Steel pipe for oil cylinder and its manufacturing method
A steel pipe with controlled elemental composition and stepwise cooling process addresses the challenge of residual stress and inner wall cracking, achieving high strength and low residual stress in oil cylinder pipes.
Patent Information
- Application Number
- JP2024530430
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-25
- Filing Date
- 2022-11-24
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2042-11-24
AI Technical Summary
Conventional methods for reducing residual stress in steel pipes for oil cylinders are costly and increase production complexity, while existing patent solutions do not adequately address the issue of inner wall cracking and residual stress in these pipes.
A steel pipe composition with specific elemental contents (Fe, C, Si, Mn, Nb, Mo, Ti, B) and a stepwise cooling process to control ferrite distribution, ensuring high strength and low residual stress, preventing inner wall cracking.
The method achieves a yield strength of 600 MPa or more, tensile strength of 730 MPa or more, and residual stress of 50 MPa or less, significantly improving the steel pipe's performance and safety by preventing cracks and reducing residual stress.
Smart Images

Figure 2024542251000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of materials, in particular to a steel pipe for oil cylinders and a method for manufacturing the same. [Background technology]
[0002] Steel pipes for oil cylinders are widely used in oil cylinders for construction machinery and air cylinder barrels, and can withstand impact fatigue, friction and other loads during use. Residual stress is an important factor that affects the fatigue life, extrusion resistance, internal pressure resistance and deformation caused by machining of seamless pipes. By reducing or eliminating the residual stress in steel pipes for oil cylinders, the service life of steel pipes for oil cylinders can be significantly improved. This is one of the important goals in the subsequent production management of steel pipes for oil cylinders.
[0003] Currently, traditional methods to reduce or eliminate residual stress include high temperature stress relief annealing and mechanical and physical methods, but these processes are costly and increase the production process.
[0004] China Patent Application Publication No. 201810365440.5 discloses a "method for removing residual stress in tempered seamless steel pipe and the adopted bidirectional chain cooling bed", which controls the straightness of the steel pipe after rolling and before tempering, and the bidirectional chain of the cooling bed after tempering to remove residual stress, thereby eliminating the need for tempering and stress relief annealing processes and achieving the goal of cost reduction.
[0005] China Patent Application Publication No. 201420805596.8 discloses an "Asymmetric Steel Pipe Straightening Roller", which designs a special straightening roller to remove residual stress and oxide film on the steel pipe by controlling the force applied to the steel pipe during the straightening process.
[0006] China Patent Application Publication No. 200910210718.2 discloses a "method for controlling the residual stress level of steel pipes for conveyors", which derives a formula and obtains the residual stress level of the steel pipe by comparing the formula with the measured elastic recovery of the steel pipe, thereby measuring and characterizing the residual stress level of the steel pipe. Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention aims to provide a steel pipe for oil cylinders and a manufacturing method thereof. Compared with conventional steel pipe products for oil cylinders, the present invention can significantly reduce the residual stress of the steel pipe for oil cylinders, and can obtain higher strength while preventing cracks from occurring on the inner wall. According to the present invention, the yield strength of the steel pipe for oil cylinders is 600 MPa or more, the tensile strength is 730 MPa or more, and the residual stress is 50 MPa or less. [Means for solving the problem]
[0008] In one aspect, the present invention provides a steel pipe for oil cylinders, which contains, in addition to 90% by weight or more of Fe and unavoidable impurities, the following chemical elements in weight percent (wt%): C: 0.16-0.3%, Si: 0.15-0.5%, Mn: 1.2-1.8%, Nb: 0.02-0.04%, Mo: 0.1-0.2%, and optionally Ti: 0.015-0.03%, and B: 0.0015-0.0035%.
[0009] Preferably, the steel pipe for oil cylinders contains, by weight, the following chemical elements: C: 0.16-0.3%, Si: 0.15-0.5%, Mn: 1.2-1.8%, Nb: 0.02-0.04%, Mo: 0.1-0.2%, optionally Ti: 0.015-0.03%, and B: 0.0015-0.0035%, with the remainder being Fe and unavoidable impurities.
