Alkoxysilanes and dense organosilica films made therefrom.

Alkoxysilane precursors in CVD methods produce dense organosilica films with low dielectric constants and high mechanical properties, addressing the challenges of plasma-induced damage and feature erosion in microelectronic devices.

JP2024541843AActive Publication Date: 2024-11-13VERSUM MATERIALS US LLC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024522400
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-13
Filing Date
2022-10-11
Publication Date
2024-11-13
Estimated Expiration
2042-10-11

Smart Images

  • Figure 2024541843000001_ABST
    Figure 2024541843000001_ABST
Patent Text Reader

Abstract

A method for fabricating a dense organosilicon film with improved mechanical properties includes providing a substrate in a reaction chamber; introducing a gaseous composition comprising an alkoxysilane into the reaction chamber; and applying energy to the gaseous composition comprising an alkoxysilane in the reaction chamber to induce reaction of the gaseous composition comprising an alkoxysilane and deposit an organosilicon film on the substrate. The organosilicon film has a dielectric constant of about 2.40 to about 3.20, an elastic modulus of about 6 GPa to about 30 GPa, and an atomic % carbon of about 10 to about 45 as measured by XPS.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of U.S. Provisional Patent Application No. 63 / 255,323, filed October 13, 2021, which is incorporated herein in its entirety. [Background technology]

[0002] Described herein are compositions and methods for forming dense organosilica dielectric films using alkoxysilanes as precursors to the films. More specifically, described herein are compositions and chemical vapor deposition (CVD) methods for forming dense films having a dielectric constant k ranging from about 2.4 to about 3.2, which films have a high elastic modulus and superior resistance to plasma-induced damage compared to films fabricated from conventional precursors.

[0003] The electronics industry utilizes dielectric materials as insulating layers between circuits and components of integrated circuits (ICs) and related electronic devices. Line dimensions are being reduced to increase the speed and memory storage capabilities of microelectronic devices (e.g., computer chips). As line dimensions decrease, the insulation requirements for the interlayer dielectric (ILD) become more stringent. Shrinking the spacing requires a lower dielectric constant to minimize the RC time constant. Here, R is the resistance of the conductive line and C is the capacitance of the insulating dielectric interlayer. The capacitance (C) is inversely proportional to the spacing and proportional to the dielectric constant (k) of the interlayer dielectric (ILD). Conventional silica (SiO2) CVD dielectric films made from SiH4 or TEOS (Si(OCH2CH3)4, tetraethyl orthosilicate) and O2 have a dielectric constant k greater than 4.0. There have been a number of approaches attempted in the industry to produce silica-based CVD films with lower dielectric constants, the most successful being the doping of insulating silicon oxide films with organic groups, which provides dielectric constants in the range of about 2.4 to about 3.5. This organosilica glass (OSG) is typically produced from organosilicon precursors such as methylsilane or siloxane, and oxidizers such as O2 or NO, to produce dense films (density about 1.5 g / cm3). 3 ) is deposited.

[0004] Patents, published applications, and publications in the field of porous ILDs by CVD techniques include: EP 1119035 and U.S. Pat. No. 6,171,945, which describe a process of depositing an OSG film from an organosilicon precursor with labile groups in the presence of an oxidizing agent such as NO and optionally a peroxide, followed by a thermal anneal to remove the labile groups and provide porous OSG; U.S. Pat. Nos. 6,054,206 and 6,238,751, which describe a process of depositing an OSG film from an organosilicon precursor with labile groups in the presence of an oxidizing agent such as NO and optionally a peroxide, followed by a thermal anneal to remove the labile groups and provide porous OSG; teaches obtaining inorganic SiO2; EP 1037275, which describes the deposition of hydrogenated silicon carbide films that are converted to porous inorganic SiO2 by post-treatment with an oxidizing plasma; and U.S. Patel, WO 00 / 24050, and the literature article Grill, A. Patel, V. Appl. Phys. Lett. (2001), 79(6), pp. 803-805, all of which teach the codeposition of films from organosilicon precursors and organic compounds, followed by thermal annealing to provide multiphase OSG / organic films with some of the polymerized organic components retained. In the latter reference, the final composition of the film shows residual porogen and a high hydrocarbon film content of approximately 80 atomic % to 90 atomic %. Furthermore, the final film retains a SiO2-like network while replacing some of the oxygen atoms with organic groups.

[0005] US201110113184 discloses a class of materials that can be used to deposit insulating films with a dielectric constant in the range of about 2.4≦k≦2.8 via a PECVD process. The materials include Si compounds with two hydrocarbon groups that can be bonded together to form a ring structure with a Si atom, or Si compounds with one or more branched hydrocarbon groups. In the branched hydrocarbon groups, α-C, which is a C atom bonded to a Si atom and constituting a methylene group, and β-C, which is a C atom bonded to a methylene group, or γ-C, which is a C atom bonded to a β-C, are branching points. Specifically, two of the alkyl groups bonded to Si include CH2CH(CH3)CH3, CH2CH(CH3)CH2CH3, CH2CH2CH(CH3)CH3, CH2C(CH3)2CH3, and CH2CH2CH(CH3)2CH3, and the third group bonded to silicon includes OCH3 and OC2H5. Although the invention claims that a high density of SiCH2Si groups is formed in the as-deposited films via plasma dissociation of the alkyl group R from SiCH2R, the examples in the patent application clearly show that a high density of SiCH2Si groups occurs only after the films are exposed to UV irradiation. The formation of SiCH2Si groups upon UV irradiation is well documented in the literature. In addition, the k values ​​reported for these films are low, below 2.8.

[0006] US2020075321 discloses a method for forming a low-k carbon-doped silicon oxide (CDO) layer with high hardness by a plasma enhanced chemical vapor deposition (PECVD) process. The method includes providing a carrier gas at a carrier gas flow rate and a CDO precursor at a precursor flow rate to a process chamber. Radio frequency (RF) power is applied to the CDO precursor at a power level and frequency. The CDO layer is deposited on a substrate in the process chamber.

