Polyimide precursor composition and polyimide film containing the same
A polyimide film with specific components and ratios addresses the issue of high dielectric loss in existing films by achieving low dielectric properties and heat resistance, enabling stable high-frequency signal transmission.
Patent Information
- Application Number
- JP2024530056
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-08-30
- Filing Date
- 2022-11-21
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-11-21
AI Technical Summary
Existing polyimide films do not possess adequate low dielectric properties, leading to insufficient insulation at high frequencies and increased stray capacitance and noise in thin circuit boards, which are crucial for high-frequency communication.
A polyimide film composed of specific components and ratios, including biphenyltetracarboxylic dianhydride, paraphenylenediamine, m-tolidine, and pyromellitic dianhydride, which form block copolymers to enhance heat resistance, low dielectric properties, and dimensional stability.
The film achieves a dielectric loss factor of 0.003 or less, a thermal expansion coefficient of 13-15 ppm/°C, and a glass transition temperature of 320°C, ensuring stable insulation and minimal signal transmission delay even at high frequencies.
Smart Images

Figure 2024541456000001 
Figure 2024541456000002 
Figure 2024541456000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyimide precursor composition and a polyimide film produced using the polyimide precursor composition, which has excellent heat resistance, low dielectric properties and dimensional stability. [Background technology]
[0002] Polyimide (PI) is a polymeric material based on imide rings, which have excellent chemical stability along with a rigid aromatic main chain, and has the highest levels of heat resistance, chemical resistance, electrical insulation, chemical resistance, and weather resistance among organic materials. In particular, due to its excellent electrical properties such as excellent insulating properties, i.e., low dielectric constant, it has been attracting attention as a highly functional polymer material in the electrical, electronic and optical fields. 2. Description of the Related Art Recently, with the trend towards lighter and smaller electronic products, flexible thin circuit boards with high integration density have been actively developed.
[0003] Such thin circuit boards tend to have a structure in which a circuit containing metal foil is formed on a polyimide film that has excellent heat resistance, low temperature resistance and insulating properties, but is also easily flexible. Flexible metal clad laminates are mainly used for such thin circuit boards, and an example is Flexible Copper Clad Laminate (FCCL), which uses a thin copper plate as a metal foil. Polyimide is also used as a protective film and insulating film for thin circuit boards. Meanwhile, as electronic devices are increasingly equipped with a variety of functions, they are required to have high operation and communication speeds. To meet this demand, thin circuit boards capable of high-speed communication at high frequencies have been developed.
[0004] To realize high-frequency and high-speed communication, insulators with high impedance that can maintain electrical insulation even at high frequencies are required. Since impedance is inversely proportional to the frequency and dielectric constant (Dk) formed in the insulator, the dielectric constant must be as low as possible to maintain insulation even at high frequencies. However, in the case of ordinary polyimide, the dielectric properties are not currently at a level excellent enough to maintain sufficient insulation for high-frequency communications. In addition, it is known that the lower the dielectric properties of the insulator, the less unwanted stray capacitance and noise can be generated in thin circuit boards, which can largely eliminate the causes of communication delays. Therefore, the low dielectric properties of polyimide are currently recognized as the most important factor in the performance of thin circuit boards.
[0005] In particular, in the case of high frequency communication, dielectric dissipation due to polyimide inevitably occurs. The dielectric dissipation factor (Df) indicates the degree of electrical energy wasted in a thin circuit board and is closely related to the signal transmission delay that determines the communication speed. Therefore, keeping the dielectric dissipation factor of polyimide as low as possible is recognized as an important factor in the performance of thin circuit boards. In addition, the more moisture a polyimide film contains, the larger its dielectric constant becomes, and the higher its dielectric loss factor becomes. Although polyimide film is suitable as a material for thin circuit boards due to its excellent inherent properties, it is relatively vulnerable to moisture due to the imide group, which exhibits polarity. This may result in a deterioration of the insulating properties. Therefore, there is a need to develop a polyimide film having dielectric properties, particularly a low dielectric loss factor, while maintaining the mechanical properties, thermal properties and dimensional stability properties inherent to polyimides at a certain level. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Republic of Korea Patent Publication No. 10-2015-0069318 Summary of the Invention [Problem to be solved by the invention]
[0007] In order to solve the above problems, an object of the present invention is to provide a polyimide film having excellent heat resistance, low dielectric properties and dimensional stability, and a polyamide precursor composition for producing the same. Therefore, a substantial object of the present invention is to provide specific examples thereof. [Means for solving the problem]
[0008] In order to achieve the above object, one embodiment of the present invention provides a polymerizable composition comprising a first block obtained by imidizing a polyamic acid derived from a polymer of a dianhydride acid component containing biphenyltetracarboxylic dianhydride (BPDA) and a diamine component containing paraphenylenediamine (PPD); a second block obtained by imidizing a polyamic acid derived from a polymer of a dianhydride component including biphenyltetracarboxylic dianhydride and a diamine component including m-tolidine; and a third block obtained by imidizing a polyamic acid derived from a polymer of a dianhydride acid component containing pyromellitic dianhydride (PMDA) and a diamine component containing m-tolidine. A polyimide film is provided.
[0009] Another embodiment of the present invention is a laminate comprising the polyimide film and a thermoplastic resin layer, A multilayer film is provided. Yet another embodiment of the present invention is a method for manufacturing a laminate comprising the polyimide film and an electrically conductive metal foil, A flexible metal foil laminate is provided. Yet another embodiment of the present invention includes the flexible metal foil laminate, Provide electronic components.
