Method for forming a circuit pattern on a substrate using metal foil with low surface roughness
By bonding a thin metal foil with low surface roughness and protrusions to an insulating base, the method addresses adhesion issues in semi-additive processes, enabling reliable and cost-effective formation of fine circuit patterns for high-frequency applications.
Patent Information
- Application Number
- JP2024527452
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-29
- Filing Date
- 2022-11-23
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-11-23
AI Technical Summary
Existing semi-additive processes face challenges in ensuring sufficient adhesion of copper seed layers to insulating bases due to non-uniform surface roughness, which affects the formation of fine circuit patterns.
A method involving bonding a thin metal foil with low surface roughness, featuring protrusions with flat ends, to an insulating base, transferring its surface roughness, and forming via holes for electroless and electroplating to create a circuit pattern.
Ensures strong adhesion to the insulating base, facilitates process control, and allows for the formation of fine circuit patterns at a lower cost, enhancing the reliability and uniformity of circuit patterns, especially for high-frequency applications like 5G devices.
Smart Images

Figure 2024542421000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for forming a circuit pattern on a substrate by a process for forming a circuit pattern, such as a semi-additive process (SAP) or a modified semi-additive process (mSAP), using a thin metal foil having a low surface roughness. [Background technology]
[0002] 2. Description of the Related Art In the manufacture of printed circuit boards, various processes for forming circuit patterns on a substrate are known, such as a subtractive process, an additive process, a full-additive process, a semi-additive process, and a modified semi-additive process.
[0003] According to the semi-additive process (SAP), via holes are processed in a substrate in which a metal base is bonded to an insulating base, electroless copper plating is performed, dry film is bonded, exposed, developed, and then copper electroplating is performed to form a circuit pattern. However, it is difficult to ensure sufficient adhesion to the insulating base by electroless copper plating. Before electroless copper plating, the surface of the insulating base is generally roughened to ensure sufficient adhesion to the insulating base by a desmear process, but there is a limit to roughening the surface of the insulating base, which is more diverse in type and characteristics. That is, when the electroless copper plating of the insulating base on which via holes are formed is performed for subsequent copper electroplating, the copper seed layer formed by electroless copper plating does not show sufficient adhesion (bonding) to the insulating base, which has a negative effect on the formation of a desired circuit pattern.
[0004] Therefore, existing processes have difficulty in ensuring sufficient adhesion to the insulating base. Furthermore, the non-uniform roughness of the insulating base makes it difficult to form microcircuits. Therefore, there is a need to develop a method for ensuring sufficient adhesion to the insulating base to facilitate controlling the process of forming fine circuit patterns. Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention provides a method for forming a circuit pattern on a substrate by a process for forming a circuit pattern, such as SAP or mSAP, using a thin metal foil having a low surface roughness. [Means for solving the problem]
[0006] One aspect of the present invention provides a method for forming a circuit pattern on a substrate, comprising: preparing a substrate having a metal base bonded to an insulating base; bonding a metal foil having one or more flat-topped protrusions onto the insulating base; and transferring the surface roughness of the metal foil to the insulating base.
[0007] In one embodiment, the metal foil may be bonded onto the insulating base such that the flat-topped projection faces a surface of the insulating base.
[0008] In one embodiment, each of the flat-topped protrusions may include a protruding portion having a truncated cone shape or a truncated polygonal pyramid shape, and a flat portion formed at an upper end of the protruding portion.
[0009] In one embodiment, the protrusion may have a plurality of microprotrusions formed on a surface thereof.
[0010] In one embodiment, the surface roughness (Rz) of the metal foil may be 0.05 to 1.5 μm.
[0011] In one embodiment, the metal foil may have a thickness of 5 μm or less.
[0012] In one embodiment, the metal foil may be formed by electroless plating.
[0013] In one embodiment, the unit area (μm 2 1 to 100 holes per 100 microns may be formed in the surface of the insulating base to which the roughness is transferred.
[0014] The present invention also provides a method for forming a circuit pattern on a substrate, the method including: preparing a substrate having a metal base bonded to an insulating base; bonding a metal foil having one or more flat-topped protrusions on the insulating base; forming one or more via holes through the insulating base and the metal foil; forming seed portions on the inner walls of the via holes; disposing a dry film on the metal foil, patterning the dry film, and electroplating the via holes exposed by patterning to form a circuit pattern.
