Multi-layer annular pore nickel-cobalt-aluminum precursor and manufacturing method thereof, and positive electrode material thereof

By controlling pH and concentration during the production of a multilayer annular pore nickel cobalt aluminum precursor, the internal structure is optimized for enhanced lithium ion diffusion and structural stability, addressing the limitations of existing cathode materials in lithium batteries.

JP2024542349AActive Publication Date: 2024-11-15HENAN KELONG NEW ENERGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024514133
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-10-26
Filing Date
2023-10-24
Publication Date
2024-11-15
Estimated Expiration
2043-10-24

AI Technical Summary

Technical Problem

Existing cathode materials for lithium batteries, such as NCA, face challenges in achieving high energy density, long life, and low cost, with previous production methods failing to effectively address the internal structure and lithium ion diffusion paths, leading to suboptimal performance.

Method used

A multilayer annular pore nickel cobalt aluminum precursor is produced by controlling the pH and concentration of aluminum solutions during coprecipitation, resulting in a spherical secondary particle structure with controlled porosity, which enhances lithium ion diffusion and structural stability.

Benefits of technology

The precursor's porosity allows for better electrolyte penetration, increasing the contact area and shortening lithium ion diffusion paths, leading to higher initial discharge capacity, reduced internal resistance, and improved cycle performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024542349000001_ABST
    Figure 2024542349000001_ABST
Patent Text Reader

Abstract

The present invention discloses a multi-layer annular pore nickel-cobalt-aluminum precursor and a preparation method thereof, and a positive electrode material thereof, in which the D50 of the precursor is 8-20μm, the cross-sectional view shows that the spherical secondary particle structure has multi-layer annular pores, and the average porosity value of the cross-section of one particle or a plurality of particles is 6-14%. The nickel-cobalt mixed salt solution, the alkali aluminum solution, the complexing agent, and the precipitating agent are co-precipitated, and the pH value and the aluminum solution concentration at each stage are strictly controlled, followed by solid-liquid separation, washing, oven drying, uniform mixing, sieving, and demagnetization processes to prepare a nickel-cobalt-aluminum precursor having multi-layer annular pores. The loose and porous morphology of the precursor is conducive to mixing and sintering lithium to obtain a positive electrode material. The positive electrode material has a multi-layer lithium ion diffusion path, which can buffer the mechanical distortion force of the crystal lattice generated in the material during charging and discharging, and improve the cycle. It has a high initial discharge specific capacity, low internal resistance, good rate performance, and good cycle stability.
Need to check novelty before this filing date? Find Prior Art

Description

CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This application claims priority from a Chinese application having CN Application No. 202211319408.6 and filing date of October 26, 2022, the disclosure of which is again incorporated herein in its entirety. [Technical field]

[0002] The present invention relates to the field of lithium battery positive electrode material technology, and particularly to a multi-layer annular pore nickel-cobalt-aluminum precursor and a preparation method thereof, and a positive electrode material thereof. [Background technology]

[0003] At present, the popularization and development of electric vehicles is restricted by problems such as the lack of driving endurance of power batteries, slow charging speed, and rather high cost, and the market popularization of electric vehicles is greatly affected by the cost-effectiveness of power lithium batteries. The positive electrode material is the core key material of power lithium batteries, and the high energy density of the positive electrode material is closely related to the driving range of electric vehicles, and its cost accounts for about 1 / 3 of the cost of lithium battery cells, so the development of high energy density, long life, high safety and low cost positive electrode materials is extremely important for the large-scale commercialization of power lithium batteries and electric vehicles.

[0004] NCA materials combine the advantages of LiNiO2 and LiCoO2, and therefore not only have a high reversible specific capacity and low material costs, but also improve the structural stability and safety of the material after doping with aluminum, and further improve the cycling stability of the material. Therefore, NCA materials are one of the most popular materials in the research of positive electrode materials that are currently commercially available.

[0005] The technical solution disclosed in the patent with publication number CN113651372A uses a discontinuous method to prepare a precursor with high sphericity and no twin particles, and this solution only improves the morphology of the precursor surface, but does not mention the internal spatial structure of the precursor, and cannot effectively explain the advantages of the precursor after sintering into a positive electrode material.

[0006] The technical solution disclosed in the patent with publication number CN113697870B provides a precursor with a binuclear twin crystal structure to improve the lithium ion diffusion path and lithium ion diffusion rate. However, when viewed from a cross-sectional electron microscope, the precursor has a dense internal structure, which is unfavorable for mixing and sintering with lithium salt, and forms multiple lithium ion diffusion paths, and is unfavorable for the elements modified by the coating to enter the surface of the primary particles. Therefore, the technical solution also fails to highlight the advantages of the improved precursor. Summary of the Invention [Problem to be solved by the invention]

[0007] Based on the above problems, the present invention has found that, during the research of nickel-cobalt-aluminum precursor, the solubility product constants between elements are different during the preparation, and the pH and concentration of the aluminum solution at each reaction stage can be strictly controlled to directly improve the morphology and porosity of the primary particles in the internal structure of the precursor particles, and this method has a simple process, low cost, is suitable for industrialized production, and the obtained product has good performance after sintering. [Means for solving the problem]

[0008] The present invention provides a multi-layer annular pore nickel cobalt aluminum precursor having the chemical formula Ni M Co N Al 1-M-NThe present invention provides a multi-layer annular pore nickel-cobalt-aluminum precursor, characterized in that (OH)2, 0.8≦M≦0.97, 0.02≦N≦0.09, 0.01≦1-MN≦0.055, with the proviso that D50 is 8-20 μm, the precursor has multi-layer annular pores in its spherical secondary particle structure, and the porosity value, which is the cross-sectional average value of one spherical secondary particle or a plurality of spherical secondary particles, is 6-14%.

[0009] The present invention further provides a method for producing the precursor, S1: Weighing nickel sulfate and cobalt sulfate powders and dissolving them in pure water to prepare a nickel-cobalt mixed salt solution; S2, weighing out aluminum salt and adding it to the sodium hydroxide solution to prepare an alkaline aluminum solution; S3, pumping the nickel-cobalt mixed salt solution of S1, the alkali aluminum solution of S2, and a complexing agent into a reaction vessel simultaneously to carry out a coprecipitation reaction stepwise; After the reaction is completed, the material obtained from the reaction is subjected to processes of solid-liquid separation, washing, oven drying, uniform mixing, sieving and demagnetization to obtain a nickel-cobalt-aluminum precursor.