[0010] Yet another embodiment of the present invention is a first block obtained by reacting a dianhydride component including biphenyltetracarboxylic dianhydride (BPDA) with a diamine component including paraphenylenediamine (PPD); a second block obtained by imidization reaction of a dianhydride component containing biphenyltetracarboxylic dianhydride with a diamine component containing m-tolidine; and a third block obtained by reacting a dianhydride component containing pyromellitic dianhydride (PMDA) with a diamine component containing m-tolidine. A polyimide precursor composition is provided. Effect of the Invention
[0011] As described above, the present invention relates to a polyimide film having specific components and specific composition ratios. The polyimide film and the polyamide precursor composition for producing the same provide a polyimide film having excellent heat resistance, low dielectric properties, and dimensional stability, and can be usefully applied in various fields where such properties are required, particularly in electronic parts such as flexible metal foil laminates. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, embodiments of the present invention will be described in more detail. Prior to this, the terms and words used in this specification and claims should not be interpreted limited to their ordinary or dictionary meanings, but should be interpreted with meanings and concepts that correspond to the technical ideas of the present invention, in accordance with the principle that an inventor can appropriately define the concepts of terms in order to explain his / her invention in the best possible way. Therefore, it should be understood that the configuration of the embodiment described in this specification is merely one of the most preferred embodiments of the present invention and does not fully represent the technical ideas of the present invention, and that there may be various equivalents and modifications that can replace them at the time of this application.
[0013] In this specification, the singular expression includes the plural expression unless the context clearly indicates otherwise. It should be understood that in this specification, the terms "comprise", "comprise", "have" and the like are intended to specify the presence of embodied features, numbers, steps, components, or combinations thereof, and do not preclude the possibility of the presence or addition of one or more other features, numbers, steps, components, or combinations thereof. Whenever an amount, concentration, or other value or parameter is given herein as a range, a preferred range or a list of an upper preferred value and a lower preferred value, it should be understood to specifically disclose all ranges formed by any pair of any upper range limit or preferred value, and any lower range limit or preferred value, regardless of whether a range is otherwise disclosed. Where a range of numerical values is recited herein, unless otherwise stated, the range is intended to include the endpoints thereof, and all integers and fractions within the range. It is not intended that the scope of the invention be limited to the specific values recited when defining a range.
[0014] As used herein, "dianhydride acid" is intended to include precursors or derivatives thereof which may not technically be dianhydrides but which nevertheless must react with a diamine to form a polyamic acid which is then converted back to a polyimide. As used herein, "diamine" is intended to include precursors or derivatives thereof, which may not technically be diamines, but which nevertheless must react with a dianhydride to form a polyamic acid, which is then converted back to a polyimide. The polyimide film according to the present invention can include a block copolymer including a first block obtained by imidizing a polyamic acid derived from a polymer of a dianhydride acid component containing biphenyltetracarboxylic dianhydride (BPDA) and a diamine component containing paraphenylenediamine (PPD), a second block obtained by imidizing a polyamic acid derived from a polymer of a dianhydride acid component containing biphenyltetracarboxylic dianhydride and a diamine component containing m-tolidine, and a third block obtained by imidizing a polyamic acid derived from a polymer of a dianhydride acid component containing pyromellitic dianhydride (PMDA) and a diamine component containing m-tolidine.
[0015] For example, the first block is obtained by imidizing a polyamic acid derived from a polymer of biphenyltetracarboxylic dianhydride and paraphenylenediamine. The second block is obtained by subjecting a polyamic acid derived from a polymer of biphenyltetracarboxylic dianhydride and m-tolidine to an imidization reaction, and the third block is obtained by subjecting a polyamic acid derived from a polymer of pyromellitic dianhydride and m-tolidine to an imidization reaction. The m-tolidine has a methyl group that exhibits hydrophobicity, and contributes to the low moisture absorption property of the polyimide film and the resulting low dielectric property of the polyimide film.
[0016] In one embodiment, the polyimide film is obtained by imidizing a polyamic acid derived from a polymer of a dianhydride component consisting of biphenyltetracarboxylic dianhydride and pyromellitic dianhydride, and a diamine component consisting of paraphenylenediamine and m-tolidine. This is because the polyimide film is made of a block copolymer containing the first block, the second block, and the third block, or made of the first block, the second block, and the third block.
[0017] In one embodiment, based on 100 mol% of the total content of the diamine components in the polyimide film, the content of m-tolidine may be 25 mol% or more and 40 mol% or less, and the content of paraphenylenediamine may be 60 mol% or more and 75 mol% or less. Preferably, based on 100 mol % of the total content of diamine components in the polyimide film, the content of m-tolidine may be 30 mol % or more and 40 mol % or less, and the content of paraphenylenediamine may be 60 mol % or more and 70 mol % or less.
[0018] In addition, based on 100 mol% of the total content of dianhydride acid components in the polyimide film, the content of biphenyltetracarboxylic dianhydride may be 50 mol% or more and 65 mol% or less, and the content of pyromellitic dianhydride may be 35 mol% or more and 50 mol% or less. Preferably, based on 100 mol% of the total content of dianhydride acid components in the polyimide film, the content of biphenyltetracarboxylic dianhydride may be 50 mol% or more and 60 mol% or less, and the content of pyromellitic dianhydride may be 40 mol% or more and 50 mol% or less.
