How to manufacture high strength steel
Direct quenching and controlled cooling in a hot strip mill, combined with subsequent tempering, produce high-strength steel with fine microstructures, addressing production limitations and achieving superior mechanical properties without additional treatments.
Patent Information
- Application Number
- JP2024529913
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-24
- Filing Date
- 2022-11-23
- Publication Date
- 2024-11-13
AI Technical Summary
Existing methods for producing high-strength steel in hot strip mills are limited by coiling temperatures exceeding 500°C, which restrict strength achievement and require additional alloy content or off-line treatments, making them costly and inefficient.
A method involving direct quenching in a hot strip mill at low coiling temperatures, followed by controlled cooling and subsequent tempering processes, to produce high-strength steel with fine microstructures like acicular ferrite or bainite, without cold rolling or annealing, and utilizing precipitation strengthening elements for enhanced properties.
This approach enables the production of high-strength steel with tensile strengths up to 1100 MPa and excellent local formability, achieving a balance of strength, ductility, and toughness through controlled thermal processes, reducing production costs and complexity.
Smart Images

Figure 2024542240000001_ABST
Abstract
Description
[Technical field]
[0001] <CROSS REFERENCE TO RELATED APPLICATIONS> This application claims the benefit of U.S. Provisional Patent Application No. 63 / 283,090, filed November 24, 2021, and is incorporated herein by reference. [Background technology]
[0002] <Background> For plate and hot strip mill products, direct quenching is typically used. Tempering is applied in direct quenching of plate, and ageing, e.g., precipitation hardening, has been employed after direct quenching in the laboratory to develop models for precipitation hardening kinetics. Many hot strip mill steels are produced using coiling temperatures in excess of 500°C. This condition limits the strength achievable in low alloy steels, requiring either increased alloy content or additional processing and expense via off-line heat treatment to achieve the required high strength levels.
[0003] For example, some manufacturing processes for high strength steels with good local formability, such as bending and hole expansion, in the tensile strength classes of 800 MPa and 1000 MPa can be produced without the need for cold rolling.
[0004] The present disclosure includes a method for producing high strength steel directly in a hot strip mill without further thermomechanical steps such as cold rolling or annealing. In some embodiments, the disclosed process includes utilizing low coiling temperatures, i.e., "direct quenching" in a hot strip mill, to produce high strength steel. In some embodiments, the process described herein includes direct quenching with reduced or no subsequent heat treatment to achieve high strength steel with fine and tough microstructure, e.g., acicular ferrite, suitable for applications requiring high local formability. In some embodiments, high strength steel is produced directly after quenching, e.g., bainite or martensite. In some embodiments, the balance of strength, ductility, or toughness can be modified by performing a subsequent tempering step, e.g., through batch annealing, continuous annealing, or hot-dip coating lines. In some embodiments, finely textured steels are produced by, for example, batch annealing, continuous annealing, or through a hot dip galvanizing line, while retaining the precipitation strengthening elements in solution for a subsequent aging treatment similar to a tempering step. In some embodiments, aging is utilized to produce a desired balance of strength, ductility, or toughness. Summary of the Invention
[0005] <Abstract> A method for producing high strength steel sheet having a tensile strength of 800-1100 MPa and a hole expansion ratio of at least 50%, comprising the steps of reheating a previously cast slab or holding heat from a directly cast slab at a temperature above Ar3, hot rolling the slab to a final desired thickness, cooling the steel sheet at a rate of 50°C per second to a temperature below 400°C, and winding the steel sheet into a coil.
[0006] A method for producing high strength steel sheet having a tensile strength of about 800 MPa and a composition containing 0.06 wt% Carbon, 1.0 wt% Mn, 0.1 wt% Si, 0.03 wt% Ti, and 0.0020 wt% Boron, comprising the steps of reheating a previously cast slab or holding the heat from a directly cast slab at a temperature above Ar3, hot rolling the slab to a final desired thickness, cooling the steel sheet at a rate of 50°C per second to a temperature below 400°C, and winding the steel sheet into a coil.