[0010] Furthermore, in step S1, the nickel-cobalt mixed salt solution has a total metal ion concentration of 1.0 to 2.0 mol / L.

[0011] Furthermore, in step S2, the aluminum salt is sodium metaaluminate, and the Al in the alkaline aluminum solution is 3+ The concentration is 0.1-0.5 mol / L, and the molar concentration of the sodium hydroxide solution is 5-10 mol / L.

[0012] Furthermore, in step S3, the concentration of the complexing agent is 10 to 15 mol / L, and the complexing agent is at least one of EDTA, ammonia water, ammonium carbonate, and ammonium hydrogen carbonate.

[0013] Further, in step S3, the coprecipitation reaction is divided into four stages: a first stage in which the nuclei are grown from the formation of the nuclei to a D150 of 25%≦D150<40% of the target value, a second stage in which the spherical secondary particles are grown to a D250 of 40%≦D250<60% of the target value, a third stage in which the spherical secondary particles are grown to a D350 of 60%≦D350<90% of the target value, and a fourth stage in which the growth reaction is immediately stopped when the spherical secondary particles grow to the target value. In each stage, the flow rate of the nickel-cobalt mixed salt solution is 1-3.5 L / h, the flow rate of the alkali aluminum solution is 1-2 L / h, the flow rate of the complexing agent is 0.5-1.5 L / h, the pH is controlled to 10-12, the reaction temperature in each stage is controlled to 55-70° C., and the stirring speed in each stage is 500-1000 rpm.

[0014] Furthermore, in step S4, the washing is specifically performed by washing the material obtained from the reaction with an alkaline solution first, and then washing with deionized water at 25 to 80°C, the resistivity of the washing water after washing is less than 0.02 cm / μs, the alkaline solution is at least one of a sodium carbonate solution and a sodium hydroxide solution, and the molar concentration of the alkaline solution is 4.0 to 5.0 mol / L.

[0015] The present invention provides a method for producing a positive electrode material for a lithium ion battery, and the method includes obtaining a nickel-cobalt-aluminum precursor by the above-mentioned method, uniformly mixing the obtained precursor with a lithium source and an additive, and performing primary sintering, crushing, pulverizing, washing with water, oven drying, coating, secondary sintering and sieving to obtain a positive electrode material.

[0016] Furthermore, the lithium source is at least one of lithium hydroxide, lithium nitrate, and lithium chloride, the additive is one or more of elements Zr, Sr, Ti, W, Mg, Y, La, B, and F, the coating agent used during coating is one or more of element D-containing oxides and element D-containing lithium compounds, element D is one or more of Co, Li, B, W, Ti, Ce, and Zr, the molar ratio of Ni+CO+Al:Li is 1:1.01-1.05, and the mass ratio of the additive used to the total mass of the precursor and lithium salt is 0.1%-2%. When performing the first sintering, the material was calcined in an oxygen atmosphere furnace, the calcination temperature was 650-800°C, the calcination time was 10-15h, and the oxygen content in the atmosphere furnace was 85%-95%, to obtain a first sintered substrate. The obtained primary sintered substrate is crushed and washed with deionized water, where the mass ratio of the primary sintered substrate to water is 1:1-3, and the temperature of the deionized water is 20-30°C, centrifuged, and oven-dried to obtain a dry substrate. The obtained dry substrate is uniformly mixed with a coating agent, where the mass ratio of the coating agent to the dry substrate is 0.01-5%. Then, the secondary sintering is performed and calcined in an oxygen atmosphere furnace, where the calcination temperature is 500-700°C, the calcination time is 6-10h, and the oxygen content in the atmosphere furnace is 90%-95%, to obtain the positive electrode material.

[0017] The present invention further provides a positive electrode material for a lithium ion battery obtained by the above production method. Effect of the Invention

[0018] The beneficial effects of the present invention are as follows: 1. NCA cathode material has higher energy density than conventional cathode materials LiNiO2 and LiCoO2, and 3+ and Co 3+ The same valence and similar ionic radius (Al 3+ The ionic radius of Co is 0.535 Å. 3+The ionic radius of Al is 0.545 Å. However, since the bond energy of the Al-O covalent bond is stronger, the doping of Al can reduce the intermixing and arrangement of lithium nickel, which is favorable for stabilizing the structure of the material. 3+ The doping of Ni is not only favorable for the transfer of heat generated by the decomposition of the electrolyte, but also reduces the oxidizing ability of the material against the electrolyte, improving the thermal stability of the material. However, the manufacturing process of the NCA precursor is technically difficult. The pH values ​​at which the elements Ni, Co, and Al precipitate are significantly different, and their solubility product constants are 10 for nickel hydroxide. -16 In the case of cobalt hydroxide, 10 -14.9 In the case of aluminum hydroxide, 10 -33 Al(OH)3 is an amphoteric hydroxide, which tends to precipitate at low pH values ​​and AlO2 at high pH values. -1 The present invention can strictly control the pH value and time of coprecipitation of the three elements in each step to prepare a nickel-cobalt-aluminum precursor having multi-layered ring pores, and the preparation method has a simple process, low cost, and is suitable for industrial production.

