Rubber-asphalt waterproof coating with high viscosity wet skid resistance and preparation method thereof
A high viscosity rubber asphalt waterproofing paint, formulated with styrene-butadiene rubber and additives, enhances adhesion and anti-slip properties on vertical walls and sloped roofs, resolving slipping issues in construction.
Patent Information
- Application Number
- JP2024523277
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-07-21
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2043-05-11
AI Technical Summary
Existing modified asphalt waterproofing coil materials exhibit poor adhesion to vertical walls of basements and sloped roofs, leading to slipping issues during construction.
A rubber asphalt waterproofing paint with high viscosity and wet skid resistance is prepared by combining modified asphalt with styrene-butadiene rubber, inorganic fillers, and specific additives, using a specific mixing process to enhance adhesion and anti-slip properties.
The resulting paint significantly improves adhesion and anti-slip performance, addressing the slipping issues on vertical walls and sloped roofs, as demonstrated by increased adhesive strength, peel strength, and sag resistance.
Smart Images

Figure 2024541864000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to the technical field of waterproof coating, particularly to a rubber-asphalt waterproof coating with high viscosity wet skid resistance and its preparation method. [Background technology]
[0002] Among the waterproof materials frequently used in the construction waterproofing process, modified asphalt waterproof coil material accounts for the highest proportion and is widely used in the above-ground and underground of existing buildings and other special architectural structures. However, the existing modified asphalt waterproof coil material on the market has the problem that the adhesion between the basement vertical wall and the sloped roof during the construction process is poor, causing slippage. Therefore, there is an urgent need to combine the new high-viscosity skid-resistant water-based rubber asphalt waterproof paint with waterproof coil material to improve the adhesive strength and anti-slip ability of the modified asphalt waterproof coil material and the underground vertical wall and sloped roof. Summary of the Invention [Problem to be solved by the invention]
[0003] The present invention provides a rubber-asphalt waterproof coating material with high viscosity wet skid resistance and a preparation method thereof, and solves the problem in related art that the modified asphalt waterproof coil material has poor adhesion to the basement vertical wall or sloped roof during construction, causing slippage. [Means for solving the problem]
[0004] The technical solution of the present invention is as follows:
[0005] The present invention relates to The composition includes 50-70 parts of modified asphalt, 20-30 parts of styrene butadiene rubber latex, 1-2 parts of thickener, 0.1-0.5 parts of defoamer, 1-5 parts of inorganic filler, 0.1-0.5 parts of dispersion medium, and 0.1-0.2 parts of aging resistance agent. The modified asphalt is a styrene butadiene rubber modified asphalt; A rubber-asphalt waterproof coating with high viscosity and skid resistance. to provide.
[0006] As a further technical proposal, in the modified asphalt, the mass ratio of asphalt to styrene-butadiene rubber is 100:(6-8).
[0007] In another technical solution, the styrene-butadiene rubber is a mixture of a first styrene-butadiene rubber and a second styrene-butadiene rubber with a mass ratio of 1:(2-3), the first styrene-butadiene rubber has a weight average molecular weight of 2500-4500, and the second styrene-butadiene rubber has a weight average molecular weight of 150,000-200,000.
[0008] Another technical idea is to mix asphalt and arene oil and heat to 150°C, add a first styrene-butadiene rubber to the mixture, stir for 30 minutes and heat to 170°C, add a second styrene-butadiene rubber to the mixture, heat to 190°C and stir for 1.5 hours, shear the mixture at a speed of 8000 rpm for 1 hour, and then stir the mixture for 30 minutes to obtain modified asphalt.
[0009] In a further technical alternative, the asphalt is No. 70 asphalt or No. 90 asphalt.
[0010] In a further technical solution, the inorganic filler is one or more of talcum powder, wollastonite, calcium carbonate, kaolin.
[0011] In a further technical solution, the thickener is a mixture of cellulose ether and polyacrylamide in a mass ratio of 1-1.5:1.
[0012] In a further technical solution, the dispersion medium is sodium oleate or sodium sulfonate, and the aging resist is antioxidant 4020 or antioxidant RD.
