Gas Sensors

A gas sensor with a functional layer of zinc oxide, titanium dioxide, or tin dioxide, deposited via inkjet printing and annealing, addresses the instability and high cost of existing sensors, offering enhanced sensitivity and stability at low gas concentrations.

JP2024541436AInactive Publication Date: 2024-11-08POLITECNICO DI MILANO
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024529802
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-22
Filing Date
2022-11-22
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing gas sensors based on semiconductors are not suitable for stable and precise gas detection, particularly at low concentrations, and their production methods are complex and expensive.

Method used

A gas sensor with a functional layer composed of zinc oxide, titanium dioxide, or tin dioxide, deposited on an insulating substrate using inkjet printing and a specific annealing process, including slow cooling, to enhance sensitivity and stability.

Benefits of technology

The sensor achieves improved sensitivity and selectivity for gases, maintaining reliability over time while being simpler and less costly to produce.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541436000001_ABST
    Figure 2024541436000001_ABST
Patent Text Reader

Abstract

A gas sensor is described, comprising an insulating substrate (2), a pattern of conductive lines (3) deposited on the insulating substrate (2) defining at least two conductive electrodes (31), and at least one functional layer (4) deposited on said insulating substrate (2) and on at least a portion of each of both conductive electrodes (31), said functional layer (4) comprising a semiconducting metal oxide selected from zinc oxide, titanium dioxide, tin dioxide and combinations thereof, said at least one functional layer (4) being obtained by inkjet printing of an ink comprising a precursor of said semiconducting metal oxide.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a gas sensor configured to detect gases and identify chemical species dispersed in an environment, which can be usefully used to implement an electronic nose for recognizing single or complex odors in a particular environment, for example to detect the presence of hazardous gases in industrial environments such as oil refineries, or more generally to detect pollutants in air quality assessment. [Background technology]

[0002] Gas sensors based on different operating principles are known in the background art, among which are, for example, electrochemical, optical, catalytic or chemiresistive gas sensors. The latter in particular envisage the presence of an at least partially conductive active layer bridged between two electrodes. Such an active layer modifies its electrical properties when in contact with certain substances, resulting in a change in resistance, which generally decreases. The materials used to realise the active layer belong to several categories, such as, for example, semiconducting metal oxides such as ZnO, SnO2, TiO2 and CuO.

[0003] The active layers are deposited in the form of a film onto a ceramic substrate using techniques such as screen printing, sputtering or drop casting.

[0004] Patent document CN103675028 A describes a gas sensor based on such a principle, comprising an active layer deposited on an insulating substrate. The insulating substrate is inkjet printed. Heating and conductive electrodes, made of gold, silver, platinum, etc., are deposited on such a substrate. The active material is obtained in the form of a nickel oxide film functionalized with carbon nanotubes, electrically connecting the conductive electrodes to each other. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] CN103675028A

[0006] Known Technical Issues Unfortunately, the semiconductors used in the above mentioned documents are not particularly suitable for realizing stable and precise gas sensors: in fact, sensors obtained from such materials exhibit detection limits when gases are present in very small, but nevertheless critical, amounts.

[0007] Unfortunately, the aforementioned deposition techniques commonly used to achieve the active layer are very complex and expensive. Summary of the Invention [Problem to be solved by the invention]

[0008] In this context, the technical problem on which the present invention is based is to provide a gas sensor which overcomes the aforementioned drawbacks of the known technology.

[0009] In particular, it is an object of the present invention to have available gas sensors which exhibit better sensitivity and good selectivity for a given gas.

[0010] It is a further object of the present invention to have available a gas sensor that proves stable and maintains its sensitivity over time, in order to provide an electronic nose whose value can be trusted over time.

[0011] It is also an object of the present invention to have available a gas sensor that is simple and cheap to produce. [Means for solving the problem]

[0012] The technical challenges and stated objectives are - with an insulating substrate; This is essentially achieved by a gas sensor comprising a pattern of conductive lines deposited on an insulating substrate and defining at least two electrodes.

[0013] At least one functional layer deposited on the insulating substrate and on at least a portion of each of both electrodes comprises a semiconducting metal oxide selected from zinc oxide, titanium dioxide, tin dioxide, and combinations thereof.

[0014] This / these layer(s) are obtained by a process comprising inkjet printing of an ink comprising a semiconducting metal oxide precursor in sol-gel or nanoparticle dispersion form, followed by a heat treatment by annealing.