[0010] Of the above unavoidable impurities, P≦0.01% and S≦0.001% are preferred.
[0011] In some embodiments, the wall thickness of the steel pipe for oil cylinders is 20 mm or more, and the steel pipe for oil cylinders contains Ti: 0.015 to 0.03% and B: 0.0015 to 0.0035%. In some embodiments, the wall thickness of the steel pipe for oil cylinders is less than 20 mm, and the steel pipe for oil cylinders may or may not contain Ti: 0.015 to 0.03% and B: 0.0015 to 0.0035%.
[0012] Preferably, the wall thickness of the steel pipe for oil cylinders is 9 mm or more.
[0013] Preferably, in the wall thickness direction of the above-mentioned steel pipe for oil cylinders, the microstructure from the outer wall to the t / 2 point is tempered sorbite, and the microstructure from the t / 2 point to the inner wall is tempered sorbite + ferrite, the ferrite is distributed with a gradient, the ferrite content increases the closer the distance to the inner wall, the ferrite content in the microstructure at the t / 2 point is 3% or more, and the ferrite content in the microstructure at the inner wall (i.e., at the surface of the inner wall) is 5% or more.
[0014] Here, unless otherwise clearly stated, t represents the wall thickness (mm) of the steel pipe for oil cylinders.
[0015] Preferably, the above-mentioned steel pipe for oil cylinders has a yield strength of 600 MPa or more, a tensile strength of 730 MPa or more, and a residual stress of 50 MPa or less.
[0016] Preferably, the residual stress of the steel pipe for oil cylinders is 40 MPa or less.
[0017] Preferably, the steel pipe for oil cylinders has a yield ratio (ie, the ratio of yield strength to tensile strength) of 0.92 or less.
[0018] Preferably, the ferrite content in the microstructure at the t / 2 point of the steel pipe for oil cylinders of the present invention is 0.5t-1.0t%.
[0019] Preferably, the ferrite content in the microstructure of the inner wall of the steel pipe for oil cylinders of the present invention is 1.5t-2.0t%.
[0020] The ferrite content is defined herein as the proportion of ferrite in the microstructure expressed as area %, and is measured by metallographic methods.
[0021] The elements in the steel pipe for oil cylinders of the present invention are designed based on the following principles.
[0022] C: C is an interstitial solid solution strengthening element and has a large effect on hardenability. If the C content is less than 0.16%, the strength becomes too low, and if the C content exceeds 0.3%, cracks will occur on the inner wall after stepwise cooling. Therefore, in the present invention, the C content is controlled to be in the range of 0.16 to 0.3%.
[0023] Si: Si is a commonly used deoxidizer and a powerful element for precipitating iron, improving hardenability to some extent. If the Si content is less than 0.15%, the above effects are not fully exhibited, and if the Si content exceeds 0.5%, Si causes problems with surface quality. Therefore, in the present invention, the Si content is controlled to be in the range of 0.15 to 0.5%.
[0024] Mn: Mn is a solid solution strengthening element and is also a powerful element that improves hardenability. If the Mn content is less than 1.2%, the hardenability is insufficient and the strength is low, and if the Mn content exceeds 1.8%, the hardenability becomes too high, so that the precipitation of ferrite content from the t / 2 point to the inner wall after stepwise cooling is reduced, and both the phase change and thermal stress of the inner wall become significant tensile stress, resulting in cracks on the inner wall. Therefore, in the present invention, the Mn content is controlled to be in the range of 1.2 to 1.8%.
[0025] Nb: Nb is a carbide precipitation strengthening element, which refines the austenite grains and acts as a nucleation point to promote the precipitation of ferrite during stepwise cooling.