[0007] WO 21050798 [EN] describes a method for producing dense organosilicon films with improved mechanical properties, comprising: providing a substrate in a reaction chamber; introducing a gaseous composition comprising a novel mono- or dialkoxysilane into the reaction chamber; and applying energy to the gaseous composition comprising a novel mono- or dialkoxysilane in the reaction chamber to induce reaction of the gaseous composition comprising a novel mono- or dialkoxysilane and deposit an organosilicon film on the substrate. The organosilicon film has a dielectric constant of about 2.8 to about 3.3, an elastic modulus of about 7 to about 30 GPa, and about 10 to about 30 atomic % carbon as measured by XPS.

[0008] WO21050659 discloses a method for producing dense organosilicon films with improved mechanical properties, comprising: providing a substrate in a reaction chamber; introducing a gaseous composition comprising a novel monoalkoxysilane into the reaction chamber; and applying energy to the gaseous composition comprising the novel monoalkoxysilane in the reaction chamber to induce reaction of the gaseous composition comprising the novel monoalkoxysilane and deposit an organosilicon film on the substrate. The organosilicon film has a dielectric constant of about 2.80 to about 3.30, an elastic modulus of about 9 GPa to about 32 GPa, and an atomic % carbon of about 10 to about 30 as measured by XPS.

[0009] Plasma or process induced damage (PID) in low-k films is caused by the removal of carbon from the film during plasma exposure, especially during etching and photoresist stripping processes. This changes the plasma damaged area from hydrophobic to hydrophilic. Exposure of a hydrophilic SiO2 like damaged layer to a dilute HF based wet chemical plasma post treatment (with or without additives like surfactants) results in rapid decomposition of this layer. In patterned low-k wafers this results in feature erosion. Process induced damage in low-k films and the resulting feature erosion are significant issues that device manufacturers must overcome when incorporating low-k materials in ULSI interconnects.

[0010] Films with improved mechanical properties (higher modulus, higher hardness) reduce line edge roughness in patterned features, reduce pattern collapse, and provide greater internal mechanical stress in interconnects, reducing defects due to electromigration. Thus, there is a need for low-k films with excellent resistance to PID and the highest possible mechanical properties for a given dielectric constant. The precursors in the present invention are targeted to films with dielectric constants for the most advanced technology nodes, typically around 2.4 to 3.2. Summary of the Invention

[0011] The methods and compositions described herein meet one or more of the above needs: Using alkoxysilane precursors, dense low-k films can be deposited with k values ​​of about 2.40 to about 3.20, and such films exhibit unexpectedly high elastic modulus / hardness and unexpectedly high resistance to plasma-induced damage.

[0012] In one aspect, a method for fabricating dense organosilica films with improved mechanical properties is provided, the method comprising: providing a substrate in a reaction chamber; introducing into the reaction chamber a gaseous composition comprising at least one alkoxysilane compound having a structure of Formula I: [ka] Here, R is a linear or branched C2-C5 alkane, a linear or branched C2-C5 alkene, a linear or branched C2-C5 alkyne, a C4-C 10 Cyclic alkanes, C4-C 10 Cyclic alkenes, C5-C 10arenes. For formula I above, the combination of alkyl groups is preferably selected such that the boiling point of the alkoxysilane compound is less than 250° C. In addition, for optimal performance, the alkyl groups are preferably selected such that the carbon atom bonded to the oxygen atom is a secondary or tertiary carbon, resulting in a more stable secondary or tertiary carbon radical upon homolytic bond dissociation (e.g., SiO-R-OSi→SiO·+SiO-R·, where SiO-R· is a primary, or a secondary or tertiary radical). Energy is then applied to the gaseous composition comprising alkoxysilane in the reaction chamber to induce reaction of the gaseous composition comprising alkoxysilane and deposit an organosilica film on the substrate. According to an exemplary embodiment, the organosilica film has a dielectric constant of about 2.40 to about 3.20 and an elastic modulus of about 6 GPa to about 30 GPa, preferably about 6 GPa to about 25 GPa. According to another embodiment, the film further comprises about 10 to about 45 atomic % carbon as measured by XPS. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is an FTIR spectrum of a film deposited using 1,4-bis(dimethylsiloxy)cyclohexane under the conditions described in Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Described herein is a chemical vapor deposition method for fabricating dense organosilica films with improved mechanical properties, the method comprising: providing a substrate in a reaction chamber; introducing a gaseous composition comprising an alkoxysilane, a gaseous oxidant such as O2 or N2O, and an inert gas such as He into the reaction chamber; and applying energy to the gaseous composition comprising an alkoxysilane in the reaction chamber to induce reaction of the gaseous composition comprising an alkoxysilane and deposit an organosilica film on the substrate. According to an exemplary embodiment, the organosilica film has a dielectric constant of about 2.40 to about 3.20, an elastic modulus of about 6 GPa to about 30 GPa, and about 10 to about 45 atomic % carbon as measured by XPS, and preferably has a dielectric constant of about 2.80 to about 3.00, an elastic modulus of about 7 GPa to about 23 GPa, and about 12 to about 43 atomic % carbon as measured by XPS.

[0015] Also described herein is a method for fabricating dense organosilica films with improved mechanical properties, the method including: providing a substrate into a reaction chamber; introducing a gaseous composition including an alkoxysilane, a gaseous oxidizer such as O2 or N2O, and an inert gas such as He into the reaction chamber; and applying energy to the gaseous composition including the alkoxysilane to deposit an organosilica film on the substrate. According to an exemplary embodiment, the organosilica film has a dielectric constant of about 2.40 to about 3.20 and an elastic modulus of about 6 GPa to about 30 GPa.

[0016] Alkoxysilanes offer unique properties that allow for the achievement of relatively low dielectric constants and surprisingly superior mechanical properties for dense organosilica films compared to prior art structure-forming precursors such as diethoxymethylsilane (DEMS) and 1-ethoxy-1-methylsilacyclopentane (MESCP). Without being bound by theory, it is believed in the present invention that alkoxysilanes can provide stable secondary or tertiary diradicals that help promote the formation of disilylmethylene groups (i.e., Si-CH2-Si moieties) in the as-deposited films.

