High-strength steel plate with excellent crashworthiness and formability and its manufacturing method

A high-strength steel plate with optimized alloying elements and microstructure addresses the challenge of achieving high yield ratio and ductility, enhancing collision resistance and formability for automotive structural members.

JP2024541988APending Publication Date: 2024-11-13POHANG IRON & STEEL CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2024525373
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-05
Filing Date
2022-11-02
Publication Date
2024-11-13

AI Technical Summary

Technical Problem

Existing high-strength steels face challenges in achieving a high yield ratio (YS/TS) while maintaining ductility and formability, leading to issues such as decreased formability and poor hole expandability, which are critical for automotive structural members requiring complex shapes and improved collision resistance.

Method used

A steel composition with specific alloying elements (C: 0.06 to 0.2%, Si: 0.4 to 1.4%, Mn: 1.8 to 3.0%, Sol.Al: 1.0% or less, Mo: 0.4% or less, Cr: 1.0% or less, Sb: 0.06% or less, B: 0.01% or less, P: 0.1% or less, S: 0.01% or less) and a microstructure of 40 to 80% tempered martensite and bainite phases with 3 to 15% retained austenite, optimized through a manufacturing process involving reheating, hot rolling, cooling, cold rolling, and continuous annealing.

Benefits of technology

The solution results in a high-strength steel plate with a yield ratio of 0.6 to 0.9, elongation rate of 10% or more, and hole expandability of 20% or more, ensuring excellent collision resistance and formability for automotive structural members.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541988000001_ABST
    Figure 2024541988000001_ABST
Patent Text Reader

Abstract

The present invention relates to a high-strength steel plate used for automobile structural members, and more particularly to a high-strength steel plate having excellent crash resistance and formability, and a method for producing the same.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a high-strength steel plate used for automobile structural members, and more particularly to a high-strength steel plate having excellent crash resistance and formability, and a method for producing the same. [Background technology]

[0002] In recent years, environmental and safety regulations in the automobile industry have become increasingly strict, and regulations on carbon dioxide emissions and fuel efficiency have also been gradually strengthened. The Insurance Institute for Highway Safety in the United States has gradually strengthened regulations on crash stability to protect passengers, and since 2013 has required severe crash performance such as 25% small overlap.

[0003] The only solution to these environmental and safety issues is to reduce the weight of automobiles. To achieve weight reduction, it is necessary to increase the strength of steel materials, and high formability is required to apply high-strength steel materials. Furthermore, a high yield ratio (YS / TS) is required to simultaneously improve the collision performance of the vehicle body.

[0004] Generally, high-strength automotive materials can be classified into precipitation hardened steel, bake hardened steel, solid-solution hardened steel, transformation hardened steel, and the like.

[0005] Examples of the transformation strengthened steel include dual phase steel (DP steel), complex phase steel (CP steel), transformation induced plasticity (TRIP steel), etc. These transformation strengthened steels are also called advance high strength steels (AHSS).

[0006] Of these, DP steel is a steel in which hard martensite is finely and homogeneously dispersed within soft ferrite to ensure high strength, while CP steel is a steel containing two or three phases of ferrite, martensite, and bainite, to which precipitation hardening elements such as Ti and Nb are added to improve strength, and TRIP steel is a steel containing finely and homogeneously dispersed retained austenite, which transforms into martensite during room temperature processing to ensure high strength and high ductility.

[0007] Meanwhile, in recent years, there has been a demand for stronger steel sheets for automobiles in order to improve fuel efficiency and durability, and from the standpoint of collision safety and passenger protection, there has been an increasing number of cases in which ultra-high strength steel sheets with a tensile strength of 980 MPa or more are used for the body structure or as reinforcing materials.

[0008] In particular, to improve the crashworthiness of the vehicle body, high-strength steel with excellent yield strength is used for structural members such as members, seat rails, pillars, etc. The higher the yield strength (YS) to tensile strength (TS), i.e., the yield ratio (YR=YS / TS), the more advantageous the crashworthiness of the structural members.

[0009] However, in general, as the strength of steel plate increases, its ductility decreases, which causes problems such as reduced formability, and the development of materials that can compensate for this is currently required. In other words, to simultaneously ensure crash stability and part formability, it is essential to develop materials with high yield strength and excellent ductility.

[0010] In addition, since most of the processed parts have internal or edge shear surfaces, only when the parts have excellent Hall Expansion Ratio (HER) can they be molded without defects such as cracks on the shear surfaces, and they can improve crash performance by absorbing shock during a collision.

[0011] Therefore, if it were possible to improve the low yield ratio and poor hole expandability of DP steel, which is the most widely used of the transformation-strengthened high-strength steels, and to ensure excellent ductility while improving the drawbacks of the low yield ratio and poor hole expandability of DP steel in order to improve the impact properties and formability of high-strength steel, the applications of high-strength steel could be further expanded.

[0012] On the other hand, in order to increase the yield ratio of steel, it is necessary to increase the yield strength relative to the tensile strength, and a representative method for achieving this is to use water cooling during continuous annealing. As an example, a steel sheet can be manufactured in which martensite is formed by soaking in water in the annealing process and then tempering in a tempered martensite phase.

[0013] However, this method has serious drawbacks, such as poor shape quality due to temperature deviations in the width and length directions during water cooling, deterioration of workability such as the occurrence of cracks during molding, and material variation depending on the position.

[0014] As a conventional technique related to the above technique, Patent Document 1 discloses a martensitic steel material in which a volume fraction of martensite is 80 to 97% by performing continuous annealing on a steel material containing 0.18% or more carbon (C), water-cooling to room temperature, and then overaging for 1 to 15 minutes at a temperature of 120 to 300° C. In this way, when ultra-high strength steel is manufactured by the water-cooling followed by tempering method, the yield ratio is very high, but problems occur in that the shape quality of the coil deteriorates due to temperature deviations in the width and length directions, and problems occur such as cracks occurring during forming and reduced workability.

[0015] Patent Document 2 discloses a method for producing a high-tensile steel sheet that is composed of a composite structure mainly composed of martensite and has fine precipitated copper particles with a particle size of 1 to 100 nm dispersed inside the structure to improve workability. However, there is a problem that excessive addition of Cu at 2 to 5% to precipitate fine copper particles may cause red brittleness due to Cu, resulting in an excessive increase in production costs.

[0016] Patent Document 3 discloses a precipitation hardened steel sheet having a ferrite matrix and containing 2 to 10% by area of ​​pearlite, and improves strength through precipitation hardening and grain refinement by adding carbonitride-forming elements such as Nb, Ti, and V. This steel sheet has good hole expandability, but there is a limit to how much tensile strength can be increased, and it has a problem of cracks occurring during press forming due to its high yield strength and low ductility.