[0019] 2. Compared with conventional precursors, the spherical secondary structure of the precursor has a large internal space between the primary particles, and the positive electrode material inherits many of the morphological structure and physical property indicators of the precursor. In the positive electrode material prepared by the present invention, the doped and coated elements penetrate not only the surface of the spherical secondary particles but also into the annular pores to protect the primary particles that compose the spherical secondary particles. The electrolyte penetrates into the multi-layer annular pores of the positive electrode material to expand the contact area between the positive electrode material and the electrolyte, and the Li + The multi-layer annular pores can reduce the volume change of the positive electrode material during charging and discharging, and can stabilize the structure and improve the cycle performance. [Brief description of the drawings]

[0020] [Figure 1] FIG. 2 is a cross-sectional scanning electron microscope view of the precursor of Example 1. [Diagram 2] FIG. 2 is a cross-sectional scanning electron microscope view of the precursor of Example 2. [Diagram 3] FIG. 2 is a cross-sectional scanning electron microscope image of the precursor of Comparative Example 1. [Figure 4] FIG. 2 is a cross-sectional scanning electron microscope image of the precursor of Comparative Example 2. [Diagram 5] FIG. 2 is a comparison diagram of the rate performance of the positive electrode materials produced in Examples 1, 2, 3, and 4 and Comparative Examples 1, 2, 3, and 4. [Figure 6] 1 is a comparison diagram of the cycle performance of the positive electrode materials prepared in Examples 1, 2, 3, 4 and Comparative Examples 1, 2, 3, 4. (Table 1) is a comparison diagram of the porosity of the precursors, the discharge capacity of the positive electrode materials, and the DCR performance of the positive electrode materials prepared in Examples 1, 2, 3, 4 and Comparative Examples 1, 2, 3, 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] The concept, specific structure and achieved technical effects of the present application will be clearly and completely described below with reference to the embodiments.

[0022] Example 1 1. A method for producing a multi-layer annular hole nickel-cobalt-aluminum precursor, comprising the following steps S1 to S5:

[0023] In S1, nickel sulfate and cobalt sulfate powders are weighed and dissolved in pure water to prepare a nickel and cobalt mixed salt solution according to a Ni:Co molar ratio of 0.875:0.09, and the molar concentration of total metal ions in the nickel and cobalt mixed salt solution is 2.0 mol / L.

[0024] In S2, sodium metaaluminate is weighed and added to the sodium hydroxide solution, and Al 3+ An alkaline aluminum solution with a molar concentration of 0.1 mol / L was prepared.

[0025] In S3, the nickel-cobalt mixed salt solution of S1, the alkali aluminum solution of S2, and 12 mol / L ammonia water complexing agent were pumped into the reaction vessel at the same time, and coprecipitation reaction was carried out while stirring. The coprecipitation reaction was divided into four stages, and the temperature was controlled at 55°C in all stages. In the first stage, the nickel-cobalt mixed salt solution with a flow rate of 2.52 L / h, the alkali aluminum solution with a flow rate of 1.8 L / h, and the complexing agent solution with a flow rate of 0.5-1.5 L / h were pumped into the reaction vessel, the pH value was controlled at 11.89±0.1, the stirring speed was set to 850 rpm, and the particles D50 in the reaction vessel were grown to 4-6 μm. In the second stage, the nickel-cobalt mixed salt solution with a flow rate of 2.45 L / h, the alkali aluminum solution with a flow rate of 1.5 L / h, and the complexing agent solution with a flow rate of 0.5-1.5 L / h were pumped into the reactor, the pH value was controlled to 11.62 ± 0.1, the stirring speed was set to 550 rpm, and the particles in the reactor D50 were grown to 6-9 μm. In the third stage, the nickel-cobalt mixed salt solution with a flow rate of 2.55 L / h, the alkali aluminum solution with a flow rate of 1.65 L / h, and the complexing agent solution with a flow rate of 0.5-1.5 L / h were pumped into the reactor, the pH value was controlled to 11.45 ± 0.1, the stirring speed was set to 650 rpm, and the particles in the reactor were grown to 9-13 μm. In the fourth stage, the nickel-cobalt mixed salt solution with a flow rate of 2.55 L / h, the alkali aluminum solution with a flow rate of 1.65 L / h, and the complexing agent solution with a flow rate of 0.5-1.5 L / h were pumped into the reaction vessel, the pH value was controlled at 11.65±0.1, the stirring speed was set to 500 rpm, and the particles D50 in the reaction vessel were grown to 15±1 μm, and then the process was stopped.

[0026] In S4, the overflow liquid of the reaction kettle in S3 is collected and concentrated, and the material obtained from the reaction is first washed with sodium hydroxide solution and then washed with deionized water at 25°C, the resistivity of the washing water after washing is less than 0.02cm / μs, and the molar concentration of the alkaline solution is 4.0-5.0mol / L. The oven drying temperature is 105°C, and the moisture is controlled to be less than 0.5wt%. The content of magnetic foreign matter in the precursor needs to be controlled to be less than 100ppb.

[0027] In this manufacturing method, a nickel-cobalt-aluminum precursor Ni having a D50 of 15.097, a porosity of 8.348, and a multi-layer annular pore structure is obtained. 0.875 Co 0.09 Al 0.035 (OH)2 can be obtained.

[0028] In S5, the nickel cobalt aluminum precursor obtained in S4, the lithium salt, and the additive are mixed uniformly. The lithium salt used in S5 is lithium hydroxide, the additive used is ZrO2, the molar ratio of (Ni+CO+Al):Li is 1:1.03, and the mass ratio of ZrO2 to the total mass of the precursor and the lithium salt is 0.3%. Calcination is performed in an oxygen atmosphere furnace, the calcination temperature is 720°C, the calcination time is 10h, and the oxygen content in the atmosphere furnace is 90%-95%, to obtain a primary sintered substrate. The obtained primary sintered substrate is crushed and washed with deionized water, where the mass ratio of the primary sintered substrate to water is 1:1.5, the temperature of the deionized water is 25°C, and the substrate is centrifuged and oven-dried to obtain a dry substrate. The obtained dry substrate is mixed uniformly with cerium oxide, which is a coating material, and the mass ratio of cerium oxide to the dry substrate is 0.1%. Then, it was calcined in an oxygen atmosphere furnace, the calcination temperature was 650°C, the calcination time was 8h, the oxygen content in the atmosphere furnace was 90%-95%, and Li 1.03 Ni 0.875 Co 0.09 Al 0.035 Zr 0.003 The positive electrode material of O2@CeO2 was obtained.

[0029] Using an argon ion cross section plotter, the Ni 0.875 Co 0.09 Al 0.035 The (OH)2 nickel cobalt aluminum precursor was cut and the cross-sectional morphology was observed using a field emission scanning electron microscope, and the test results are shown in Figure 1.