[0013] The present invention relates to Step S1: mixing styrene butadiene rubber latex, inorganic filler, dispersion medium and defoamer for 0.2-0.5 hours to obtain a premixed material; Step S2: mixing the premixed material and the modified asphalt and grinding it for 1-1.5 hours to obtain a mixed material; Step S3 of adding thickener and anti-aging agent to the mixed material and mixing them evenly to obtain a rubber waterproof coating with high viscosity wet skid resistance. The method for preparing the high viscosity wet skid resistant rubber asphalt waterproof coating is characterized in that Also provided.
[0014] The present invention relates to The application of the high viscosity wet skid resistant rubber asphalt waterproof coating to basement upright walls and sloped roofs is also provided. Effect of the Invention
[0015] The operating principle and beneficial effects of the present invention are as follows.
[0016] The present invention uses styrene-butadiene rubber to modify asphalt, and the styrene-butadiene rubber is composed of a mixture of first styrene-butadiene rubber and second styrene-butadiene rubber with a mass ratio of 1:(2-3). The modified asphalt obtained can be further mixed with styrene-butadiene rubber latex, thickener and other auxiliaries to obtain a water-based rubber asphalt waterproof coating. The adhesive performance and anti-slip properties of the water-based rubber asphalt waterproof coating are greatly improved, and a high-viscosity skid-resistant water-based rubber asphalt waterproof coating is obtained. This solves the problem in related technologies that the modified asphalt waterproof coil material has poor adhesion to the basement vertical walls and sloped roofs during construction, causing slippage. [Brief description of the drawings]
[0017] [Figure 1]FIG. 1 is a test chart of the skid resistance after the water-based rubber asphalt waterproof coating in Example 1 of the present invention is adhered to the self-adhesive coil material. [Diagram 2] FIG. 2 is a front view of the water-based rubber asphalt waterproof coating in Example 1 of the present invention adhered to the self-adhesive coil material and subjected to a skid resistance test under a load of 100 kg. [Diagram 3] FIG. 3 is a left view of the water-based rubber asphalt waterproof coating in Example 1 of the present invention adhered to the self-adhesive coil material and subjected to a skid resistance test under a load of 100 kg. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Combining with the embodiments of the present invention, the technical solutions in the embodiments of the present invention are clearly and completely described. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without original work are all within the protection scope of the present invention.
[0019] In the following examples and comparative examples, the first styrene butadiene rubber has a weight average molecular weight of 2500-4500, model number is HTBS, I type, and is purchased from Shandong Zhuo Qilong Chemical Engineering Co., Ltd. The second styrene butadiene rubber has a weight average molecular weight of 176000, model number is ESBR1739E, and is purchased from China Petroleum Lanzhou Petrochemical Co., Ltd. The defoamer is BASF A10. EXAMPLES
[0020] Example 1 The high viscosity wet skid resistance performance rubber asphalt waterproof coating contains 50 parts modified asphalt, 20 parts styrene butadiene rubber latex, 1 part thickener, 0.1 part defoamer, 1 part talcum powder, 0.1 part sodium oleate, and 0.1 part antioxidant 4020.
[0021] Among them, No. 70 asphalt and arene oil are mixed and heated to 150°C, the first styrene butadiene rubber is added to the mixture, stirred for 30 minutes, heated to 170°C, the second styrene butadiene rubber is added to the mixture, heated to 190°C and stirred for 1.5 hours, the mixture is sheared at a speed of 8000 rpm for 1 hour, and then stirred for 30 minutes to obtain modified asphalt. The mass ratio of asphalt, aromatic oil, first styrene butadiene rubber, and second styrene butadiene rubber is 100:15:2:4. The thickener is a mixture of cellulose ether and polyacrylamide in a mass ratio of 1:1.