[0017] Patent Document 4 discloses a method for producing a cold-rolled steel sheet that utilizes tempered martensite to simultaneously ensure high strength and high ductility and has excellent sheet shape after continuous annealing. However, the carbon content is high at 0.2% or more, which results in poor weldability, and the steel sheet contains a large amount of Si, which may cause dent defects in the furnace. [Prior art documents] [Patent documents]

[0018] [Patent Document 1] JP 1992-289120 A [Patent Document 2] JP 2005-264176 A [Patent Document 3] Korean Patent Publication No. 2015-0073844 [Patent Document 4] JP 2010-090432 A Summary of the Invention [Problem to be solved by the invention]

[0019] One aspect of the present invention is to provide a steel sheet suitable for use in automobile structural components and the like, which is excellent not only in strength but also in ductility, and has improved crash resistance and formability, and a method for producing the same.

[0020] The object of the present invention is not limited to the above. The object of the present invention can be understood from the entire contents of this specification, and a person having ordinary skill in the art to which the present invention pertains will have no difficulty in understanding further object of the present invention. [Means for solving the problem]

[0021] One aspect of the present invention contains, by weight, 0.06 to 0.2% carbon (C), 0.4 to 1.4% silicon (Si), 1.8 to 3.0% manganese (Mn), 1.0% or less acid-soluble aluminum (Sol.Al), 0.4% or less molybdenum (Mo), 1.0% or less chromium (Cr), 0.06% or less antimony (Sb), 0.01% or less boron (B), 0.1% or less phosphorus (P), 0.01% or less sulfur (S), with the balance being Fe and other unavoidable impurities, wherein the C, Si, and Al satisfy the following relational formula 1: The microstructure contains tempered martensite and bainite phases with a total area fraction of 40 to 80%, retained austenite phase of 3 to 15%, and the remaining ferrite and fresh martensite phases. The retained austenite phase is the total retained austenite fraction (A T ), the retained austenite (A TM+B ) share (A TM+B / A T The present invention provides a high-strength steel plate having excellent crash resistance and formability, characterized in that the ratio of Cr-Si alloy to Cr-Si alloy is 90% or more.

[0022] [Equation 1] (8×C)+(1.1×Si)+(0.8×Al)≧1.7 (Here, each element means its weight content.)

[0023] Another aspect of the present invention includes the steps of heating a steel slab satisfying the above-mentioned alloy composition and Relational Formula 1 in a temperature range of 1050 to 1250°C, finish hot rolling the reheated steel slab in a temperature range of Ar3 to Ar3+50°C at the outlet side of the finish hot rolling to produce a hot rolled steel sheet, coiling the hot rolled steel sheet in a temperature range of 400 to 700°C, cooling the hot rolled steel sheet to room temperature at a cooling rate of 0.1°C / s after the coiling, and cooling the hot rolled steel sheet to room temperature after the cooling. The method includes the steps of cold rolling a hot-rolled steel sheet at a total rolling reduction of 30 to 80% to produce a cold-rolled steel sheet, subjecting the cold-rolled steel sheet to continuous annealing, subjecting the continuously annealed cold-rolled steel sheet to a primary cooling at a cooling rate of 10°C / s or less to 450 to 700°C, and after the primary cooling, subjecting the cold-rolled steel sheet to a secondary cooling at a cooling rate of 3°C / s or more to 250 to 500°C, and reheating the secondary cooled cold-rolled steel sheet to a temperature of 490°C or less and holding the temperature for 30 seconds or more, The cold rolling is performed at a cumulative reduction rate of 20% or more in the first three stands, and thus provides a method for producing a high-strength steel sheet having excellent crash resistance and formability. Effect of the Invention

[0024] According to the present invention, it is possible to provide a steel sheet having high strength and excellent ductility. In particular, the steel sheet of the present invention is characterized by having a higher yield ratio, excellent hole expandability, excellent crash resistance and excellent formability compared to existing DP steels.

[0025] The steel sheet of the present invention has an advantage that it can be suitably applied to materials for automobile structural members and the like that require processing into complex shapes. [Brief description of the drawings]

[0026] [Figure 1] 1 is a graph showing changes in mechanical properties (relationship 2) according to relationship 1 according to an embodiment of the present invention. [Diagram 2] 1 is a photograph showing a microstructure measurement of an inventive steel according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] The inventors of the present invention have conducted intensive research to provide a high-strength steel plate that has improved crash resistance and formability by increasing the yield ratio (YR) and hole expandability compared to existing DP steels while still satisfying the high ductility characteristic of existing DP steels.

[0028] As a result, the inventors confirmed that by optimizing the alloy composition system and manufacturing conditions of the steel, it is possible to obtain a structure that is advantageous for ensuring the target physical properties, and that this makes it possible to provide steel sheet suitable for automotive structural components that require processing into complex shapes, and thus completed the present invention.

[0029] The present invention will be described in detail below.

[0030] A high-strength steel plate with excellent crash resistance and formability according to one embodiment of the present invention can contain, by weight, carbon (C): 0.06 to 0.2%, silicon (Si): 0.4 to 1.4%, manganese (Mn): 1.8 to 3.0%, acid-soluble aluminum (Sol.Al): 1.0% or less, molybdenum (Mo): 0.4% or less, chromium (Cr): 1.0% or less, antimony (Sb): 0.06% or less, boron (B): 0.01% or less, phosphorus (P): 0.1% or less, and sulfur (S): 0.01% or less.

[0031] The reasons for restricting the alloy composition of the steel plate provided in the present invention as described above will be described in detail below.

[0032] On the other hand, unless otherwise specified in the present invention, the content of each element is based on weight, and the proportion of the structure is based on area.

[0033] Carbon (C): 0.06~0.2% Carbon (C) is a very important element that is added to strengthen the transformed structure. C increases the strength of steel and promotes the formation of martensite in dual-phase steel. As the C content increases, the amount of martensite increases.

[0034] If the C content exceeds 0.2%, the strength increases due to the formation of martensite, but the strength difference with ferrite, which has a low carbon concentration, becomes large. Such a strength difference causes problems in that fracture is likely to occur at the interface between phases during plastic deformation, resulting in reduced ductility and work hardening rate. In addition, poor weldability causes welding defects during part processing, and LME (Liquid Metal Embrittlement) cracking occurs during welding, hindering part performance. On the other hand, if the C content is less than 0.06%, it becomes difficult to ensure the target level of strength, and it becomes difficult to ensure a certain fraction of the retained austenite phase required for ductility.

[0035] Therefore, in the present invention, the C content can be contained in a range of 0.06 to 0.20%, and more advantageously, the C content can be contained in an amount of 0.08% or more and 0.18% or less.