[0017] It is well known to those skilled in the art of organic chemistry that more energy must be supplied to generate a primary hydrocarbon radical (such as the ethyl radical CH3CH2·) than a secondary hydrocarbon radical (such as the isopropyl radical (CH3)2CH·). This is due to the greater stability of the isopropyl radical with respect to the ethyl radical. The same principle applies to the homolytic bond dissociation of oxygen-carbon bonds in silicon alkoxy groups; it takes less energy to dissociate the oxygen-carbon bond in isopropoxysilane than in ethoxysilane. Similarly, it takes less energy to dissociate the silicon-carbon bond in isopropylsilane than in ethylsilane. It is assumed that bonds that require less energy to break are more likely to dissociate in a plasma. Thus, the Si-OPr i , or Si-OBu s or Si-OBu t Alkoxysilanes with Si-OEt groups can provide a higher density of SiO radicals in plasma than alkoxysilanes with Si-Et or Si-Pr groups. i , Si-Bu s Or Si-Bu t Alkoxysilanes bearing groups can provide a higher density of Si·-type radicals in plasma compared to alkoxysilanes bearing simple Si-Me groups. This is probably due to the fact that alkoxysilanes bearing Si-OMe groups have Si-OEt, Si-OPr, which constitute the R group of formula I, are more efficient at reacting with alkoxysilanes bearing Si-OMe groups. i , or Si-OBu s or Si-OBu t This contributes to the differentiated properties of the films deposited using alkoxysilanes bearing the SiO-R-OSi moiety. Importantly, the SiO-R-OSi bond can provide more stable SiO-R radicals than the hydrocarbon radicals resulting from oxygen-carbon bonds, thus potentially enabling the generation of more disilylmethylene bonds in the as-deposited silicon-containing films.

[0018] Without intending to be bound by theory, it is believed that alkoxysilane compounds having formula I may have advantages over simple alkoxysilanes such as TEOS (tetraethoxysilane), MTES (methyltriethoxysilane), DEMS (diethoxymethylsilane), or dimethylmethoxysilane with respect to their use as precursors for the deposition of dense organosilica films. Specifically, the alkoxysilane compounds having formula I described herein have two silicon atoms instead of one, which may lead to higher deposition rates and / or more efficient deposition of silicon atoms onto the substrate surface. In addition, the alkoxy moieties in these molecules are derived from diols and bridge the two silicon atoms into close proximity to each other when the precursor reacts with the plasma reactant gas and the substrate surface. Also, the radicals believed to be generated on the carbon atoms of the R groups in formula I may have better stability and / or better ability to form dense network organosilica films on substrates compared to those radical species generated from terminal alkoxy groups such as methoxy, ethoxy, iso-propoxy, sec-butoxy, and tert-butoxy.

[0019] Some of the advantages over the prior art that are achieved using alkoxysilanes as silicon precursors include, but are not limited to: Low cost and ease of synthesis High elastic modulus Wide range XPS carbon High disilylmethylene density A high percentage of Si(CH3)2 or Si(CH3)CH2Si in the Si(CH3)x IR bands, and High deposition rate.

[0020] In one aspect, a method is provided for the fabrication of dense organosilica films with improved mechanical properties, the method comprising: providing a substrate in a reaction chamber; introducing a gaseous composition into the reaction chamber comprising at least one alkoxysilane compound having a structure of Formula I: [ka] Here, R is a linear or branched C2-C5 alkane, a linear or branched C2-C5 alkene, a linear or branched C2-C5 alkyne, a C4-C 10 Cyclic alkanes, C4-C 10 Cyclic alkenes, C5-C 10 arenes, with or without an oxygen source. For formula I above, the combination of alkyl groups is selected such that the boiling point of the molecule is less than 200° C. In addition, for optimal performance, the R groups are selected from those that can form secondary or tertiary carbon radicals upon homolytic bond dissociation (e.g., SiO-R-OSi→SiO·+SiO-R·, where SiO-R· is a primary, or secondary or tertiary radical). The resulting SiO-R· radical is expected to react with the Si-Me group to generate Si-CH2-Si bonds that help increase the disilylmethylene density. Energy is then applied to the gaseous composition comprising alkoxysilane in the reaction chamber to induce reaction of the gaseous composition comprising alkoxysilane and deposit the organosilicon film on the substrate. According to an exemplary embodiment, the organosilicon film has a dielectric constant of about 2.40 to about 3.20 and an elastic modulus of about 6 GPa to about 25 GPa. The substrate temperature also has an effect on the properties of the resulting dense organosilica film, and higher temperatures may be preferred, such as, for example, 300° C. to 400° C., or 350° C. to 400° C. In certain embodiments, the oxygen source is selected from the group consisting of water vapor, water plasma, ozone, oxygen, oxygen plasma, oxygen / helium plasma, oxygen / argon plasma, nitrogen oxide plasma, carbon dioxide plasma, hydrogen peroxide, organic peroxides, and mixtures thereof.

[0021] In yet another embodiment, a composition is provided that includes at least one alkoxysilane compound having a structure of Formula I: [ka] Here, R is a linear or branched C2-C5 alkane, a linear or branched C2-C5 alkene, a linear or branched C2-C5 alkyne, a C4-C 10Cyclic alkanes, C4-C 10 Cyclic alkenes, C5-C 10 The organic moiety is derived from the group consisting of arenes. Table 1 lists preferred alkoxysilanes having formula I.