[0007] A method for producing a high strength steel sheet having a tensile strength of about 1000 MPa and a composition containing 0.06 wt% C, 1.0 wt% Mn, 0.1 wt% Si, 0.03 wt% Ti, and 0.0020 wt% B, comprising the steps of reheating a previously cast slab or holding the heat from a directly cast slab at a temperature above Ar3, hot rolling the slab to a final desired thickness, cooling the steel sheet at a rate of 50°C per second to a temperature below 400°C, and winding the steel sheet into a coil. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a graph showing modeling of conventional cooling methods at various locations within a coil.
[0009] [Diagram 2] FIG. 2 is a graph showing hole expansion as a function of tensile strength for the experimental steels without subsequent annealing.
[0010] [Diagram 3] FIG. 3 is a graph showing hole expansion as a function of tensile strength for the experimental steels after different annealing cycles.
[0011] [Figure 4]FIG. 4 is a graph showing the aging response from hardness testing, and is used to determine whether there is agreement with the P* modeling, batch annealing paradigm.
[0012] [Figure 5-1] FIG. 5-1 is a graph showing the aging treatment carried out to determine the sensitivity to annealing. [Figure 5-2] FIG. 5-2 is a graph showing aging treatments performed to determine sensitivity to annealing.
[0013] [Figure 6] FIG. 6 is a graph of a low temperature aging treatment performed to temper the microstructure for the purpose of improving hole expansion.
[0014] [Figure 7] FIG. 7 is a graph showing a simulation of batch annealing to determine sensitivity to annealing temperature.
[0015] [Figure 8-1] FIG. 8-1 is a graph of the aging response based on batch annealing. [Figure 8-2] FIG. 8-2 is a graph of the aging response based on batch annealing.
[0016] [Figure 9] FIG. 9 is a graph showing the results of an aging study in which batch annealing simulations were performed with hot spots and cold spots.
[0017] [Figure 10-1] FIG. 10-1 is a graph of an annealing screen to examine sensitivity to batch annealing temperature. [Figure 10-2] FIG. 10-2 is a graph of an annealing screen to examine sensitivity to batch annealing temperature.
[0018] [Figure 11] FIG. 11 is a graph of an annealing simulation with hot spot and cold spot cycles.
[0019] [Figure 12] FIG. 12 is a graph of low temperature annealing temperatures. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] <Detailed Description> In some embodiments, the process for producing high strength steels is required to produce a ferritic structure that is substantially strengthened by precipitation hardening. The primary precipitation hardening is either titanium-based or vanadium-based in conventional processes. These techniques employ a typical hot strip mill (HSM) process, with coiling temperatures of at least 600°C (1112°F). Free cooling of the hot coil is conventionally performed, resulting in different time-temperature histories at different locations in the coil. The ends of the coil (especially the edges, the outer wraps) cool faster than the coil interior. Such variations that can be estimated by conventional methods are shown in Figure 1. An example is for an initial coiling temperature of 1325°F, a coil ID of 30 inches, an OD of 65.6 inches, and a thickness of 0.371 inches. This is closely related to the precipitation hardening reaction on which this material design is based, causing undesirable variations in mechanical properties.
[0021] In some conventional methods, molybdenum is added to mitigate the variability of titanium carbide precipitates and the variability of vanadium-based precipitates. Acicular ferrite structures are known to provide both strength and toughness. These microstructures are the basis for linepipe products. Local formability, as disclosed herein, is useful as a measure of steels that have toughness and high strength.
[0022] Acicular ferrite can be produced by quenching low carbon steels, and quenching the strip to a low temperature before winding on the coiler can mitigate cooling variability after coiling. This disclosure discusses direct quenching of steels after the hot strip mill process. In some embodiments, direct quenching can preserve precipitation hardening species in solution (unprecipitated).
[0023] The main purpose of a hot strip mill is to reheat thick steel slabs into thin sheets of various thicknesses. The thick steel slabs pass through several rolling mill stands driven by powerful motors. The rolled steel sheet then passes through a coiler after which the coils are transferred to the next process in the mill. From start-up to finish, the steel undergoes several treatments at each stage which are the main features of a hot strip mill:
[0024] The disclosure includes methods to induce precipitation strengthening reactions under controlled thermal conditions, such as batch annealing, continuous annealing, or to tailor properties with improved uniformity. Additionally, the disclosure includes data showing that a combination of strength and toughness can be achieved by annealing quenched and tempered products.