[0030] ImageJ was used to perform particle porosity analysis on the cross-sectional view of the precursor, and the calculation of particle cross-sectional porosity was mainly based on the proportion of pores in the particle. ImageJ needs to make one copy of the original image, the original image is used to extract the pore area, and the copy image is used to extract the area of ​​the particle after filling the pores, and the ratio of the two is the particle cross-sectional porosity. The test results are shown in Table 1.

[0031] 2. Electrical performance test A full cell 18650 was constructed and used to test the electrical performance of the cathode materials in Example 1, with the cathode material (96.5%), SuperP (1.2%), CNT (0.5%), PVDF (1.8%), and the anode material graphite, with the anode material graphite (94.8%), CMC (1.7%), SBR (2%), and SuperP (1.5%). The capacity ratio of the cathode / anode in the full cell design is 1 / 1.2.

[0032] 1) Gram capacity test: Assembled into an 18650 cylindrical battery, then formed and capacity graded. The formation voltage was 2.75 to 4.2 V, and the initial efficiency (initial efficiency % = 0.2 C discharge capacity / initial charge capacity) and 0.2 C discharge gram capacity were calculated, and the results are shown in Table 1.

[0033] 2) Rate performance test: After the assembled 18650 cylindrical battery was subjected to chemical formation and capacity grading, the formed battery was subjected to discharge tests at different rates at a room temperature of 25°C and within a voltage range of 2.75 to 4.2V. The charge rate was 0.5C, and the discharge rates were 0.5C, 1C, 2C, and 3C, respectively. The discharge capacity retention rates at different rates were calculated, and the results are shown in Table 1.

[0034] 3) Cycle performance test: After the assembled 18650 cylindrical battery was subjected to conventional formation and capacity grading, the formed battery was charged at a rate of 0.5 C and discharged at a rate of 1 C at a room temperature of 25° C. and within a voltage range of 2.75 to 4.2 V. The results of the capacity retention are shown in FIG. 6.

[0035] 4) DCR performance test: After the assembled 18650 cylindrical battery was subjected to conventional formation and capacity grading, a room temperature DCR test was performed. The process of the room temperature DCR test is as follows: The formed battery was fully charged at 1C rate at room temperature of 25°C and within the voltage range of 2.75 to 4.2V, and then left to stand, and then discharged to 50% SOC and 10% SOC at 1C rate and left to stand, and then pulse discharged at 1C for 10s, and the voltage change before and after the pulse discharge was recorded, and the DCR data at room temperature 50% SOC and 10% SOC was obtained according to the calculation formula DCR = (end voltage of standing - voltage after pulse discharge) / pulse current, and the results are shown in Table 1.

[0036] Example 2 In S1, nickel sulfate and cobalt sulfate powders are weighed and dissolved in pure water to prepare a nickel and cobalt mixed salt solution according to a Ni:Co molar ratio of 0.92:0.03, and the molar concentration of total metal ions in the nickel and cobalt mixed salt solution is 2.0 mol / L.

[0037] In S2, sodium metaaluminate is weighed and added to the sodium hydroxide solution, and Al 3+ An alkaline aluminum solution with a molar concentration of 0.5 mol / L was prepared.

[0038] In S3, the nickel-cobalt mixed salt solution of S1, the alkali aluminum solution of S2, and 12 mol / L ammonia water complexing agent were pumped into the reaction vessel at the same time, and coprecipitation reaction was carried out while stirring. The coprecipitation reaction was divided into four stages, and the temperature was controlled at 55°C in all stages. In the first stage, the nickel-cobalt mixed salt solution with a flow rate of 2.55 L / h, the alkali aluminum solution with a flow rate of 1.85 L / h, and the complexing agent solution with a flow rate of 0.5-1.5 L / h were pumped into the reaction vessel, the pH value was controlled at 11.92±0.1, the stirring speed was set to 850 rpm, and the particles D50 in the reaction vessel were grown to 4-6 μm. In the second stage, the nickel-cobalt mixed salt solution with a flow rate of 2.43 L / h, the alkali aluminum solution with a flow rate of 1.45 L / h, and the complexing agent solution with a flow rate of 0.5-1.5 L / h were pumped into the reaction vessel simultaneously, the pH value was controlled to 11.65 ± 0.1, the stirring speed was set to 550 rpm, and the particle D50 in the reaction vessel was grown to 6-9 μm. In the third stage, the nickel-cobalt mixed salt solution with a flow rate of 2.5 L / h, the alkali aluminum solution with a flow rate of 1.65 L / h, and the complexing agent solution with a flow rate of 0.5-1.5 L / h were pumped into the reaction vessel simultaneously, the pH value was controlled to 11.48 ± 0.1, the stirring speed was set to 650 rpm, and the particle in the reaction vessel was grown to 9-13 μm. In the fourth stage, the nickel-cobalt mixed salt solution with a flow rate of 2.5 L / h, the alkali aluminum solution with a flow rate of 1.6 L / h, and the complexing agent solution with a flow rate of 0.5 to 1.5 L / h were simultaneously pumped into the reaction vessel, the pH value was controlled at 11.54 ± 0.1, the stirring speed was set to 500 rpm, and the particles D50 in the reaction vessel were grown to 15 ± 1 μm, and then the process was stopped.

[0039] In S4, the overflow liquid from the reaction kettle in S3 is collected and concentrated, and the material obtained from the reaction is first washed with sodium hydroxide solution and then washed with deionized water at 25°C, the resistivity of the washing water after washing is less than 0.02cm / μs, and the molar concentration of the alkaline solution is 4.0-5.0mol / L. The oven drying temperature is 105°C, and the moisture is controlled to be less than 0.5wt%. The content of magnetic foreign matter in the precursor needs to be controlled to be less than 100ppb.

[0040] In this manufacturing method, a nickel-cobalt-aluminum precursor Ni having a D50 of 14.792, a porosity of 9.465, and a multi-layer ring pore structure is obtained. 0.92 Co 0.03 Al 0.05 (OH)2 can be obtained.