[0022] [Table 1-1] [Table 1-2] [Table 1-3]

[0023] The alkoxysilanes described herein can be synthesized by a variety of routes. One route involves reacting the corresponding diol (containing two -OH groups) with tetramethyldisilazane, as shown in formula (1). [ka] Another route involves the reaction of an aminodimethylsilane, such as dimethylaminodimethylsilane, with the corresponding diol, as shown in equation (2). [ka] An alternative route involves the reaction of tetramethyldisiloxane with the corresponding diol, as shown in equation (3). [ka] An alternative route involves the reaction of an alkoxydimethylsilane, such as dimethylethoxysilane, with the corresponding diol, as shown in equation (4). [ka] An alternative route involves the reaction of chlorodimethylsilane with the corresponding diol, as shown in equation (5). [ka]

[0024] Alternatively, the reaction depicted in equation (5) can be carried out in the presence of an amine base or some other type of HCl scavenger to drive the reaction to completion.

[0025] An alternative route involves a two-step process, where the first step is the reaction of the corresponding diol with an organolithium reagent (e.g., n-butyllithium), a different organometallic reagent (e.g., dibutylmagnesium), a metal amide (e.g., LiN i The reaction involves first generating a metallated diolate intermediate by metallation with a diamine such as Pr2 or NaN(SiMe3)2, a Grignard reagent (e.g., MeMgCl), or a metal hydride reagent (e.g., LiH, NaH, KH, CaH2). The second step involves reacting the metallated diolate with either an alkoxydimethylsilane, tetramethyldisiloxane, or chlorodimethylsilane. An example of this two-step process is shown in equation (6). [ka]

[0026] In the formula above and throughout this specification, the term "alkane" refers to a straight or branched chain functional group having 1 to 10 carbon atoms bonded to two oxygen atoms. Exemplary straight chain alkyl groups include, but are not limited to, ethane, propane, and n-butane. Exemplary branched chain alkyl groups include, but are not limited to, isobutane and 2,3-dimethylbutane.

[0027] In the formula above and throughout this specification, the term "cyclic alkane" refers to a cyclic functional group having 3 to 10 carbon atoms bonded to two oxygen atoms. Exemplary cyclic alkyl groups include, but are not limited to, cyclopentane and cyclohexane.

[0028] In the formula above and throughout this specification, the term "alkene" refers to a group having one or more carbon-carbon double bonds and having 2 to 10 or 2 to 6 carbon atoms bonded to two oxygen atoms.

[0029] In the formula above and throughout this specification, the term "alkyne" refers to a group having one or more carbon-carbon triple bonds and having 2 to 10 or 2 to 6 carbon atoms bonded to two oxygen atoms.

[0030] In the formula above and throughout this specification, the term "arene" refers to an aromatic cyclic functional group having 3-10 carbon atoms, 5-10 carbon atoms, or 6-10 carbon atoms bonded to two oxygen atoms. Exemplary aryl groups include, but are not limited to, benzene and toluene.

[0031] In the formula above and throughout this specification, the term "secondary carbon" refers to a carbon that is bonded to two carbon atoms.

[0032] In the formula above and throughout this specification, the term "tertiary carbon" refers to a carbon that is bonded to three carbon atoms.

[0033] Throughout this specification the symbol "~" indicates a deviation of about 5.0% from the value, for example ~3.00 indicates about 3.00 (±0.15).

[0034] The alkoxysilanes having formula I according to the present invention and compositions comprising alkoxysilane compounds having formula I according to the present invention are preferably substantially free of halide ions. As used herein, the term "substantially free" with respect to halide ions (or halides), such as, for example, chloride (i.e., chloride-containing species such as HCl or silicon compounds having at least one Si-Cl bond) and fluoride, bromide, and iodide, means less than 5 ppm (by weight) as measured by ion chromatography (IC), preferably less than 3 ppm as measured by IC, more preferably less than 1 ppm as measured by IC, and most preferably 0 ppm as measured by IC. Chloride is known to act as a decomposition catalyst for silicon precursor compounds having formula I. High levels of chloride in the final product can cause the decomposition of silicon precursor compounds. The gradual decomposition of silicon precursor compounds can directly affect the film deposition process and make it difficult for semiconductor manufacturers to meet film specifications. Moreover, the faster decomposition rate of silicon precursor compounds adversely affects the shelf life or stability, making it difficult to guarantee a shelf life of 1 to 2 years. Accelerated decomposition of silicon precursor compounds therefore poses safety and performance concerns associated with the formation of these flammable and / or pyrophoric gaseous by-products. The alkoxysilanes having formula I are preferably Li + , Na + , K + , Mg 2+ , Ca 2+ , Al 3+ , Fe 2+ , Fe 3+ , Ni 2+ , Cr 3+ As used herein, the term "substantially free" with respect to Li, Na, K, Mg, Ca, Al, Fe, Ni, Cr means less than 5 ppm (by weight), preferably less than 3 ppm, more preferably less than 1 ppm, and most preferably 0.1 ppm, as measured by ICP-MS. In some embodiments, the silicon precursor compound having formula I is Li + , Na + , K+ , Mg 2+ , Ca 2+ , Al 3+ , Fe 2+ , Fe 3+ , Ni 2+ , Cr 3+ As used herein, the term "free" of metal impurities with respect to Li, Na, K, Mg, Ca, Al, Fe, Ni, Cr means less than 1 ppm by weight as measured by ICP-MS, preferably less than 0.1 ppm, and most preferably less than 0.05 ppm by weight as measured by ICP-MS or other analytical method for metal measurement.

[0035] Furthermore, the alkoxysilanes having formula I, when used as precursors for depositing dense organosilica films, preferably have a purity of 98% by weight or more, more preferably 99% by weight, as measured by GC. Importantly, the alkoxysilane compounds having formula I are preferably substantially free of oxygen-containing or nitrogen-containing impurities, either from the starting materials used during synthesis or from by-products produced during synthesis. Examples include, but are not limited to, water, tetramethyldisiloxane, organic amines such as triethylamine, pyridine and other organic amines used to facilitate the reaction. As used herein, the term "free" of oxygen-containing or nitrogen-containing impurities, when referring to tetramethyldisiloxane, tetramethyldisilazane, water, organic amines such as triethylamine, pyridine and other organic amines, means 1000 ppm or less (by weight) as measured by GC, preferably 500 ppm or less (by weight), and most preferably 100 ppm or less (by weight) as measured by GC or other analytical methods. Oxygen-containing impurities as defined herein are compounds having at least one oxygen atom, either originating from the starting material or resulting from the synthesis of the alkoxysilane compound having formula I. These oxygen-containing impurities may have a boiling point close to that of the alkoxysilane compound having formula I, and therefore may remain in the product after purification. Similarly, nitrogen-containing impurities as defined herein are compounds having at least one nitrogen atom, either originating from the starting material or resulting from the synthesis of the alkoxysilane compound having formula I. These nitrogen-containing impurities may have a boiling point close to that of the alkoxysilane compound having formula I, and therefore may remain in the product after purification.