[0015] In addition to the specific heating operating conditions, this annealing treatment is particularly characterized by the cooling method common to both types, which is slow cooling carried out partly in a furnace and partly in air.

[0016] The annealing process includes the following steps. i) if the precursor is a nanoparticle dispersion, the annealing step comprises the steps of: A first step which assumes a first temperature ramp of -10°C / min from room temperature to 200°C; a second step at a constant temperature of 200° C. for a period of 60 minutes; - A final step of slow cooling in the furnace to 75°C, after which the sample is left in air until it reaches room temperature. ii) if the precursor is a sol-gel, said annealing comprises the steps of: A first step which assumes a first temperature ramp of -10°C / min from room temperature to 200°C; an intermediate step at constant temperature for a period of 15 minutes at -200°C; a second step of heating from 200° C. to 400° C. with a second temperature ramp of −10° C. / min; a further intermediate step at a constant temperature of 400° C. for a period of 60 minutes; - 75°C in an oven, followed by a final step of slow cooling to room temperature in air. [Brief description of the drawings]

[0017] [Figure 1] 1A-1D are schematic diagrams illustrating possible gas sensor configurations according to the present invention; [Figure 2a] - [Figure 2c] 4 is a graph showing how the resistance changes over a range of time for an embodiment of a sensor gas according to the present invention when contacted with different concentrations of n-butanol, dimethyl disulfide, and trimethylamine, respectively. [Figure 3a] - [Figure 3c] 1 is a graph showing the R / R0 patterns for various embodiments of a gas sensor according to the present invention when exposed to increasing amounts of n-butanol. [Figure 4] 4 is a graph showing the temperature pattern over time at the final cooling step of the annealing process for a gas sensor according to the present invention obtained through a sol-gel precursor. [Diagram 5] 4 is a graph showing the temperature pattern over time for a first heating step and for a second step at constant temperature in an annealing process for a gas sensor according to the present invention obtained through a nanoparticle dispersion. [Figure 6] 1 is a graph showing the temperature pattern over time of a first heating step, followed by a step at constant temperature, a second heating step, and a further step at constant temperature in an annealing process for a gas sensor according to the present invention obtained through a sol-gel precursor. [Figure 7] 1 is a graph showing the desorption isotherms of the sensor as a function of the relative pressure P / P0 (P0 represents the saturation pressure of 759,339 mmHg). The bottom curve identified with the small square markers represents the desorption isotherm for a sensor according to the invention in which the functional layer is ZnO deposited by inkjet printing, the middle curve identified with the small circular markers represents the desorption isotherm for the commercial sensor Figaro TGS2600, and the top curve identified with the small square markers represents the desorption isotherm for an alumina substrate (Al2O3) without active material. [Figure 8a] and [Figure 8b]1A and 1B are microstructures of the commercial sensor Figaro TGS2600 obtained through scanning electron microscopy (SEM) at magnifications of 100,000x and 400,000x, respectively. [Figure 9a] and [Figure 9b] 1A and 1B are images of the microstructure of a sensor according to the invention, the functional layer being ZnO deposited by inkjet printing, taken through scanning electron microscopy (SEM) at magnifications of 100,000x and 500,000x, respectively. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] For purposes of the present invention, the words "comprising" and "including" do not exclude the presence of additional elements in addition to those specifically listed after such words, while the words "comprising" and "consisting of" exclude the presence of additional elements in addition to those specifically listed after such words.

[0019] The subject of the present invention is a gas sensor designated hereinafter with the reference numeral 1.

[0020] The gas sensor 1 according to the invention is configured to detect gases and is particularly useful for realizing an electronic nose, so that an electronic nose comprising the gas sensor described below also falls within the scope of the invention.

[0021] A gas sensor 1 according to the invention has a structure which corresponds to known gas sensor structures, for example as shown in FIG.

[0022] The gas sensor 1 includes an insulating substrate 2. The insulating substrate 2 includes a first surface 21 and an opposing second surface 22.

[0023] Preferably, the insulating substrate 2 is made of an inorganic material. More preferably, the insulating substrate 2 is made of an inert material capable of sustaining high temperatures. Therefore, the insulating substrate 2 is preferably made of a ceramic material. For example, the insulating substrate 2 is made of alumina.

[0024] The gas sensor 1 comprises a pattern of conductive lines 3 deposited on an insulating substrate 2. Such conductive lines 3 are in particular deposited on a first surface 21.

