ammonium periodate, potassium periodate, sodium periodate, ammonium persulfate, iodic acid, iodate salts, perchloric acid, perchlorate salts, hydroxylamine and hydroxylamine salts, and any combination thereof.

13. 13. The polishing composition of claim 12, wherein the oxidizing agent is in an amount of about 0.001% to about 5% by weight of the composition.

14. 2. The polishing composition of claim 1, further comprising an azole-containing rust inhibitor selected from the group consisting of triazole, tetrazole, benzotriazole, tolyltriazole, 1,2,4-triazole, ethylbenzotriazole, propylbenzotriazole, butylbenzotriazole, pentylbenzotriazole, hexylbenzotriazole, dimethylbenzotriazole, chlorobenzotriazole, dichlorobenzotriazole, chloromethylbenzotriazole, chloroethylbenzotriazole, phenylbenzotriazole, benzylbenzotriazole, aminotriazole, aminobenzimidazole, pyrazole, imidazole, aminotetrazole, isothiazole, and mixtures thereof.

15. 15. The polishing composition of claim 14, wherein the azole-containing rust inhibitor is in an amount of about 0.0001% to about 1% by weight of the composition.

16. 2. The polishing composition of claim 1, wherein the water is in an amount of about 20% to about 99% by weight of the composition.

17. 13. The method of claim 1, further comprising the steps of: applying the polishing composition of claim 1 to a surface of a substrate, the surface comprising ruthenium or a hard mask material; and contacting a pad with the surface of the substrate and moving the pad relative to the substrate; 16. A method for polishing a substrate, comprising:

18. 20. The method of claim 17, further comprising manufacturing a semiconductor device from the substrate treated with the polishing composition.