[0036] Low-k dielectric films such as organosilicates are organosilica glass ("OSG") films or materials. Organosilicates are employed in the electronics industry, for example, as low-k materials. Material properties depend on the chemical composition and structure of the film. The type of organosilicon precursor has a strong effect on the structure and composition of the film, so it is beneficial to use a precursor that provides the necessary film properties to ensure that the addition of the amount of porosity required to reach the desired dielectric constant does not produce a mechanically robust film. The methods and compositions described herein provide a means to produce low-k dielectric films with the desired balance of electrical and mechanical properties, as well as other beneficial film properties such as high carbon content to integrally improve plasma resistance.

[0037] In certain embodiments of the methods and compositions described herein, a layer of silicon-containing dielectric material is deposited on at least a portion of a substrate via a chemical vapor deposition (CVD) process using a reaction chamber. Thus, the method includes providing a substrate in a reaction chamber. Suitable substrates include, but are not limited to, semiconductor materials such as gallium arsenide ("GaAs"), silicon, and silicon-containing compositions such as crystalline silicon, polysilicon, amorphous silicon, epitaxial silicon, silicon dioxide ("SiO2"), silicon glass, silicon nitride, fused silica, glass, quartz, borosilicate glass, and combinations thereof. Other suitable materials include chromium, molybdenum, and other metals commonly used in semiconductor, integrated circuit, flat panel display, and flexible display applications. The substrate may have additional layers such as, for example, silicon, SiO2, organosilicate glass (OSG), fluorosilicate glass (FSG), boron carbonitride, silicon carbide, hydrogenated silicon carbide, silicon nitride, hydrogenated silicon nitride, silicon carbonitride, hydrogenated silicon carbonitride, boronitride, organic-inorganic composites, photoresists, organic polymers, porous organic and inorganic materials and composites, and metal oxides such as aluminum oxide and germanium oxide. The additional layers can be germanosilicates, aluminosilicates, copper and aluminum, and diffusion barrier materials such as, but not limited to, TiN, Ti(C)N, TaN, Ta(C)N, Ta, W, or WN.

[0038] The reaction chamber is typically, for example, a thermal CVD or plasma CVD reactor, or a batch furnace type reactor in various ways. In an embodiment, a liquid transport system may be utilized. In a liquid transport formulation, the precursors described herein may be transported in neat liquid form, or alternatively, may be used in a solvent formulation or composition containing the same. Thus, in certain embodiments, the precursor formulation may include a solvent component(s) of suitable properties as may be desirable and advantageous in a given end use application of forming a film on a substrate.

[0039] The method disclosed herein includes introducing a gaseous composition including an alkoxysilane into a reaction chamber. In some embodiments, the composition includes additional reactants such as, for example, oxygen-containing species, e.g., O2, O3, and N2O, gaseous or liquid organic substances, CO2, or CO. In one detailed embodiment, the reaction mixture introduced into the reaction chamber includes at least one oxidizing agent selected from the group consisting of O2, N2O, NO, NO2, CO2, water, H2O2, ozone, and combinations thereof. In an alternative embodiment, the reaction mixture does not include an oxidizing agent.

[0040] The compositions for depositing the dielectric films described in this disclosure include from about 40% to about 100% by weight of an alkoxysilane in a solvent and can be delivered to a reaction chamber via direct liquid injection (DLI).

[0041] In embodiments, the gaseous composition including alkoxysilanes may be used in conjunction with a curing additive to further increase the elastic modulus of the deposited film.

[0042] In embodiments, the gaseous composition comprising the alkoxysilane is substantially free or free of halides, such as, for example, chlorides.

[0043] In addition to alkoxysilanes, additional materials can be introduced into the reaction chamber before, during, and / or after the deposition reaction. Such materials include, for example, inert gases (e.g., He, Ar, N2, Kr, Xe, etc., which can be used as carrier gases for low volatility precursors and / or can promote curing of the deposited materials to provide a more stable final film).

[0044] The reagents used, including the alkoxysilanes, can be delivered to the reactor separately from separate sources or as a mixture. The reagents can be delivered to the reactor system by any number of means, preferably using a pressurizable stainless steel vessel fitted with appropriate valves and fittings to allow the delivery of liquids to the process reactor. Preferably, the precursor is delivered to the process vacuum chamber as a gas, i.e., the liquid must be vaporized before it is delivered to the process chamber.

[0045] In another embodiment, the method disclosed herein includes introducing a gaseous composition comprising a mixture of 1-alkoxy-1-methylsilacyclopentane and an alkoxysilane into a reaction chamber.

[0046] The method disclosed herein includes applying energy to a gaseous composition comprising an alkoxysilane in a reaction chamber to induce reaction of the gaseous composition comprising an alkoxysilane and deposit an organosilica film on a substrate, where the organosilica film has a dielectric constant of about 2.40 to about 3.20 in some embodiments, about 2.40 to about 3.00 in other embodiments, and in more preferred embodiments, about 2.40 to about 2.90, or about 2.80 to about 3.00; an elastic modulus of about 2 GPa to about 30 GPa, preferably 3 GPa to 23 GPa; and about 10 atomic % carbon to about 45 atomic % carbon as measured by XPS. Energy is applied to the gaseous reagents to induce reaction of the alkoxysilane and, if present, other reactants to form a film on the substrate. Such energy can be provided by, for example, plasma, pulsed plasma, helicon plasma, high density plasma, inductively coupled plasma, remote plasma, hot filament, and thermal (i.e., non-filament) and methods. A secondary rf frequency source can be used to modify the plasma characteristics at the substrate surface.Preferably, the film is formed by plasma enhanced chemical vapor deposition ("PECVD").