[0041] In S5, the nickel cobalt aluminum precursor obtained in S4, the lithium salt, and the additive are mixed uniformly. The lithium salt used in S5 is lithium hydroxide, the additive used is ZrO2, the molar ratio of (Ni+CO+Al):Li is 1:1.03, and the mass ratio of ZrO2 to the total mass of the precursor and the lithium salt is 0.3%. Calcination is performed in an oxygen atmosphere furnace, the calcination temperature is 700°C, the calcination time is 10h, and the oxygen content in the atmosphere furnace is 90%-95%, to obtain a primary sintered substrate. The obtained primary sintered substrate is crushed and washed with deionized water, where the mass ratio of the primary sintered substrate to water is 1:1.5, the temperature of the deionized water is 25°C, and the substrate is centrifuged and oven-dried to obtain a dry substrate. The obtained dry substrate is mixed uniformly with cerium fluoride, which is a coating material, and the mass ratio of cerium fluoride to the dry substrate is 0.2%. Then, it was calcined in an oxygen atmosphere furnace, the calcination temperature was 650°C, the calcination time was 8h, the oxygen content in the atmosphere furnace was 90%-95%, and Li 1.03 Ni 0.92 Co 0.03 Al 0.05 Zr 0.003 The O2@CeF4 cathode material was obtained.

[0042] Using an argon ion cross section plotter, the Ni 0.92 Co 0.03 Al 0.05 The (OH)2 nickel cobalt aluminum precursor was cut and the cross-sectional morphology was observed using a field emission scanning electron microscope, and the test results are shown in Figure 2.

[0043] The precursor cross-sectional porosity test method was the same as in Example 1, and the results were shown in Table 1.

[0044] The manufacturing process of the 18650 cylindrical battery was the same as in Example 1, and the electrical performance was tested under the same test conditions. The results are shown in Table 1, Figures 5 and 6.

[0045] Example 3 Referring to S1 to S4 in Example 1, the nickel-cobalt-aluminum precursor Ni had a D50 of 15.097, a porosity of 8.348, and a multi-layer annular pore structure. 0.875 Co 0.09 Al 0.035 (OH)2 can be obtained.

[0046] In S5, the nickel cobalt aluminum precursor obtained in S4, the lithium salt, and the additive are mixed uniformly. The lithium salt used in S5 is lithium hydroxide, the additive used is B2O3, the molar ratio of (Ni+CO+Al):Li is 1:1.03, and the mass ratio of B2O3 to the total mass of the precursor and the lithium salt is 0.15%. Calcination is performed in an oxygen atmosphere furnace, the calcination temperature is 720°C, the calcination time is 10h, and the oxygen content in the atmosphere furnace is 90%-95%, to obtain a primary sintered substrate. The obtained primary sintered substrate is crushed and washed with deionized water, where the ratio of the primary sintered substrate to water is 1:1.5, the temperature of the deionized water is 25°C, and the substrate is centrifuged and oven-dried to obtain a dry substrate. The obtained dry substrate is mixed uniformly with zirconia, which is a coating material, and the mass ratio of zirconia to the dry substrate is 0.1%. Then, it was calcined in an oxygen atmosphere furnace, the calcination temperature was 600°C, the calcination time was 8h, the oxygen content in the atmosphere furnace was 90%-95%, and Li 1.03 Ni 0.875 Co 0.09 Al 0.035 B 0.0015 The positive electrode material of O2@ZrO2 was obtained.

[0047] The precursor cross-sectional porosity test method was the same as in Example 1, and the results were shown in Table 1.

[0048] The manufacturing process of the 18650 cylindrical battery was the same as in Example 1, and the electrical performance was tested under the same test conditions. The results are shown in Table 1, Figures 5 and 6.

[0049] Example 4 Referring to S1 to S4 in Example 2, the nickel-cobalt-aluminum precursor Ni had a D50 of 14.792, a porosity of 9.465, and a multi-layer annular pore structure. 0.92 Co 0.03 Al 0.05 (OH)2 was obtained.

[0050] In S5, the nickel cobalt aluminum precursor obtained in S4, the lithium salt, and the additive are mixed uniformly. The lithium salt used in S5 is lithium hydroxide, the additive used is B2O3, the molar ratio of (Ni+CO+Al):Li is 1:1.03, and the mass ratio of B2O3 to the total mass of the precursor and the lithium salt is 0.1%. Calcination is performed in an oxygen atmosphere furnace, the calcination temperature is 700°C, the calcination time is 10h, and the oxygen content in the atmosphere furnace is 90%-95%, to obtain a primary sintered substrate. The obtained primary sintered substrate is crushed and washed with deionized water, where the mass ratio of the primary sintered substrate to water is 1:1.5, the temperature of the deionized water is 25°C, and the substrate is centrifuged and oven-dried to obtain a dry substrate. The mass ratio of boric acid to the dry substrate is 0.05%. Then, it is calcined in an oxygen atmosphere furnace, the calcination temperature is 350°C, the calcination time is 5h, the oxygen content in the atmosphere furnace is 80%~95%, and Li 1.03 Ni 0.92 Co 0.03 Al 0.05 B 0.001 The O2@Li3BO3 positive electrode material was obtained.

[0051] The precursor cross-sectional porosity test method was the same as in Example 1, and the results were shown in Table 1.

[0052] The manufacturing process of the 18650 cylindrical battery was the same as in Example 1, and the electrical performance was tested under the same test conditions. The results are shown in Table 1, Figures 5 and 6.

[0053] Comparative Example 1 1. A conventional method for producing a nickel-cobalt-aluminum precursor and sintering a positive electrode material, which includes the following steps S1 to S5:

[0054] In S1, nickel sulfate and cobalt sulfate powders are weighed and dissolved in pure water to prepare a nickel and cobalt mixed salt solution according to a Ni:Co molar ratio of 0.875:0.09, and the molar concentration of total metal ions in the nickel and cobalt mixed salt solution is 2.0 mol / L.

[0055] In S2, sodium metaaluminate is weighed and added to the sodium hydroxide solution, and Al 3+ An alkaline aluminum solution with a molar concentration of 0.1 mol / L was prepared.