[0025] The present disclosure is applicable across a wide range of hot rolling processes for steel. In some embodiments, the steel is hot rolled when it is primarily in the austenitic state, and the rolled strip is then cooled at a sufficient rate to a sufficiently low temperature to achieve an acicular ferrite or bainite structure. In some embodiments, the precursor to the final hot roll can be produced in parallel with the final rolling sequence (direct casting and rolling technique with or without intermediate reheating before final rolling), or in a facility independent of the slab or transfer bar that is reheated for processing in the hot strip mill.
[0026] In some embodiments, the temperature of the final rolling step should be such that the steel is in the austenitic start state, so that the final rolling pass is completed above the austenite-ferrite transformation temperature, also known as the Ar3 temperature.
[0027] In some embodiments, after completion of the final rolling step, the steel is rapidly cooled to achieve the desired acicular ferrite and / or bainite microstructure (depending on the strength class). Rapid cooling continues until the steel is below 400° C. The steel strip is then wound into a coil. The rate of rapid cooling should be greater than 50° C. / sec.
[0028] In some embodiments, a secondary treatment process is applied to the steel strip to promote precipitation reactions for retention or increase of strength. In this embodiment, the hot rolled strip should be reheated to a temperature above 500°C below the ferrite-austenite phase transformation temperature, e.g., the Acl temperature. The appropriate temperature depends on the expected time of the process to be carried out. For example, continuous annealing of steel strip requires shorter heating times than batch annealing of coils. In a continuous annealing process (for hot-dip galvanized or ungalvanized strip), the shorter heating times allow the strip to reach the Acl temperature and achieve the desired properties.
[0029] In some embodiments, the steel composition includes carbon. In some embodiments, the steel composition includes carbon in the range of about 0.03 to 0.07 weight percent. Carbon levels below about 0.03 weight percent may not achieve the desired strength levels. Higher carbon levels may result in poor hole expansion performance and may make the steel more susceptible to deleterious peritectic reactions during continuous casting.
[0030] In some embodiments, the steel composition includes manganese. In some embodiments, the steel composition includes manganese in the range of up to about 2.0 weight percent. Manganese is one of the more economical strengthening elements and sequesters sulfur to prevent the formation of harmful iron sulfides. The minimum practical level for high strength steels is about 0.5 weight percent, and higher levels are often used for economic reasons to avoid the use of more expensive elements. Too high a level of manganese can result in chemical segregation patterns that can adversely affect performance.
[0031] In some embodiments, the steel composition includes molybdenum. In some embodiments, the steel composition includes molybdenum in the range of up to about 0.5 wt.%. Molybdenum is a potent strengthening element, but is often expensive to use. Molybdenum may be selected to limit the maximum manganese content used or to add thermal stability to precipitation hardening species. If not technically necessary, residual levels will be used for economic reasons.
[0032] In some embodiments, the steel composition includes chromium. In some embodiments, the steel composition includes chromium at less than about 2.0 weight percent. Chromium is a strong strengthening element. Economics suggest its use after manganese and before molybdenum. Chromium can be used to limit the maximum amount of manganese used. Additions of less than about 2.0 weight percent are appropriate for this technology.
[0033] In some embodiments, the steel composition includes silicon. In some embodiments, the steel composition includes up to about 1 weight percent or less of silicon, which is an efficient strengthening element. Higher levels of silicon can induce surface features in the hot strip that are undesirable in some applications. Higher levels of silicon can also interfere with galvanizing operations.
[0034] In some embodiments, the steel composition includes boron. In some embodiments, the steel composition includes boron in the range of about 10-30 ppm or less. The strengthening effect is ensured by the use of a nitrogen-sequestering element, most typically titanium. The nitrogen sequestration results in coarse nitride particles that can impair the toughness of the steel. Therefore, the use of boron may not be suitable for applications where toughness is paramount.
[0035] In some embodiments, the steel composition includes titanium. In some embodiments, the steel composition includes titanium as a strong strengthening element. In this disclosure, titanium is utilized primarily as a nitrogen sequestering element to facilitate the use of boron, or as a precipitation strengthener for secondary thermal processing. A suitable level for use in nitrogen sequestering is a level of 3.4 times the nitrogen content of the steel. A practical maximum addition for precipitation strengthening purposes would be 0.2 wt.%.
[0036] In some embodiments, the steel composition includes vanadium. In some embodiments, the steel composition includes about 0.2 wt.% vanadium. Vanadium can be a strong strengthening element. In the present disclosure, vanadium is used as a secondary thermal process precipitation strengthener.