[0036] Silicon (Si): 0.4-1.4% Silicon (Si) is a ferrite stabilizing element that promotes the transformation of ferrite and promotes the concentration of carbon (C) in untransformed austenite, thereby contributing to the formation of martensite. In addition, the above-mentioned Si has excellent solid solution strengthening ability, and is effective in increasing the strength of ferrite and reducing the hardness difference between phases. When held in the bainite region, it effectively suppresses the precipitation of carbides in bainite, thereby promoting the concentration of C in untransformed austenite, and delays the transformation of martensite during low-temperature quenching, thereby forming retained austenite necessary for ductility, and is therefore a useful element for improving the ductility of steel sheets. In other words, the above-mentioned Si is a useful element that can ensure strength without reducing the ductility of steel sheets.

[0037] If the Si content exceeds 1.4%, it will cause surface scale defects, adversely affecting the quality of the plating surface, impede chemical conversion treatment, and deteriorate weldability, resulting in welding defects during part processing. In particular, LME cracking will occur during welding, reducing part performance. On the other hand, if the Si content is less than 0.4%, it will be difficult to secure a certain fraction of the retained austenite phase required for ductility, and the solution hardening ability will be poor, reducing the strength of ferrite, limiting the reduction of the hardness difference between phases.

[0038] Therefore, in the present invention, the Si content can be 0.4 to 1.4%, and more advantageously, the Si content can be 0.5% or more and 1.2% or less.

[0039] Manganese (Mn): 1.8-3.0% Manganese (Mn) is an effective element for strengthening steel, as it refines grains without reducing ductility, completely precipitates sulfur (S) in steel as MnS, and prevents hot embrittlement due to the formation of FeS. Mn also makes it easier to form martensite in dual-phase steels by lowering the critical cooling rate at which the martensite phase is obtained.

[0040] If the Mn content is less than 1.8%, it is difficult to ensure the strength targeted in the present invention. On the other hand, if the Mn content exceeds 3.0%, problems such as weldability and hot rolling are likely to occur, and martensite is excessively formed, making the material unstable. In addition, manganese oxide bands (Mn-Bands) are formed in the structure, increasing the risk of defects such as processing cracks and plate breakage. In addition, there is a problem that Mn oxide dissolves on the surface during the annealing process, significantly impairing the surface quality.

[0041] Therefore, in the present invention, the Mn content can be 1.8 to 3.0%, and more advantageously, the Mn content can be 2.0% or more and 2.9% or less.

[0042] Acid-soluble aluminum (Sol.Al): 1.0% or less Acid-soluble aluminum (Sol.Al) is an element added to refine the grain size of steel and to deoxidize it, and is a ferrite stabilizing element like Si. The above-mentioned Al is an element that is useful for distributing carbon in ferrite to austenite to improve the hardening ability of martensite. In addition, during annealing, when held in the bainite region, it effectively suppresses the precipitation of carbides in bainite, promotes the concentration of C in untransformed austenite, delays martensite transformation during low-temperature quenching, and generates a retained austenite phase to improve the ductility of the steel sheet.

[0043] If the Al content exceeds 1.0%, excessive inclusions are formed during continuous casting of steel, which not only increases the possibility of surface defects on the surface of the steel sheet, but also increases the manufacturing cost. Furthermore, the weldability is poor, which may cause welding defects during part processing.

[0044] Therefore, the Al content may be 1.0% or less, excluding 0%, and more preferably 0.01% or more.

[0045] Molybdenum (Mo): 0.4% or less Molybdenum (Mo) is an element that delays the transformation of austenite to pearlite, refines ferrite, and improves strength. Mo has the advantage of improving the hardening ability of steel and forming fine martensite at grain boundaries, making it possible to control the yield ratio. However, Mo is an expensive element, and the higher its content, the higher the manufacturing cost becomes, which is economically disadvantageous.

[0046] To fully obtain the above-mentioned effects, the above-mentioned Mo can be added up to 0.4%. If the above-mentioned Mo content exceeds 0.4%, there is a problem that the alloy cost increases sharply, resulting in a decrease in economic efficiency, and the effects of grain refinement and solid solution strengthening are excessively produced, resulting in a decrease in the ductility of the steel.

[0047] Therefore, in the present invention, Mo can be contained at 0.4% or less. In the present invention, the intended microstructure, physical properties, etc. can be secured without adding Mo, so the content may be 0%. However, when Mo is added, it is more advantageous to include Mo at 0.01% or more.

[0048] Chromium (Cr): 1.0% or less Chromium (Cr) is an element added to improve the hardenability of steel and ensure high strength, and plays an important role in the formation of martensite. It also minimizes the loss of elongation relative to the increase in strength, which is advantageous for the production of dual-phase steels with high ductility.

[0049] If the Cr content exceeds 1.0%, not only the above-mentioned effects become saturated, but also there are problems that the hot-rolling strength increases excessively and the cold-rolling property deteriorates, and there are problems that the size of martensite after annealing becomes coarse due to the excessive formation and coarsening of Cr-based carbides, resulting in a decrease in elongation.

[0050] Therefore, in the present invention, the Cr content can be 1.0% or less. In the present invention, the intended microstructure and physical properties can be secured without adding the Cr content, so the Cr content may be 0%. However, when the Cr content is added, it is more advantageous to add the Cr content at 0.1% or more.

[0051] Antimony (Sb): 0.06% or less Antimony (Sb) is distributed in the grain boundaries and retards the diffusion of oxidizing elements such as Mn, Si, and Al through the grain boundaries, thereby suppressing the surface segregation of oxides. It is also highly effective in suppressing the coarsening of surface segregated oxides due to temperature rise and changes in the hot rolling process. If the Sb content exceeds 0.06%, not only will the above-mentioned effects saturate, but there will also be problems such as an increase in manufacturing costs and deterioration of workability.

[0052] Therefore, the Sb content can be 0.06% or less. In the present invention, the intended microstructure and physical properties can be secured without adding the Sb, so the content may be 0%. However, when Sb is added, it is more advantageous to add 0.01% or more.

[0053] Boron (B): 0.01% or less Boron (B) is an element that delays the transformation of austenite to pearlite during the cooling process during annealing, and is a hardening element that suppresses the formation of ferrite and promotes the formation of martensite. If the content of B exceeds 0.01%, there is a problem that B is excessively concentrated on the steel surface, deteriorating the plating adhesion, etc.

[0054] Therefore, the above B can be contained at 0.01% or less. In the present invention, since the intended microstructure, physical properties, etc. can be secured without adding the above B, the content may be 0%. However, when adding the above B, it is more advantageous to include the above B at 0.0005% or more.

[0055] Phosphorus (P): 0.1% or less Phosphorus (P) is a substitutional element with a large solid solution strengthening effect, and is the most advantageous element for improving in-plane anisotropy and ensuring strength without significantly impairing formability. However, if the P content is excessive, there is a problem that the possibility of brittle fracture occurring increases significantly, which may cause plate breakage of the slab during hot rolling and impair the plating surface properties.

[0056] Therefore, the P content may be 0.1% or less, and 0% may be excluded in consideration of the level of P that is inevitably added during the steel manufacturing process.