[0026] Mo: Mo significantly improves hardenability, as well as improving the balance between strength and toughness and tempering stability. When the Mo content is in the range of 0.1%-0.2%, the effect of Mo on hardenability controls the distribution of ferrite from the t / 2 point to the inner wall in a gradient, which ensures strength while preventing cracks from occurring on the inner wall during the stepwise cooling process.
[0027] Ti and B: The combined addition of Ti and B significantly improves the hardenability. For pipes with a wall thickness of 20 mm or more, it is necessary to improve the hardenability of the steel pipe for oil cylinders, and to avoid a significant increase in the ferrite content from the t / 2 point to the inner wall, which reduces the strength. On the other hand, Ti precipitates as carbonitride, but can function as a nucleation point of ferrite in the stepwise cooling process, and can effectively control the precipitation rate of ferrite. If the Ti content is less than 0.015% or the B content is less than 0.0015%, the above effect is not fully exerted, and if the Ti content exceeds 0.03% or the B content exceeds 0.0035%, there is no significant improvement effect in improving the hardenability. Therefore, in the present invention, the Ti content is controlled to be in the range of 0.015 to 0.03%, and the B content is controlled to be in the range of 0.0015 to 0.0035%.
[0028] It should be noted that the unavoidable impurities include P and S, both of which are harmful elements in steel. If the mass fraction of P is too high, it may cause bias in the grain boundaries, making them brittle and significantly reducing toughness. If the mass fraction of S is too high, the amount of inclusions in the steel will increase, which will have a negative effect on low-temperature toughness. Therefore, the contents of P and S in steel should be minimized.
[0029] The present invention controls the distribution of ferrite in a steel pipe for oil cylinders by controlling the content of elements such as Nb, Mo, and Ti. In the wall thickness direction of the steel pipe for oil cylinders, the microstructure from the outer wall to the t / 2 point is tempered sorbite, and the microstructure from the t / 2 point to the inner wall is tempered sorbite + ferrite, the ferrite is distributed with a gradient, and the content of the ferrite increases as the distance to the inner wall decreases. The ferrite content in the microstructure at the t / 2 point is 3% or more, and the ferrite content in the microstructure at the inner wall is 5% or more. Here, t is the wall thickness (mm) of the steel pipe for oil cylinders. The microstructure from the outer wall to the t / 2 point is tempered sorbite, and the strength and toughness levels of the tempered sorbite are good, and the rigidity of the outer layer of the steel pipe for oil cylinders can be sufficiently ensured. The microstructure from the t / 2 point to the inner wall is tempered sorbite + ferrite, and the good toughness and low yield ratio of the steel pipe for oil cylinders can be ensured.
[0030] In addition, the precipitation of ferrite structure is distributed with a gradient, and the closer to the inner wall, the higher the ferrite content. Ferrite has good ductility and toughness, so that the residual stress of the inner wall of the steel pipe for oil cylinders can be well controlled in the cooling process, and the cracks on the inner wall can be prevented in the water quenching process. In addition, the residual stress of the steel pipe for oil cylinders can be significantly reduced while ensuring high strength of the steel pipe for oil cylinders.
[0031] As a result of intensive research, the present inventors have found that the amount of ferrite precipitated in a steel pipe for oil cylinders and the wall thickness of the steel pipe for oil cylinders are directly related in a specific manner. The ferrite content at the t / 2 point of the wall thickness of the steel pipe for oil cylinders is in the range of 0.5t to 1.0t%, and the ferrite content in the microstructure of the inner wall is in the range of 1.5t to 2.0t%. If the ferrite content is too low, the yield ratio becomes too high, the residual stress becomes too large, the safety of use decreases, and the risk of cracks occurring in the inner wall during water quenching increases. If the ferrite content is too high, the strength of the steel pipe for oil cylinders becomes too low and the requirements for use cannot be met. In addition, if the wall thickness is large, if sufficient ferrite is not precipitated, the residual stress of the steel pipe for oil cylinders increases, and there is a strong tendency for cracks to occur in the inner wall.
[0032] In another aspect, the present invention provides a method for producing a steel pipe for an oil cylinder as described above, comprising the steps of: (1) Smelting and casting process: a process of smelting and casting molten steel having the above-mentioned elemental composition to obtain a cast billet; (2) heating the cast billet; (3) drilling holes into the heated cast billet; (4) A process of continuously rolling the pierced cast billet to obtain a steel pipe; (5) forced air cooling and reheating of the steel pipe; (6) Step of tension reduction and cooling of the reheated steel pipe: After tension reduction (i.e., diameter reduction by stretch reducing) of the reheated steel pipe, only the outer wall of the steel pipe is water-cooled (i.e., the inner wall of the steel pipe is not water-cooled in this step), and the cooling start temperature of the steel pipe is set to ≧Ar 3 The cooling end temperature of the steel pipe is controlled to ≧B f And ≦B s a step of controlling the temperature to −100° C. and controlling the cooling rate to be in the range of 25 to 35° C. / s; (7) straightening the cooled steel pipe; (8) Quenching the straightened steel pipe: The straightened steel pipe is quenched with Ac 3+30~Ac 3 +60℃ (i.e., quenching temperature is Ac 3 +30≦and≦Ac 3 After quenching, the steel pipe is rotated and cooled stepwise by water cooling. First, water is sprayed on the outside, then Ar 3 -70℃≦Inner wall temperature≦Ar 3 When the temperature falls below -30℃, inject water into the steel pipe from one end until the inner bore of the steel pipe is filled with cooling water, and then cool the steel pipe to room temperature; (9) tempering the quenched steel pipe; and (10) The process of straightening the steel pipes after they are discharged from the furnace to obtain steel pipes for oil cylinders. The present invention provides a method comprising:
[0033] Preferably, in step (2), the heating is carried out at a temperature of 1250 to 1280° C. for 3 to 4 hours.
[0034] Preferably, in step (3), the piercing is carried out at a temperature of 1100 to 1230°C.
[0035] Preferably, in step (4), the finish rolling is carried out at a temperature of 900 to 1000°C.
[0036] Preferably, in step (5), the steel pipe is treated with Ar 3 Cool by forced air to below -50℃, then reheat to 950~980℃.
[0037] Preferably, in step (6), the tension drawing is carried out at a temperature of 850 to 900°C.
[0038] Preferably, in step (7), the straightened steel pipe is naturally cooled to room temperature.
[0039] Preferably, in step (9), the tempering is carried out at a temperature of (550-2×t)° C.
[0040] Preferably, in step (10), straightening is carried out at a temperature of ≧400° C.
[0041] By designing the composition of a steel pipe for oil cylinders and controlling the cooling process during water quenching, the present invention makes it possible to reduce the residual stress in the steel pipe for oil cylinders and improve the usage performance of the steel pipe for oil cylinders without adding any additional manufacturing processes.
[0042] After the steel pipe is tension-drawn at 850 to 900°C, only the outer wall of the steel pipe is water-cooled, and the cooling start temperature is set to ≧Ar 3 and the cooling end temperature is controlled to ≧B f And ≦B s Controlled at -100℃ (here, B f is the temperature at the end of the bainite phase transformation during the cooling process, and B s is the temperature at which the phase change of bainite begins in the cooling process. ) In the cooling process, the cooling rate is controlled to be 25-35°C / s. The main purpose of this process is to rapidly cool and harden the steel tube by uniform cooling. This allows the steel tube to have a straightness of 2mm / m or less, preferably less than 1.5mm / m, and at the same time refines the as-rolled structure, laying the foundation for a good balance of performance after subsequent tempering. Moreover, this cooling reduces the residual stress level in the as-rolled state.
[0043] The steel tube is immediately straightened after being rapidly cooled to the finishing cooling temperature. The temperature straightening helps to ensure the straightness and at the same time reduces the residual stress level in the rolled state, so that the straightness of the straightened steel tube is less than 2 mm / m, preferably less than 1.5 mm / m. The steel tube is then sent onto a cooling bed to cool naturally to room temperature.
[0044] The steel pipe of the present invention is cooled stepwise by water cooling after quenching, and rotated during the cooling process. During cooling, the outer wall of the steel pipe is first cooled by external water spraying, and then cooled by Ar 3 -70℃≦Inner wall temperature≦Ar 3 When the temperature drops below -30°C, the internal water sprinkler is turned on to inject water into the steel pipe, cooling the inner wall of the steel pipe until the inner bore of the steel pipe is filled with cooling water, and the steel pipe is cooled to room temperature.
[0045] The present invention performs cooling on a steel tube for an oil cylinder by a stepwise cooling process based on the following principle.
[0046] 1) The entire length of the steel pipe is cooled simultaneously by external water spraying, so the cooling uniformity is good. When cooling the inner wall of the steel pipe, one end of the steel pipe is cooled first, and the other end is cooled later, so the rigidity of the steel pipe is increased, and the good cooling uniformity can better ensure the straightness level of the steel pipe, and avoid the large residual stress caused by the straightening deformation due to the subsequent bending of the pipe.
[0047] 2) The residual stress of the steel pipe is closely related to the phase change and thermal stress in the cooling process. Through stepwise cooling, the distribution of phase change and thermal stress throughout the wall thickness of the steel pipe can be effectively controlled, the phase change stress and thermal stress of martensite can be mutually eliminated, and the residual stress level of the steel pipe can be effectively reduced. In the technical solution of the present invention, by using a stepwise cooling method of external water spraying followed by internal water spraying, the phase change stress is tensile stress and the thermal stress is compressive stress for the outer wall of the steel pipe, and the phase change stress is compressive stress and the thermal stress is tensile stress for the center of the steel pipe, and the two can be offset each other.
[0048] 3) The cooling transformation structure of the inner wall partially precipitates ferrite instead of a complete martensite structure, so that the residual stress of the inner wall can be effectively reduced. In the technical solution of the present invention, the phase change stress and thermal stress of the inner wall are both tensile stresses, but the inner wall is a surface that is cooled later. The cooling of the inner wall is performed by cooling with external water spraying, followed by Ar 3 -70℃≦Inner wall temperature≦Ar 3 It starts when the temperature drops to -30°C. At this time, ferrite structure is precipitated on the inner wall, the transformation ratio of martensite structure is reduced, and the phase change stress on the inner wall is reduced. Therefore, the residual stress level on the inner wall is effectively reduced, and cracks do not occur on the inner wall.
[0049] In the present invention, rapid cooling is adopted in the cooling process after tension drawing to increase the hardness and uniformity of the steel pipe for oil cylinders and reduce the residual stress level of the steel pipe for oil cylinders in the rolled state. In addition, by performing stepwise cooling after quenching, a cooling rate gradient is formed in the wall thickness direction. In the cooling process, the outer wall is cooled first, and then the center and inner wall are cooled. The cooling rate of the center and inner wall is slower than that of the outer wall. The transformation of ferrite structure occurs first, and then the transformation of martensite occurs. As it approaches the inner wall, the cooling rate gradually slows down, and the amount of ferrite precipitation increases. In addition, as the wall thickness of the steel pipe for oil cylinders increases, the cooling rate of the center and inner wall is further reduced, which promotes the precipitation of ferrite, and the amount of ferrite precipitation increases accordingly.
[0050] Ar 3 -70℃≦Inner wall temperature≦Ar 3 When the temperature drops to -30°C, water is injected into the inner wall to cool it. At this time, ferrite structures have precipitated on the inner wall, and the rate of transformation of martensite structures decreases. Therefore, the residual stress level within 1 mm from the inner wall is effectively reduced.
[0051] The present invention controls the precipitation of ferrite in the microstructure of the steel pipe for oil cylinder by a stepwise cooling process, and the ferrite content is higher near the inner wall. Since ferrite has good ductility and toughness, the residual stress of the inner wall of the steel pipe for oil cylinder can be well controlled during cooling, and the inner wall will not crack during the water quenching process.
[0052] The present invention provides the following beneficial effects:
[0053] In the composition design of the steel pipe for oil cylinders of the present invention, the contents of C, Si and Mn are controlled to improve the hardenability of the steel pipe for oil cylinders, and prevent cracks from occurring on the inner wall of the steel pipe for oil cylinders in the subsequent stepwise cooling process. Meanwhile, the contents of Nb and Mo are controlled to control the distribution of ferrite in the steel pipe for oil cylinders, and thus prevent further cracks from occurring on the inner wall in the stepwise cooling process.
[0054] Also, depending on the wall thickness of the steel pipe for oil cylinders, Ti and B may be added to improve hardenability. This makes it possible to avoid a significant increase in the ferrite content from the t / 2 point to the inner wall, which would result in a decrease in strength, when the wall thickness of the steel pipe for oil cylinders is 20 mm or more.
[0055] According to the present invention, after tension drawing and quenching are performed on the steel tube based on the composition design, different stepwise cooling processes are adopted. On the one hand, the rigidity and straightness of the steel tube are increased, so that the large residual stress caused by the subsequent bending deformation of the tube is avoided. On the other hand, the distribution of phase change and thermal stress throughout the wall thickness of the steel tube for oil cylinders can be controlled, so that the mutual elimination of martensite phase change stress and thermal stress can be realized, and the residual stress level of the steel tube can be effectively reduced. Finally, the distribution of ferrite in the microstructure of the steel tube for oil cylinders is reduced, so that the phase change stress in the inner wall is effectively reduced, and the residual stress level of the inner wall is prevented from cracking. As a result, a steel tube for oil cylinders with high strength and low residual stress is obtained. The yield strength of the steel tube for oil cylinders is 600 MPa or more, the tensile strength is 730 MPa or more, and the residual stress is 0 MPa or more and 50 MPa or less. [Brief description of the drawings]
[0056] [Figure 1] 1 is a photograph showing the residual stress of a steel pipe for oil cylinders manufactured in Comparative Example 1 of the present invention, measured by the slit method. [Diagram 2]1 is a photograph showing the residual stress of a steel pipe for oil cylinders manufactured in Example 1 of the present invention, measured by the slit method. [Diagram 3] 1 is a photograph of the metal structure of the outer wall surface of a steel pipe for an oil cylinder according to Example 1 of the present invention. [Figure 4] 1 is a photograph of the metal structure at a point of 1 / 2 the wall thickness of a steel pipe for oil cylinders in Example 1 of the present invention. [Diagram 5] 1 is a photograph of the metal structure of the inner wall surface of a steel pipe for an oil cylinder according to Example 1 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0057] The present invention will now be further described with reference to examples.
[0058] The steel pipes for oil cylinders of Examples 1 to 8 of the present invention were manufactured according to the above-mentioned method. The steel pipes for oil cylinders of Comparative Examples 1 to 8 were manufactured by substantially the same method as that of Examples 1 to 8, but one or more of the elemental compositions and / or manufacturing process parameters of Comparative Examples 1 to 8 were not included in the scope of protection of the present invention.
[0059] Table 1 shows the chemical compositions of Examples 1 to 8 of the present invention and Comparative Examples 1 to 8.
[0060] Specific manufacturing process parameters for Examples 1 to 8 of the present invention and Comparative Examples 1 to 8 are shown in Table 2. In step (1), molten steel was smelted and cast to obtain a cast billet according to the element composition shown in Table 1. In step (7), the treated steel pipe obtained in step (6) was straightened, and the straightened steel pipe was naturally cooled to room temperature.
[0061] Table 3 shows the performance parameters of the steel pipes for oil cylinders obtained in Examples 1 to 8 of the present invention and Comparative Examples 1 to 8.
[0062] In this application, the yield strength and tensile strength are measured according to GB / T228, and the residual stress is measured according to ISO / TR10400 standard.
[0063] 1 and 2 are photographs showing the measurement of the residual stress by the slit method of the steel pipe for oil cylinders produced in Comparative Example 1 and Example 1 of the present invention, respectively. As can be seen from the figures, it is clear that the residual stress of the steel pipe for oil cylinders of the present invention is significantly smaller than the residual stress of the conventional steel pipe for oil cylinders, the slit of the seamless pipe obtained by the method of the present invention is smaller than the slit of the seamless pipe produced by the conventional process, and the residual stress of the seamless pipe obtained by the present invention (e.g., Example 1) is significantly smaller than the residual stress of the seamless pipe produced by the conventional process (e.g., Comparative Example 1).
[0064] Figures 3 to 5 are photographs of the metal structure of each part of the steel pipe for oil cylinders of the present invention. As can be seen from the photographs, the metal structure from the outer wall to the t / 2 point was tempered sorbite, and at the t / 2 point, ferrite structure was precipitated at a ratio of t%. The ferrite was distributed with a gradient from the t / 2 point to the inner wall. The ferrite content increased as the distance to the inner wall approached. The ferrite content in the metal structure of the inner wall reached 2t%.
[0065] As can be seen from Table 3, the inner wall of the steel pipe for oil cylinders obtained by the present invention is free of cracks, and the residual stress is less than 50 MPa, and the residual stress can even be reduced to zero.
[0066] Since one or more of the elemental composition and / or manufacturing process parameters were not included in the scope of protection of the present invention, the steel pipes for oil cylinders obtained in Comparative Examples 1 to 8 exhibited higher residual stress and may even have cracks on the inner wall. When the wall thickness was more than 20 mm, the steel pipes for oil cylinders in Comparative Examples 4 and 5 did not contain Ti and B elements, so that although the residual stress of the steel pipes for oil cylinders was low, the strength of the steel pipes for oil cylinders did not meet the requirements of the present invention.
[0067] In summary, the present invention provides a steel pipe for oil cylinders with superior overall performance compared to the prior art by designing the chemical element composition of the steel pipe for oil cylinders in combination with a specific manufacturing process.
[0068]
Table 1
[0069]
Table 2
[0070]
Table 3
Claims
1. A steel pipe for oil cylinders further containing, in addition to 90% by weight or more of Fe and unavoidable impurities, the following chemical elements, by weight: C: 0.16-0.3%, Si: 0.15-0.5%, Mn: 1.2-1.8%, Nb: 0.02-0.04%, Mo: 0.1-0.2%, and optionally Ti: 0.015-0.03%, and B: 0.0015-0.0035%.
2. 2. The steel pipe for oil cylinders according to claim 1, containing, by weight, the following chemical elements: C: 0.16-0.3%, Si: 0.15-0.5%, Mn: 1.2-1.8%, Nb: 0.02-0.04%, Mo: 0.1-0.2%, optionally Ti: 0.015-0.03% and B: 0.0015-0.0035%, with the balance being Fe and unavoidable impurities.
3. 3. The steel pipe for oil cylinders according to claim 1 or 2, wherein the wall thickness of the steel pipe for oil cylinders is 20 mm or more, and the steel pipe for oil cylinders contains Ti: 0.015 to 0.03% and B: 0.0015 to 0.0035%.
4. 4. A steel pipe for oil cylinders according to claim 1, wherein in the wall thickness direction of the steel pipe for oil cylinders, the microstructure from the outer wall to the t / 2 point is tempered sorbite, and the microstructure from the t / 2 point to the inner wall is tempered sorbite + ferrite, the ferrite is distributed with a gradient, the ferrite content increases as the distance to the inner wall decreases, the ferrite content in the microstructure at the t / 2 point is 3% or more, and the ferrite content in the microstructure at the inner wall is 5% or more, where t is the wall thickness (mm) of the steel pipe for oil cylinders.
5. The steel pipe for oil cylinders according to any one of claims 1 to 4, wherein the steel pipe for oil cylinders has a yield strength of 600 MPa or more, a tensile strength of 730 MPa or more, and a residual stress of 50 MPa or less, preferably 40 MPa or less, and preferably the steel pipe for oil cylinders has a yield ratio of 0.92 or less.
6. 6. A steel pipe for oil cylinders according to claim 1, wherein the ferrite content in the microstructure at the t / 2 point of the steel pipe for oil cylinders is 0.5t to 1.0t%.
7. The steel pipe for oil cylinders according to any one of claims 1 to 6, wherein the ferrite content in the microstructure in the inner wall of the steel pipe for oil cylinders is 1.5t to 2.0t%.
8. The steel pipe for oil cylinders according to any one of claims 1 to 7, wherein the wall thickness of the steel pipe for oil cylinders is 9 mm or more.
9. A method for producing a steel pipe for oil cylinders according to any one of claims 1 to 8, (1) Smelting and casting step: smelting and casting a molten steel having the elemental composition according to claim 1 to obtain a cast billet; (2) heating the cast billet; (3) piercing the heated cast billet; (4) A step of continuously rolling the pierced cast billet to obtain a steel pipe; (5) Forced air cooling and reheating the steel pipe; (6) A step of tension drawing and cooling the reheated steel pipe: After the tension drawing, the outer wall of the steel pipe is water-cooled, and the cooling start temperature of the steel pipe is set to ≧Ar 3 and the cooling end temperature of the steel pipe is controlled to ≧B f And ≦B s a step of controlling the temperature at −100° C. and controlling the cooling rate to be in the range of 25 to 35° C. / s; (7) A step of straightening the cooled steel pipe; (8) A step of quenching the straightened steel pipe: the quenching temperature is Ac 3 +30≦and≦Ac 3 After the quenching, the steel pipe is rotated and gradually cooled by water cooling. The water cooling is first performed by spraying water on the outside, and then by cooling with Ar. 3 -70℃≦Inner wall temperature≦Ar 3 When the temperature falls below −30° C., injecting water into the steel pipe from one end until the inner bore of the steel pipe is filled with cooling water, thereby cooling the steel pipe to room temperature; (9) tempering the quenched steel pipe; and (10) A process of straightening the steel pipe after it is discharged from the furnace to obtain the steel pipe for oil cylinders. The method includes:
10. The following conditions: In step (2), the heating is carried out at a temperature of 1250 to 1280° C. for 3 to 4 hours; In step (3), the piercing is carried out at a temperature of 1100 to 1230°C; In step (4), the finish rolling is carried out at a temperature of 900 to 1000°C; In step (5), the steel pipe is 3 Forced air cooling to below -50°C, then reheating to 950-980°C; In step (6), the tension drawing is carried out at a temperature of 850 to 900°C; In step (7), the straightened steel pipe is naturally cooled to room temperature; In step (9), the tempering is performed at a temperature of (550-2×t)° C.; and In step (10), the straightening is carried out at a temperature of ≧400° C. The method according to claim 9 , wherein one or more of the following is satisfied:
Citation Information
Patent Citations
High-strength and high-toughness N80Q petroleum casing pipe and manufacturing method thereof
CN105925883A
Oil sleeve resistant to carbon dioxide corrosion and manufacturing method thereof
CN108004461A
Manufacture of high strength resistance welded tube for automobile use hardly causing softening in heat affected zone
JP1990197525A
Method for producing seamless steel tube
JP2008221250A
Seamless precision steel pipe for hydraulic cylinders with improved isotropic toughness at low temperature and method for obtaining same
JP2009541589A