[0025] Preferably, the conductive lines 3 have a symmetrical arrangement.

[0026] In particular, the conductive line 3 defines at least two conductive electrodes 31. Such conductive electrodes 31 are made of a noble metal such as gold, platinum, palladium, etc. The conductive electrodes 31 are spaced from each other by strips of the insulating substrate 2.

[0027] The conductive line 3 also defines a heating electrode 32 configured to act as a resistor and to provide a thermal field. The gas sensor 1 therefore comprises such a heating electrode 32. Preferably, the heating electrode 32 is also made of a noble metal such as gold, platinum, palladium, etc. The heating electrode 32 has, for example, a coil arrangement.

[0028] The conductive electrode 31 is at least partially surrounded by a heating electrode 32 .

[0029] The gas sensor 1 further comprises at least one functional layer 4. The functional layer 4 or active layer is deposited on the insulating substrate 2 and on at least a portion of each of both conductive electrodes 31. In particular, the functional layer 4 is arranged to bridge between the conductive electrodes 31 and to electrically connect both conductive electrodes 31. More particularly, the conductive electrodes 31 are interposed between the functional layer 4 and the insulating substrate 2 at the places where the functional layer 4 is arranged on the conductive electrodes 31. Otherwise, the functional layer 4 contacts the first surface 21 of the insulating substrate 2.

[0030] The functional layer 4 comprises a metal oxide that is a semiconductor. According to the invention, the semiconducting metal oxide is selected from zinc oxide, titanium dioxide, tin dioxide and combinations thereof. In particular, the gas sensor 1 may comprise one functional layer 4 or one or more functional layers 4 stacked with each other. If the gas sensor 1 comprises one functional layer 4, this may be a mono-material or mixed layer. If the gas sensor 1 instead comprises one or more functional layers 4 stacked with each other, these may be the same or different from each other.

[0031] The at least one functional layer 4 is in particular obtained by inkjet printing of an ink comprising a semiconducting metal oxide precursor. Preferably, the ink is composed of such a precursor.

[0032] In the gas sensor 1, gas detection is performed by detecting the change in resistance when a current flows between two conductive electrodes 31 made of a noble metal deposited on an insulating substrate 2, on which a functional layer 4 comprising a semiconducting metal oxide is deposited by inkjet printing.

[0033] More specifically, according to the present invention, the precursor contained in the ink is a nanoparticle dispersion or a sol-gel precursor.

[0034] Such precursors are interchangeable and therefore the first embodiment of the invention envisages the metal oxide / metal oxides of the functional layer 4 being obtained from a sol-gel precursor.

[0035] A second embodiment of the present invention envisages instead obtaining the metal oxide / metal oxides from a nanoparticle dispersion.

[0036] These two precursors offer different advantages: for example, in the case of the sol-gel precursor, there is a better control of the crystallinity and of the final properties of the functional layer 4, better printability and easier possible doping, whereas in the case of the nanoparticles, the layers deposited with metal oxides are characterized by a higher purity and lower temperatures are required for the thermal treatment.

[0037] Preferably, the process for obtaining a gas sensor according to the invention comprises a first step a) of preparing a sol-gel precursor or a nanoparticle dispersion.

[0038] More preferably, the process also comprises a step b) of depositing by inkjet printing the nanoparticle dispersion or sol-gel precursor(s) on the insulating substrate 2 and on at least a part of the conductive electrodes 31. Such step b) may be repeated as many times as the number of functional layers 4 to be obtained.

[0039] The process then envisages an annealing heat treatment according to the present invention.

[0040] According to a first embodiment, preferably the zinc oxide and / or tin dioxide sol-gel precursor is prepared from a zinc and / or tin salt solution in an amount ranging from 10 to 30% by weight, preferably 20%, in a mixture of a C2-C5 alcohol and a C2-C4 alkylene glycol, by a process comprising the steps described below.

[0041] The first step comprises a-1-1) dissolving the salt in said C2-C4 alkylene glycol, and then the second step envisages a-1-2) adding a C2-C5 alcohol to the solution obtained in a-1-1).

[0042] Hereinafter, the process envisages a step a-1-3) of sonicating the mixture from a-1-2) for a period ranging from 10 to 50 minutes, preferably for 30 minutes.

[0043] The next step involves a-1-4) removing the residues formed in step a-1-3), which is preferably carried out by filtration through a paper filter.

[0044] The final solution obtained by such steps is homogeneous and transparent and represents a sol-gel precursor that can be used as an inkjet printing ink to deposit a homogeneous metal oxide film, i.e., the functional layer 4.

[0045] In particular, the salts are preferably zinc and / or stannous chloride, or more preferably zinc acetate and / or stannous acetate, which may be anhydrous or hydrated.

[0046] According to the present invention, it is envisioned that different chlorides or acetates may also be mixed together to provide a mixed solution.

[0047] Preferably, the solvent is a mixture of ethylene glycol and ethanol.

[0048] Thus, a C2-C4-alkylene glycol is ethylene glycol and a C2-C5 alcohol is ethanol.

[0049] More preferably, the C2-C4-alkylene glycol is present in an amount of 30% by weight based on the final weight of the solution.More preferably, the C2-C5 alcohol is present in an amount of 50% by weight based on the final weight of the solution.

[0050] Optionally, between steps a-1-1) and a-1-2), a step is envisaged in which the mixture is stirred at elevated temperature. Preferably, such a step envisages stirring the mixture at a temperature in the range of 120-160° C., preferably at 140° C., for a period in the range of 20-40 minutes, preferably 30 minutes.

[0051] Further according to the first embodiment, the sol-gel precursor of titanium dioxide is preferably prepared from a solution containing A) a C2-C5 titanium alkoxide in a concentration ranging from 30 to 70% by weight based on the total weight of the solution. Preferably, the concentration of the titanium alkoxide is 50% by weight based on the total weight of the solution.

[0052] Optionally, the solution also comprises 3-6% by weight of lactic acid B), based on the total weight of the solution. Preferably, the solution comprises 4.3% by weight of lactic acid, based on the total weight of the solution.

[0053] The solution further comprises C) a mixture of C2-C4 alcohol and water.

[0054] Preferably, the alkoxide is titanium isopropoxide and tert-butoxide. More preferably, the alcohol is isopropanol. More preferably, the water is demineralized water.

[0055] Preferably, such a titanium dioxide precursor solution is obtained by a process comprising the following steps:

[0056] According to the first step, it is envisaged a-2-1) to mix a C2-C5 titanium alkoxide with a C2-C4 alcohol to form a first solution.

[0057] The process then comprises a second step a-2-2) of pouring the solution into water and stirring for several minutes. In particular, the water is included in an amount ranging from 2 to 3 times the weight of the C2-C5 titanium alkoxide.

[0058] Preferably, the water is present in an amount 2.5 times the weight of the C2-C5 titanium alkoxide. Such a step envisages that the solution is stirred for a period ranging from 3 to 6 minutes, preferably 4 or 5 minutes. In particular, the solution is kept stirred until it becomes clear. Optionally, lactic acid is added.

[0059] According to the third step, a-2-3) is envisaged, which involves stirring at a temperature in the range of 60-100° C., preferably at 80° C., for 24 hours.

[0060] Alternatively, the titanium dioxide sol-gel precursor is prepared from a solution obtainable through the so-called "reverse micelle" technique. Such a solution additionally contains a titanium alkoxide, but envisages the use of a different solvent, such as xylene. Furthermore, the xylene is preferably mixed with a surfactant, preferably a non-ionic surfactant. For example, the non-ionic surfactant is Trione-X. Such a solution also comprises deionized water.

[0061] Preferably, such a titanium dioxide precursor solution is obtained by a process comprising the following steps:

[0062] According to a first step, a-3-1) it is envisaged to mix and stir xylene and a surfactant to form a first solution.

[0063] The process then includes a second step a-3-2) of adding deionized water to the solution formed in a-3-1) and stirring for a few minutes.

[0064] This is followed by step a-3-3) in which titanium alkoxide is added dropwise to the solution formed in a-3-2).

[0065] Furthermore, according to a first embodiment which envisages a sol-gel precursor, the sol-gel precursor comprises transition metal ions, preferably selected from iron, copper or nickel ions. The transition metal ions are preferably added in the form of a salt selected from chloride, nitrate, acetate or sulfate. In particular, the transition metal ions are added to the sol-gel precursor in a concentration ranging from 1 to 4 g / l. Preferably, the concentration of the transition metal ions in the solution is 2 g / l. Such transition metal ions are added to the solution before step b) of depositing the precursor.

[0066] Advantageously, it is possible to dope the solution and obtain a final doped oxide, the electrical characteristics of which are better than the same oxide that is not doped.

[0067] According to a second embodiment, preferably in step a), the nanoparticle dispersion is prepared by dispersing zinc oxide and / or tin dioxide and / or titanium dioxide nanoparticles in a mixture comprising water and a polyhydric alcohol or a C1-C4 monoalkyl ether thereof.

[0068] Preferably, the nanoparticles have a diameter in the range of 1 to 100 nm.

[0069] More preferably, the polyhydric alcohol is ethylene glycol, or the C1-C4 monoalkyl ether is triethylene glycol monomethyl ether.

[0070] Preferably, the mixture of polyhydric alcohol or its C1-C4 monoalkyl ether and water comprises 10-30% by weight of polyhydric alcohol or its C1-C4 monoalkyl ether, more preferably 20%.

[0071] According to a preferred embodiment, the nanoparticles are included in an amount ranging from 2 to 4% by weight, based on the total weight of the dispersion.

[0072] Preferably, the nanoparticles are included in an amount of 3% by weight based on the total weight of the dispersion.

[0073] The mixture further comprises a surfactant, preferably present in an amount in the range of 0.5 to 1.5%, preferably 1% by weight based on the total weight of the dispersion.

[0074] More preferably, the surfactant is an anionic or neutral organic surfactant, preferably selected from polyacrylic acid sodium salt, polyethylene glycol, polyvinyl alcohol.

[0075] Following step a) of preparing a precursor, i.e. an ink, the ink is loaded in an inkjet printing setup for step b) of depositing by inkjet printing a sol-gel solution or a nanoparticle dispersion to achieve a homogenous film representing the functional layer 4.

[0076] For printing, the use of piezoelectric or thermal printheads can be envisaged.

[0077] Optionally, prior to printing, the insulating substrate 2 can be subjected to a treatment intended to improve its wettability, such as a corona treatment.

[0078] More preferably, during step b) of depositing the precursor by inkjet printing, the insulating substrate 2 may be kept heated at a temperature in the range of 40°C to 80°C, preferably at 60°C.

[0079] The precursors prepared according to the above mentioned stages and steps show good stability over time leading to high print quality.

[0080] After deposition of the metal oxide film, the method comprises a step of carrying out a heat treatment, i.e. an annealing step c) according to the invention.

[0081] 5-6 represent the individual heating steps with two different metal oxide precursors, and FIG. 4 represents the cooling curve in the annealing step c) for a functional layer 4 obtained through a sol-gel precursor.

[0082] According to an embodiment, the semiconducting metal oxide is surface functionalized with noble or transition metal nanoparticles in order to improve the selectivity of the gas sensor 1 to a given substrate and / or to improve its stability.

[0083] The method then optionally comprises a functionalization step d), before the annealing treatment c) and after the deposition step b), which is carried out by immersing the gas sensor 1 in a solution containing nanoparticles of the noble or transition metal with which the functional layer 4 is intended to be functionalized. Alternatively, the functionalization step d) is carried out by depositing metal nanoparticles on the functional layer 4 deposited on the insulating substrate 2. Such nanoparticles can be deposited by various methods, such as sputtering or evaporation.

[0084] The gas sensor 1 realized according to the present invention shows good sensitivity even at low gas concentrations. Figures 2a-2c show how the resistance changes over a given time range at various gas concentrations for the gas sensor 1 according to the present invention, where the functional layer 4 is contacted with gases such as n-butanol, dimethyl disulfide, and trimethylamine, respectively. In this specific case, the functional layer 4 has three TiO2 layers obtained through a sol-gel precursor according to Example 7 described below.

[0085] Practical examples Example 1 A gas sensor with ZnO active layer was obtained from a sol-gel precursor of 0.4 moles of zinc acetate dihydrate dissolved in 120 ml of ethylene glycol. Such a mixture was stirred at 140°C for 30 minutes. Afterwards, the mixture was cooled at room temperature and, once cooling was complete, 280 ml of ethanol was added. The solution was then sonicated for 30 minutes and filtered through a paper filter. A total of 400 ml of solution was obtained, i.e., precursor ink solution. Such a precursor was filled into a 10pl cartridge of a Dimatix materials printer DMP-2850 (by Fujifilm).

[0086] The printer comprises in particular a support for the substrate, which can be heated. Such a support was heated to reach 60° C. before the substrate was placed on it. The substrate was also previously corona treated for 4 minutes. The substrate used is made of alumina with a platinum conductive line containing two platinum electrodes.