[0037] In some embodiments, the steel composition includes copper. In some embodiments, the steel composition includes copper in the range of about 0.3-0.5 wt.% when atmospheric corrosion resistance is desired. Copper is not considered a significant strengthening element. In this disclosure, copper is used only when atmospheric weathering resistance is desired. Adequate mechanical properties are obtained without this expensive alloying element. Copper must be used with caution because it can lose ductility during hot rolling (hot brittleness). Depending on the hot rolling process used, the co-addition of nickel may be required to mitigate the loss of hot ductility.
[0038] In some embodiments, the steel composition includes nickel. In some embodiments, the steel composition includes nickel at a level approximately half the copper addition. This level has been found to be suitable for reducing low ductility at hot rolling temperatures. The nickel addition can be employed to strengthen, toughen, or reduce low ductility during hot rolling. In the present disclosure, nickel is only used in conjunction with the copper addition when weathering resistance is desired. Adequate mechanical properties can be obtained without the use of this expensive alloying element.
[0039] In some embodiments, the steel composition has a tensile strength of about 800 MPa, and a very economical steel composition is approximately 0.06C-1.0Mn-0.1Si-0.03Ti-0.0020B (all values in weight percent) with no intentional addition of additional elements. Using a similar alloy design to obtain a nominal tensile strength of 1000 MPa, the composition is approximately 0.06C-1.0Mn-0.1Si-0.03Ti-0.0020B (all values in weight percent) with no intentional addition of additional elements. Alternative designs without boron additions can be considered. For example, a steel with a tensile strength of 800 MPa would be approximately 0.06C-1.5Mn-0.1Si (all values in weight percent) with no intentional addition of additional elements. To reach a tensile strength of 1000 MPa, the manganese level would be increased to a practical maximum of 2.0 weight percent, and chromium would be added at a level of 0.5 weight percent.
[0040] As described herein, direct quenching is the first step of the heat treatment process, and the subsequent tempering step is performed in a separate process step (batch annealing, continuous annealing). This method does not rely on precipitation hardening reactions and is an alternative implementation of the known quench-and-temper concept.
[0041] FIG. 2 shows a combination of two important properties of primary interest: hole expansion and tensile strength. FIG. 2 is a graph showing hole expansion as a function of tensile strength. The graph shows properties for steels produced according to embodiments of the process of the present disclosure, directly as quenched and after annealing. The present disclosure is configured to produce steels with tensile strengths of at least 800 MPa and with at least 50% hole expansion. The graph shown in FIG. 2 shows the properties without annealing and the second graph shows the properties after applying different annealing cycles. The graph shown in FIG. 2 shows that there are various batches with good hole expansion with tensile strengths of over 800 MPa.
[0042] The following examples are intended to illustrate various aspects of the present disclosure, but are not intended to limit the scope of the present disclosure. Many different steel alloys were examined. The strength of the direct quenched product is expected to vary as a function of composition. Table 1 shows the regression model of tensile strength as a function of composition. The data is sorted by increasing P-value, with the most significant elements in the regression placed at the top of the list (higher P-values indicate a higher probability of random contribution).
[0043] Table 1 shows the regression results of tensile strength vs. composition for the directly quenched plates. [Table 1]
[0044] The inclusion of C, B, Mn, Mo, and Cr is used to enhance the hardenability of the steel. In some embodiments, the contribution of Cb, especially shown by the negative coefficient, reflects the grain refinement contribution of this element and its negative contribution to hardenability. In some embodiments, the addition of Cu and Ni is expected to contribute to hardenability, but was not reported as a reliable contribution (P values are quite high). Similarly, in some embodiments, V and Ti showed high P values. This is reasonable for V and Ti, since their contribution in these steels is mainly from precipitation hardening, and they are not expected to be active in the as-quenched state. It is through subsequent aging that V and Ti, as well as Cb, contribute to maintaining or increasing strength.
[0045] Tables 2 and 3 show the data for Campaign 1. Plates were hot rolled and directly quenched to room temperature. All heat compositions are in weight percent. [Table 2] [Table 3]
[0046] Tables 4 and 5 show the data for Campaign 2. The plates were hot rolled and directly quenched to room temperature, after which they were aged to determine their sensitivity to annealing. [Table 4] [Table 5]
[0047] Figure 4 shows a graph of the aging response with hardness testing to determine if there was agreement with the P* modeling. Batch annealing paradigm times ranged from 1 hour to 48 hours and 3600 seconds to 172800 seconds. Hardness testing was performed on the HRA scale and converted to HRC.