[0047] Flow rates for each of the gaseous reagents preferably range from 10 sccm to 5000 sccm, more preferably 30 sccm to 3000 sccm, for a single 300 mm wafer. The actual flow rates required may depend on the wafer size and chamber configuration, and are not limited to 300 mm wafers or single wafer chambers.

[0048] In certain embodiments, the film is deposited at a deposition rate of about 5 nanometers (nm) to about 200 nanometers (nm) per minute. In other embodiments, the film is deposited at a deposition rate of about 30 nanometers (nm) to about 200 nanometers (nm) per minute.

[0049] The pressure in the reaction chamber during deposition typically ranges from about 0.01 Torr to about 600 Torr, or from about 1 Torr to about 15 Torr.

[0050] Although thickness can vary as desired, films are preferably deposited to a thickness of 0.001 microns to 500 microns. Blanket films deposited on non-patterned surfaces have excellent uniformity, e.g., less than 3% thickness variation for 1 standard deviation across the substrate, with reasonable edge exclusion where the 5 mm outermost edge of the substrate is not included in statistical calculations of uniformity.

[0051] In addition to the OSG products of the invention, the invention includes processes by which the products are made, methods of using the products and compounds, and compositions useful for preparing the products. For example, a process for fabricating integrated circuits on semiconductor devices is disclosed in U.S. Patent No. 6,583,049, which is incorporated herein by reference.

[0052] The dense organosilica films produced by the disclosed methods exhibit excellent resistance to plasma-induced damage, especially during etching and photoresist strip processes.

[0053] The dense organosilica films produced by the disclosed methods exhibit superior mechanical properties for a given dielectric constant relative to dense organosilica films made from precursors having the same dielectric constant but that are not alkoxysilanes. Typically, the resulting organosilica films (as deposited) have a dielectric constant of about 2.40 to about 3.20 in some embodiments, about 2.80 to about 3.10 in other embodiments, and about 2.40 to about 3.00 in still other embodiments, an elastic modulus of about 6 GPa to about 30 GPa, and about 10 atomic % carbon to about 45 atomic % carbon as measured by XPS. In some embodiments, the incorporation of nitrogen is believed to potentially increase the dielectric properties of the dense organosilica films, and therefore the nitrogen content is expected to be 0.1 atomic % or less, preferably 0.1 atomic % or less, and most preferably 0.01 atomic % or less, as measured by XPS, SIMS or RBS, or any analytical method. In addition, the organosilica film has a relative disilylmethylene density of about 1 to about 30, about 5 to about 30, about 10 to about 30, or about 1 to about 20, as calculated from FTIR spectra. In some embodiments, the organosilica film deposits at a rate of about 5 nm / min to about 1000 nm / min, or about 50 nm / min to about 1000 nm / min. In other embodiments, the organosilica film deposits at a higher rate of about 100 nm / min to about 2000 nm / min, about 200 nm / min to about 2000 nm / min, or about 500 nm / min to about 2000 nm / min. Importantly, alkoxysilanes having formula I are expected to provide higher deposition rates than other alkoxysilanes because the other alkoxysilanes have existing Si-R-Si bonds.

[0054] The resulting dense organosilica films may be subjected to post-treatment processes after deposition. Thus, the term "post-treatment" as used herein refers to treating the film with energy (e.g., heat, plasma, photons, electrons, microwaves, etc.) or chemicals to further enhance the material properties.

[0055] The conditions under which post-treatment is carried out may vary widely, for example, post-treatment may be carried out under elevated pressure or reduced pressure.

[0056] UV annealing is the preferred method, which is carried out under the following conditions:

[0057] The environment may be inert (e.g., nitrogen, CO2, noble gases (He, Ar, Ne, Kr, Xe), etc.), oxidizing (e.g., oxygen, air, dilute oxygen environment, enriched oxygen environment, ozone, nitrous oxide, etc.), or reducing (dilute or concentrated hydrogen, hydrocarbons (saturated, unsaturated, straight or branched chain, aromatic), etc.). The pressure is preferably from about 1 Torr to about 1000 Torr. However, reduced pressure environments are preferred for thermal annealing as well as other post-treatment procedures. The temperature is preferably from 200° C. to 500° C. with a ramp rate of 0.1 deg° C. / min to 100 deg° C. / min. The total UV anneal time is preferably from 0.01 min to 12 h.

[0058] The present invention is illustrated in more detail with reference to the following examples, but it should be understood that it is not to be considered limited thereto. It is also recognized that the precursors described in the present invention can also be used to deposit porous low-k films with similar process advantages (i.e., higher elastic modulus for a given value of dielectric constant and greater resistance to plasma-induced damage) relative to existing porous low-k films. EXAMPLES

[0059] Some experiments were performed on a 300mm AMAT Producer SE, which deposits films on two wafers simultaneously. The precursor and gas flow rates therefore correspond to the flow rates required to deposit films on two wafers simultaneously. Each wafer processing station has its own independent RF power source, so the RF power shown per wafer is accurate. Both wafer processing stations are maintained at the same pressure, so the deposition pressure shown is accurate. Other experiments were performed on a 200mm AMAT P5000 Platform, which provided a variety of dense organo-silica films on a single wafer. The deposition chamber is fitted with an RF power source suitable for industry standard PECVD processes.

[0060] Although shown and described above with respect to certain specific embodiments and examples, the present invention is nevertheless not intended to be limited to the details shown. Rather, various changes may be made in the details within the scope and range of equivalents of the claims without departing from the spirit of the present invention. For example, all ranges broadly described in this document are expressly intended to include all narrower ranges within that broad range. It is also recognized that the hydrido-dimethyl-alkoxysilanes disclosed in the present invention can be used as structure-forming agents for the deposition of porous low-k films with high elastic modulus, high XPS carbon content, and high resistance to plasma-induced damage.