[0019] The polyimide chain derived from the biphenyltetracarboxylic dianhydride of the present invention has a structure called a charge transfer complex (CTC), i.e., a regular linear structure in which an electron donor and an electron acceptor are located close to each other, and intermolecular interactions are strengthened. This structure has the effect of preventing hydrogen bonding with moisture, which has an effect of lowering the moisture absorption rate, thereby maximizing the effect of lowering the moisture absorption of the polyimide film. In one embodiment, the dianhydride component may further include a pyromellitic dianhydride, which is a dianhydride component having a relatively rigid structure and is preferred in that it can impart suitable elasticity to the polyimide film.
[0020] In order for the polyimide film to simultaneously satisfy the appropriate elasticity and moisture absorption rate, the content ratio of the dianhydride is particularly important. For example, the lower the content ratio of biphenyltetracarboxylic dianhydride, the less likely it is that the low moisture absorption rate due to the CTC structure will be achieved. In addition, biphenyltetracarboxylic dianhydride contains two benzene rings corresponding to the aromatic moiety, whereas pyromellitic dianhydride does not contain any aromatic moiety. It contains one corresponding benzene ring.
[0021] An increase in the content of pyromellitic dianhydride in the dianhydride acid component can be understood as an increase in the imide groups in the molecule based on the same molecular weight, which can be understood as a relative increase in the ratio of imide groups derived from the pyromellitic dianhydride in the polyimide polymer chain compared to the imide groups derived from biphenyltetracarboxylic dianhydride. That is, an increase in the content of pyromellitic dianhydride is seen as a relative increase in imide groups with respect to the entire polyimide film, which makes it difficult to expect a low moisture absorption rate. Conversely, if the content ratio of the pyromellitic dianhydride is decreased, the components having a relatively rigid structure are decreased, and the elasticity of the polyimide film may be decreased below a desired level.
[0022] For this reason, when the content of the biphenyltetracarboxylic dianhydride is higher than the above range or the content of the pyromellitic dianhydride is lower than the above range, the mechanical properties of the polyimide film are deteriorated, and it is not possible to ensure a suitable level of heat resistance for producing a flexible metal foil laminate. Conversely, if the content of the biphenyltetracarboxylic dianhydride is below the above range or the content of the pyromellitic dianhydride is above the above range, it is difficult to achieve an appropriate level of dielectric constant and dielectric loss factor, which is not preferable.
[0023] In one embodiment, the content of the biphenyltetracarboxylic dianhydride in the first block may be 40 mol % or more and 55 mol % or less based on 100 mol % of the total content of dianhydride acid components in the polyimide film, and the content of the biphenyltetracarboxylic dianhydride in the second block may be 10 mol % or more based on 100 mol % of the total content of dianhydride acid components in the polyimide film. If the content of the biphenyltetracarboxylic dianhydride in the first block is less than the above range, it may be difficult to ensure a sufficiently low dielectric loss factor (Df), and if it exceeds the above range, it may be difficult to ensure necessary heat resistance.
[0024] When the content of the biphenyltetracarboxylic dianhydride in the second block is less than the above range, it may be difficult to ensure a sufficiently low dielectric loss factor (Df). On the other hand, the content of the biphenyltetracarboxylic dianhydride in the second block may be 25 mol % or less based on 100 mol % of the total content of dianhydride acid components in the polyimide film.
[0025] If the content of the biphenyltetracarboxylic dianhydride in the second block exceeds the above range, it may be difficult to ensure the required heat resistance. Alternatively, the biphenyltetracarboxylic dianhydride in the first block may all be imidized with paraphenylenediamine, and the biphenyltetracarboxylic dianhydride in the second block may all be imidized with m-tolidine.
[0026] On the other hand, the content of the m-tolidine in the third block may be 10 mol % or more and 35 mol % or less based on 100 mol % of the total content of diamine components in the polyimide film. If the content of m-tolidine in the third block is less than the above range, it may be difficult to ensure a sufficiently low dielectric loss factor (Df), and if it exceeds the above range, it may be difficult to ensure the required heat resistance. . Furthermore, all of the m-tolidines in the third block may be imidized with pyromellitic dianhydride.
[0027] In one embodiment, the polyimide film may have a dielectric loss factor (Df) of 0.003 or less, a coefficient of thermal expansion (CTE) of 13 ppm / °C or more and 23 ppm / °C or less, and a glass transition temperature (Tg) of 320°C or more. In this regard, polyimide film that satisfies all of the requirements for dielectric loss factor (Df), thermal expansion coefficient, and glass transition temperature can be used as an insulating film for flexible metal foil laminates. Furthermore, even if the manufactured flexible metal foil laminates are used as electrical signal transmission circuits that transmit signals at high frequencies of 10 GHz or more, the insulation stability is ensured and signal transmission delay can be minimized. The polyimide film satisfying all of the above requirements is a novel polyimide film that has not been known before. The dielectric loss factor (Df) of the polyimide film will be described in detail below.
[0028] <Dielectric loss factor> "Dielectric loss factor" refers to the force dissipated by a dielectric (or insulator) when molecular friction impedes molecular motion induced by an alternating electric field. The dielectric loss factor is usually used as an index of how easily a charge is lost (dielectric loss): the higher the dielectric loss factor, the easier it is to lose a charge, and conversely, the lower the dielectric loss factor, the harder it is to lose a charge. In other words, the dielectric loss factor is a measure of power loss, and the lower the dielectric loss factor, the faster the communication speed can be maintained while mitigating signal transmission delays caused by power loss. This is a strong requirement for polyimide films, which are insulating films, and the polyimide film of the present invention has a dielectric loss factor of 0.003 or less at a very high frequency of 10 GHz.
[0029] In the present invention, the polyamic acid can be produced, for example, by (1) A method in which the entire amount of the diamine component is placed in a solvent, and then the dianhydride component is added in an amount substantially equimolar to the diamine component to polymerize it; (2) A method in which the entire amount of the dianhydride component is placed in a solvent, and then a diamine component is added in an amount substantially equimolar to the dianhydride component to polymerize it; (3) A method in which a part of the diamine component is placed in a solvent, a part of the dianhydride component is mixed with the reaction components in a ratio of about 95 to 105 mol %, the remaining diamine component is added, and the remaining dianhydride component is added successively thereto, so that the diamine component and the dianhydride component are polymerized in substantially equimolar amounts; (4) A method in which a dianhydride component is placed in a solvent, a part of the components in the diamine compound is mixed in a ratio of 95 to 105 mol % relative to the reactive components, and then another dianhydride component is added, followed by the remaining diamine component, so that the diamine component and the dianhydride component are substantially equimolar, thereby polymerizing the mixture; (5) A method of forming a first composition by reacting some diamine components and some dianhydride acid components in a solvent so that one of them is in excess, and forming a second composition by reacting some diamine components and some dianhydride acid components in another solvent so that one of them is in excess, and then mixing the first and second compositions to complete polymerization, in which if the diamine component is in excess when the first composition is formed, the dianhydride acid component is in excess in the second composition, and if the dianhydride acid component is in excess in the first composition, the diamine component is in excess in the second composition, and the first and second compositions are mixed to polymerize so that the total diamine components and dianhydride acid components used in these reactions are substantially equimolar.
[0030] In the present invention, the polymerization method of the polyamic acid as described above can be defined as a random polymerization method, and the polyamic acid of the present invention produced by the above process can be used to produce the polymerizable composition. The polyimide film thus produced can be preferably applied in terms of maximizing the effect of the present invention, which is to reduce the dielectric loss factor (Df) and moisture absorption rate. However, in the above polymerization method, the length of the repeating unit in the polymer chain is relatively short as described above, so that there may be a limit to the excellent properties of the polyimide chain derived from the dianhydride acid component. Therefore, the polymerization method of polyamic acid that can be particularly preferably used in the present invention is the block polymerization method.
[0031] On the other hand, the solvent for synthesizing the polyamic acid is not particularly limited, and any solvent that dissolves the polyamic acid can be used, but an amide-based solvent is preferable. Specifically, the solvent may be an organic polar solvent, more specifically, an aprotic polar solvent, for example, one or more selected from the group consisting of N,N-dimethylformamide (DMF), N,N-dimethylacetamide, N-methyl-pyrrolidone (NMP), gamma-butyrolactone (GBL), and diglyme, but is not limited thereto, and may be used alone or in combination of two or more kinds as needed.
[0032] In one example, the solvent is preferably N,N-dimethylformamide or N,N-dimethylacetamide. In addition, in the process for producing the polyamic acid, a filler may be added for the purpose of improving various properties of the film such as sliding properties, thermal conductivity, corona resistance, loop hardness, etc. The filler to be added is not particularly limited, but preferred examples include silica, titanium oxide, alumina, silicon nitride, boron nitride, calcium hydrogen phosphate, calcium phosphate, mica, etc.
[0033] The particle size of the filler is not particularly limited and may be determined depending on the film properties to be modified and the type of filler to be added. In general, the average particle size is 0.05 to 100 μm, preferably 0.1 to 75 μm, more preferably 0.1 to 50 μm, and particularly preferably 0.1 to 25 μm. If the particle size is below this range, the modifying effect is unlikely to be achieved, whereas if it exceeds this range, the surface properties may be significantly damaged or the mechanical properties may be significantly reduced. The amount of the filler to be added is not particularly limited, and may be determined depending on the film properties to be modified, the particle size of the filler, etc. In general, the amount of the filler to be added is 0.01 to 100 parts by weight, preferably 0.01 to 90 parts by weight, and more preferably 0.02 to 80 parts by weight, relative to 100 parts by weight of polyimide.
[0034] If the amount of the filler added is less than this range, the modifying effect of the filler is unlikely to be exhibited, and if the amount exceeds this range, the mechanical properties of the film may be significantly damaged. The method of adding the filler is not particularly limited, and any known method may be used. In the production method of the present invention, the polyimide film is produced by a thermal imidization method and a chemical imidization method.
[0035] Alternatively, the imidization method may be a hybrid imidization method in which a thermal imidization method and a chemical imidization method are performed in parallel. The thermal imidization method is a method in which a chemical catalyst is excluded and the imidization reaction is induced by a heat source such as hot air or an infrared dryer. The thermal imidization method can imidize the amic acid groups present in the gel film by heat-treating the gel film at a variable temperature in the range of 100 to 600°C, specifically, 200 to 500°C, more specifically, 300 to 500°C.
[0036] However, even during the process of forming the gel film, a portion of the amic acid (approximately 0.1 mol % to 10 mol %) is imidized, and therefore the polyamic acid composition can be dried at a variable temperature in the range of 50°C to 200°C, which also falls within the category of the thermal imidization method. In the case of the chemical imidization method, a polyimide film can be produced using a dehydrating agent and an imidization agent by methods known in the art.
[0037] As an example of the composite imidization method, a polyimide film can be produced by adding a dehydrating agent and an imidization agent to a polyamic acid solution, heating the solution at 80 to 200°C, preferably 100 to 180°C, partially curing and drying the solution, and then heating the solution at 200 to 400°C for 5 to 400 seconds. The polyimide film of the present invention produced by the above-mentioned production method may have a dielectric loss factor (Df) of 0.004 or less, a coefficient of thermal expansion (CTE) of 15 ppm / °C or less, and a glass transition temperature (Tg) of 320°C or more. The present invention provides a multilayer film comprising the above-mentioned polyimide film and a thermoplastic resin layer, and a flexible metal foil laminate comprising the above-mentioned polyimide film and an electrically conductive metal foil.
[0038] As the thermoplastic resin layer, for example, a thermoplastic polyimide resin layer can be used. The metal foil used is not particularly limited, but when the flexible metal foil laminate of the present invention is used for electronic or electrical equipment, the metal foil may be, for example, copper or a copper alloy, stainless steel or an alloy thereof, nickel or a nickel alloy (including alloy 42), aluminum or an aluminum alloy. In general flexible metal foil laminates, copper foils such as rolled copper foils and electrolytic copper foils are often used, and are also preferably usable in the present invention. In addition, the surface of these metal foils may be coated with an anti-rust layer, a heat-resistant layer, or an adhesive layer.
[0039] In the present invention, the thickness of the metal foil is not particularly limited, and may be any thickness that allows the metal foil to exhibit sufficient function depending on the application. The flexible metal foil laminate according to the present invention may have a structure in which a metal foil is laminated on one side of the polyimide film, or an adhesive layer containing a thermoplastic polyimide is added to one side of the polyimide film, and the metal foil is laminated in a state of being attached to the adhesive layer. The present invention further provides an electronic component including the flexible metal foil laminate as an electrical signal transmission circuit, the electrical signal transmission circuit being an electronic component that transmits signals at a high frequency of at least 2 GHz, particularly at least 5 GHz, and more particularly at least 10 GHz.
[0040] The electronic component may be, for example, but is not limited to, a communication circuit for a mobile terminal, a communication circuit for a computer, or a communication circuit for an aerospace application. Meanwhile, the polyimide precursor composition according to the present invention may include a block copolymer including a first block obtained by reacting a dianhydride component including biphenyltetracarboxylic dianhydride (BPDA) with a diamine component including paraphenylenediamine (PPD), a second block obtained by reacting a dianhydride component including biphenyltetracarboxylic dianhydride with a diamine component including m-tolidine, and a third block obtained by reacting a dianhydride component including pyromellitic dianhydride (PMDA) with a diamine component including m-tolidine.
[0041] The dianhydride and diamine components of the block copolymer consist solely of biphenyltetracarboxylic dianhydride, pyromellitic dianhydride, paraphenylenediamine, and m-tolidine. In one embodiment, based on 100 mol% of the total content of the diamine components in the block copolymer, the content of m-tolidine may be 25 mol% or more and 40 mol% or less, the content of paraphenylenediamine may be 60 mol% or more and 75 mol% or less, and based on 100 mol% of the total content of the dianhydride components in the block copolymer, the content of biphenyltetracarboxylic dianhydride may be 50 mol% or more and 65 mol% or less, and the content of pyromellitic dianhydride may be 35 mol% or more and 50 mol% or less.
[0042] In one embodiment, the content of the biphenyltetracarboxylic dianhydride in the first block of the block copolymer may be 40 mol % or more and 55 mol % or less based on 100 mol % of a total content of dianhydride acid components in the polyimide film, and the content of the biphenyltetracarboxylic dianhydride in the second block may be 10 mol % or more based on 100 mol % of a total content of dianhydride acid components in the polyimide film. On the other hand, the content of the biphenyltetracarboxylic dianhydride in the second block may be 25 mol % or less based on 100 mol % of the total content of dianhydride acid components in the polyimide film.
[0043] The content of the m-tolidine in the third block of the block copolymer may be 10 mol % or more and 35 mol % or less, based on 100 mol % of the total content of diamine components in the polyimide film. The polyimide precursor composition of the present invention can contain the block copolymer (polyamic acid) and an organic solvent. The organic solvent is not particularly limited, and any solvent that dissolves the block copolymer (polyamic acid) can be used, but an amide-based solvent is preferable.
[0044] Specifically, the organic solvent may be a polar organic solvent, more specifically, an aprotic polar solvent, or may be, for example, one or more selected from the group consisting of N,N-dimethylformamide (DMF), N,N-dimethylacetamide, N-methyl-pyrrolidone (NMP), gamma-butyrolactone (GBL), and diglyme, but is not limited thereto, and may be used alone or in combination of two or more kinds as needed. In one example, the solvent is preferably N,N-dimethylformamide or N,N-dimethylacetamide.
[0045] Meanwhile, the block copolymer (polyamic acid) is included in about 5 wt% to about 35 wt% (for example, about 5 wt%, about 10 wt%, about 15 wt%, about 20 wt%, about 25 wt%, about 30 wt%, or about 35 wt%) based on the total weight of the polyimide precursor composition. In this range, the polyimide precursor composition can have a molecular weight and solution viscosity suitable for forming a film and can have excellent storage stability. Based on the total weight of the polyimide precursor composition, the block copolymer (polyamic acid) is included in, for example, about 10 wt% to about 30 wt%, and another example, about 15 wt% to 20 wt%, but is not limited thereto. The polyimide precursor composition is heated at 23° C. for 1 s -1 The viscosity of the composition may be from about 100,000 cP to about 300,000 cP (e.g., about 100,000 cP, about 150,000 cP, about 200,000 cP, about 250,000 cP, or about 300,000 cP) at a shear rate of about 100,000 cP to about 300,000 cP.
[0046] Within the above range, the block copolymer (polyamic acid) can have a predetermined weight average molecular weight while providing excellent processability during the formation of a polyimide film. Here, the "viscosity" can be measured using a HAAKE Mars Rheometer. The polyimide precursor composition was heated at 23° C. for 1 s-1 At a shear rate of about 150,000 cP to about 250,000 cP, for example, and as another example, a viscosity of about 200,000 cP to about 250,000 cP, but this is not limiting. The block copolymer (polyamic acid) may have a weight average molecular weight (Mw) of about 100,000 g / mol or more, for example, about 100,000 g / mol to about 500,000 g / mol, and within the above range, it may be advantageous for producing a better polyimide coating film or film, but is not limited thereto. Here, the "weight average molecular weight" can be measured using gel permeation chromatography (GPC).
[0047] The polyimide precursor composition of the present invention may be provided as a varnish and used to produce a polyimide coating film, or may be used to produce the polyimide film of the present invention. To obtain a polyimide coating film, a polyimide precursor composition can be applied onto a substrate by a conventional method such as spin coating, spray coating, screen printing, immersion, curtain coating, dip coating, or die coating, and then dried at a temperature of 250° C. or less to remove the solvent, followed by imidization.
[0048] The polyimide precursor composition of the present invention may contain other components within the scope of not impairing the object of the present invention. Examples of the other components include a base generator component, a polymerizable component such as a monomer, a surfactant, a plasticizer, a viscosity modifier, a defoamer, a colorant, and a filler. The filler is not particularly limited, but preferred examples include silica, titanium oxide, alumina, silicon nitride, boron nitride, calcium hydrogen phosphate, calcium phosphate, and mica. A method for producing a polyimide precursor composition according to the present invention includes the steps of: (a) polymerizing biphenyltetracarboxylic dianhydride and paraphenylenediamine in an organic solvent to produce a first polyamic acid including a first block of a block copolymer; (b) polymerizing biphenyltetracarboxylic dianhydride and m-tolidine with the first polyamic acid formed in step (a) to produce a second polyamic acid including the first and second blocks of the block copolymer; and (c) polymerizing pyromellitic dianhydride and m-tolidine with the second polyamic acid formed in step (b) to produce a third polyamic acid including the first, second, and third blocks of the block copolymer.
[0049] In one embodiment, based on 100 mol% of the total content of the diamine components in the block copolymer, the content of m-tolidine may be 25 mol% or more and 40 mol% or less, the content of paraphenylenediamine may be 60 mol% or more and 75 mol% or less, and based on 100 mol% of the total content of the dianhydride components in the block copolymer, the content of biphenyltetracarboxylic dianhydride may be 50 mol% or more and 65 mol% or less, and the content of pyromellitic dianhydride may be 35 mol% or more and 50 mol% or less. In one embodiment, the content of the biphenyltetracarboxylic dianhydride in the first block of the block copolymer is 40 mol % or more and 55 mol % or less based on 100 mol % of the total content of the dianhydride acid components of the block copolymer, and the content of the biphenyltetracarboxylic dianhydride in the second block is The dianhydride acid component content of the polyimide film may be 10 mol % or more based on 100 mol % of the total content of the dianhydride acid components.
[0050] On the other hand, the content of the biphenyltetracarboxylic dianhydride in the second block may be 25 mol % or less based on 100 mol % of the total content of dianhydride acid components in the polyimide film. The content of the m-tolidine in the third block of the block copolymer may be 10 mol % or more and 35 mol % or less, based on 100 mol % of the total content of diamine components in the polyimide film. EXAMPLES
[0051] The functions and effects of the present invention will be described in more detail below through specific examples of the present invention, however, these examples are merely presented as examples of the present invention and do not define the scope of the invention.
[0052] <Production Example> NMP was added to a 500 ml reactor equipped with a stirrer and nitrogen inlet / outlet tubes while injecting nitrogen, and the temperature of the reactor was set to 30°C. Then, paraphenylenediamine and m-tolidine as diamine components, and biphenyltetracarboxylic dianhydride and pyromellitic dianhydride as dianhydride components were added in a specified order, and the temperature was raised to 40°C under a nitrogen atmosphere and the mixture was stirred for 120 minutes while heating to carry out block copolymerization, thereby producing a polyamic acid having a viscosity of 200,000 cP at 23°C. The prepared polyamic acid was rotated at a high speed of 1,500 rpm or more to remove air bubbles. The degassed polyimide precursor composition was then applied to a glass substrate using a spin coater. The composition was then dried for 30 minutes at 120°C under a nitrogen atmosphere to prepare a gel film. The gel film was then heated to 450°C at a rate of 2°C / min, heat-treated at 450°C for 60 minutes, and cooled to 30°C at a rate of 2°C / min to obtain a polyimide film.