[0048] Tables 6 and 7 show the data for Campaign 3. Plates were hot rolled and direct quenched. [Table 6] [Table 7]
[0049] Tables 8 and 9 show the data for Campaign 4. Initial testing was performed by hot rolling to heavy gauge. [Table 8] [Table 9]
[0050] Table 10 shows data for plates ground to a thickness of 5 mm to facilitate hole expansion testing. Sub-sized longitudinal tensile specimens taken from the ends were tested. [Table 10]
[0051] Figure 5 shows a graph of the aging treatments used to investigate sensitivity to annealing. All tests were performed in a salt pot and hardness was measured as HRA, which was converted to VHN to provide a more direct estimate of tensile strength. Figures 6 and 7 show simulated hot and cold spot batch annealing with low temperature aging to temper the microstructure for improved hole expansion.
[0052] Table 11 shows the hole expansion after low temperature tempering. [Table 11]
[0053] Tables 12 and 13 show the data for Campaign 5. Plates were hot rolled and directly quenched to room temperature. [Table 12] [Table 13]
[0054] Tables 14 and 15 show the data for Campaign 6. Plates were hot rolled and quenched to room temperature. [Table 14] [Table 15]
[0055] Tables 16 and 17 show the direct quench portion of the 780 Developmental Bainite Process. The laboratory heats were hot rolled at two different finishing temperatures and direct quenched to room temperature. [Table 16] [Table 17]
[0056] 8 is a graph showing the aging response under the batch annealing paradigm, in which batch annealing was performed, for example, at 100° F. / hr, hold for 24 hours, and furnace cool, to determine sensitivity to annealing temperature.
[0057] Figure 9 shows results based on aging studies with batch annealing simulations performed with hot and cold spots. In some embodiments, the hot spot temperature was 1100°F, near peak age for Mo steel and overaged without Mo. In some embodiments, the cold spot was 1000°F, below peak age when peak age was 1000°F for 24 hours.
[0058] Table 18 shows the results based on the aging study results where batch annealing simulation was performed with hot and cold spots, a hot spot of 1100°F was tested near peak age for the Mo steel and overaged without Mo. Additionally, a cold spot of 1000°F was tested, which is below peak age if the peak age was 1000°F for 24 hours. [Table 18]
[0059] Tables 19 and 20 show the results of the direct quench portion of the HR780 development, a hybrid of FM13 and KSL780R. The data includes laboratory heats for CAL / HD grades. Plates were hot rolled at different finishing temperatures and direct quenched to room temperature. [Table 19] [Table 20]
[0060] Figure 10 is a graph of the annealing screen to examine sensitivity at 24 hours to batch annealing temperatures of 900, 1000, 1100, and 1200° F. Figure 11 shows a simulation of batch annealing with hot spot and cold spot cycles. Table 21 contains data from the batch annealing simulation with hot spot and cold spot cycles. [Table 21]
[0061] Figure 12 shows the data for the low anneal temperature in heat 30, 900°F, 24 hours, approximately 755 MPa. Table 22 shows the direct quench portion of the HR780 development, which contains Ti and has different N levels. These heats are to tailor FM13 / FM44. The lab heats were directly quenched to room temperature after hot rolling. [Table 22]
[0062] Notwithstanding that the numerical ranges and parameters setting forth the broad scope of the invention are approximations, the numerical values set forth in the specific examples are reported as precisely as possible, however, any numerical value inherently contains certain errors necessarily resulting from the standard deviation found in their respective testing measurements.
[0063] It should also be understood that all numerical ranges recited herein are intended to include all subranges subsumed therein. For example, a range "1 to 10" is intended to include the recited minimum value of 1 and the recited maximum value of 10, as well as all subranges between 1 and 10, i.e., minimum values equal to or greater than 1 and maximum values equal to or less than 10.
[0064] As used herein, the use of the singular includes the plural and the plural encompasses the singular, unless specifically stated otherwise. Also, as used herein, the use of "or" means "and / or" unless specifically stated otherwise, even if "and / or" is expressly used in a particular instance. As used herein and in the appended claims, the articles "a," "an," and "the" include plural items unless expressly and unambiguously limited to one item.