[0056] In S3, the nickel-cobalt mixed salt solution of S1, the alkali aluminum solution of S2, and 12 mol / L ammonia water complexing agent were pumped into the reaction vessel at the same time, and coprecipitation reaction was carried out while stirring. No stage process adjustment was made during the growth of precursor D50, and the temperature in the reaction vessel was controlled to 55°C overall, the pH value of the entire reaction was maintained at 11.2-12.2, and the stirring speed was 600±100 rpm. When the particles D50 in the reaction vessel grew to 15±1 μm, the reaction was stopped.

[0057] In S4, the overflow liquid of the reaction kettle in S3 is collected and concentrated, and the material obtained from the reaction is first washed with sodium hydroxide solution and then washed with deionized water at 25°C, the resistivity of the washing water after washing is less than 0.02cm / μs, and the molar concentration of the alkaline solution is 4.0-5.0mol / L. The oven drying temperature is 105°C, and the moisture is controlled to be less than 0.5wt%. The content of magnetic foreign matter in the precursor needs to be controlled to be less than 100ppb.

[0058] In this manufacturing method, D50=14.837, porosity is 2.12, and Ni with conventional dense morphology is obtained. 0.875 Co 0.09 Al 0.035 (OH)2 nickel cobalt aluminum precursor was obtained.

[0059] In S5, the nickel cobalt aluminum precursor obtained in S4, the lithium salt, and the additive are mixed uniformly. The lithium salt used in S5 is lithium hydroxide, the additive used is ZrO2, the molar ratio of (Ni+CO+Al):Li is 1.01-1.05:1, and the mass ratio of ZrO2 to the total mass of the precursor and the lithium salt is 0.3%. Calcination is performed in an oxygen atmosphere furnace, the calcination temperature is 720°C, the calcination time is 10h, and the oxygen content in the atmosphere furnace is 90%-95%, to obtain a primary sintered substrate. The obtained primary sintered substrate is crushed and washed with deionized water, where the mass ratio of the primary sintered substrate to water is 1:1.5, the temperature of the deionized water is 25°C, and the substrate is centrifuged and oven-dried to obtain a dry substrate. The obtained dry substrate is mixed uniformly with cerium oxide, which is a coating material, and the mass ratio of cerium oxide to the dry substrate is 0.1%. Then, it was calcined in an oxygen atmosphere furnace, the calcination temperature was 650°C, the calcination time was 8h, the oxygen content in the atmosphere furnace was 90%-95%, and Li 1.03 Ni 0.875 Co 0.09 Al 0.035 Zr 0.003 The positive electrode material of O2@CeO2 was obtained.

[0060] Using an argon ion cross section plotter, the Ni 0.875 Co 0.09 Al 0.035 The (OH)2 nickel cobalt aluminum precursor was cut and the cross-sectional morphology was observed using a field emission scanning electron microscope, and the test results are shown in Figure 3.

[0061] The precursor cross-sectional porosity test method was the same as in Example 1, and the results were shown in Table 1.

[0062] The manufacturing process of the 18650 cylindrical battery was the same as in Example 1, and the electrical performance was tested under the same test conditions. The results are shown in Table 1, Figures 5 and 6.

[0063] Comparative Example 2 In S1, nickel sulfate and cobalt sulfate powders are weighed and dissolved in pure water to prepare a nickel and cobalt mixed salt solution according to a Ni:Co molar ratio of 0.92:0.03, and the molar concentration of total metal ions in the nickel and cobalt mixed salt solution is 2.0 mol / L.

[0064] In S2, sodium metaaluminate is weighed and added to the sodium hydroxide solution, and Al 3+ An alkaline aluminum solution with a molar concentration of 0.5 mol / L was prepared.

[0065] In S3, the nickel-cobalt mixed salt solution in S1, the alkali aluminum solution in S2, and 12 mol / L ammonia water complexing agent were simultaneously pumped into a reaction vessel, and coprecipitation reaction was carried out while stirring.

[0066] No stage adjustment was made during the growth of the precursor D50, the temperature in the reactor was controlled at 55°C, the pH value of the whole reaction was maintained at 11.2-12.2, and the stirring speed was 600±100 rpm. The reaction was stopped when the particles D50 in the reactor grew to 15±1 μm.

[0067] In S4, the overflow liquid of the reaction kettle in S3 is collected and concentrated, and the material obtained from the reaction is first washed with sodium hydroxide solution and then washed with deionized water at 25°C, the resistivity of the washing water after washing is less than 0.02cm / μs, and the molar concentration of the alkaline solution is 4.0-5.0mol / L. The oven drying temperature is 105°C, and the moisture is controlled to be less than 0.5wt%. The content of magnetic foreign matter in the precursor needs to be controlled to be less than 100ppb.

[0068] In this manufacturing method, D50=15.167, porosity is 1.95, and Ni with conventional dense morphology is obtained. 0.92 Co 0.03 Al 0.05 (OH)2 nickel cobalt aluminum precursor was obtained.

[0069] In S5, the nickel cobalt aluminum precursor obtained in S4, the lithium salt, and the additive are mixed uniformly. The lithium salt used in S5 is lithium hydroxide, the additive used is ZrO2, the molar ratio of (Ni+CO+Al):Li is 1.01-1.05:1, and the mass ratio of ZrO2 to the total mass of the precursor and the lithium salt is 0.3%. Calcination is performed in an oxygen atmosphere furnace, the calcination temperature is 700°C, the calcination time is 10h, and the oxygen content in the atmosphere furnace is 90%-95%, to obtain a primary sintered substrate. The obtained primary sintered substrate is crushed and washed with deionized water, where the mass ratio of the primary sintered substrate to water is 1:1.5, the temperature of the deionized water is 25°C, and the substrate is centrifuged and oven-dried to obtain a dry substrate. The mass ratio of cerium fluoride to the dry substrate is 0.2%. Then, it was calcined in an oxygen atmosphere furnace, the calcination temperature was 650°C, the calcination time was 8h, the oxygen content in the atmosphere furnace was 90%-95%, and Li 1.03 Ni 0.92 Co 0.03 Al 0.05 Zr 0.003 The O2@CeF4 cathode material was obtained.

[0070] Using an argon ion cross section plotter, the Ni 0.92 Co 0.03 Al 0.05 The (OH)2 nickel cobalt aluminum precursor was cut and the cross-sectional morphology was observed using a field emission scanning electron microscope, and the test results are shown in Figure 4.