[0022] The preparation method of the high viscosity wet skid resistant rubber asphalt waterproof coating material includes: Step S1: Styrene butadiene rubber latex, talcum powder, sodium oleate and antifoaming agent are added to a mixing tank, the mixing tank is started to stir, and the obtained mixture is dispersed for 20 minutes, and the rotation speed of the stirrer is set to 400 rpm to obtain a premixed material; Step S2 of mixing the premixed material and the modified asphalt and grinding it for 1 hour to obtain a mixed material; Step S3: add thickener and aging resistance agent 4020 to the mixed material, disperse the mixture for 40 minutes, and set the rotation speed of the stirring to 800 rpm to obtain high viscosity wet skid resistance rubber waterproof paint; Includes. EXAMPLES
[0023] Example 2 The high viscosity wet skid resistance performance rubber asphalt waterproof coating contains 60 parts modified asphalt, 25 parts styrene butadiene rubber latex, 1.5 parts thickener, 0.3 parts defoamer, 3 parts talcum powder, 0.3 parts sodium sulfonate, and 0.15 parts antioxidant RD.
[0024] Among them, No. 70 asphalt and arene oil are mixed and heated to 150°C, the first styrene butadiene rubber is added to the mixture, stirred for 30 minutes, heated to 170°C, the second styrene butadiene rubber is added to the mixture, heated to 190°C and stirred for 1.5 hours, the mixture is sheared at a speed of 8000 rpm for 1 hour, and then stirred for 30 minutes to obtain modified asphalt. The mass ratio of asphalt, aromatic oil, first styrene butadiene rubber, and second styrene butadiene rubber is 100:15:2:4. The thickener is a mixture of cellulose ether and polyacrylamide in a mass ratio of 1:1.
[0025] The preparation method of the high viscosity wet skid resistant rubber asphalt waterproof coating material includes: Step S1: Styrene butadiene rubber latex, talcum powder, sodium sulfonate and antifoaming agent are added to a mixing tank, the mixing tank is started to stir, and the mixture is dispersed for 20 minutes, and the rotation speed of the stirrer is set to 400 rpm to obtain a premixed material; Step S2 of mixing the premixed material and the modified asphalt and grinding it for 1 hour to obtain a mixed material; Step S3: add thickener and antioxidant RD to the mixed material, disperse the mixture for 40 minutes, and set the rotation speed of the stirring to 800 rpm to obtain a rubber waterproof paint with high viscosity wet skid resistance; Includes. EXAMPLES
[0026] Example 3 The high viscosity wet skid resistance performance rubber asphalt waterproof coating contains 70 parts modified asphalt, 30 parts styrene butadiene rubber latex, 2 parts thickener, 0.5 parts defoamer, 5 parts wollastonite, 0.5 parts sodium sulfonate, and 0.2 parts antioxidant RD.
[0027] Among them, No. 90 asphalt and arene oil are mixed and heated to 150°C, the first styrene butadiene rubber is added to the mixture, stirred for 30 minutes, heated to 170°C, the second styrene butadiene rubber is added to the mixture, heated to 190°C and stirred for 1.5 hours, the mixture is sheared at a speed of 8000 rpm for 1 hour, and then stirred for 30 minutes to obtain modified asphalt. The mass ratio of asphalt, aromatic oil, first styrene butadiene rubber, and second styrene butadiene rubber is 100:15:2:4. The thickener is a mixture of cellulose ether and polyacrylamide in a mass ratio of 1:1.
[0028] The preparation method of the high viscosity wet skid resistant rubber asphalt waterproof coating material includes: Step S1: Styrene butadiene rubber latex, wollastonite, sodium sulfonate and defoamer are added into a mixing tank, the mixing tank is started to stir, and the mixture is dispersed for 20 minutes, and the rotation speed of the stirrer is 400 rpm to obtain a premixed material; Step S2 of mixing the premixed material and the modified asphalt and grinding it for 1 hour to obtain a mixed material; Step S3: add thickener and antioxidant RD to the mixed material, disperse the mixture for 40 minutes, and set the rotation speed of the stirring to 800 rpm to obtain a rubber waterproof paint with high viscosity wet skid resistance; Includes. EXAMPLES
[0029] Example 4 The high viscosity wet skid resistance performance rubber asphalt waterproof coating contains 50 parts modified asphalt, 20 parts styrene butadiene rubber latex, 1 part thickener, 0.1 part defoamer, 1 part talcum powder, 0.1 part sodium oleate, and 0.1 part antioxidant 4020.