[0065] As used herein, terms such as "including, comprising," "containing," and the like are open-ended terms and are understood to not exclude the presence of additional elements, materials, phases, or process steps not recited in this application. As used herein, the term "consisting of" is understood to exclude the presence of any unspecified element, material, phase, or process step. As used herein, the term "consisting essentially of" is understood to include the specified elements, materials, phases, or process steps, where applicable, and to include any unspecified elements, materials, phases, or process steps that do not materially affect the basic or novel characteristics of the invention.
[0066] While particular embodiments of the invention have been described above for purposes of illustration, it will be apparent to those skilled in the art that many changes in the details of the invention can be made without departing from the invention.
Claims
1. A method for producing a high strength steel sheet having a tensile strength of 800-1100 MPa and a hole expansion ratio of at least 50%, comprising the steps of: reheating a previously cast slab to a temperature above Ar3 or holding the heat of a directly cast slab above Ar3; hot rolling the slab to a final desired thickness; cooling the steel sheet at a rate of 50°C per second to a temperature below 400°C; winding the steel sheet into a coil; A method for producing a high strength steel sheet, comprising:
2. The method for producing a high strength steel sheet according to claim 1, wherein the Ar3 temperature is higher than the austenite-ferrite transformation temperature.
3. The method of claim 1 further comprising cooling the steel sheet to an acicular ferrite structure. Manufacturing method of high strength steel sheet.
4. The method of claim 1 further comprising cooling the steel sheet to a bainite structure.
5. 10. The method of claim 1 further comprising subjecting the steel sheet to a secondary treatment to promote precipitation reactions for strength retention or improvement.
6. The method of claim 5 further comprising reheating the steel coil to a temperature below AcI.
7. The method of claim 6, wherein the Ac1 temperature is higher than 500° C. and lower than the ferrite-austenite phase transformation temperature.
8. A method for producing high strength steel sheet according to claim 6, wherein the temperature depends on the expected length of time of the process used.
9. The method of claim 6 further comprising continuous annealing the steel sheet to achieve a reduced heating time.
10. The method of claim 9, wherein the heating time during the successive annealing steps can be reduced to bring the steel sheet closer to the Ac1 temperature to achieve the desired properties.
11. 1. A method for producing a high strength steel sheet having a tensile strength of about 800 MPa and a composition of 0.06 wt.% carbon, 1.0 wt.% Mn, 0.1 wt.% Si, 0.03 wt.% Ti, and 0.0020 wt.% boron, comprising: reheating a previously cast slab to a temperature above Ar3 or holding the heat of a directly cast slab above Ar3; hot rolling the slab to a final desired thickness; cooling the steel sheet at a rate of 50°C per second to a temperature below 400°C; winding the steel sheet into a coil; A method for producing a high strength steel sheet, comprising:
12. The method of claim 11 further comprising cooling the steel sheet to acicular ferrite.
13. 12. The method of claim 11 further comprising subjecting the steel sheet to a secondary treatment to promote precipitation reactions for strength retention or improvement.
14. The method of claim 13 further comprising reheating the steel coil to a temperature below AcI.
15. The method of claim 14, wherein the Ac1 temperature is higher than 500° C. and lower than the ferrite-austenite phase transformation temperature.
16. A method of manufacturing high strength steel sheet according to claim 11, wherein the temperature depends on the expected length of time of the process used.
17. The method of claim 11 further comprising continuous annealing the steel sheet to achieve a reduced heating time.
18. 18. The method of claim 17, wherein the heating time during the successive annealing steps can be reduced to bring the steel sheet closer to the Ac1 temperature to achieve the desired properties.
19. A method for producing a high strength steel sheet having a tensile strength of about 1000 MPa and a composition of 0.06 wt% C, 1.0 wt% Mn, 0.1 wt% Si, 0.03 wt% Ti, and 0.0020 wt% B, comprising: reheating a previously cast slab to a temperature above Ar3 or holding the heat of a directly cast slab above Ar3; hot rolling the slab to a final desired thickness; cooling the steel sheet at a rate of 50°C per second to a temperature below 400°C; winding the steel sheet into a coil; A method for producing a high strength steel sheet, comprising: