Binders, electrode mixtures, and electrodes
A tailored binder for non-aqueous electrolyte secondary batteries, using specific vinylidene fluoride polymers, addresses viscosity and flexibility issues, ensuring stable production and increased capacity by suppressing slurry thickening and maintaining electrode integrity.
Patent Information
- Application Number
- JP2024547804
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-12-28
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2041-12-28
AI Technical Summary
Existing vinylidene fluoride polymers used in non-aqueous electrolyte secondary battery electrodes tend to increase viscosity, leading to handling issues during production and potential electrode cracking or current collector breakage due to increased thickness, which limits the capacity and flexibility of the batteries.
A binder comprising specific vinylidene fluoride polymers with controlled turbidity, dissolution rate, inherent viscosity, and infrared absorption spectrum ratios, along with a blend of polymers with varying hexafluoropropylene content, is used to suppress slurry thickening and enhance electrode flexibility.
The proposed binder effectively prevents electrode mixture thickening and ensures flexibility, reducing the risk of cracking and improving handling properties during battery production, thereby enhancing the capacity and safety of non-aqueous electrolyte secondary batteries.
Smart Images

Figure 2024542289000001 
Figure 2024542289000002 
Figure 2024542289000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a binder, an electrode mixture, and an electrode. [Background technology]
[0002] There is a demand for high capacity electrodes for non-aqueous electrolyte secondary batteries. For example, by using a binder (binding agent) with high binding properties, the amount of binder in the electrode can be reduced. In addition, the amount of active material can be increased with the reduction in the amount of binder in the electrode, so that the capacity of the non-aqueous electrolyte secondary battery can be increased.
[0003] Currently, vinylidene fluoride polymers that mainly contain repeating units derived from vinylidene fluoride (VDF) are mainly used as the binder.
[0004] As an example of such a binder, Patent Document 1 describes a vinylidene fluoride polymer obtained by copolymerizing vinylidene fluoride with a specific compound, and also describes that the vinylidene fluoride polymer has excellent adhesiveness to metal foil. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2012 / 090876 Summary of the Invention [Problem to be solved by the invention]
[0006] In order to increase the capacity of non-aqueous electrolyte secondary batteries, a method of increasing the thickness of the electrode and increasing the amount of active material mounted on the electrode has been carried out. When an electrode with increased thickness is produced using a vinylidene fluoride polymer as described in Patent Document 1, the electrode is likely to become hard. For example, when the electrode is deformed by rolling or the like to fit into a cylindrical can, or when a wound electrode is deformed by pressing to fit into a rectangular can, the electrode may crack and / or the current collector may break.
[0007] In addition, the viscosity of the electrode mixture slurry containing the vinylidene fluoride polymer as described in Patent Document 1 is likely to increase, and the viscosity of the vinylidene fluoride polymer may become high at the stage of coating with the current collector. If the viscosity of the electrode mixture is high, problems may occur in terms of handling during battery production.
[0008] Thus, there is a need for further improvements in vinylidene fluoride polymers for use in binders.
[0009] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide a binder that can suppress thickening of an electrode mixture slurry and provide an electrode having flexibility. [Means for solving the problem]
[0010] As a result of intensive research, the present inventors have found that a binder that satisfies certain requirements can provide a flexible electrode. They have also found that an increase in the viscosity of an electrode mixture slurry containing the binder can be suppressed, and have completed the present invention.
[0011] A binder according to one embodiment of the present invention is a binder that contains at least one vinylidene fluoride polymer and satisfies the following requirements (A) to (E): (A) the turbidity of an N-methylpyrrolidone solution containing 5% by mass of the binder at 25°C is 5.0 or less; (B) in a binder solution obtained by adding 6 parts by mass of the binder to 94 parts by mass of a 95% by mass aqueous acetone solution and stirring at 30°C for 2 hours, the solubility of the binder as represented by the following formula (1) is 10% or more and 70% or less: Dissolution rate (%) = ((input amount - undissolved substance amount) / input amount) × 100 (1) (C) the inherent viscosity of the dissolved components of the binder solution is 0.5 dL / g or more and less than 2.5 dL / g; (D) 1735 cm of the dissolved components of the binder solution -1 Infrared absorption spectrum absorbance A at 1735cm -1 And, 3025cm -1 Infrared absorption spectrum absorbance A3025cm -1 Ratio to A1735cm -1 / A3025cm -1 is greater than or equal to 0.20 and less than or equal to 0.80; and (E) the inherent viscosity of the binder is greater than the inherent viscosity of the dissolved components of the binder solution.
[0012] A binder according to one embodiment of the present invention contains a first vinylidene fluoride polymer having a constituent unit derived from vinylidene fluoride as a main constituent component and optionally containing a constituent unit derived from hexafluoropropylene, and a second vinylidene fluoride polymer containing a constituent unit derived from vinylidene fluoride, a constituent unit derived from hexafluoropropylene, and a constituent unit containing a polar functional group; the first vinylidene fluoride polymer has an inherent viscosity of 2.5 dL / g or more and 6.0 dL / g or less, and a content of structural units derived from hexafluoropropylene in all structural units of the first vinylidene fluoride polymer is 0 mass% or more and less than 0.5 mass%, the second vinylidene fluoride polymer has an inherent viscosity of 0.5 dL / g or more and less than 2.5 dL / g, and the content of structural units derived from hexafluoropropylene in all structural units of the second vinylidene fluoride polymer is 6% by mass or more and 40% by mass or less; The second vinylidene fluoride polymer has a peak at 1735 cm -1Infrared absorption spectrum absorbance A at 1735cm -1 And, 3025cm -1 Infrared absorption spectrum absorbance A3025cm -1 Ratio to A1735cm -1 / A3025cm -1 is 0.20 or more and 0.80 or less, The mass ratio of the second vinylidene fluoride polymer to the first vinylidene fluoride polymer (second vinylidene fluoride polymer / first vinylidene fluoride polymer) in the binder is 3 / 7 or more and 7 / 3 or less. Effect of the Invention
[0013] The binder according to one aspect of the present invention can suppress thickening of the electrode mixture slurry, and can provide an electrode having flexibility. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, one embodiment of the present invention will be described in detail.
[0015] <Binder> The binder according to the present embodiment is a binder used to bind an electrode active material to a current collector in an electrode in which an electrode mixture layer containing an electrode active material is formed on a current collector. The binder according to the present embodiment contains at least one vinylidene fluoride polymer.
[0016] (Vinylidene fluoride polymer) In terms of obtaining a flexible electrode, the vinylidene fluoride polymer is preferably a copolymer of a constituent unit derived from vinylidene fluoride and a constituent unit derived from another monomer. A flexible electrode can be evaluated, for example, by whether or not the electrode breaks when a force such as bending is applied to the electrode.
[0017] The other monomer may be one or more. The other monomer may or may not contain fluorine. Specific examples of the other monomer include fluorine-containing monomers (e.g., vinyl fluoride, trifluoroethylene, tetrafluoroethylene, chlorotrifluoroethylene, hexafluoropropylene, perfluoroalkyl vinyl ether), ethylene, unsaturated dibasic acid derivatives (e.g., monomethyl maleate, dimethyl maleate), vinyl acetate, (meth)acrylamide, (meth)dimethylacrylamide, allyl glycidyl ether, (meth)acrylic acid alkyl compounds (e.g., methyl (meth)acrylate), carboxyl group-containing acrylate compounds (e.g., (meth)acrylic acid, 2-carboxyethyl acrylate, (meth)acryloyloxypropyl succinic acid, (meth)acryloyloxyethyl succinic acid), 2-hydroxyethyl acrylate, and hydroxypropyl acrylate.
[0018] From the viewpoint of obtaining an electrode having flexibility, the other monomer is preferably a fluorine-containing monomer or a monomer containing a polar functional group. The fluorine-containing monomer is more preferably hexafluoropropylene (HFP). The monomer containing a polar functional group is more preferably an unsaturated dibasic acid derivative. Furthermore, the other monomer is more preferably a monomer containing a polar functional group and HFP.
[0019] In the case of containing a vinylidene fluoride polymer containing a structural unit derived from HFP, when the total structural units of the vinylidene fluoride polymer contained in the binder according to the present embodiment are taken as 100% by mass, the ratio of the structural units derived from HFP is preferably 3% by mass or more, more preferably 3.5% by mass or more. In addition, the ratio of the structural units is preferably 15% by mass or less, more preferably 6.5% by mass or less. Within the above range, an electrode having flexibility and being less likely to break can be provided. Here, "all structural units of the vinylidene fluoride polymer contained in the binder" means the sum of all structural units of the vinylidene fluoride polymer, including the structural units of the vinylidene fluoride polymer not containing a structural unit derived from HFP, when the binder contains a vinylidene fluoride polymer not containing a structural unit derived from HFP in addition to the vinylidene fluoride polymer containing a structural unit derived from HFP (i.e., when the binder contains a plurality of vinylidene fluoride polymers).
[0020] The ratio of each structural unit of vinylidene fluoride polymer is 1 H NMR spectrum or 19 It can be determined by F NMR spectroscopy or neutralization titration.
[0021] In the case of containing a vinylidene fluoride polymer containing a structural unit derived from HFP, when the total structural units of the vinylidene fluoride polymer contained in the dissolved components of the binder solution (a solution obtained by adding 6 parts by mass of the binder to 94 parts by mass of a 95% by mass aqueous acetone solution and stirring at 30° C. for 2 hours) are taken as 100% by mass, the proportion of the structural units derived from HFP contained in the dissolved components of the binder solution is preferably 5% by mass or more, more preferably 6% by mass or more. In addition, the proportion of the structural units is preferably 40% by mass or less, more preferably 15% by mass or less. If it is within the above range, it is possible to provide an electrode having flexibility that is unlikely to break. In this specification, the binder solution is prepared separately using the binder according to this embodiment in order to show the physical properties of the binder according to this embodiment.
[0022] In terms of further suppressing thickening of the slurry of the electrode mixture and further enabling the provision of an electrode having sufficient flexibility such that electrode breakage is unlikely to occur, it is more preferable that the proportion of structural units derived from HFP among all structural units of the vinylidene fluoride polymer is 3 mass% or more and 15 mass% or less, and that the proportion of structural units derived from HFP among all structural units of the vinylidene fluoride polymer contained in the dissolved components of the binder solution is 5 mass% or more and 40 mass% or less.
[0023] As the vinylidene fluoride polymer, a commercially available vinylidene fluoride polymer may be used. Examples of the method for producing the vinylidene fluoride polymer include polymerization methods such as suspension polymerization, mini-emulsion polymerization, and solution polymerization. Among these, suspension polymerization is preferred from the viewpoint of reducing impurities.
[0024] (Physical properties of binder) The binder according to the present embodiment satisfies the following requirements (A) to (E). By satisfying the requirements (A) to (E), it is possible to suppress thickening of the electrode mixture slurry. In addition, by satisfying the requirements (A) to (E), it is possible to obtain an electrode having flexibility.
[0025] [Requirement (A): Turbidity of NMP solution containing binder] Requirement (A): The turbidity of the binder according to this embodiment in an N-methylpyrrolidone solution (NMP solution) containing 5% by mass of the binder at 25° C. is 5.0 or less.
[0026] If the turbidity is greater than 5.0, thickening of the electrode mixture slurry cannot be suppressed, and therefore, from this viewpoint, the turbidity is preferably 4.0 or less, and more preferably 3.5 or less.
[0027] The turbidity of the binder can be determined by a known method for measuring turbidity, for example, by integrating sphere photoelectric photometry.
[0028] [Requirement (B): Dissolution rate of binder] Requirement (B): The dissolution rate of the binder according to this embodiment, measured by the following measurement method, is 10% or more and 70% or less.
[0029] (Method of measuring binder dissolution rate) 6 parts by mass of binder is added to 94 parts by mass of 95% by mass acetone aqueous solution, and the mixture is stirred at 30°C for 2 hours to obtain a binder solution. The binder solution is filtered to separate the undissolved matter from the dissolved liquid. The solvent contained in the undissolved matter is then dried and removed, and the mass is measured. The dissolution rate of the binder is then calculated using the following formula (1). Dissolution rate (%) = ((input amount - undissolved substance amount) / input amount) × 100 (1)
[0030] In this specification, the term "dissolved component of the binder solution" refers to a component obtained by reprecipitating a vinylidene fluoride polymer from a solution obtained by removing undissolved matter from the binder solution by a process such as filtration.
[0031] The dissolution rate of the binder is preferably 10% or more and 70% or less, so that the flexibility of the electrode can be improved. From this viewpoint, the dissolution rate of the binder is preferably 30% or more. Also, the dissolution rate is preferably 50% or less.
[0032] [Requirement (C): Inherent viscosity of the dissolved components of the binder solution] Requirement (C): The inherent viscosity of the dissolved components of the binder solution is 0.5 dL / g or more and less than 2.5 dL / g.
[0033] By having the inherent viscosity of 0.5 dL / g or more and less than 2.5 dL / g, thickening of the electrode mixture slurry can be suppressed, and an electrode having flexibility can be provided. From this viewpoint, the inherent viscosity of the dissolved component of the binder solution is preferably 1.0 dL / g or more. In addition, the inherent viscosity is preferably 2.2 dL / g or less.
[0034] The inherent viscosity can be determined using a known viscometer such as an Ubbelohde viscometer.
[0035] [Requirement (D): IR spectrum ratio of dissolved components in binder solution] Requirement (D): 1735 cm of the soluble components of the binder solution -1 Infrared absorption spectrum (IR spectrum) absorbance A1735cm -1 And, 3025cm -1 Absorbance of IR spectrum at A3025cm -1 Ratio to A1735cm -1 / A3025cm -1 is greater than 0.20 and less than 0.80.
[0036] 1735cm -1 The absorbance in the IR spectrum at 3025cm is due to the stretching vibration of the carbonyl group. -1 The absorbance in the IR spectrum is due to the stretching vibration of CH. Therefore, A1735cm -1 / A3025cm -1 is a measure of the amount of carbonyl groups present in the vinylidene fluoride polymer.
[0037] A1735cm -1 / A3025cm -1 By being within the above range, it is possible to suppress the thickening of the electrode mixture slurry. -1 / A3025cm -1 is preferably 0.25 or more. -1 / A3025cm -1 is preferably 0.4 or less.
[0038] The IR spectrum absorbance of the dissolved components of the binder solution can be determined by a known method using, for example, an infrared spectrophotometer.
[0039] [Requirement (E): Inherent viscosity of binder] Requirement (E): The inherent viscosity of the binder is greater than the inherent viscosity of the dissolved components of the binder solution.
[0040] The requirement (E) makes it possible to suppress thickening of the electrode mixture slurry and further to provide a flexible electrode.
[0041] The inherent viscosity of the binder is preferably 2.0 dL / g or more, more preferably 2.5 dL / g or more, from the viewpoint of suppressing thickening of the electrode mixture slurry, and is preferably 5.0 dL / g or less, more preferably 4.5 dL / g or less.
[0042] Preferred embodiments of the physical properties of the binder other than the above requirements (A) to (E) are shown below.
[0043] The binder according to the present embodiment preferably has at least one crystallization peak (Tc) in the range of 85° C. or more and less than 125° C. and in the range of 125° C. or more and 150° C. or less when a first temperature drop measurement is performed using a differential scanning calorimeter under conditions of 10° C. / min. This configuration makes it possible to suppress thickening of the electrode mixture slurry and provide an electrode having flexibility.
[0044] Tc can be confirmed by a differential scanning calorimeter (DSC) from the presence or absence of a peak in the DSC curve during the first temperature drop process when a temperature rise-lowering cycle is carried out under conditions of 10° C. / min.
[0045] <Binder containing two or more types of vinylidene fluoride polymer> A binder according to another embodiment of the present invention contains two or more kinds of vinylidene fluoride polymers. Hereinafter, a binder containing two or more kinds of vinylidene fluoride polymers may be referred to as a "blend binder."
[0046] The blend binder includes a vinylidene fluoride polymer having vinylidene fluoride as its main constituent component (hereinafter, sometimes referred to as a first vinylidene fluoride polymer), and a copolymer of a constituent unit derived from vinylidene fluoride and a constituent unit derived from another monomer, which is different from the first vinylidene fluoride polymer (hereinafter, referred to as a second vinylidene fluoride polymer).
[0047] [First vinylidene fluoride polymer] In this specification, "containing vinylidene fluoride as a main component" refers to a polyvinylidene fluoride resin containing 50% by mass or more of constituent units derived from vinylidene fluoride. A vinylidene fluoride polymer containing vinylidene fluoride as a main component may be a homopolymer of vinylidene fluoride containing substantially 100% by mass of constituent units derived from vinylidene fluoride. In addition, a vinylidene fluoride polymer containing vinylidene fluoride as a main component may optionally contain a constituent unit derived from HFP.
[0048] The proportion of the structural units derived from HFP in the total structural units of the first vinylidene fluoride polymer is preferably less than 0.1% by mass, more preferably 0.05% by mass or less. Within the above range, thickening of the electrode mixture slurry is further suppressed, and further, an electrode having sufficient flexibility that is unlikely to break can be provided.
[0049] The first vinylidene fluoride polymer has an inherent viscosity of 2.5 dL / g or more, preferably 3.0 dL / g or more. Also, the inherent viscosity is 6.0 dL / g or less, preferably 4.5 dL / g or less. When the viscosity is within the above range, the thickening of the electrode mixture slurry is further suppressed, and further, an electrode having sufficient flexibility that is unlikely to break can be provided.
[0050] The first vinylidene fluoride polymer has a ratio of structural units derived from HFP to all structural units of the first vinylidene fluoride polymer of 0% by mass or more and less than 0.5% by mass, and has an inherent viscosity of 2.5 dL / g or more and 6.0 dL / g or less. This configuration further suppresses the increase in viscosity of the electrode mixture slurry, and further provides an electrode having sufficient flexibility that is unlikely to break.
[0051] [Second vinylidene fluoride polymer] The preferred embodiments of the other monomers in the second vinylidene fluoride polymer are as described above. By including a structural unit derived from vinylidene fluoride, a structural unit derived from HFP, and a structural unit containing a polar functional group, it is possible to provide an electrode having sufficient flexibility that is unlikely to break.
[0052] When the second vinylidene fluoride polymer contains a structural unit derived from HFP, the proportion of the structural unit derived from HFP in the total structural units of the second vinylidene fluoride polymer is 6% by mass or more, preferably 6.5% by mass or more. Also, the proportion of the structural unit is 40% by mass or less, preferably 20% by mass or less. Within the above range, the thickening of the electrode mixture slurry is further suppressed, and further, an electrode having sufficient flexibility that is unlikely to break can be provided.
[0053] The second vinylidene fluoride polymer has an inherent viscosity of 0.5 dL / g or more, preferably 1.0 dL / g or more. Also, the inherent viscosity is less than 2.5 dL / g, preferably 2.3 dL / g or less. When the viscosity is within the above range, the thickening of the electrode mixture slurry is further suppressed, and further, an electrode having sufficient flexibility that is unlikely to break can be provided.
[0054] The second vinylidene fluoride polymer has a proportion of HFP-derived structural units in all structural units of the second vinylidene fluoride polymer of 6% by mass or more and 40% by mass or less, and has an inherent viscosity of 0.5 dL / g or more and less than 2.5 dL / g, so that the thickening of the electrode mixture slurry is further suppressed, and further, an electrode having sufficient flexibility that is less likely to break can be provided.
[0055] 1735cm of the second vinylidene fluoride polymer -1 Absorbance of IR spectrum at 1735cm -1 And, 3025cm -1 Absorbance of IR spectrum at A3025cm -1 Ratio to A1735cm -1 / A3025cm-1 is 0.20 or more, and preferably 0.25 or more. -1 / A3025cm -1 is preferably 0.80 or less and less than 0.4. By being within the above range, thickening of the electrode mixture slurry can be suppressed.
[0056] In the blend binder, the mass ratio of the second vinylidene fluoride polymer to the first vinylidene fluoride polymer (second vinylidene fluoride polymer / first vinylidene fluoride polymer) is 3 / 7 or more, and preferably 4 / 6. Also, the mass ratio is 7 / 3 or less. By being within the above range, thickening of the electrode mixture slurry is further suppressed, and further, an electrode having sufficient flexibility that is unlikely to break can be provided.
[0057] The form of the binder according to the present embodiment is not particularly limited, and may be in powder form or liquid form.
[0058] <Electrode mixture> The electrode mixture according to this embodiment contains the binder according to this embodiment, a positive electrode active material, and a conductive assistant.
[0059] (Cathode active material) Lithium composite metal oxides are typically used as the positive electrode active material. Examples of lithium composite metal oxides include LiMnO2, LiMn2O4, LiCoO2, LiNiO2, and LiNi x Co 1-x O2(0 <x<1)、LiNi x Co y Mn 1-x-y O2(0 <x<1、0<y<1)、LiNi x Co y AlZO2(0.55≦x<1, 0 <y2<0.55、0<z<0.55であり、かつx / (x+y+z)≧0.55である。)、Li x Ni 1-y M y O2, LiFePO4, LiFe x Mn 1-xPO4 (0.05≦x≦0.40, 1-x≧0) and the like.
[0060] The positive electrode active material has an average particle diameter Dv50 of 6.0 μm or less. This range of values allows for the production of an electrode with high flexibility. The average particle diameter Dv50 refers to the particle diameter at a particle size cumulative rate of 50% in a particle size cumulative line diagram based on volume. The particle size cumulative line diagram may be created in accordance with JISK 1474.
[0061] (Conductive assistant) The conductive assistant is added for the purpose of improving the conductivity of the electrode mixture layer when an active material with low electronic conductivity such as LiCoO2 is used. Examples of the conductive assistant include carbon materials such as carbon black, carbon nanotubes, graphene, graphite fine powder, and graphite fiber, as well as metal fine powders or metal fibers such as nickel and aluminum.
[0062] (Other ingredients) The electrode mixture according to the present embodiment may contain a solvent such as a non-aqueous solvent. Examples of the non-aqueous solvent include N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethylsulfoxide, hexamethylphosphoramide, dioxane, tetrahydrofuran, tetramethylurea, triethylphosphate, trimethylphosphate, acetone, ethyl acetate, n-butyl acetate, n-butanol, dipropylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, and cyclohexanone. These solvents may be used alone or in combination of two or more.
[0063] In addition, the electrode mixture according to this embodiment may contain, as other components, for example, a pigment dispersant such as polyvinylpyrrolidone, a dispersion stabilizer, and the like.
[0064] In the electrode mixture, when the amount of the positive electrode active material is taken as 100 parts by mass, the vinylidene fluoride polymer is preferably contained in an amount of 0.2 to 15 parts by mass, and more preferably 0.5 to 10 parts by mass.
[0065] (Preparation of electrode mixture) For example, the electrode mixture may be prepared by mixing the binder according to the present embodiment, the electrode active material, and the solvent to form a uniform slurry, and the order of mixing is not particularly limited. For example, the electrode active material may be added to the binder, and then the solvent may be added, and the mixture may be stirred and mixed to obtain the electrode mixture. Alternatively, the electrode active material may be dispersed in a solvent, and then the binder may be added thereto, and the mixture may be stirred and mixed to obtain the electrode mixture. Alternatively, the solvent may be added to the binder, and then the electrode active material may be added, and the mixture may be stirred and mixed to obtain the electrode mixture. Furthermore, the kneading may be performed in multiple steps, for example, secondary kneading may be performed.
[0066] <Electrode> The electrode according to the present embodiment includes a current collector and an electrode mixture layer formed from the electrode mixture according to the present embodiment on both sides of the current collector. Unless otherwise specified, the term "electrode" in this specification means an electrode of a battery in which an electrode mixture layer formed from the electrode mixture according to the present embodiment is formed on a current collector.
[0067] (current collector) The current collector is the base material of the electrode and is a terminal for extracting electricity. Examples of the material of the current collector include iron, stainless steel, steel, copper, aluminum, nickel, and titanium. The shape of the current collector is preferably a foil or a mesh.
[0068] (Electrode mixture layer) The electrode mixture layer is a layer obtained by applying a slurry-like electrode mixture to a current collector and drying it. The electrode mixture can be applied by a method known in the art, and can include a method using a bar coater, a die coater, a comma coater, or the like. The drying temperature for forming the electrode mixture layer is preferably 50°C to 170°C, and more preferably 50°C to 150°C. The electrode mixture layer may be formed on both sides of the current collector, or only on one side.
[0069] The thickness of the electrode mixture layer is usually 20 to 600 μm, preferably 20 to 350 μm per side. The electrode mixture layer may be pressed to increase its density. The weight per unit area of the electrode mixture layer on both sides is usually 20 to 700 g / m 2 and preferably 30 to 600 g / m 2 It is.
[0070] In order to increase the capacity of batteries such as non-aqueous electrolyte secondary batteries, the thickness of the electrode is preferably 150 μm or more, more preferably 170 μm or more, and is preferably 270 μm or less, more preferably 220 μm or less.
[0071] The electrode according to this embodiment can be suitably used as a positive electrode for a non-aqueous electrolyte secondary battery such as a lithium ion secondary battery.
[0072] <Nonaqueous electrolyte secondary battery> The nonaqueous electrolyte secondary battery according to the present embodiment includes the electrode according to the present embodiment. Other members in the nonaqueous electrolyte secondary battery are not particularly limited, and for example, conventionally used members can be used. One aspect of the nonaqueous electrolyte secondary battery has a cylindrical battery structure in which a power generating element in which a separator is arranged between a positive electrode and a negative electrode and the resulting laminate is wound in a spiral shape is housed in a metal casing. Another aspect of the nonaqueous electrolyte secondary battery may be a nonaqueous electrolyte secondary battery of other shapes such as a coin shape, a square shape, or a paper shape.
[0073] A method for producing a non-aqueous electrolyte secondary battery includes, for example, stacking a negative electrode layer and a positive electrode layer with a separator interposed therebetween, placing the resulting stack in a battery container, injecting an electrolyte into the battery container, and sealing the container.
[0074] <Summary> The binder according to the present embodiment contains at least one vinylidene fluoride polymer and satisfies the following requirements (A) to (E): (A) an N-methylpyrrolidone solution containing 5% by mass of the binder has a turbidity of 5.0 or less at 25° C.; (B) a binder solution obtained by adding 6 parts by mass of the binder to 94 parts by mass of a 95% by mass aqueous acetone solution and stirring at 30° C. for 2 hours has a solubility of the binder, as represented by the following formula (1), of 10% or more and 70% or less; (C) an inherent viscosity of a soluble component of the binder solution is 0.5 dL / g or more and less than 2.5 dL / g; (D) a viscosity of the soluble component of the binder solution is 1735 cm -1 Infrared absorption spectrum absorbance A at 1735cm -1 And, 3025cm -1 Infrared absorption spectrum absorbance A3025cm -1 Ratio to A1735cm -1 / A3025cm -1 is greater than or equal to 0.20 and less than or equal to 0.80; and (E) the inherent viscosity of the binder is greater than the inherent viscosity of the dissolved components of the binder solution. Dissolution rate (%) = ((input amount - undissolved substance amount) / input amount) × 100 (1)
[0075] Furthermore, the binder according to this embodiment preferably has at least one crystallization peak (Tc) in the range of 85° C. or more and less than 125° C. and in the range of 125° C. or more and 150° C. or less when a first temperature drop measurement is performed using a differential scanning calorimeter under conditions of 10° C. / min.
[0076] Furthermore, in the binder according to the present embodiment, when all the constituent units of the vinylidene fluoride polymer contained in the binder are taken as 100 mass%, the proportion of constituent units derived from hexafluoropropylene is preferably 3 mass% or more and 15 mass% or less, and when all the constituent units of the vinylidene fluoride polymer contained in the dissolved component of the binder solution are taken as 100 mass%, the proportion of constituent units derived from hexafluoropropylene contained in the dissolved component of the binder solution is preferably 5 mass% or more and 40 mass% or less.
[0077] The binder according to the present embodiment contains a first vinylidene fluoride polymer having a structural unit derived from vinylidene fluoride as a main structural component and optionally containing a structural unit derived from hexafluoropropylene, and a second vinylidene fluoride polymer containing a structural unit derived from vinylidene fluoride, a structural unit derived from hexafluoropropylene, and a structural unit containing a polar functional group, and the first vinylidene fluoride polymer has an inherent viscosity of 2.5 dL / g or more and 6.0 dL / g or less. The first vinylidene fluoride polymer has a hexafluoropropylene-derived structural unit of 0% by mass or more and less than 0.5% by mass in all structural units of the first vinylidene fluoride polymer, the second vinylidene fluoride polymer has an inherent viscosity of 0.5 dL / g or more and less than 2.5 dL / g, the second vinylidene fluoride polymer has a hexafluoropropylene-derived structural unit of 6% by mass or more and 40% by mass or less in all structural units of the second vinylidene fluoride polymer, and the second vinylidene fluoride polymer has a 1735 cm -1 Infrared absorption spectrum absorbance A at 1735cm -1 And, 3025cm -1 Infrared absorption spectrum absorbance A3025cm -1 Ratio to A1735cm -1 / A3025cm -1 is 0.20 or more and 0.80 or less, and the mass ratio of the second vinylidene fluoride polymer to the first vinylidene fluoride polymer in the binder (second vinylidene fluoride polymer / first vinylidene fluoride polymer) is 3 / 7 or more and 7 / 3 or less.
[0078] The electrode mixture according to this embodiment includes the binder according to this embodiment, a positive electrode active material, and a conductive assistant, and the average particle diameter Dv50 of the positive electrode active material is 6.0 μm or less.
[0079] The electrode according to this embodiment is an electrode including a current collector and electrode mixture layers formed from the electrode mixture according to this embodiment on both sides of the current collector.
[0080] A nonaqueous electrolyte secondary battery including the electrode according to this embodiment can achieve high capacity. Furthermore, this nonaqueous electrolyte secondary battery, which is highly safe and can be used for a long time, will promote the spread of electric vehicles (EVs) and contribute to the reduction of CO2 emissions associated with them. In addition, it is expected that the use of this battery will contribute to the mitigation of global warming through resource conservation and reduction of greenhouse gas emissions, as well as the foundation of industry and technological innovation. This will contribute to the achievement of the Sustainable Development Goals (SDGs).
[0081] The following examples are provided to further explain the embodiments of the present invention. Of course, the present invention is not limited to the following examples, and various modifications are possible in detail. Furthermore, the present invention is not limited to the above-mentioned embodiments, and various modifications are possible within the scope of the claims. The technical scope of the present invention also includes embodiments obtained by appropriately combining the technical means disclosed in the different embodiments. In addition, all of the documents described in this specification are incorporated by reference. EXAMPLES
[0082] In the following examples, % means % by mass unless otherwise specified.
[0083] [Preparation Example 1] Preparation of VDF / HFP / MMM copolymer In a 2-liter autoclave, 1027 g of ion-exchanged water, 0.8 g of Metolose SM-100 (Shin-Etsu Chemical Co., Ltd.), 7.08 g of 50% diisopropyl peroxydicarbonate-Flon HFE-347pc-f solution, 344 g of vinylidene fluoride (VDF), 54 g of hexafluoropropylene (HFP), and 1.99 g of monomethyl maleic acid (MMM) were charged and heated to 29°C. The obtained polymer slurry was dehydrated and dried to obtain a vinylidene fluoride copolymer (VDF / HFP / MMM). Hereinafter, the 50% diisopropyl peroxydicarbonate-Flon HFE-347pc-f solution is referred to as solution A.
[0084] [Preparation Example 2] Preparation of VDF / HFP / MMM copolymer Into a 2-L autoclave were charged 1,072 g of ion-exchanged water, 0.62 g of Metrose SM-100 (Shin-Etsu Chemical Co., Ltd.), 2.66 g of solution A, 311 g of VDF, 103 g of HFP, and 2.08 g of MMM, and the mixture was heated to 29° C. The resulting polymer slurry was dehydrated and dried to obtain a vinylidene fluoride copolymer (VDF / HFP / MMM).
[0085] [Preparation Example 3] Preparation of VDF homopolymer Into a 14-liter autoclave were charged 7614.5 g of ion-exchanged water, 1.755 g of Metolose SM-100, 9.83 g of solution A, and 3509 g of VDF, and the temperature was adjusted to 26° C. The obtained polymer slurry was dehydrated and dried to obtain vinylidene fluoride homopolymer (pVDF).
[0086] [Preparation Example 4] Preparation of VDF / HFP polymer Into a 2-liter autoclave, 1100.8 g of ion-exchanged water, 0.22 g of Metolose SM-100 (Shin-Etsu Chemical Co., Ltd.), 1.85 g of solution A, 374 g of VDF, and 0.61 g of HFP were charged and heated to 43° C. The obtained polymer slurry was dehydrated and dried to obtain a vinylidene fluoride copolymer (VDF / HFP).
[0087] [Preparation Example 5] Preparation of VDF homopolymer Into a 14-liter autoclave were charged 7614.5 g of ion-exchanged water, 1.755 g of Metolose SM-100, 6.32 g of solution A, and 3509 g of VDF, and the temperature was adjusted to 26° C. The obtained polymer slurry was dehydrated and dried to obtain pVDF.
[0088] [Preparation Example 6] Preparation of VDF / HFP / MMM copolymer Into a 2-L autoclave were charged 1,054 g of ion-exchanged water, 0.62 g of Metolose SM-100 (Shin-Etsu Chemical Co., Ltd.), 3.49 g of solution A, 374 g of VDF, 40 g of HFP, and 2.08 g of MMM, and the mixture was heated to 29° C. The resulting polymer slurry was dehydrated and dried to obtain a vinylidene fluoride copolymer (VDF / HFP / MMM).
[0089] [Preparation Example 7] Preparation of VDF / HFP / MMM copolymer A 2-L autoclave was charged with 1061 g of ion-exchanged water, 0.62 g of Metolose SM-100, 1.65 g of solution A, 370 g of VDF, 41 g of HFP, and 1.24 g of MMM, and heated to 29° C. The resulting polymer slurry was dehydrated and dried to obtain a vinylidene fluoride copolymer (VDF / HFP / MMM).
[0090] [Preparation Example 8] Preparation of VDF / HFP / MMM copolymer A 2-L autoclave was charged with 1188 g of ion-exchanged water, 0.44 g of Metolose SM-100, 3.96 g of solution A, 418 g of VDF, 22 g of HFP, and 2.42 g of MMM, and heated to 43° C. The resulting polymer slurry was dehydrated and dried to obtain a vinylidene fluoride copolymer (VDF / HFP / MMM).
[0091] [Preparation Example 9] Preparation of VDF homopolymer In a 2-liter autoclave, 1153.6 g of ion-exchanged water, 2.06 g of perfluorooctanoic acid (PFOA), a small amount of ethyl acetate, and 103 g of VDF were placed. After heating to 80°C, 2.06 g of ammonium persulfate was added and polymerized, and 309 g of VDF was further added. The resulting polymer slurry was dehydrated and dried to obtain vinylidene fluoride polymer (pVDF).
[0092] [Preparation Example 10] Preparation of VDF / HFP / MMM copolymer A 2-L autoclave was charged with 1,060 g of ion-exchanged water, 0.63 g of Metolose SM-100, 2.35 g of solution A, 391 g of VDF, 20 g of HFP, and 0.78 g of MMM, and heated to 29° C. The resulting polymer slurry was dehydrated and dried to obtain a vinylidene fluoride copolymer (VDF / HFP / MMM).
[0093] [Preparation Example 11] Preparation of VDF / HFP / MMM copolymer A 2-liter autoclave was charged with 1060.7 g of ion-exchanged water, 0.63 g of Metolose SM-100, 2.35 g of solution A, 391 g of VDF, 20 g of HFP, and 0.41 g of MMM, and heated to 29° C. The resulting polymer slurry was dehydrated and dried to obtain a vinylidene fluoride copolymer (VDF / HFP / MMM).
[0094] [Preparation Example 12] Preparation of VDF / HFP / AA copolymer Into a 2-liter autoclave, 1071.2 g of ion-exchanged water, 0.58 g of Metolose SM-100, 3.5 g of solution A, 82 g of VDF, and 41 g of HFP were added. After heating to 45°C, 289 g of VDF and 2.06 g of acrylic acid (AA) were added. At that time, AA was used in the form of a 5% by mass aqueous solution, and the AA aqueous solution was added at a rate of 3.4 g / h. The obtained polymer slurry was dehydrated and dried to obtain a vinylidene fluoride copolymer (VDF / HFP / AA).
[0095] [Preparation Example 13] Preparation of VDF / HFP / MMM copolymer A 2-L autoclave was charged with 1,061 g of ion-exchanged water, 0.62 g of Metolose SM-100, 2.27 g of solution A, 391 g of VDF, 19 g of HFP, and 1.03 g of MMM, and heated to 29° C. The resulting polymer slurry was dehydrated and dried to obtain a vinylidene fluoride copolymer (VDF / HFP / MMM).
[0096] [Example 1] Preparation of binder and electrode mixture and fabrication of electrode A binder was obtained by mixing the first vinylidene fluoride polymer and the second vinylidene fluoride polymer shown in Table 1 in the ratio (mass ratio) shown in Table 2. The second vinylidene fluoride polymer used was the vinylidene fluoride polymer prepared in Preparation Example 1. #4300 is a vinylidene fluoride homopolymer (suspension polymerization) manufactured by Kureha Corporation.
[0097] The binder was dissolved in N-methyl-2-pyrrolidone (hereinafter referred to as NMP) to prepare a vinylidene fluoride polymer solution containing 6 mass % of vinylidene fluoride copolymer. Then, a CNT (carbon tube) dispersion (tube diameter 7 nm, specific surface area 300 m) was added as a conductive assistant to the polymer solution. 2 A NMP mixed solution containing 4.3 mass% of MWCNT (1.0 mass% / g) and NMP were added, and a primary kneading was performed. Next, lithium iron phosphate (LFP), which is a positive electrode active material having a Dv50 shown in Table 4, was added to adjust the solid content concentration to 50%. Then, a secondary kneading was performed at 2000 rpm for 5 minutes to obtain an electrode mixture. The mass ratio of the positive electrode active material, CNT, and vinylidene fluoride polymer in the obtained electrode mixture, in this order, was 100:2:3.
[0098] The obtained electrode mixture was applied to both sides of an aluminum foil having a thickness of 15 μm using a TH-C type coater manufactured by Thank Metals Co., Ltd., so that the weight of the electrode mixture on one side in a dry state was approximately 190 g / m. 2 The electrodes were prepared as follows.
[0099] [Examples 2 to 7] Preparation of binder and electrode mixture and fabrication of electrodes A binder was obtained by mixing the first vinylidene fluoride polymer and the second vinylidene fluoride polymer shown in Table 1 in the ratio (mass ratio) shown in Table 2. The second vinylidene fluoride polymer of Example 2, the first vinylidene fluoride polymer of Example 3, the first vinylidene fluoride polymer of Example 4, the first vinylidene fluoride polymer of Example 7, and the second vinylidene fluoride polymer of Example 7 were the vinylidene fluoride polymers prepared in Preparation Examples 2 to 6, respectively. The second vinylidene fluoride polymer of Examples 3 to 6 was the vinylidene fluoride polymer prepared in Preparation Example 1.
[0100] In addition, an electrode mixture was prepared using the LFP having a Dv50 shown in Table 4 in the same manner as in Example 1. Then, an electrode was produced using each of the prepared electrode mixtures. The weight per surface of the electrode produced in Example 6 was approximately 210 g / m 2 It was.
[0101] [Comparative Examples 1 to 8 and Reference Example 1] Preparation of binder and electrode mixture and fabrication of electrodes The first vinylidene fluoride polymer and the second vinylidene fluoride polymer shown in Table 1 were mixed in the ratio (mass ratio) shown in Table 2 to obtain a binder. The first vinylidene fluoride polymer in Comparative Example 3 and 5 to 8 used the vinylidene fluoride polymers prepared in Preparation Examples 9, 10, 11, 5 and 13, respectively. The second vinylidene fluoride polymer in Comparative Examples 1 and 7 used the vinylidene fluoride polymers prepared in Preparation Examples 7 and 12, respectively. The second vinylidene fluoride polymer in Comparative Examples 2 and 6 used the vinylidene fluoride polymer prepared in Preparation Example 8, and the second vinylidene fluoride polymer in Comparative Examples 3, 4 and Reference Example 1 used the vinylidene fluoride polymer prepared in Preparation Example 1. In Comparative Examples 5 and 8, the second vinylidene fluoride polymer was not used.
[0102] #1300 is a vinylidene fluoride homopolymer (suspension polymerization) manufactured by Kureha Corporation.
[0103] Further, an electrode mixture was prepared using an LFP having a Dv50 shown in Table 4 in the same manner as in Example 1. The mass ratio of the positive electrode active material, CNT, and vinylidene fluoride polymer in the electrode mixtures obtained in Example 7 and Comparative Examples 7 and 8 was 100:2:2.5, in this order.
[0104] Then, electrodes were fabricated using each of the prepared electrode mixtures.
[0105] [Evaluation Example 1] Inherent viscosity (η i ) Measurement A polymer solution was prepared by dissolving 80 mg of vinylidene fluoride polymer in 20 mL of N,N-dimethylformamide. The viscosity η of the prepared polymer solution was measured using an Ubbelohde viscometer in a thermostatic bath at 30°C. The inherent viscosity (η i ) was calculated. η i =(1 / C)·ln(η / η0) In the above formula, η0 is the viscosity of the solvent, N,N-dimethylformamide, and C is 0.4 g / dL.
[0106] [Evaluation Example 2] Measurement of HFP content in vinylidene fluoride copolymer Approximately 40 mg of a PVDF sample and approximately 750 μL of DMSO-d6 as a solvent were added, and the mixture was stirred at 600 rpm for approximately 30 minutes at 40°C using a magnetic stirrer. The dissolved sample was transferred to a 5 mm NMR measurement tube and analyzed using a Bruker AVANCE-400. 19 F NMR measurement was performed. The ratio of HFP to VDF (molar ratio) was calculated from the integral ratio of each peak area when the peak area of the internal standard was set to 6, assuming that the total amount of VDF and HFP introduced was 100 mol%.
[0107] In addition, 19 As with F NMR measurements, 1H NMR measurement was performed, and the ratio of MMM to VDF (molar ratio) was calculated based on the integrated intensity of a signal observed at 4.19 ppm, which is mainly derived from a monomer containing a polar functional group, and signals observed at 2.24 ppm and 2.87 ppm, which are mainly derived from vinylidene fluoride, assuming that the total of the amount of VDF introduced and the amount of MMM introduced is 100 mol %.
[0108] The above 19 The HFP to VDF ratio obtained by F NMR measurement and the 19 The VDF / HFP / MMM composition ratio in the vinylidene fluoride copolymer was calculated from the MMM ratio to VDF obtained by F NMR measurement, and then the amount of each component introduced [mol%] was calculated when the total amount of VDF, HFP, and MMM introduced was 100 mol%. The amount of each component introduced [mol] obtained was multiplied by the molar mass [g / mol] to calculate the mass [g] of each component.
[0109] Furthermore, the amount of HFP [mass %] was calculated using formula (2). HFP amount [mass%] = (HFP mass / (HFP mass + VDF mass + MMM mass)) × 100 (2)
[0110] [Evaluation Example 3] Measurement of absorbance ratio of second vinylidene fluoride polymer The second vinylidene fluoride copolymer was heat-pressed at 200° C. to form a 30 mm×30 mm film. -1 ~4000cm -1 The IR spectrum of each of the above films was measured in the range of 1735 cm -1 The absorbance of the IR spectrum at (A1735cm -1 ) and 3025cm -1 The absorbance of the IR spectrum at 25 cm -1 ) (A1735cm -1 / A3025cm -1 ) was sought.
[0111] [Evaluation Example 4] Measurement of crystallization peak (Tc) of binder by differential scanning calorimetry (DSC) 10 mg of the binder was placed in an aluminum pan for DSC and measured under a nitrogen atmosphere using a Mettler Toledo DSC-1 under the following conditions: <Measurement conditions> First temperature rise: From 30°C to 230°C at a rate of 10°C per minute (After reaching 230℃, maintain 230℃ for 10 minutes) 1st cooling: Decrease temperature from 230℃ to 30℃ at a rate of 10℃ per minute (After reaching 30°C, maintain 30°C for 10 minutes) Second temperature rise: From 30°C to 230°C at a rate of 10°C per minute
[0112] After the measurement, the top temperature of the crystallization peak detected in the first cooling process was defined as Tcx (x≧1).
[0113] [Evaluation Example 5] Measurement of turbidity of binder Each binder was added to NMP so as to be 5% by mass, and the mixture was heated and stirred at 50° C. to prepare a 5% by mass NMP solution. The prepared 5% by mass NMP solution was stirred at 25° C., and immediately after stopping the stirring, the turbidity was measured by integrating sphere photoelectric photometry.
[0114] [Evaluation Example 6] Evaluation of binder solution 12 g of binder was placed in 188 g of acetone containing 5% water (95% by mass acetone aqueous solution) and stirred for 2 hours with a magnetic stirrer heated to 30°C to obtain a binder solution. After that, filtration was performed to separate the undissolved matter from the dissolved liquid. The solvent contained in the undissolved matter was removed by drying, and the mass of the undissolved matter was measured. The dissolution rate of the binder solution was then calculated using the following formula (1). Dissolution rate (%) = ((input amount - undissolved substance amount) / input amount) × 100 (1)
[0115] The solvent was removed by heating from the solution after removing the undissolved matter to obtain a precipitated polymer (a dissolved component of the binder solution). The amount of HFP and the absorbance ratio (A1735cm -1 / A3025cm -1 ) measurements were carried out.
[0116] [Evaluation Example 7] Measurement of the average particle diameter Dv50 of the positive electrode active material 0.1 g of dispersant (cationic surfactant "SN Wet 366" (manufactured by San Nopco)) was added to 0.01 g of LFP sample, and the dispersant was allowed to soak into the sample. Next, 20 mL of pure water was added, and the sample was dispersed in an ultrasonic cleaner for about 5 minutes. The particle size distribution was then measured in the particle size distribution range of 0.1 to 1000 μm using a particle size distribution measuring device (manufactured by Microtrac: MT3300EXII). The dispersion medium was pure water, and the refractive index of the dispersion medium was 1.333. From the obtained particle size distribution, the particle size at which the cumulative frequency was 50% on a volume basis was calculated, and Dv50 was obtained.
[0117] [Evaluation Example 8] Measurement of viscosity of electrode mixture slurry The slurry viscosity of the electrode mixture was measured at 25°C using a B-type viscometer (BROOKFIELD's "DVS+"). A certain amount of the slurry was placed in a 1.2 cm diameter polytube and left to stand at 25°C and humidity of 10% or less to be used as the measurement sample. In this measurement, a No. 64 spindle was used, and the sample was pre-stirred at a rotation speed of 0.5 rpm for 1 minute, followed by 1 rpm for 2 minutes, and then stirred at 6 rpm for 30 seconds, at which point the viscosity was recorded as the slurry viscosity (mPa s). Viscosity measurements were taken immediately after sample preparation and 24 hours after the start of static storage.
[0118] [Evaluation Example 9] Measurement of electrode break density Each electrode was cut to a length of 5 cm × 2 cm to prepare an unpressed electrode sample. The unpressed electrode sample was pressed using a roll press under conditions of 0.4 m / min and a linear pressure of 1 t / cm to obtain a density of the electrode mixture of 2.25 g / cm. 3 A pressed electrode sample was prepared with an electrode density of 2.25 g / cm. 3For each of the pressed electrode samples, the short sides of the test pieces were joined with double-sided tape so as not to overlap, forming a cylindrical shape. The cylindrical samples were then crushed at a compression speed of 30 mm / min. The electrodes were then opened and the bent parts were visually inspected. Electrodes in which light transmission was confirmed were judged to have fractures. Electrodes in which light transmission was not confirmed were judged to have no fractures.
[0119] Details of the first vinylidene fluoride polymer and the second vinylidene fluoride polymer used in each of the Examples, Comparative Examples, and Reference Examples are shown in Table 1. In Table 1, η i indicates the inherent viscosity (dL / g) of each vinylidene fluoride polymer. The HFP content indicates the proportion (mass%) of structural units derived from HFP in the total structural units of each vinylidene fluoride polymer. IR is A1735cm -1 / A3025cm -1 It is to be noted that the inherent viscosity of the first vinylidene fluoride polymer of Comparative Example 3 was not measurable.
[0120] [Table 1]
[0121] The evaluation results of the binders obtained in each of the Examples, Comparative Examples, and Reference Examples are shown in Table 2. In Table 2, the "first polymer / second polymer" indicates the ratio (mass ratio) of the first vinylidene fluoride polymer to the second vinylidene fluoride polymer in the binder. η i indicates the inherent viscosity (dL / g) of the binder. The inherent viscosity is a value calculated based on the inherent viscosity of each vinylidene fluoride polymer measured in Evaluation Example 1 and the ratio of the first polymer / second polymer in the binder.
[0122] In Table 2, the HFP amount is the ratio (mass%) of structural units derived from HFP to all structural units of the vinylidene fluoride polymer contained in the binder. The HFP amount is a value calculated based on the amount of HFP in each vinylidene fluoride copolymer measured in Evaluation Example 2 and the ratio of the first polymer / second polymer in the binder.
[0123] In Table 2, Tc1 is the peak temperature of the heat change due to crystallization detected on the low temperature side in the differential scanning calorimetry curve obtained in the first cooling run. Tc2 is the peak temperature of the heat change due to crystallization detected on the high temperature side in the differential scanning calorimetry curve obtained in the first cooling run. In Comparative Examples 4 to 6 and 8, Tc1 was not detected.
[0124] [Table 2]
[0125] Table 3 shows the binder solutions obtained in the respective Examples, Comparative Examples, and Reference Examples, and the evaluation results of the dissolved components in the binder solutions.
[0126] [Table 3]
[0127] Table 4 shows the evaluation results of the electrode mixtures and electrodes obtained in each of the Examples, Comparative Examples, and Reference Examples. In Table 4, the viscosity of the slurry is the viscosity immediately after the sample was prepared. The viscosity increase (%) indicates the rate of increase in the slurry viscosity after standing for 24 hours, calculated using the following formula. "Excessive" indicates that the slurry viscosity after standing for 24 hours was 100,000 mPa s (upper limit of measurement) or more. The unit of electrode density is g / cm. 3 The unit of weight is g / m 2 The unit of electrode thickness is μm. Viscosity (%) = Slurry viscosity after standing for 24 hours / Slurry viscosity immediately after sample preparation × 100
[0128] [Table 4]
[0129] <Result> As shown in Table 4, the electrode mixtures obtained using the binders of Examples 1 to 7, which satisfied the above requirements (A) to (E), suppressed thickening of the slurry. Furthermore, although the electrodes obtained using the electrode mixtures were thick, no breakage was observed, and it was found that the electrodes had flexibility that could withstand bending.
[0130] When a binder containing a first vinylidene fluoride polymer having a low HFP content and a second vinylidene fluoride polymer having a high HFP content is dissolved in a 95% by mass acetone aqueous solution, the second vinylidene fluoride polymer having a high HFP content dissolves. Therefore, the soluble component of the binder solution corresponds to the second vinylidene fluoride polymer.
[0131] The dissolution rate of the binder solution in Comparative Examples 2 and 6 was less than 10%. This is believed to be due to the fact that the HFP content of the second vinylidene fluoride polymer was less than 6% by mass. It was also suggested that the HFP content of the second vinylidene fluoride polymer must be 6% by mass or more, regardless of the HFP content of the first vinylidene fluoride polymer and the content of the first vinylidene fluoride polymer in the binder.
[0132] The first vinylidene fluoride polymer of Comparative Example 3 was a polymer obtained by emulsion polymerization. The turbidity of the binder containing the polymer exceeded 5.0, and the thickening of the electrode mixture slurry became excessive.
[0133] The binder in Comparative Examples 5 and 8 was only the first vinylidene fluoride polymer. Even if the amount of HFP in the first vinylidene fluoride polymer was increased, the dissolution rate of the binder solution was less than 10%. The thickening of the slurry of the electrode mixture in Comparative Examples 5 and 8 became excessive, and breakage was observed in the electrode. These results suggested that the presence of a soluble component (second vinylidene fluoride polymer) in the binder solution was necessary.
[0134] It was also found that if the dissolution rate of the binder solution was less than 10%, no crystallization peak was observed in the range of 85° C. or more and less than 125° C. in the DSC analysis.
[0135] The binders in Examples 1 to 7 are all binders of a first vinylidene fluoride polymer (low HFP amount, high inherent viscosity) and a second vinylidene fluoride polymer (high HFP amount, low inherent viscosity). However, from the above evaluation examples, etc., a person skilled in the art can understand that the thickening of the slurry viscosity of an electrode mixture containing one type of vinylidene fluoride polymer satisfying the above requirements (A) to (E) is suppressed. In addition, from the above evaluation examples, a person skilled in the art can understand that an electrode obtained using the electrode mixture has flexibility. [Industrial Applicability]
[0136] The present invention can be used in non-aqueous electrolyte secondary batteries.
Claims
1. A binder comprising at least one vinylidene fluoride polymer, A binder that satisfies the following requirements (A) to (E): (A) the turbidity of an N-methylpyrrolidone solution containing 5% by mass of the binder at 25° C. is 5.0 or less; (B) In a binder solution obtained by adding 6 parts by mass of the binder to 94 parts by mass of a 95% by mass aqueous acetone solution and stirring the mixture at 30° C. for 2 hours, the dissolution rate of the binder represented by the following formula (1) is 10% or more and 70% or less: Dissolution rate (%) = ((input amount - undissolved substance amount) / input amount) x 100... (1) (C) the inherent viscosity of the dissolved component of the binder solution is 0.5 dL / g or more and less than 2.5 dL / g; (D) 1735 cm of the dissolved component of the binder solution -1 Infrared absorption spectrum absorbance A1735 cm -1 And 3025 cm -1 Infrared absorption spectrum absorbance A3025cm -1 Ratio to A1735cm -1 / A3025cm -1 is equal to or greater than 0.20 and equal to or less than 0.80; and (E) the inherent viscosity of the binder is greater than the inherent viscosity of the dissolved components of the binder solution.
2. 2. The binder according to claim 1, wherein the binder has at least one crystallization peak (Tc) in the range of 85° C. or more and less than 125° C. and in the range of 125° C. or more and 150° C. or less when a first temperature drop measurement is performed using a differential scanning calorimeter under conditions of 10° C. / min.
3. a ratio of structural units derived from hexafluoropropylene is 3% by mass or more and 15% by mass or less, when all structural units of the vinylidene fluoride polymer contained in the binder are taken as 100% by mass, 2. The binder according to claim 1, wherein a ratio of structural units derived from hexafluoropropylene contained in the dissolved components of the binder solution is 5% by mass or more and 40% by mass or less, when all structural units of the vinylidene fluoride polymer contained in the dissolved components of the binder solution are taken as 100% by mass.
4. A first vinylidene fluoride polymer having a structural unit derived from vinylidene fluoride as a main structural component and optionally including a structural unit derived from hexafluoropropylene; a second vinylidene fluoride polymer including a structural unit derived from vinylidene fluoride, a structural unit derived from hexafluoropropylene, and a structural unit containing a polar functional group; the first vinylidene fluoride polymer has an inherent viscosity of 2.5 dL / g or more and 6.0 dL / g or less, and a content of structural units derived from hexafluoropropylene in all structural units of the first vinylidene fluoride polymer is 0 mass% or more and less than 0.5 mass%, the second vinylidene fluoride polymer has an inherent viscosity of 0.5 dL / g or more and less than 2.5 dL / g, and a content of structural units derived from hexafluoropropylene in all structural units of the second vinylidene fluoride polymer is 6% by mass or more and 40% by mass or less; The second vinylidene fluoride polymer has a peak at 1735 cm -1 Infrared absorption spectrum absorbance A1735 cm -1 And 3025 cm -1 Infrared absorption spectrum absorbance A3025cm -1 Ratio to A1735cm -1 / A3025cm -1 is equal to or greater than 0.20 and equal to or less than 0.80, A binder, wherein a mass ratio of the second vinylidene fluoride polymer to the first vinylidene fluoride polymer (second vinylidene fluoride polymer / first vinylidene fluoride polymer) in the binder is 3 / 7 or more and 7 / 3 or less.
5. A binder according to any one of claims 1 to 4, a positive electrode active material, and a conductive assistant, The electrode mixture, wherein the average particle diameter Dv50 of the positive electrode active material is 6.0 μm or less.
6. A current collector; An electrode comprising: an electrode mixture layer formed from the electrode mixture according to claim 5 on both sides of the current collector.
Citation Information
Patent Citations
Binder for forming nonaqueous electrochemical element electrode, electrode mix, electrode structure, and electrochemical element
JP2005310747A
Core-shell type particle, and use and manufacturing method thereof
JP2018174105A
Binder composition, non-aqueous electrolyte secondary battery electrode, and non-aqueous electrolyte secondary battery
WO2017056974A1
Nonaqueous secondary battery separator and nonaqueous secondary battery
WO2019107521A1
Resin composition and coating composition containing same, electrode for lamination, separator for lamination, and nonaqueous electrolyte secondary battery and production method for same
WO2022044592A1