[0053] Then, the polyimide film was peeled off from the glass substrate by dipping in distilled water. The thickness of the polyimide film was 15 μm. The thickness of the polyimide film was measured using an Anritsu Electric Film Thickness Tester. Hereinafter, the content of the diamine component in the examples indicates the mol% of each diamine component based on 100 mol% of the total content of the diamine components in the polyimide film, and the content of the dianhydride acid component in the examples indicates the mol% of each dianhydride acid component based on 100 mol% of the total content of the dianhydride acid components in the polyimide film.
[0054] <Example 1> According to the above-mentioned production example, the diamine component and the dianhydride acid component were added in the following order: paraphenylenediamine (70 mol%), biphenyltetracarboxylic dianhydride (45 mol%), m-tolidine (15 mol%), biphenyltetracarboxylic dianhydride (15 mol%), m-tolidine (15 mol%), and pyromellitic dianhydride (40 mol%), and copolymerized to produce a polyimide film.
[0055] <Example 2> According to the above-mentioned production example, the diamine component and the dianhydride acid component were added in the following order: paraphenylenediamine (70 mol%), biphenyltetracarboxylic dianhydride (50 mol%), m-tolidine (10 mol%), biphenyltetracarboxylic dianhydride (10 mol%), m-tolidine (20 mol%), and pyromellitic dianhydride (40 mol%), and copolymerized to produce a polyimide film.
[0056] <Example 3> According to the above-mentioned production example, the diamine component and the dianhydride acid component were added in the following order: paraphenylenediamine (65 mol%), biphenyltetracarboxylic dianhydride (40 mol%), m-tolidine (10 mol%), biphenyltetracarboxylic dianhydride (10 mol%), m-tolidine (25 mol%), and pyromellitic dianhydride (50 mol%), and copolymerized to produce a polyimide film.
[0057] <Example 4> According to the above-mentioned production example, the diamine component and the dianhydride acid component were added in the following order: paraphenylenediamine (60 mol%), biphenyltetracarboxylic dianhydride (40 mol%), m-tolidine (15 mol%), biphenyltetracarboxylic dianhydride (15 mol%), m-tolidine (25 mol%), and pyromellitic dianhydride (45 mol%), and copolymerized to produce a polyimide film.
[0058] <Example 5> According to the above-mentioned production example, the diamine component and the dianhydride acid component were added in the following order: paraphenylenediamine (60 mol%), biphenyltetracarboxylic dianhydride (40 mol%), m-tolidine (10 mol%), biphenyltetracarboxylic dianhydride (10 mol%), m-tolidine (30 mol%), and pyromellitic dianhydride (50 mol%), and copolymerized to produce a polyimide film.
[0059] <Comparative Example 1> According to the above-mentioned manufacturing example, the diamine component and the dianhydride component were added in the order of paraphenylenediamine (55 mol%), biphenyltetracarboxylic dianhydride (50 mol%), m-tolidine (45 mol%), and pyromellitic dianhydride (50 mol%), and copolymerized to produce a polyimide film.
[0060] <Comparative Example 2> According to the above-mentioned manufacturing example, the diamine component and the dianhydride component were added in the order of m-tolidine (80 mol%), biphenyltetracarboxylic dianhydride (40 mol%), paraphenylenediamine (20 mol%), and pyromellitic dianhydride (60 mol%), and copolymerized to produce a polyimide film.
[0061] <Comparative Example 3> According to the above-mentioned manufacturing example, the diamine component and the dianhydride component were added in the order of m-tolidine (80 mol%), biphenyltetracarboxylic dianhydride (30 mol%), paraphenylenediamine (20 mol%), and pyromellitic dianhydride (70 mol%), and copolymerized to produce a polyimide film.
[0062] <Comparative Example 4> According to the above-mentioned manufacturing example, the diamine component and the dianhydride component were added in the order of m-tolidine (60 mol%), biphenyltetracarboxylic dianhydride (40 mol%), paraphenylenediamine (40 mol%), and pyromellitic dianhydride (60 mol%), and copolymerized to produce a polyimide film.
[0063] <Comparative Example 5> According to the above-mentioned production example, the diamine component and the dianhydride component were prepared by mixing paraphenylenediamine (80 mol%), biphenyltetracarboxylic dianhydride (70 mol%), m-tolidine (20 mol%), pyromellitic dianhydride (30 mol%), and the like. %) were added in this order and copolymerized to produce a polyimide film. The components and contents of the polyimide films produced in Examples 1 to 5 and Comparative Examples 1 to 5 are shown in Table 1 below. [Table 1]
[0064] <Experimental Example>Evaluation of dielectric constant, dielectric loss factor, thermal expansion coefficient and glass transition temperature The polyimide films produced in Examples 1 to 5 and Comparative Examples 1 to 5 were measured for dielectric constant, dielectric loss factor, thermal expansion coefficient, and glass transition temperature, and the results are shown in Table 2 below.
[0065] (1) Measurement of dielectric constant (Dk) The dielectric constant (Dk) was measured at 10 GHz using a Keysight network analyzer and a QWED SPDR resonator after drying the sample in an oven at 130°C for 30 minutes and leaving it in an environment at 23°C and 50% relative humidity for 24 hours.
[0066] (2) Measurement of dielectric loss factor (Df) The dielectric loss factor (Df) was measured at 10 GHz using a Keysight network analyzer and a QWED SPDR resonator after drying the sample for 30 minutes in an oven at 130°C and leaving it in an environment at 23°C and 50% relative humidity for 24 hours.
[0067] (3) Measurement of coefficient of thermal expansion (CTE) The coefficient of thermal expansion (CTE) was measured using a TA thermomechanical analyzer, model Q400. After cutting the polyimide film to a width of 4 mm and a length of 20 mm, the film was heated from room temperature to 300°C at a rate of 10°C / min while applying a tension of 0.05 N under a nitrogen atmosphere, and then cooled again at a rate of 10°C / min to measure the slope in the range from 100°C to 200°C.
[0068] (4) Measurement of glass transition temperature Glass transition temperature (T g ) measured the loss modulus and storage modulus of each film using DMA, and determined the inflection point in the tangent graph of these values as the glass transition temperature. [Table 2]
[0069] As shown in Table 2, the polyimide films prepared according to the embodiments of the present invention not only exhibit a significantly low dielectric loss factor of 0.003 or less, but also have desired levels of thermal expansion coefficient and glass transition temperature. Such results are achieved by the components and composition ratios specified in this application, and it is understood that the content of each component plays a decisive role. In contrast, it is expected that the polyimide films of Comparative Examples 1 to 5, which have components different from those of Examples 1 to 5, will be difficult to use in electronic components in which signal transmission is performed at high frequencies in the gigahertz range in terms of one or more of the dielectric loss factor, thermal expansion coefficient, and glass transition temperature. The present invention has been described above with reference to an embodiment thereof. However, a person having ordinary knowledge in the field to which the present invention pertains will be able to make various applications and modifications within the scope of the present invention based on the above content. [Industrial Applicability]
[0070] As described above, the present invention provides a polyimide film having excellent heat resistance, low dielectric properties and dimensional stability by using a polyimide film having specific components and a specific composition ratio and a polyamide precursor composition for producing the polyimide film. The polyimide film can be usefully applied in various fields requiring such properties, particularly to electronic parts such as flexible metal foil laminates.
Claims
1. a first block obtained by imidizing a polyamic acid derived from a polymer of a dianhydride acid component including biphenyltetracarboxylic dianhydride (BPDA) and a diamine component including paraphenylenediamine (PPD); a second block obtained by imidizing a polyamic acid derived from a polymer of a dianhydride component including biphenyltetracarboxylic dianhydride and a diamine component including m-tolidine; and a third block obtained by imidizing a polyamic acid derived from a polymer of a dianhydride acid component containing pyromellitic dianhydride (PMDA) and a diamine component containing m-tolidine. Polyimide film.
2. The polyimide film is obtained by imidizing a polyamic acid derived from a polymer of a dianhydride component consisting of biphenyltetracarboxylic dianhydride and pyromellitic dianhydride, and a diamine component consisting of paraphenylenediamine and m-tolidine. The polyimide film according to claim 1 .
3. the content of m-tolidine is 25 mol% or more and 40 mol% or less, and the content of p-phenylenediamine is 60 mol% or more and 75 mol% or less, based on 100 mol% of the total content of diamine components in the polyimide film; The polyimide film according to claim 1 .
4. The content of biphenyltetracarboxylic dianhydride is 50 mol % or more and 65 mol % or less based on 100 mol % of the total content of dianhydride acid components in the polyimide film; 2. The polyimide film according to claim 1, wherein the content of the pyromellitic dianhydride is from 35 mol % to 50 mol %.
5. the content of the biphenyltetracarboxylic dianhydride in the first block is 40 mol % or more and 55 mol % or less based on 100 mol % of the total content of the dianhydride acid components in the polyimide film; the content of the biphenyltetracarboxylic dianhydride in the second block is 10 mol % or more based on 100 mol % of the total content of the dianhydride acid components in the polyimide film; The polyimide film according to claim 1 .
6. the content of the m-tolidine in the third block is 10 mol % or more and 35 mol % or less based on 100 mol % of the total content of diamine components in the polyimide film; The polyimide film according to claim 1 .
7. The dielectric loss factor (Df) is 0.003 or less, A coefficient of thermal expansion (CTE) of 13 ppm / °C or more and 23 ppm / °C or less; The glass transition temperature (Tg) is 320° C. or higher. The polyimide film according to claim 1 .
8. A multilayer film comprising the polyimide film according to any one of claims 1 to 7 and a thermoplastic resin layer.
9. A laminate comprising the polyimide film according to any one of claims 1 to 7 and an electrically conductive metal foil. Flexible metal foil laminate.
10. The flexible metal foil laminate of claim 9, Electronic components.
11. A first block obtained by reacting a dianhydride component including biphenyltetracarboxylic dianhydride (BPDA) with a diamine component including paraphenylenediamine (PPD); a second block obtained by reacting a dianhydride component containing biphenyltetracarboxylic dianhydride with a diamine component containing m-tolidine; and a third block obtained by reacting a dianhydride component including pyromellitic dianhydride (PMDA) with a diamine component including m-tolidine. A polyimide precursor composition.
Citation Information
Patent Citations
Polyimide film
JP2017179150A
HMD-based PC game expansion system
KR1020220148027A
Apparatus for assisting driving of a host vehicle and method therof
KR1020220148378A
Highly heat-resistant and low dialectric-polyimide film and method for producing same
WO2021091011A1
Poly-imide resin with low dielectric constant and flexible metal laminate using the same
KR1020150069318A