[0087] The precursor was deposited on the surface of a substrate, 0.5 mm x 0.7 mm, to form the active layer. In this case, a single metal oxide layer was formed.

[0088] After printing, heat treatment in an oven was performed as follows: a first heating ramp at 10°C / min to reach 200°C, a step at constant temperature at 200°C for 15 minutes, a second heating ramp at 10°C / min to reach 400°C, a further step at constant temperature at 400°C for 60 minutes, and slow cooling in the oven to reach 75°C and subsequent cooling in air to reach room temperature.

[0089] Variation of Example 1: Procedure as above but including deposition of 3 or 6 metal oxide layers.

[0090] Example 2 Same as Example 1 for solution preparation. 2 g / l of copper chloride dihydrate was added to the final solution to obtain the precursor ink.

[0091] The printing, substrate and heat treatment are the same as in Example 1.

[0092] Example 3 The solution was prepared as in Example 2. The printing and the substrate were the same as in Example 1. The number of functional layers deposited was 6. After deposition, the active part thus realized was immersed in a 0.05M PdCl2 solution in ethanol. A heat treatment was carried out after this step as described in Example 1.

[0093] Example 4 A gas sensor with an active layer of SnO2 was obtained from a sol-gel precursor of 90.25 g (i.e. 0.4 mol) of tin(II) acetate dihydrate dissolved in 120 ml of ethylene glycol. Such a mixture was stirred at 140°C for 30 minutes. Afterwards, the mixture was cooled at room temperature and, once cooling was complete, 280 ml of ethanol was added. The solution was then sonicated for 30 minutes and filtered through a paper filter. A total of 400 ml of solution was obtained, i.e. the precursor ink solution. Such a precursor was filled into a 10pl cartridge of a Dimatix materials printer DMP-2850 (by Fujifilm).

[0094] The printer comprises, inter alia, a support for the substrate, which can be heated.

[0095] Such a support was heated to reach 60° C. before the substrate was placed on it.

[0096] The substrate was also previously corona treated for 4 minutes.The substrate used is made of alumina equipped with a platinum conductive wire containing two platinum electrodes.

[0097] The precursor was deposited on the surface of the substrate at 0.5 mm x 0.7 mm to form an active layer.

[0098] After printing, heat treatment in an oven was performed as follows: a first heating ramp at 10°C / min to reach 200°C, a step at constant temperature at 200°C for 15 minutes, a second heating ramp at 10°C / min to reach 400°C, a further step at constant temperature at 400°C for 60 minutes, and slow cooling in the oven to reach 75°C and subsequent cooling in air to reach room temperature.

[0099] Example 5 A gas sensor whose active layer is a mixed layer ZnO / SnO2. The mixed precursor was obtained from a sol-gel precursor of 3.66 g (i.e., 0.017 mol) of zinc acetate dihydrate dissolved with 11.28 g (i.e., 0.05 mol) of tin chloride dihydrate in 30 ml of ethylene glycol. Such a mixture was stirred at 140°C for 30 minutes. After that, the mixture was cooled at room temperature and, once cooling was complete, 70 ml of ethanol was added. The solution was then sonicated for 30 minutes and filtered through a paper filter. 60 ml of solution, i.e., precursor ink, was obtained in total.

[0100] The printing and substrate as well as the heat treatment are the same as in Example 1.

[0101] Example 6 Gas sensors with a mixed layer ZnO active layer were obtained from a nanoparticle suspension precursor. The nanoparticle suspension was prepared from a mixture of 20% by weight ethylene glycol in water to which 3% by weight ZnO nanoparticles and 1% by weight polyacrylic acid sodium salt were added. The suspension was stirred for 30 minutes and then sonicated for 15 minutes. The suspension thus obtained was printed. The printing and the substrate are similar to those of the previous examples. One or two active material layers are deposited.

[0102] After printing, heat treatment in an oven was performed as follows: a first heating ramp at 10°C / min to reach 200°C, a constant temperature step at 200°C for 60 min, and slow cooling in the oven to reach 75°C and subsequent cooling in air to reach room temperature.

[0103] Example 7 Gas sensors with TiO2 as the active layer were obtained by stirring a sol-gel precursor from a mixture of 5.1 ml xylene and 2.5 ml Triton-X. Then, 60 μl water was added to the mixture. The mixture was stirred for a few minutes until it became transparent. Then, 1 ml titanium isopropoxide was added to the mixture, forming a yellow solution. The solution represented the precursor ink, which was filled into a 10 pl cartridge of a Dimatix materials printer DMP-2850 (by Fujifilm).

[0104] The substrate and printing were the same as in the previous example. The heat treatment performed after the deposition of the active layer was the same as in examples 1-5.

[0105] 3a-3c show graphs depicting the R / R0 patterns for several embodiments of a gas sensor according to the present invention when exposed to increasing amounts of n-butanol.

[0106] Data collected Below, tables are reported that show how the efficiency changes over time, along with the drift time, for several gas sensors implemented according to the invention and for two commercially available sensors.

[0107] It should be pointed out that all of the sensors mentioned in the table below are zinc oxide based.

[0108] To fabricate the two commercial sensors, metallic Zn thin films were deposited through RF magnetron sputtering (13.56 MHz) on 2 mm square alumina and silicon substrates. The thickness of the Zn thin films was 600 nm. The Zn thin films were anodized in a two-electrode system at room temperature. A platinum sheet was used as the counter electrode. The anodization was carried out in a 2 M concentrated electrolyte of oxalic acid dihydrate (C2H2O4·2H2O) containing ethanol. The applied voltage was 30 V and the anodization time was 20 min. The prepared samples were zinc oxalate dihydrate (ZnC2O4·2H2O). The samples were then annealed in a tube furnace at 400 °C in an atmosphere of 50% O2 and 50% Ar for 5 h. 1 .

[0109] It should be noted that the efficiency remains unchanged even after 10 months for the gas sensor implemented according to the invention, whereas the commercial sensor suffers from a noticeable efficiency loss after a few months. [Table 1] [Table 2]

[0110] Sensor characteristics Desorption isotherm Comparing the desorption isotherms depicted in the graphs of Figure 7, it is clear that the sensor according to the invention is able to desorb significantly larger amounts (see Figure 7, bottom curve with small square markers) of substances (mostly water) with respect to the commercial sensor (middle graph with small circular markers), thus indicating a higher porosity of the sensor according to the invention. Measurements carried out on an alumina substrate (used as substrate for the sensor according to the invention - top diagram with small square markers) were carried out as a control test.

[0111] Microscopic analysis (SEM) Comparing Figures 8a-8b and 9a-9b, which are characterized by similar and completely comparable magnification levels, it is clear that the sensor according to the invention is characterized by nanometer-sized pores that are too small to be resolved by SEM microscopy. Such nanometer porosity is also evident to be uniform in the sample being analyzed. In contrast, the commercial sensor appears to be characterized by pores that are significantly larger and more dimensionally non-uniform.

[0112] Image comparison shows that the sensor according to the invention is characterized by a higher and dimensionally finer porosity, an observation which fully confirms the previously discussed results obtained with the desorption isotherms (FIG. 7).

Claims

1. A gas sensor (1) configured to detect a gas, comprising: An insulating substrate (2); a pattern of conductive lines (3) deposited on said insulating substrate (2) and defining at least two conductive electrodes (31); At least one functional layer (4) deposited on the insulating substrate (2) and on at least a portion of each of the at least two conductive electrodes (31), the functional layer (4) comprising a semiconducting metal oxide selected from zinc oxide, titanium dioxide, tin dioxide, and combinations thereof; Equipped with The at least one functional layer (4) Inkjet printing with an ink comprising a sol-gel precursor or a precursor of said semiconducting metal oxide in nanoparticle dispersion form, followed by Annealing, heat treatment and and The process comprises: i) if the precursor is a nanoparticle dispersion, the annealing comprises: A first step, which assumes heating from room temperature to 200° C. via a first temperature ramp of 10° C. / min; a second step of constant temperature at 200° C. for 60 minutes; The final step is to gradually cool the material to 75°C in the furnace and then return it to room temperature in the air. or ii) if the precursor is a sol-gel, the annealing comprises the steps of: A first step, which assumes heating from room temperature to 200° C. via a first temperature ramp of 10° C. / min; an intermediate step of 15 minutes at a constant temperature of 200°C; a second step of heating from 200° C. to 400° C. via a second temperature ramp of 10° C. / min; a further intermediate step of constant temperature at 400° C. for 60 minutes; The final step is to gradually cool the material to 75°C in the furnace and then return it to room temperature in the air. Equipped with Gas sensor (1).

2. A gas sensor (1), comprising: The process comprising: a) preparing a precursor of the sol-gel or a precursor of the nanoparticle dispersion; b) depositing the precursor(s) of said nanoparticle dispersion or said sol-gel on said insulating substrate (2) and on at least a part of said conductive electrodes (31) by inkjet printing, said depositing step being performed a number of times equal to the number of functional layers (4) to be obtained; c) annealing the material of step b); The gas sensor (1) according to claim 1, comprising:

3. In step a), The sol-gel precursor of zinc oxide and / or tin dioxide comprises a zinc and / or tin salt solution in a mixture of C2-C5 alcohol and C2-C4 alkylene glycol in an amount ranging from 10 to 30% by weight, preferably 20% by weight, the precursor comprising the following: a-1-1) dissolving the salt in the C2-C4-alkylene glycol; a-1-2) adding the C2-C5 alcohol to the solution obtained in a-1-1); a-1-3) sonicating the mixture of step a-1-2) for 30 minutes; a-1-4) removing the residue formed in step a-1-3); 3. The gas sensor (1) according to claim 2, prepared by a process comprising:

4. 4. The gas sensor (1) according to claim 3, wherein the salt in the salt solution is zinc chloride and / or tin chloride and / or zinc acetate and / or tin acetate, and the solvent in the salt solution is a mixture of ethylene glycol and ethanol.

5. In step a), A) a C2-C5 titanium alkoxide in a concentration ranging from 30 to 70% by weight, preferably 50% by weight, based on the total weight of the solution; B) 3 to 6% by weight, preferably 4.3% by weight, of lactic acid based on the total weight of the solution; C) A tin dioxide sol-gel precursor is prepared, which is composed of a solution comprising a mixture of C2-C4 alcohol and water, said precursor being prepared by the following steps: a-2-1) mixing the C2-C5 titanium alkoxide and a C2-C4 alcohol to form a first solution; a-2-2) pouring the solution into water under stirring, stirring for 5 minutes, and adding lactic acid; a-2-3) stirring at 80° C. for 24 hours; 3. The gas sensor (1) according to claim 2, obtained by a process comprising:

6. The gas sensor (1) according to claim 5, wherein the alkoxide is titanium isopropoxide and tert-butoxide and the alcohol is isopropanol.

7. 7. The gas sensor (1) according to any one of claims 1 to 6, wherein the sol-gel precursor comprises transition metal ions, preferably selected from iron, copper or nickel ions, the transition metal ions being in salt form selected from chloride, nitrate, acetate or sulfate, and the transition metal ions being added to the sol-gel precursor in a concentration in the range of 1 to 4 g / l, preferably 2 g / l.

8. 3. The gas sensor (1) according to claim 2, wherein in step a) the nanoparticle dispersion is prepared by dispersing zinc oxide and / or tin dioxide and / or titanium dioxide nanoparticles, preferably having a diameter in the range of 1 to 100 nm, in a mixture comprising water and a polyhydric alcohol or a C1-C4 monoalkyl ether thereof.

9. The gas sensor (1) according to claim 8, wherein the polyhydric alcohol is ethylene glycol or the C1-C4 monoalkyl ether thereof is ethylene glycol monomethyl ether.

10. 10. The gas sensor (1) according to claim 8 or claim 9, wherein the nanoparticles are contained in an amount ranging from 2 to 4%, preferably 3% by weight based on the total amount of the dispersion, and the mixture comprises a surfactant in an amount ranging from 0.5 to 1.5%, preferably 1% by weight based on the total amount of the dispersion.

11. 11. The gas sensor (1) according to claim 10, wherein the surfactant is an anionic or neutral organic surfactant, preferably selected from polyacrylic acid sodium salt, polyethylene glycol, polyvinyl alcohol.

12. The gas sensor (1) according to any one of the preceding claims, wherein the semiconducting metal oxide is functionalized with noble metal or transition metal nanoparticles prior to said step c) of annealing.

13. 13. The gas sensor (1) according to any one of claims 1 to 12, wherein the gas detection is performed through the conductive electrode (31) made of a noble metal deposited on the insulating substrate (2) and on which at least a functional layer (4) comprising a semiconducting oxide selected from the group consisting of zinc oxide, titanium dioxide, tin dioxide and combinations thereof is deposited by inkjet printing.

14. An electronic nose comprising a gas sensor (1) according to any one of the preceding claims.

Citation Information

Patent Citations

  • Semiconductor gas sensor as well and preparation method thereof

    CN103675028A