[0057] Sulfur (S): 0.01% or less Sulfur (S) is an impurity that is inevitably added to steel and is an element that impairs ductility and weldability, so it is advantageous to control its content as low as possible. In particular, since there is a high possibility of causing red shortness, it is preferable to control its content to 0.01% or less. However, 0% can be excluded in consideration of the level that is inevitably added during the steel manufacturing process.

[0058] In addition to the above-mentioned alloy composition, the steel sheet of the present invention may further contain one or more of Ti and Nb for the purpose of further improving the mechanical properties of the steel sheet.

[0059] Titanium (Ti): 0.05% or less and Niobium (Nb): 0.05% or less Titanium (Ti) and niobium (Nb) are effective elements in increasing the strength of steel and refining grains by forming nano-precipitates. When these elements are added, they combine with carbon to form very fine nano-precipitates, which strengthen the matrix structure and reduce the hardness difference between phases.

[0060] When Ti and Nb are added, if the content exceeds 0.05%, there are problems in that the manufacturing cost increases and the ductility is significantly reduced due to the excessive formation of precipitates.

[0061] Therefore, when one or more of Ti and Nb are added, each can be contained in an amount of 0.05% or less.

[0062] The remaining component of the present invention is iron (Fe). However, in a normal manufacturing process, there is a possibility that unintended impurities are inevitably mixed in from the raw materials or the surrounding environment, and this cannot be excluded. Since these impurities are known to anyone skilled in the normal manufacturing process, the contents of all of them will not be mentioned in this specification.

[0063] In the steel sheet of the present invention having the above-mentioned alloy composition, it is preferable that the relationship between the contents of C, Si and Al satisfies the following Relational Formula 1.

[0064] [Equation 1] (8×C)+(1.1×Si)+(0.8×Al)≧1.7 (Here, each element means its weight content.)

[0065] Silicon and aluminum in steel are ferrite stabilizing elements that promote ferrite transformation and contribute to the formation of retained austenite and martensite by promoting the concentration of carbon in untransformed austenite. Carbon also contributes to the formation and fraction adjustment of martensite by promoting the concentration of carbon in untransformed austenite.

[0066] Specifically, when the value of the above-mentioned relational expression 1 is controlled to be 1.7 or more, the fraction of retained austenite that can contribute to ductility can be secured, and thus the ductility and formability of the steel sheet can be improved. On the other hand, when the above-mentioned relational expression 1 is not satisfied, the fraction of retained austenite is insufficient, and the distribution of the generated retained austenite is not uniform, making it difficult to secure ductility and formability.

[0067] As will be described in detail later, the present invention, in addition to the above-mentioned alloy composition system, optimizes the manufacturing process of the steel sheet to finely distribute the generated retained austenite around the hard phase, thereby alleviating local stress concentration, thereby improving ductility and ensuring excellent formability.

[0068] The steel sheet of the present invention may contain, as its microstructure, a tempered martensite and a bainite phase in total area fraction of 40 to 80%, a retained austenite phase in 3 to 15%, and the remainder being ferrite and fresh martensite phase.

[0069] In the present invention, the tempered martensite and bainite structures are useful for the formation of retained austenite in addition to the effect of contributing to strength. Specifically, when Si and Al are added to steel, the precipitation of carbides during bainite transformation is delayed, and carbon (C) is accumulated in the untransformed austenite around the bainite, so that the martensite transformation temperature drops below room temperature. At this time, the retained austenite can be secured at room temperature. In addition, when the martensite is tempered, the carbon (C) introduced into the martensite moves to and accumulates in the surrounding untransformed austenite, so that the martensite transformation temperature drops below room temperature, and the retained austenite can also be secured at room temperature.

[0070] As a result, the steel sheet of the present invention can contain 3 to 15% of the retained austenite phase. Ensuring that the retained austenite phase is 3% or more is advantageous in ensuring the ductility of the steel sheet by causing transformation-induced plasticity during forming. However, if the fraction is excessive, the plated steel sheet tends to become brittle to liquid metal embrittlement (LME) during spot welding for assembling the plated steel sheet into automobile parts, etc. Therefore, it is preferable that the retained austenite phase is contained in an amount of 15% or less.

[0071] On the other hand, the above-mentioned retained austenite phase is the total retained austenite fraction (A T ), the retained austenite (A TM+B ) share (A TM+B / A T ) is characterized by being 90% or more.

[0072] Here, "adjacent to tempered martensite and bainite" refers to the periphery of these phases, more specifically, the interface between these phases. As an example, it means that the retained austenite phase is mainly distributed around the grain boundary between the tempered martensite and bainite phase, as shown in Figure 2.

[0073] By distributing the retained austenite phase finely and uniformly around the tempered martensite and bainite as described above, it is possible to improve ductility by alleviating local stress concentration, and as a result, it is possible to ensure excellent formability without the occurrence of cracks during part forming.

[0074] If the total fraction of the tempered martensite and bainite is less than 40%, the retained austenite cannot be uniformly distributed around the tempered martensite and bainite, and the amount of the retained austenite is reduced, making it difficult to improve formability.On the other hand, if the fraction exceeds 80%, not only does the fraction of ferrite that contributes to ductility decrease significantly, but the fraction of the retained austenite also decreases, making it difficult to improve ductility and formability.

[0075] More advantageously, the tempered martensite phase may be contained in an amount of 25 to 65% of the total fraction.

[0076] In the present invention, in addition to the above-mentioned tempered martensite, bainite and retained austenite phases, ferrite and fresh martensite phases may be included. In this case, the ferrite phase may be included at 40% or less, and the fresh martensite phase may be included at 20% or less. Here, the ferrite phase and fresh martensite phase are excluded from 0%.

[0077] If the fraction of the ferrite phase exceeds 40%, not only is it impossible to secure the target level of strength, but it is also difficult to improve the yield ratio, and if the fraction of the fresh martensite phase exceeds 20%, the fraction of the retained austenite phase decreases, resulting in a problem of reduced ductility, making it impossible to secure formability.

[0078] The steel sheet of the present invention having the above-mentioned alloy composition and fine structure not only has a high strength of tensile strength of 980 MPa or more, but also has the effects of a yield ratio of 0.6 to 0.9, an elongation of 10% or more, and a hole expandability of 20% or more. If the yield ratio is less than 0.6, the hole expandability is poor, while if it exceeds 0.9, the ductility is reduced.

[0079] Furthermore, the steel sheet of the present invention can provide a steel sheet having both a high yield ratio and high ductility, since the relationship between the yield ratio, elongation and tensile strength satisfies the following Relational Formula 2.

[0080] The high yield ratio of the steel plate gives the material excellent crash resistance and contributes to improved stability during a vehicle collision, and the high ductility prevents processing defects such as cracks and wrinkles that occur during press processing of parts, ensuring excellent formability.