[0030] Among them, No. 70 asphalt and arene oil are mixed and heated to 150°C, the first styrene butadiene rubber is added to the mixture, stirred for 30 minutes, heated to 170°C, the second styrene butadiene rubber is added to the mixture, heated to 190°C and stirred for 1.5 hours, the mixture is sheared at a speed of 8000 rpm for 1 hour, and then stirred for 30 minutes to obtain modified asphalt. The mass ratio of asphalt, aromatic oil, first styrene butadiene rubber, and second styrene butadiene rubber is 100:15:2:6. The thickener is a mixture of cellulose ether and polyacrylamide in a mass ratio of 1:1.
[0031] The preparation method of the high viscosity wet skid resistant rubber asphalt waterproof coating material is the same as that in Example 1. EXAMPLES
[0032] Example 5 The high viscosity wet skid resistance performance rubber asphalt waterproof coating contains 50 parts modified asphalt, 20 parts styrene butadiene rubber latex, 1 part thickener, 0.1 part defoamer, 1 part talcum powder, 0.1 part sodium oleate, and 0.1 part antioxidant 4020.
[0033] Among them, No. 70 asphalt and arene oil are mixed and heated to 150°C, the first styrene butadiene rubber is added to the mixture, stirred for 30 minutes, heated to 170°C, the second styrene butadiene rubber is added to the mixture, heated to 190°C and stirred for 1.5 hours, the mixture is sheared at a speed of 8000 rpm for 1 hour, and then stirred for 30 minutes to obtain modified asphalt. The mass ratio of asphalt, aromatic oil, first styrene butadiene rubber, and second styrene butadiene rubber is 100:15:3:3. The thickener is a mixture of cellulose ether and polyacrylamide in a mass ratio of 1:1.
[0034] The preparation method of the high viscosity wet skid resistant rubber asphalt waterproof coating material is the same as that in Example 1. EXAMPLES
[0035] Example 6 The high viscosity wet skid resistance performance rubber asphalt waterproof coating contains 50 parts modified asphalt, 20 parts styrene butadiene rubber latex, 1 part thickener, 0.1 part defoamer, 1 part talcum powder, 0.1 part sodium oleate, and 0.1 part antioxidant 4020.
[0036] Among them, No. 70 asphalt and arene oil are mixed and heated to 150°C, the first styrene butadiene rubber is added to the mixture, stirred for 30 minutes, heated to 170°C, the second styrene butadiene rubber is added to the mixture, heated to 190°C and stirred for 1.5 hours, the mixture is sheared at a speed of 8000 rpm for 1 hour, and then stirred for 30 minutes to obtain modified asphalt. The mass ratio of asphalt, aromatic oil, first styrene butadiene rubber, and second styrene butadiene rubber is 100:15:1.2:4.8. The thickener is a mixture of cellulose ether and polyacrylamide in a mass ratio of 1:1.
[0037] The preparation method of the high viscosity wet skid resistant rubber asphalt waterproof coating material is the same as that in Example 1. EXAMPLES
[0038] Example 7 The high viscosity wet skid resistance performance rubber asphalt waterproof coating contains 50 parts modified asphalt, 20 parts styrene butadiene rubber latex, 1 part thickener, 0.1 part defoamer, 1 part talcum powder, 0.1 part sodium oleate, and 0.1 part antioxidant 4020.
[0039] Among them, No. 70 asphalt and arene oil are mixed and heated to 150°C, the first styrene butadiene rubber is added to the mixture, stirred for 30 minutes, heated to 170°C, the second styrene butadiene rubber is added to the mixture, heated to 190°C and stirred for 1.5 hours, the mixture is sheared at a speed of 8000 rpm for 1 hour, and then stirred for 30 minutes to obtain modified asphalt. The mass ratio of asphalt, aromatic oil, first styrene butadiene rubber and second styrene butadiene rubber is 100:15:2:4. The thickener is a mixture of cellulose ether and polyacrylamide with a mass ratio of 1:1.5.
[0040] The preparation method of the high viscosity wet skid resistant rubber asphalt waterproof coating material is the same as that of Example 1.
[0041] Comparison 1 The only difference between this comparative example and Example 1 is as follows: No. 70 asphalt and arene oil are mixed and heated to 150°C, the first styrene-butadiene rubber is added to the resulting mixture, the temperature is further increased to 190°C and stirred for 1.5 hours, the resulting mixture is sheared at a speed of 8000 rpm for 1 hour, and then the resulting mixture is stirred for 30 minutes to obtain a modified asphalt. The mass ratio of asphalt, aromatic oil, and first styrene-butadiene rubber is 100:15:6. Comparative Example 2
[0042] Comparison 2 The only difference between this comparative example and Example 1 is as follows: No. 70 asphalt and arene oil are mixed and heated to 170°C, the resulting mixture is added with secondary styrene-butadiene rubber, and the temperature is further increased to 190°C and stirred for 1.5 hours, the resulting mixture is sheared at a speed of 8000 rpm for 1 hour, and then the resulting mixture is stirred for 30 minutes to obtain a modified asphalt. The mass ratio of asphalt, aromatic oil, and secondary styrene-butadiene rubber is 100:15:6. Comparative Example 3
[0043] Comparison 3 The only difference between this comparative example and Example 1 is as follows: No. 70 asphalt and arene oil are mixed and heated to 170°C, the first styrene-butadiene rubber and the second styrene-butadiene rubber are added to the mixture, the temperature is further increased to 190°C and stirred for 1.5 hours, the mixture is sheared at a speed of 8000 rpm for 1 hour, and then the mixture is stirred for 30 minutes to obtain a modified asphalt. The mass ratio of asphalt, aromatic oil, first styrene-butadiene rubber, and second styrene-butadiene rubber is 100:15:2:4.
[0044] The following performance tests were carried out on the water-based rubber-asphalt waterproof coatings of Examples 1-7 and Comparative Example 1-2.
[0045] 1. Adhesive strength: The adhesive strength of the sample is measured according to the method specified in GB / T 16777-2008 "Test method for architectural waterproof coatings".
[0046] 2. Peel strength: The peel strength of the sample is measured according to the method specified in JC / T1069-2008 "Primer for asphalt-based waterproof coil material".
[0047] 3. Dripping resistance: The dripping resistance of the test sample is measured according to the method specified in GB / T9264-2012 "Assessment of Dripping Resistance of Color-Developing Coatings and Varnishes".
[0048] The test results are shown in the table below.
[0049] Table 1: Performance test results of water-based rubber asphalt waterproofing paint for Examples 1-7 and Comparative Example 1-2 TIFF2024541864000002.tif109123
[0050] From the data in the above table, it can be seen that the adhesive strength, peel strength and sagging resistance of the water-based rubber asphalt waterproof coating of Example 1-7 are significantly improved when compared with Comparative Example 1-2, and this is especially true for the water-based rubber asphalt waterproof coating of Example 1-3 and Example 7. It can be asserted that the present invention can modify asphalt by using ethylene butadiene rubber, while the styrene butadiene rubber is formed as a mixture of primary styrene butadiene rubber and secondary styrene butadiene rubber with a mass ratio of 1:(2-3), which significantly improves the adhesive performance and anti-slip properties of the water-based rubber asphalt waterproof coating, and prepares a high-viscosity skid-resistant water-based rubber asphalt waterproof coating, thereby improving the construction performance of the water-based rubber asphalt waterproof coating for the application of basement vertical walls and sloped roofs.
[0051] Compared with Example 1, the adhesive strength, peel strength and sagging resistance of the water-based rubber asphalt waterproof coating of Comparative Example 3 are all poor. The reason is that the first styrene-butadiene rubber and the second styrene-butadiene rubber are added to the modified asphalt at the same time during the preparation of the water-based rubber asphalt waterproof coating of Comparative Example, which leads to the inability to fully exert the modifying effect of styrene-butadiene rubber on asphalt. It can be asserted that the present invention can fully exert the modifying effect of styrene-butadiene rubber on asphalt by adjusting the preparation method of modified asphalt, thereby improving the adhesiveness and anti-slip performance of the water-based rubber asphalt waterproof coating.
[0052] Examples of construction applications: The water-based rubber asphalt waterproofing paint and the self-adhesive coil material of Example 1 are used in combination. As shown in Figures 1 and 2, the process example shows that when a 1m wide coil material supports an adult, there is no falling off or slipping down, and when a 1m wide coil material supports a balancing weight of 100 kg, there is no slipping within 7 days.
[0053] The water-based rubber asphalt waterproof coating prepared in Example 1 was sent to the National Building Materials Industry Building Cladding and Tubular Products Quality Supervision and Testing Center for commissioned testing, and the testing report is shown in the table below.
[0054] Table 2. Detection report for water-based rubber asphalt waterproofing paint in Example 1 TIFF2024541864000003.tif5598TIFF2024541864000004.tif5398
[0055] Report Number: JC2021MJ0536
[0056] The above are only preferred embodiments of the present invention, and are not intended to limit the present invention. Any modifications, equivalent replacements, improvements, etc. within the spirit and principle of the present invention shall be included within the protection scope of the present invention.
Claims
1. The composition contains 50-70 parts of modified asphalt, 20-30 parts of styrene butadiene rubber latex, 1-2 parts of thickener, 0.1-0.5 parts of defoamer, 1-5 parts of inorganic filler, 0.1-0.5 parts of dispersion medium, and 0.1-0.2 parts of aging resistance agent. The modified asphalt is a styrene-butadiene rubber modified asphalt, and in the modified asphalt, the mass ratio of asphalt to styrene-butadiene rubber is 100:(6-8); The styrene butadiene rubber is a mixture of a first styrene butadiene rubber and a second styrene butadiene rubber in a mass ratio of 1:(2-3), the first styrene butadiene rubber has a weight average molecular weight of 2500-4500 and a model number of HTBS, I type, the second styrene butadiene rubber has a weight average molecular weight of 176000 and a model number of ESBR1739E, Mix asphalt and arene oil and heat to 150°C, add first styrene butadiene rubber to the mixture, stir for 30 minutes and heat to 170°C, add second styrene butadiene rubber to the mixture, heat to 190°C and stir for 1.5 hours, shear the mixture at a speed of 8000 rpm for 1 hour, and then stir the mixture for 30 minutes to obtain modified asphalt. The thickener is a mixture of cellulose ether and polyacrylamide in a mass ratio of 1 to 1.5:1; The present invention relates to a rubber-asphalt waterproof coating material having high viscosity and wet skid resistance.
2. The high viscosity wet skid resistant rubber asphalt waterproof coating as claimed in claim 1, wherein the asphalt is No. 70 asphalt or No. 90 asphalt.
3. The high viscosity wet skid resistant rubber asphalt waterproof coating as claimed in claim 1, wherein said inorganic filler is one or more of talcum powder, wollastonite, calcium carbonate, and kaolin.
4. The high viscosity wet skid resistant rubber asphalt waterproof coating as claimed in claim 1, wherein the dispersion medium is sodium oleate or sodium sulfonate, and the aging resistance agent is antioxidant 4020 or antioxidant RD.
5. Step S1: mixing styrene butadiene rubber latex, inorganic filler, dispersion medium, and defoaming agent for 0.2-0.5 hours to obtain a premixed material; Step S2: mixing the premixed material and the modified asphalt and grinding for 1-1.5 hours to obtain a mixed material; Step S3: adding a thickener and an anti-aging agent to the mixed material and mixing them evenly to obtain a rubber waterproof coating material with high viscosity and wet skid resistance. A method for preparing the high viscosity wet skid resistant rubber asphalt waterproof coating material according to any one of claims 1 to 4.
6. The application of the high viscosity wet skid resistant rubber asphalt waterproof coating according to any one of claims 1 to 4 to basement upright walls and sloped roofs.
Citation Information
Patent Citations
Emulsified SBS modified asphalt and reparation method thereof, waterproof coating and reparation method thereof
CN105315471A
High-performance modified asphalt waterproof coating and preparation method thereof
CN113004794A
Aqueous protective coating composition
JP1983217550A
Aqueous asphalt coating composition
JP2008513580A
Modified asphalt composition, hardened film using the same, and waterproofing method
JP2010174229A