[0071] The precursor cross-sectional porosity test method was the same as in Example 1, and the results were shown in Table 1.

[0072] The manufacturing process of the 18650 cylindrical battery was the same as in Example 1, and the electrical performance was tested under the same test conditions. The results are shown in Table 1, Figures 5 and 6.

[0073] Comparative Example 3 With reference to S1 to S4 in Comparative Example 1, D50=14.837, porosity is 2.12, and Ni has a conventional dense form. 0.875 Co 0.09 Al 0.035(OH)2 nickel cobalt aluminum precursor was obtained.

[0074] In S5, the nickel cobalt aluminum precursor obtained in S4, the lithium salt, and the additive are mixed uniformly. The lithium salt used in S5 is lithium hydroxide, the additive used is B2O3, the molar ratio of (Ni+CO+Al):Li is 1.03:1, and the mass ratio of B2O3 to the total mass of the precursor and the lithium salt is 0.15%. Calcination is performed in an oxygen atmosphere furnace, the calcination temperature is 720°C, the calcination time is 10h, and the oxygen content in the atmosphere furnace is 90%-95%, to obtain a primary sintered substrate. The obtained primary sintered substrate is crushed and washed with deionized water, where the mass ratio of the primary sintered substrate to water is 1:1.5, the temperature of the deionized water is 25°C, and the substrate is centrifuged and oven-dried to obtain a dry substrate. The obtained dry substrate is mixed uniformly with zirconia, which is a coating material, and the mass ratio of zirconia to the dry substrate is 0.1%. Then, it was calcined in an oxygen atmosphere furnace, the calcination temperature was 600°C, the calcination time was 8h, the oxygen content in the atmosphere furnace was 90%-95%, and Li 1.03 Ni 0.875 Co 0.09 Al 0.035 B 0.0015 The positive electrode material of O2@ZrO2 was obtained.

[0075] The precursor cross-sectional porosity test method was the same as in Example 1, and the results were shown in Table 1.

[0076] The manufacturing process of the 18650 cylindrical battery was the same as in Example 1, and the electrical performance was tested under the same test conditions. The results are shown in Table 1, Figures 5 and 6.

[0077] Comparative Example 4 With reference to S1 to S4 in Comparative Example 2, D50=15.167, porosity is 3.34, and Ni has a conventional dense form. 0.92 Co 0.03 Al 0.05 (OH)2 nickel cobalt aluminum precursor was obtained.

[0078] In S5, the nickel cobalt aluminum precursor obtained in S4, the lithium salt, and the additive are mixed uniformly. The lithium salt used in S5 is lithium hydroxide, the additive used is B2O3, the molar ratio of (Ni+CO+Al):Li is 1.03:1, and the mass ratio of B2O3 to the total mass of the precursor and the lithium salt is 0.1%. Calcination is performed in an oxygen atmosphere furnace, the calcination temperature is 700°C, the calcination time is 10h, and the oxygen content in the atmosphere furnace is 90%-95%, to obtain a primary sintered substrate. The obtained primary sintered substrate is crushed and washed with deionized water, where the mass ratio of the primary sintered substrate to water is 1:1.5, the temperature of the deionized water is 25°C, and the substrate is centrifuged and oven-dried to obtain a dry substrate. The mass ratio of boric acid to the dry substrate is 0.05%. Then, it was calcined in an oxygen atmosphere furnace, the calcination temperature was 350°C, the calcination time was 5h, and the oxygen content in the atmosphere furnace was 80%-95%. 1.03 Ni 0.92 Co 0.03 Al 0.05 B 0.001 The O2@Li3BO3 positive electrode material was obtained.

[0079] The precursor cross-sectional porosity test method was the same as in Example 1, and the results were shown in Table 1.

[0080] The manufacturing process of the 18650 cylindrical battery was the same as in Example 1, and the electrical performance was tested under the same test conditions. The results are shown in Table 1, Figures 5 and 6. [Table 1]

[0081] The experimental data are divided into two sets, Example 1 and Comparative Example 1, and Example 2 and Comparative Example 2. As can be seen from the experimental data results, the precursor coprecipitation reaction process can be obtained by strictly controlling the pH value, rotation speed, and solution flow rate during the reaction in separate steps, and the precursor with multi-layer annular pores can be obtained. In the comparative example, the precursor with this morphology cannot be obtained by not adjusting the reaction steps or adjusting it in a manner that does not follow this method. The morphology has a large effect on the porosity index. Among the positive electrode materials with the same nickel-cobalt-aluminum ratio, those with relatively large porosity values ​​have high initial discharge gram capacity. The positive electrode material inherits the internal space structure of the precursor, which allows more electrolyte to penetrate and provides more lithium ion diffusion paths, and can accelerate the absorption and release rate of lithium ions. Therefore, Examples 1 and 2 have higher initial discharge specific capacity and lower internal resistance than Comparative Examples 1 and 2. Furthermore, comparing the two sets of data between Example 3 and Comparative Example 3, and between Example 4 and Comparative Example 4, it can be seen that doping or coating with different elements can improve the electrical performance of the cathode materials to a certain extent, but still cannot improve the advantages inherited from the precursor structure itself.

[0082] The experimental data results further show that among the positive electrode materials with the same nickel-cobalt-aluminum ratio, those with a relatively large porosity value have excellent cycle performance, and the positive electrode inherits the porous structure between the primary particles from the precursor, and after the precursor is lithiated and sintered, there are many voids between the primary particles, and the elements coated by the secondary sintering also penetrate to the surface of the primary particles, which can protect the positive electrode material and improve the side reaction caused by the electrolyte. It is known that the change in morphology has a significant impact on the cycle stability of nickel-rich NCA positive electrodes, and the phase change near the end of charging causes crystal lattice shrinkage in the positive electrode. The appropriate voids between the primary particles allow the internal strain caused by the phase change to be distributed evenly, which ensures the dissipation of the strain force, thereby improving the cycle characteristics.

Claims

1. A multi-layer annular pore nickel cobalt aluminum precursor comprising: The chemical formula is Ni M Co N A 1-M-N (OH) 2 0.8≦M≦0.97, 0.02≦N≦0.09, 0.01≦1−M−N≦0.055, with the proviso that D50 is 8 μm to 20 μm, and the spherical secondary particle structure of the precursor has multi-layer annular pores, and the porosity value, which is the cross-sectional average value of one spherical secondary particle or a plurality of spherical secondary particles, is 6% to 14%. A multi-layer annular pore nickel-cobalt-aluminum precursor comprising:

2. 2. A method for producing the multi-layer annular hole nickel-cobalt-aluminum precursor of claim 1, comprising: S1: Weighing nickel sulfate and cobalt sulfate powders and dissolving them in pure water to prepare a nickel-cobalt mixed salt solution; S2: weighing aluminum salt and adding it to the sodium hydroxide solution to prepare an alkaline aluminum solution; S3, in which the nickel-cobalt mixed salt solution of S1, the alkali aluminum solution of S2, and a complexing agent are simultaneously pumped into a reaction vessel to carry out a coprecipitation reaction stepwise; After the reaction is completed, the material obtained from the reaction is subjected to solid-liquid separation, washing, oven drying, uniform mixing, sieving, and demagnetization to obtain a nickel-cobalt-aluminum precursor. A method for producing a multi-layer annular hole nickel-cobalt-aluminum precursor, comprising:

3. In step S1, the concentration of total metal ions in the nickel-cobalt mixed salt solution is 1.0 mol / L to 2.0 mol / L; The method for producing a multi-layer annular hole nickel-cobalt-aluminum precursor according to claim 2 .

4. In step S2, the aluminum salt is sodium metaaluminate, and the Al in the alkaline aluminum solution is 3+The concentration is 0.1 mol / L to 0.5 mol / L, and the molar concentration of the sodium hydroxide solution is 5 mol / L to 10 mol / L; The method for producing a multi-layer annular hole nickel-cobalt-aluminum precursor according to claim 2 .

5. In step S3, the concentration of the complexing agent is 10 mol / L to 15 mol / L, and the complexing agent is at least one of EDTA, ammonia water, ammonium carbonate, and ammonium bicarbonate. The method for producing a multi-layer annular hole nickel-cobalt-aluminum precursor according to claim 2 .

6. In step S3, after the nuclei are formed, the target value is set to 25% or less. 1 50 < 40% of the target value D 1 The first stage is to grow the secondary particles to 40% of the target value D in the reaction vessel. 2 50 < 60% of the target value D 2 The second stage is to grow the secondary particles to 60% of the target value D in the reaction vessel. 3 50 < 90% of the target value D 3 The coprecipitation reaction is carried out in four stages: the third stage is to grow the secondary particles to a size of 50; and the fourth stage is to immediately stop the growth reaction when the secondary particles in the reaction vessel grow to the target size. In each step, the flow rate of the nickel-cobalt mixed salt solution is 1-3.5L / h, the flow rate of the alkali aluminum solution is 1-2L / h, the flow rate of the complexing agent is 0.5-1.5L / h, the pH is controlled at 10-12, the reaction temperature in each step is controlled at 55-70°C, and the stirring speed in each step is 500-1000rpm. The method for producing a multi-layer annular hole nickel-cobalt-aluminum precursor according to claim 2 .

7. In step S4, the washing is specifically performed by washing the material obtained from the reaction with an alkaline solution first, and then washing with deionized water at 25°C to 80°C, the resistivity of the washing water after washing is less than 0.02 cm / μs, the alkaline solution is at least one of a sodium carbonate solution and a sodium hydroxide solution, and the molar concentration of the alkaline solution is 4.0 mol / L to 5.0 mol / L; The method for producing a multi-layer annular hole nickel-cobalt-aluminum precursor according to claim 2 .

8. The nickel-cobalt-aluminum precursor is obtained by the method of claim 2, and then the obtained precursor is uniformly mixed with a lithium source and an additive, and the mixture is subjected to primary sintering, crushing, pulverization, water washing and oven drying, coating, secondary sintering and sieving to obtain a positive electrode material. A method for producing a positive electrode material for a lithium ion battery, comprising the steps of:

9. The lithium source is at least one of lithium hydroxide, lithium nitrate, and lithium chloride, the additive is one or more of elements Zr, Sr, Ti, W, Mg, Y, La, B, and F, the coating agent used during coating is one or more of oxides containing element D and lithium compounds containing element D, element D being one or more of Co, Li, B, W, Ti, Ce, and Zr, the molar ratio of Ni+CO+Al:Li is 1:1.01 to 1.05, and the mass ratio of the additive used to the total mass of the precursor and the lithium salt is 0.1% to 2%, during the first sintering, calcination is performed in an oxygen atmosphere furnace, the calcination temperature is 650°C-800°C, the calcination time is 10h-15h, and the oxygen content in the atmosphere furnace is 85%-95%; a first sintering substrate is obtained; the obtained first sintering substrate is crushed and washed with deionized water, where the mass ratio of the first sintering substrate to the water is 1:1-3, and the temperature of the deionized water is 20°C-30°C; centrifuged and oven-dried to obtain a dry substrate; the obtained dry substrate is uniformly mixed with a coating agent, where the mass ratio of the coating agent to the dry substrate is 0.01%-5%; Then, the secondary sintering is carried out and calcined in an oxygen atmosphere furnace, the calcination temperature is 500°C to 700°C, the calcination time is 6h to 10h, and the oxygen content in the atmosphere furnace is 90% to 95%, to obtain the positive electrode material; The method for producing a positive electrode material for a lithium ion battery according to claim 8.

10. A positive electrode material for a lithium ion battery produced by the method according to claim 8 or 9.

Citation Information

Patent Citations

  • Precursor for lithium ion battery, positive electrode material and preparation method of precursor

    CN109473667A

  • Nickel-based active material for lithium secondary battery, method of preparing the same, and lithium secondary battery including positive electrode including the same

    JP2020074264A

  • Nickel-based active material precursor for lithium secondary batteries, method for producing the same, nickel-based active material for lithium secondary batteries formed therefrom, and lithium secondary batteries including positive electrodes containing the same

    JP2020513658A

  • Positive electrode active substance for lithium ion secondary battery and method for producing same

    WO2019194150A1