[0081] In the present invention, when the value of the following relational expression 2 is 9 or more, impact resistance and formability can be ensured simultaneously, whereas when the value is less than 9, impact resistance and formability cannot be ensured simultaneously.

[0082] [Equation 2] (YR×El×1000) / TS≧9 (Here, units of each physical property are excluded.)

[0083] The steel sheet of the present invention having the above mechanical properties can prevent processing defects such as cracks and wrinkles during processing into parts, and can be used in a variety of applications as structural members for automobiles having complex shapes. Furthermore, the steel sheet of the present invention can contribute to improving the safety of structural parts and vehicles by improving crash resistance and delaying crack generation during a collision.

[0084] On the other hand, the steel sheet of the present invention may be a cold-rolled steel sheet, a hot-dip galvanized steel sheet including a zinc-based plating layer on at least one surface of the above-mentioned cold-rolled steel sheet, or an alloyed hot-dip galvanized steel sheet obtained by alloying the above-mentioned hot-dip galvanized steel sheet.

[0085] Although there is no particular limitation, the zinc-based plating layer may be a zinc plating layer containing mainly zinc, or a zinc alloy plating layer containing aluminum and / or magnesium in addition to zinc.

[0086] Hereinafter, a method for producing a high-strength steel plate excellent in crash resistance and formability provided by the present invention, which is another embodiment of the present invention, will be described in detail.

[0087] In short, the present invention can produce a target steel sheet through the steps of [steel slab reheating-hot rolling-coil-cooling-cold rolling-continuous annealing-cooling-reheating and holding], and then further steps such as [hot-dip galvanizing-alloying heat treatment] can be carried out.

[0088] The conditions for each stage are explained in detail below.

[0089] [Steel slab heating] First, a steel slab that satisfies all of the above-mentioned alloy composition systems is prepared, and then heated. This process is performed to smoothly carry out the subsequent hot rolling process and to sufficiently obtain the desired physical properties of the steel sheet.

[0090] The heating step can be carried out at a temperature range of 1050 to 1250°C. If the heating temperature is less than 1050°C, there is a problem that friction between the steel sheet and the rolling mill increases, and the load on the roller during hot rolling increases rapidly. On the other hand, if the temperature exceeds 1250°C, not only does the energy cost required for temperature increase increase, but the amount of surface scale increases, which may lead to material loss.

[0091] Therefore, the heating step can be carried out at a temperature in the range of 1050 to 1250°C.

[0092] [Hot rolling] The steel slab heated as described above can be finish hot-rolled at a temperature equal to or higher than the Ar3 transformation point to produce a hot-rolled steel sheet. In this case, the outlet side temperature preferably satisfies Ar3 to Ar3+50°C.

[0093] If the exit temperature during the above-mentioned finish hot rolling is less than Ar3, rolling in the two-phase region of ferrite and austenite may occur, which may lead to non-uniformity in the material. On the other hand, if the temperature exceeds Ar3+50°C, the formation of abnormally coarse grains due to high-temperature rolling may lead to non-uniformity in the material, which may cause a problem of coil distortion during the subsequent cooling.

[0094] More specifically, the finish hot rolling can be carried out in the temperature range of 800 to 1000°C.

[0095] [Winding] The hot-rolled steel sheet produced as described above can be coiled at a temperature in the range of 400 to 700°C.

[0096] If the coiling temperature is less than 400°C, the strength of the hot-rolled steel sheet becomes excessively high, which may induce rolling load during subsequent cold rolling. In addition, it takes excessive cost and time to cool the hot-rolled steel sheet to the coiling temperature, which causes an increase in process cost. On the other hand, if the temperature exceeds 700°C, there is a high possibility that scale will be excessively generated on the surface of the hot-rolled steel sheet, which may induce surface defects and cause weakening of galvanizability.

[0097] Therefore, the winding step can be carried out at a temperature in the range of 400 to 700°C.

[0098] [cooling] The coiled hot-rolled steel sheet is cooled to room temperature at an average cooling rate of preferably 0.1° C. / s or less (excluding 0° C. / s), more preferably 0.05° C. / s or less, and even more preferably 0.015° C. / s or less. Here, cooling means the average cooling rate.

[0099] In this way, by cooling the coiled hot-rolled steel sheet at a constant speed, it is possible to obtain a hot-rolled steel sheet in which carbides that become austenite nucleation sites are finely dispersed. That is, fine carbides are uniformly dispersed in the steel during the hot rolling process, and during the subsequent annealing, the carbides are dissolved and austenite phase is finely dispersed and formed in the steel. As a result, a uniformly dispersed fine martensite phase is obtained after the annealing is completed.

[0100] [Cold rolling] The hot-rolled steel sheet coiled as described above can be cold-rolled to produce a cold-rolled steel sheet, at a cold reduction (total reduction) of 30 to 80%.

[0101] In particular, the present invention controls the cumulative reduction rate of the initial stands, preferably the first to third stands, during the cold rolling to 20% or more, thereby increasing the stored energy inside the steel, which acts as a driving force to promote the recrystallization of ferrite in the subsequent annealing process, thereby providing the effect of reducing the fraction of unrecrystallized ferrite in the steel.

[0102] When unrecrystallized ferrite is present in steel, deformation and stress are concentrated locally, resulting in poor ductility of the steel, whereas recrystallized ferrite contributes to improving ductility by alleviating the concentration of deformation and stress.

[0103] During the cold rolling, if the cumulative reduction rate of the first to third stands is less than 20% or the cold reduction rate (total reduction rate) up to the final stand is less than 30%, not only is it difficult to secure the target thickness, but it is also difficult to correct the shape of the steel sheet. In addition, the proportion of unrecrystallized ferrite increases, resulting in a decrease in ductility. On the other hand, if the cold reduction rate up to the final stand exceeds 80%, the strength increases, resulting in a load on the rolls during cold rolling, and there is a high possibility of cracks occurring at the edges of the steel sheet.

[0104] In the present invention, the cold rolling can be performed using a rolling mill configured with 5 or 6 stands, but it is clear that the present invention is not limited thereto.

[0105] [Continuous annealing] It is preferable that the cold-rolled steel sheet produced as described above is subjected to a continuous annealing treatment. As an example, the continuous annealing treatment can be performed in a continuous alloying hot-dip galvanizing furnace.

[0106] The continuous annealing step is a process for recrystallizing and simultaneously forming ferrite and austenite phases and decomposing carbon.

[0107] The continuous annealing treatment is preferably carried out in the temperature range of Ac1+30°C to Ac3+30°C, and more advantageously in the temperature range of 800 to 870°C.

[0108] If the temperature during the continuous annealing is less than Ac1+30°C, sufficient recrystallization does not occur, and furthermore, it becomes difficult to form sufficient austenite, and the target level of martensite phase and bainite phase fraction after annealing cannot be ensured. On the other hand, if the temperature exceeds Ac3+30°C, the size of the austenite crystal grains becomes coarse, and it becomes impossible to uniformly form fine retained austenite phase around the hard phase. In addition, productivity decreases, and the high-temperature annealing causes the formation of surface concentrates due to elements such as Si, Mn, and B that reduce the wettability of hot-dip galvanizing, making it impossible to ensure the quality of the plated surface.