[0061] The thickness and refractive index were measured with a Woollam Model M2000 Spectroscopic Ellipsometer. The dielectric constant was determined using the Hg probe technique on medium resistivity p-type wafers (ranging from 8 ohm cm to 12 ohm cm). FTIR spectra were measured using a Thermo Fisher Scientific Model iS50 spectrometer equipped with a nitrogen purged Pike Technologies Map300 to handle 12-inch wafers. The FTIR spectra were used to calculate the relative density of bridging disilylmethylene groups in the films. The relative density of bridging disilylmethylene groups in the films (i.e., SiCH2Si density), as determined by infrared spectroscopy, was calculated using the FTIR spectrum at 1360 cm -1 The area of ​​the SiCH2Si infrared band centered around 1250 cm -1 From 920cm -1 SiO X The peaks corresponding to the CH3 stretch, asymmetric bending, and symmetric bending are at approximately 2960 cm -1 , 1410cm -1 , and 1274 cm -1 The focus is on H X The bond stretching vibration mode for SiO is 2100 -1 cm to 2300cm -1The mechanical properties were determined using a KLA iNano Nano Indenter.

[0062] Compositional data was obtained by X-ray photoelectron spectroscopy (XPS) using either a PHI 5600 (73560, 73808) or a Thermo K-Alpha (73846) and is provided in atomic weight percent. Hydrogen is not included in the atomic weight percent (%) values ​​reported in the tables.

[0063] Although shown and described above with respect to certain specific embodiments and examples, the present invention is nevertheless not intended to be limited to the details shown. Rather, various changes may be made in the details within the scope and range of equivalents of the claims without departing from the spirit of the present invention. For example, all ranges broadly described in this document are expressly intended to include all narrower ranges within that broad range. It is also recognized that the alkoxysilanes disclosed in the present invention can be used as structure-forming agents for the deposition of porous low-k films with high elastic modulus, high XPS carbon content, and high resistance to plasma-induced damage.

[0064] Example 1: Synthesis of 1,4-bis(dimethylsiloxy)cyclohexane.

[0065] To 0.77 g (5.78 mmol) of 1,1,3,3-tetramethyldisilazane was added 0.67 g (5.78 mmol) of 1,4-cyclohexanediol directly. After 16 h, GC-MS showed product with the following peaks: m / z=232 (M+), 217 (M-15), 207, 189, 175, 149, 133, 117, 102, 87, 75, 59, 45.

[0066] Example 2: Synthesis of 1,2-bis(dimethylsiloxy)cyclohexane.

[0067] To 0.77 g (5.78 mmol) of 1,1,3,3-tetramethyldisilazane was added 0.67 g (5.78 mmol) of 1,2-cyclohexanediol directly. After 16 h, GC-MS showed product with the following peaks: m / z=232 (M+), 217 (M-15), 207, 189, 173, 149, 133, 113, 101, 85, 75, 59, 41.

[0068] Example 3: Deposition of dense organosilica films from 1,4-bis(dimethylsiloxy)cyclohexane.

[0069] Using similar processing conditions as DEMS low-k dielectric film deposition, a variety of dense organo-silica films can be deposited on 200 mm wafers. 1,4-bis(dimethylsiloxy)cyclohexane precursor is delivered to the reaction chamber via direct liquid injection (DLI) at flow rates of 100 mg / min to 2000 mg / min using He carrier gas flow rates of 100 standard cubic centimeters per minute (sccm) to 1000 standard cubic centimeters per minute (sccm), low flow rates of 10 mg / min to 50 mg / min or high flow rates of O2 of 100 mg / min to 1000 mg / min with a pedestal spacing of 350 mils. Films were grown at a range of pressures from 2 Torr to 9 Torr and at a variety of temperatures from 300 °C to 400 °C, as summarized in Table 2.

[0070] [Table 2]

[0071] Following the deposition conditions listed here, films grown from 1,4-bis(dimethylsiloxy)cyclohexane were compared to films derived from DEMS under the same process conditions. Although the films derived from 1,4-bis(dimethylsiloxy)cyclohexane were observed to have similar refractive index values, the k values ​​of the 1,4-bis(dimethylsiloxy)cyclohexane-based organosilica films were significantly lower than the films derived from DEMS, at 2.76 and 3.1, respectively, as shown in Table 3. The results in Table 3 show that the deposition rate for 1,4-bis(dimethylsiloxy)cyclohexane is also much higher than DEMS under similar conditions. FTIR analysis produced a spectrum with peaks consistent with a film composition including carbon, silicon, and oxygen. -1 From about 2960cm -1 The peak at 1250 cm corresponds to the bending and stretching bond vibrations of -CH. The film is mainly composed of SiO features, with a peak at 1250 cm. -1 From 920cm -1 Si-O-Si network band and 1250cm -1 A shoulder peak is observed due to the vibrational mode of the Si-O-Si cage bond.

[0072] [Table 3]

[0073] Example 4: Deposition of SiOC films at O2 flow rates of 100 mg / min and 750 mg / min to lower carbon uptake.

[0074] Furthermore, when the process was repeated using higher O2 flow rates of 100 mg / min and 750 mg / min, the resulting films were found to have lower carbon incorporation. FTIR spectra of films grown at different O2 flow rates while keeping all other process parameters constant indicate that the amount of O2 introduced into the reaction chamber significantly alters the k value, deposition rate, and refractive index as well as the carbon concentration in the film. Adjusting the O2 flow rate can be used to optimize the composition, growth rate, and physical properties of films derived from 1,4-bis(dimethylsiloxy)cyclohexane.