[0109] [Stepwise cooling] It is preferable to cool the cold-rolled steel sheet subjected to the above-mentioned continuous annealing treatment stepwise.

[0110] Specifically, the cooling is preferably performed by first cooling to 450 to 700°C at an average cooling rate of 10°C / s or less (excluding 0°C / s) (this cooling is called primary cooling), and then cooling to 250 to 500°C at an average cooling rate of 3°C / s or more (this cooling is called secondary cooling).

[0111] Primary cooling In the present invention, when tempered martensite and bainite phases are formed as the final structure with a total area fraction of 40 to 80%, the fractions of martensite and bainite generated during this process can be controlled by controlling the end temperature in the subsequent secondary cooling process.

[0112] Specifically, when the subsequent secondary cooling is terminated at or below Ms (martensitic transformation start temperature), a relatively large amount of martensite phase can be formed, and in order to achieve this, it is advantageous to control the end temperature of the primary cooling as low as possible.Also, when the subsequent secondary cooling is terminated in the bainite temperature region, a relatively large amount of bainite phase can be formed advantageously, and in order to achieve this, it is advantageous to control the end temperature of the primary cooling to be higher.

[0113] Preferably, when the subsequent secondary cooling is completed below Ms, the primary cooling can be performed to a temperature range of 450 to 600°C, and when the subsequent secondary cooling is completed in the bainite temperature region, the primary cooling is preferably performed to a temperature range of 550 to 700°C.

[0114] If the end temperature of the primary cooling is less than 450°C, a large load is placed on the equipment for cooling the atmospheric gas in the annealing furnace, and the cooling rate becomes too fast to ensure a sufficient amount of ferrite phase formed during cooling.On the other hand, if the end temperature exceeds 700°C, there is a disadvantage that an excessively high cooling rate is required during the subsequent cooling (secondary cooling).

[0115] Furthermore, if the average cooling rate during the primary cooling exceeds 10°C / s, carbon diffusion will not be sufficient. On the other hand, in consideration of productivity, the primary cooling can be performed at an average cooling rate of 1°C / s or more.

[0116] Secondary cooling After completing the primary cooling under the above-mentioned conditions, it is preferable to carry out secondary cooling. In this case, the cooling end temperature and the cooling rate can be controlled to induce the formation of a targeted microstructure.

[0117] If the secondary cooling is performed below Ms, quenched martensite is formed, and the lower the temperature, the higher the proportion of quenched martensite, which can lead to improved strength of the steel sheet. In addition, the martensite is tempered during the subsequent heat treatment (the reheating process of the present invention) to form tempered martensite, and the carbon supersaturated in the martensite is distributed to the surrounding untransformed austenite to increase the stability of the retained austenite and improve ductility.

[0118] If the secondary cooling is performed at a temperature above Ms, the bainite fraction can be increased. During this time, the effects of Si and Al delay the precipitation of carbides during the bainite transformation process, and carbon is distributed from the bainite to the surrounding untransformed austenite, increasing the stability of the retained austenite and improving ductility.

[0119] If the end temperature of the secondary cooling is less than 250°C, the proportion of quenched martensite increases excessively, and the proportion of the retained austenite phase decreases, resulting in deterioration of the shape of the steel sheet. On the other hand, if the temperature exceeds 500°C, bainite is not sufficiently formed, the proportion of the retained austenite phase decreases, and the proportion of the fresh martensite phase increases significantly in the subsequent process, resulting in excessive strength. More preferably, the secondary cooling can be ended at 400°C or less.

[0120] In addition, if the average cooling rate during the secondary cooling is less than 3°C / s, the pearlite phase is formed, and the bainite phase may not be formed to the target level. On the other hand, the upper limit of the average cooling rate is not particularly limited, and can be appropriately selected by an ordinary engineer in consideration of the specifications of the cooling equipment. As an example, the cooling rate can be 100°C / s or less.

[0121] Furthermore, the secondary cooling can be performed using a hydrogen cooling facility that uses hydrogen gas (H2 gas). In this way, by performing cooling using the hydrogen cooling facility, it is possible to obtain an effect of suppressing surface oxidation that may occur during the secondary cooling. In this case, the hydrogen cooling facility can be controlled with 60 to 70% hydrogen (H2) and the balance nitrogen (N2).

[0122] On the other hand, as described above, when cooling is performed stepwise, the cooling rate in the secondary cooling can be made faster than the cooling rate in the primary cooling.

[0123] retention After completing the secondary cooling as described above, a step of maintaining the cooled temperature range for 30 seconds or more may be further carried out.

[0124] The above-mentioned holding step can provide the effect of tempering the quenched martensite or increasing the amount of bainite transformation. If the holding time is less than 30 seconds, the above-mentioned effect is difficult to achieve.

[0125] [Reheating and holding] The microstructure intended in the present invention can be formed by the process of reheating and holding the cold-rolled steel sheet after the stepwise cooling as described above. Specifically, it is preferable to reheat the cold-rolled steel sheet after the second cooling to a temperature of 490°C or less and hold the temperature for 30 seconds or more.

[0126] Reheating to and holding at the aforementioned temperatures allows the hardened martensite produced during the previous cooling process to transform into tempered martensite, with a bainite transformation also occurring.

[0127] During the tempering process, the carbon that was supersaturated in the martensite is redistributed to the surrounding untransformed austenite. In addition, if the secondary cooling is completed above Ms, the bainite fraction increases significantly during the reheating and holding process, but the carbon expelled from the bainite during this process is redistributed to the untransformed austenite, improving the stability of the retained austenite and increasing ductility.

[0128] Furthermore, during the reheating and holding process, dislocations are fixed in the tempered martensite and bainite, increasing the yield strength, and as a result, a steel sheet having a yield ratio of 0.6 to 0.9 can be obtained.

[0129] However, if the temperature during the reheating is excessively high, the carbides in the tempered martensite and bainite will become coarse, reducing the strength, and the effect of carbon redistribution to untransformed austenite due to the formation of coarse carbides will decrease, reducing the fraction of retained austenite, and ultimately making it difficult to expect an improvement in ductility.

[0130] Therefore, the reheat temperature can be limited to less than or equal to 490°C, and more advantageously can be greater than or equal to 350°C.

[0131] It is preferable that the cold-rolled steel sheet reheated to 490° C. or less as described above is held at that temperature for 30 seconds or more so that the above-mentioned effects can be fully realized.

[0132] If the holding time is excessive and exceeds 5 minutes, the tempering effect of martensite becomes excessive, resulting in a problem of reduced strength.

[0133] In the present invention, by optimizing the above-mentioned alloy composition system and manufacturing conditions, tempered martensite and bainite are formed as a microstructure as a base structure, and a certain fraction of retained austenite is formed finely and uniformly around the tempered martensite and bainite, thereby increasing the yield ratio and ductility compared to existing DP steels, and improving the formability for part processing of the steel sheet and the crash resistance performance during vehicle collision. The steel sheet of the present invention, which is precisely controlled in this way, can ensure ductility while maintaining the yield ratio compared to existing DP steels. As a result, a high-strength steel sheet having excellent ductility, hole expansibility, formability, and crash resistance can be provided.

[0134] On the other hand, the present invention can provide a plated steel sheet by plating the cold rolled steel sheet produced as described above.

[0135] [Hot-dip galvanizing] After undergoing the reheating and holding steps as described above, the steel sheet is preferably immersed in a hot-dip galvanized bath to produce a hot-dip galvanized steel sheet.

[0136] At this time, the hot-dip galvanizing can be performed under normal conditions, for example, in a temperature range of 430 to 490° C. The composition of the hot-dip galvanizing bath used in the hot-dip galvanizing is not particularly limited, and may be a pure zinc plating bath or a zinc-based alloy plating bath containing Si, Al, Mg, etc.

[0137] [Alloying heat treatment] If necessary, the hot-dip galvannealed steel sheet can be subjected to alloying heat treatment to obtain a hot-dip galvannealed steel sheet. In the present invention, the alloying heat treatment step conditions are not particularly limited, and may be normal conditions. As an example, the alloying heat treatment step can be performed in a temperature range of 480 to 600°C.

[0138] Furthermore, a final cooling and temper rolling process may be carried out after the hot dip galvanizing or alloying heat treatment.

[0139] [Final cooling] The steel sheet that has been hot-dip galvanized or heat-treated for alloying as described above can be final-cooled to further introduce fresh martensite. In this case, the final cooling is preferably performed to room temperature at a cooling rate of 3° C. / s or more.

[0140] If the cooling rate is less than 3° C. / s, the intended level of fresh martensite cannot be secured during the cooling process. On the other hand, the upper limit of the cooling rate is not particularly limited, but the cooling rate can be 50° C. / s or less in order to form a constant fraction of fresh martensite.

[0141] [Temper rolling] Furthermore, if necessary, the final-cooled hot-dip galvanized steel sheet or galvannealed hot-dip galvanized steel sheet can be subjected to temper rolling to form a large amount of dislocations in the steel and further improve the bake hardenability. In this case, the rolling reduction is preferably less than 2% (excluding 0%). If the rolling reduction is 2% or more, it is advantageous in terms of dislocation formation, but side effects such as sheet breakage may occur due to the limits of the equipment capacity.

[0142] The present invention will be described in more detail below with reference to examples. However, it should be noted that the following examples are intended to illustrate and explain the present invention in more detail, and are not intended to limit the scope of the present invention. The scope of the present invention is determined by the matters described in the claims and matters that can be reasonably inferred therefrom. EXAMPLES

[0143] Steel slabs having the alloy composition shown in Table 1 below were heated at temperatures of 1050 to 1250°C, and then each heated slab was finish hot rolled at Ar3 to Ar3+50°C to produce hot rolled steel sheets. Then, each hot rolled steel sheet was coiled at 400 to 700°C, and cooled to room temperature at a cooling rate of 0.1°C / s or less. Then, the cooled hot rolled steel sheet was cold rolled at a cold reduction rate of 45 to 75% to produce cold rolled steel sheet.

[0144] The cold rolling was carried out using a rolling mill having six stands, and the cumulative rolling reductions of stands 1 to 3 were as shown in Table 2 below.

[0145] Then, each cold-rolled steel sheet was subjected to continuous annealing under the conditions shown in Table 2 below, and then to stepwise cooling (primary-secondary cooling and holding). After the secondary cooling and holding process was completed, the steel sheet was reheated to a temperature of 490°C or less and held at that temperature. The holding process after the secondary cooling was performed for 30 seconds.

[0146] Then, the steel sheets were galvanized in a hot-dip galvanizing bath at 430 to 490°C, and finally cooled to room temperature at a cooling rate of 5°C / s, and then temper rolled to less than 2% to produce hot-dip galvanized steel sheets. At this time, some of the steel sheets were subjected to an alloying heat treatment after the above-mentioned galvanizing treatment.

[0147] [Table 1]

[0148] [Table 2]

[0149] The microstructure of each steel sheet manufactured as described above was observed and is shown in Table 3 below. The microstructure of each steel sheet was measured at 1 / 4t (t: thickness of steel sheet (unit: mm)) of the steel sheet thickness by Nital etching, and the fractions of tempered martensite (TM), bainite (B), ferrite (F), fresh martensite (FM) and retained austenite (A) were measured using FE-SEM, image analyzer, EBSD and XRD. The occupancy rate of retained austenite was also measured using EBSD.

[0150] In addition, the test pieces taken for the tensile test of each steel plate were evaluated for tensile properties in the L direction according to the DIN standard.

[0151] The hole expandability (HER) was measured by pushing up a circular hole (Hall) with a diameter of 10 mm punched according to the procedure of ISO 16630 with a conical punch until a crack occurred in the test piece, measuring the ratio of the initial hole diameter to the hole diameter after the change, and calculating it using the following formula.

[0152] [formula] Hole expansion ratio (HER,%) = {(D-D0) / D0} x 100 (Here, D means the hole diameter (mm) when the crack penetrates the steel plate along the thickness direction, and D0 means the initial hole diameter (mm).)

[0153] [Table 3]

[0154] As shown in Tables 1 to 3, in Examples 1 to 6, which satisfy all of the alloy composition systems and manufacturing conditions proposed in the present invention, the tempered martensite phase and the bainite phase were formed at a total area of ​​40 to 80%, as intended, and the retained austenite phase was formed mainly around the tempered martensite phase and the bainite phase. As a result, not only was a high strength of 980 MPa or more achieved, but a yield ratio of 0.6 to 0.9 was achieved, and an elongation rate of 10% or more and a hole expandability of 20% or more were ensured.

[0155] That is, the steel plate manufactured according to the present invention has significantly improved strength and ductility at the same time, and in particular, by satisfying the value of Relational Formula 2, it is possible to ensure the crash resistance and formability targeted by the present invention.

[0156] On the other hand, in the comparative steels 1 to 5 which do not satisfy the manufacturing conditions and do not satisfy the relational formula 1 proposed in the present invention, the intended microstructure was not formed and at least one of the physical properties was inferior.

[0157] Comparative steel 1 had an excessive ferrite phase, and was unable to ensure the target level of strength, had poor hole expandability, and was unable to ensure crash resistance and formability due to a deviation from Relational Formula 2.

[0158] In the comparative steels 2 and 5, the fresh martensite phase was formed in an excessive amount, so that high strength could be ensured, but since the relational expression 2 was not satisfied, the impact resistance performance and formability could not be ensured.

[0159] In comparative steel 3, the ferrite phase was small, and the retained austenite phase was not formed around the hard phase, so that the ductility was greatly reduced.

[0160] In Comparative Steel 4, the retained austenite phase was not formed around the hard phase, and the elongation was relatively low, which resulted in deviation from Relational Formula 2, making it impossible to ensure crash resistance and formability.

[0161] FIG. 1 is a graph showing the change in mechanical properties (relationship 2) depending on the value of relationship 1.

[0162] As shown in FIG. 1, when the value of Relational Expression 1 proposed in the present invention satisfies 1.7 or more, it is possible to ensure that the value of Relational Expression 2 is 9 or more.

[0163] FIG. 2 shows a photograph of the microstructure of Inventive Steel 4 measured by EBSD.

[0164] As shown in Fig. 2, it can be seen that the retained austenite phase was mainly formed around the tempered martensite phase and the bainite phase, and the ferrite phase and fresh martensite phase were properly formed.

Claims

1. In weight percent, carbon (C): 0.06 to 0.2%, silicon (Si): 0.4 to 1.4%, manganese (Mn): 1.8 to 3.0%, acid soluble aluminum (Sol.Al): 1.0% or less, molybdenum (Mo): 0.4% or less, chromium (Cr): 1.0% or less, antimony (Sb): 0.06% or less, boron (B): 0.01% or less, phosphorus (P): 0.1% or less, sulfur (S): 0.01% or less, the balance being Fe and other unavoidable impurities, The C, Si, and Al satisfy the following relational formula 1: The microstructure contains tempered martensite and bainite phases in total area fraction of 40 to 80%, retained austenite phase of 3 to 15%, and the remainder ferrite and fresh martensite phases. The residual austenite phase is a total residual austenite fraction (A T ), the retained austenite (A) adjacent to the tempered martensite and bainite TM+B ) Occupancy rate (A TM+B / A T ) is 90% or more. [Relationship 1] (8×C)+(1.1×Si)+(0.8×Al)≧1.7 (Here, each element means its weight content.)

2. The high strength steel plate having excellent crash resistance and formability according to claim 1, further comprising at least one of titanium (Ti): 0.05% or less and niobium (Nb): 0.05% or less.

3. The high-strength steel plate having excellent crash resistance and formability according to claim 1 , wherein the ferrite is contained in an area fraction of 40% or less.

4. The high-strength steel plate having excellent crash resistance and formability according to claim 1 , wherein the fresh martensite is contained in an area fraction of 20% or less.

5. The high-strength steel plate having excellent collision resistance and formability according to claim 1, wherein the steel plate has a tensile strength of 980 MPa or more, a yield ratio of 0.6 to 0.9, an elongation rate of 10% or more, and a hole expandability of 20% or more.

6. 2. The high-strength steel plate having excellent crash resistance and formability according to claim 1, wherein the relationship between the yield ratio, the elongation and the tensile strength of the steel plate satisfies the following Relational Expression 2. [Relationship 2] (YR×El×1000) / TS≧9 (Here, units of each physical property are excluded.)

7. heating a steel slab containing, by weight, 0.06-0.2% carbon (C), 0.4-1.4% silicon (Si), 1.8-3.0% manganese (Mn), 1.0% or less acid-soluble aluminum (Sol.Al), 0.4% or less molybdenum (Mo), 1.0% or less chromium (Cr), 0.06% or less antimony (Sb), 0.01% or less boron (B), 0.1% or less phosphorus (P), 0.01% or less sulfur (S), and the balance being Fe and other inevitable impurities, wherein the C, Si, and Al satisfy the following relational expression 1, at a temperature range of 1050-1250°C; Finish hot rolling the reheated steel slab at an outlet temperature of finish hot rolling in a temperature range of Ar3 to Ar3+50° C. to produce a hot-rolled steel sheet; coiling the hot-rolled steel sheet at a temperature in the range of 400 to 700°C; After the coiling, cooling the hot-rolled steel sheet to room temperature at a cooling rate of 0.1 ° C. / s; After cooling, the hot-rolled steel sheet is cold-rolled at a total rolling reduction of 30 to 80% to produce a cold-rolled steel sheet; subjecting the cold rolled steel sheet to a continuous annealing treatment; a step of primarily cooling the continuously annealed cold-rolled steel sheet to 450 to 700° C. at a cooling rate of 10° C. / s or less; After the primary cooling, secondary cooling is performed to 250 to 500° C. at a cooling rate of 3° C. / s or more; reheating the second-cooled cold-rolled steel sheet to a temperature of 490° C. or less and holding the temperature for 30 seconds or more; The cold rolling is performed at a cumulative reduction rate of 20% or more in the first to third stands. [Relationship 1] (8×C)+(1.1×Si)+(0.8×Al)≧1.7 (Here, each element means its weight content.)

8. The method for producing a high strength steel plate having excellent crash resistance and formability according to claim 7, wherein the continuous annealing treatment is carried out in a temperature range of Ac1+30°C to Ac3+30°C.

9. The method for producing a high strength steel plate having excellent crash resistance and formability according to claim 7, wherein the cooling rate in the secondary cooling is faster than the cooling rate in the primary cooling.

10. The secondary cooling is performed using hydrogen (H 2 8. The method for producing a high strength steel plate having excellent crash resistance and formability according to claim 7, wherein the process is carried out in a hydrogen quenching facility using hydrogen gas.

11. The method for producing a high strength steel plate having excellent crash resistance and formability according to claim 7, further comprising a step of holding the steel plate for 30 seconds or more after the secondary cooling.

12. The method of claim 7, further comprising the step of hot-dip galvanizing in a coating bath at 430 to 490°C after the reheating and holding.

13. The method for producing a high strength steel plate having excellent crash resistance and formability according to claim 12, further comprising the step of performing an alloying heat treatment after the hot dip galvanizing.

14. The method for producing a high strength steel plate having excellent crash resistance and formability according to claim 13, further comprising a step of final cooling to room temperature at an average cooling rate of 3° C. / s or more after the hot dip galvanizing or alloying heat treatment.

15. The method for producing a high strength steel plate having excellent crash resistance and formability according to claim 14, further comprising a step of temper rolling at a rolling reduction of less than 2% after the final cooling.

Citation Information

Patent Citations

  • Steel sheet and method of producing the same

    JP2014034716A

  • High-strength steel plate with excellent crashworthiness and formability and its manufacturing method

    JP2021504576A

  • Steel plate with excellent formability and work hardening rate

    JP2023534825A

  • Cold rolled and heat-treated steel sheet and method of manufacturing thereof

    US20230243007A1

  • High-strength steel sheet having superior impact resistance, method for producing same, high-strength galvanized steel sheet, and method for producing same

    WO2013018740A1