[0075] Table 4: Dense organosilica films using bis(dimethylsiloxy)cyclohexane at higher O2 flow rates. [Table 4]

Claims

1. 1. A method for fabricating a dense organosilica film with improved mechanical properties, the method comprising: providing a substrate into a reaction chamber; introducing into said reaction chamber a gaseous composition comprising at least one alkoxysilane compound having a given structure of Formula I: [Formula 1] where R is a linear or branched C 2 ~C 5 Alkanes, linear or branched C 2 ~C 5 Alkenes, linear or branched C 2 ~C 5 Alkyne, C 4 ~C 10 Cyclic alkanes, C 4 ~C 10 Cyclic alkenes, C 5 ~C 10 arenes; and applying energy to the gaseous composition comprising the at least one alkoxysilane in the reaction chamber to induce reaction of the gaseous composition comprising the at least one alkoxysilane and deposit an organosilica film on the substrate; wherein the organosilica film has a dielectric constant of about 2.40 to about 3.20 and an elastic modulus of about 6 GPa to about 30 GPa.

2. 2. The method of claim 1, wherein the at least one alkoxysilane comprises at least one selected from the group consisting of 2,3-bis(dimethylsiloxy)butane, 1,4-bis(dimethylsiloxy)cyclohexane, 1,2-bis(dimethylsiloxy)cyclohexane, 1,4-bis(dimethylsiloxy)-cis-2-butene, 1,4-bis(dimethylsiloxy)-2-butyne, 1,4-bis(dimethylsiloxy)benzene, 1,4-bis(dimethylsiloxymethyl)cyclohexane, 1,3-bis(dimethylsiloxy)propane, 1,3-bis(dimethylsiloxy)-2-methylpropane, 1,2-bis(dimethylsiloxy)propane, 1,3-bis(dimethylsiloxy)butane, and 1,4-bis(dimethylsilyl)butane.

3. The method of claim 1 , wherein the gaseous composition comprising the alkoxysilane does not contain a curing additive.

4. The method of claim 1 which is a chemical vapor deposition process.

5. The method of claim 1 , which is a plasma enhanced chemical vapor deposition method.

6. 2. The method of claim 1, wherein the gaseous composition comprising the alkoxysilane further comprises at least one oxidizer selected from the group consisting of water vapor, water plasma, ozone, oxygen, oxygen plasma, oxygen / helium plasma, oxygen / argon plasma, nitrogen oxide plasma, carbon dioxide plasma, hydrogen peroxide, organic peroxides, and combinations thereof.

7. The method of claim 1 , wherein the gaseous composition comprising the alkoxysilane does not include an oxidizer.

8. The reaction chamber in the application step is filled with He, Ar, N 2 , Kr, Xe, CO 2 2. The method of claim 1 , further comprising at least one gas selected from the group consisting of CO and H 2 .

9. 10. The method of claim 1, wherein the organosilica film has a refractive index (RI) at 632 nm of about 1.3 to about 1.6 and a carbon content of about 10 atomic % to about 45 atomic % as measured by XPS.

10. The method of claim 1 , wherein the organosilica film is deposited at a rate of about 5 nm / min to about 2000 nm / min.

11. The method of claim 1 , wherein the organosilica film has a relative disilylmethylene density of about 10 to about 30.

12. 1. A composition for vapor deposition of a dielectric film, the composition comprising at least one alkoxysilane compound having a structure of Formula I: [chemical 2] where R is a linear or branched C 2 ~C 5 Alkanes, linear or branched C 2 ~C 5 Alkenes, linear or branched C 2 ~C 5 Alkyne, C 4 ~C 10 Cyclic alkanes, C 4 ~C 10 Cyclic alkenes, C 5 ~C 10 1. A composition comprising: an alkoxysilane, an alkoxysilane derivative of an alkoxysilane that is substantially free of one or more impurities selected from the group consisting of halides, water, nitrogen-containing impurities, oxygen-containing impurities, and metals.

13. 13. The composition of claim 12, wherein the at least one alkoxysilane comprises at least one selected from the group consisting of 2,3-bis(dimethylsiloxy)butane, 1,4-bis(dimethylsiloxy)cyclohexane, 1,2-bis(dimethylsiloxy)cyclohexane, 1,4-bis(dimethylsiloxy)-cis-2-butene, 1,4-bis(dimethylsiloxy)-2-butyne, 1,4-bis(dimethylsiloxy)benzene, 1,4-bis(dimethylsiloxymethyl)cyclohexane, 1,3-bis(dimethylsiloxy)propane, 1,3-bis(dimethylsiloxy)-2-methylpropane, 1,2-bis(dimethylsiloxy)propane, 1,3-bis(dimethylsiloxy)butane, and 1,4-bis(dimethylsilyl)butane.

14. The composition of claim 12 , wherein the halide comprises chloride ions.

15. 15. The composition of claim 14, wherein the chloride ions, if present, are present at a concentration of 50 ppm or less as measured by IC.

16. 16. The composition of claim 15, wherein the chloride ions, if present, are present at a concentration of 5 ppm or less as measured by IC.

17. 13. The composition of claim 12, wherein the alkoxysilane compound is substantially free of nitrogen-containing impurities.

18. 20. The composition of claim 17, wherein the nitrogen-containing species, if present, is present in a concentration of less than or equal to 1000 ppm as measured by GC.

19. The method of claim 6, further comprising adjusting the carbon content in the resulting film by adjusting the flow rate of the oxidizer.

20. 1. A composition comprising at least one alkoxysilane compound having a structure of Formula I: [C3] where R is a linear or branched C 2 ~C 5Alkanes, linear or branched C 2 ~C 5 Alkenes, linear or branched C 2 ~C 5 Alkyne, C 4 ~C 10 Cyclic alkanes, C 4 ~C 10 Cyclic alkenes, and C 5 ~C 10 The composition, wherein the organic moiety is derived from the group consisting of arenes.

Citation Information

Patent Citations

  • Insulation film, forming method thereof and semiconductor device using the insulation film

    JP2000357690A

  • Very low permittivity plasma-enhanced cvd film

    JP2001298023A

  • Method of forming low dielectric constant interlayer dielectric film

    JP2002256434A

  • Method for manufacturing silicon oxide film from organic amino silane precursor

    JP2007318142A

  • Novel silicon precursor for fabricating ultra-low K films with high mechanical properties by plasma-accelerated chemical deposition.

    JP2011530174A