[0015] The present invention also provides a method for forming a circuit pattern on a substrate, the method including: preparing a substrate having a metal base bonded to an insulating base; bonding a metal foil having one or more protrusions with flat upper ends onto the insulating base; peeling off the metal foil having a surface roughness formed by the protrusions to transfer the surface roughness of the metal foil to the insulating base; forming one or more via holes penetrating the insulating base; forming seed portions on a surface of the insulating base having the via holes and on inner walls of the via holes; disposing a dry film on the insulating base on which the seed portions are formed, patterning the dry film; and electroplating the via holes exposed by the patterning to form a circuit pattern. Effect of the Invention
[0016] According to each of the methods of the present invention, the circuit pattern is formed on the substrate by bonding a thin metal foil having a small surface roughness onto an insulating base, forming via holes, and performing electroless plating and / or electroplating. Therefore, the circuit pattern can be formed at low cost while ensuring sufficient adhesive strength (bonding strength) to the insulating base and facilitating process control. [Brief description of the drawings]
[0017] [Figure 1]FIG. 1 is a flow diagram showing a method for forming a circuit pattern on a substrate according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a reference diagram for illustrating the metal foil used in the method of the present invention. [Diagram 3] FIG. 3 is a reference diagram for illustrating the metal foil used in the method of the present invention. [Figure 4] FIG. 4 is a flow diagram illustrating a method for forming a circuit pattern on a substrate according to a further embodiment of the present invention. [Diagram 5] FIG. 5 is an image for explaining the first experimental example. [Figure 6] FIG. 6 is an image for explaining the first experimental example. [Figure 7] FIG. 7 is an image for explaining the second experimental example. [Figure 8] FIG. 8 illustrates a method for forming a circuit using a primer according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] It should be understood that the terms and phrases used in the present specification and claims are not to be construed as having common and dictionary meanings, but are to be construed as having meanings and concepts that correspond to the technical spirit of the present invention in light of the principle that the inventor can appropriately define the concepts of terms and phrases in order to describe the inventor's invention in the best possible manner.
[0019] When an element is described as being "on" another element, it will be understood that it may be directly on the other element or there may be intervening elements. When the element and the other element are in varying positions relative to each other, "on" may be interpreted as "under."
[0020] The individual steps described herein may be performed sequentially, in reverse order, or by appropriately altering the order during processing.
[0021] The present invention is directed to a method for forming a circuit pattern on a substrate, comprising: providing a substrate having a metal foil bonded to an insulating base; bonding a metal foil having one or more flat-topped protrusions onto the insulating base; and transferring the surface roughness of the metal foil to the insulating base.
[0022] With particular reference to FIG. 1, an insulating base is bonded to the top surface of the metallic base to provide the base portion of the substrate.
[0023] The metal base 10 ensures the heat dissipation performance of the board and serves to electrically connect between the multi-layer circuit patterns. The metal base 10 may include one or more metal components generally known in the art. Specifically, the metal base 10 may include one or more metals selected from the group consisting of copper (Cu) and titanium (Ti).
[0024] The insulating base 20 serves to ensure the insulating performance of the board. The insulating base 20 may be made of a material generally known in the art, specifically, a prepreg in which an insulating resin such as an epoxy resin or a polyimide resin is impregnated into a fiber base such as carbon fiber or glass fiber.
[0025] A metal foil 30 having one or more flat-topped projections is bonded onto the insulating base 20 .
[0026] To bond the metal foil 30 onto the insulating base 20, any conventional method for laminating metal foils may be used without particular limitation. Specifically, the metal foil is laminated at a temperature of 100° C. and a pressure of 5 kg / m 2 The laminate was laminated by pressing for 60 seconds at a temperature of 100°C and a pressure of 5 kg / m 2 After pressing, curing may be carried out at 130° C. for 30 minutes and 165° C. for 30 minutes.
[0027] The formation of one or more, i.e., multiple protrusions with flat tops, results in the metal foil 30 having a particular surface feature (structure). With specific reference to Fig. 2, the metal foil 30 may have a structure in which multiple surface protrusions 31 are present (formed) on the surface. The protrusions 31 may be metal crystal particles protruding vertically upward from the surface of the metal foil 30. Specifically, each of the protrusions 31 may include a protruding portion 31b and a flat portion 31a.
[0028] The protruding portion 31b of the projection 31 is a portion protruding from the surface of the metal foil 30, and may have a truncated cone shape or a truncated polygonal pyramid shape. Specifically, as shown in Fig. 3, the protruding portion 31b has a truncated cone shape with a flat surface (outer surface) or a truncated polygonal pyramid shape with a squared surface. This shape enhances the fixation of the metal foil to the insulating base 20 so that the metal foil 30 can be bonded to the insulating base 20 with high adhesive strength. More specifically, the protruding portion 31b may have at least one truncated polygonal pyramid shape selected from the group consisting of a pentagonal truncated pyramid shape, a hexagonal truncated pyramid shape, a heptagonal truncated pyramid shape, and an octagonal truncated pyramid shape.
[0029] Each of the protrusions 31b may have a plurality of micro-projections 31b' to enhance adhesion to the insulating base 20 by increasing the surface area of the insulating base 20. The formation of the micro-projections 31b' enables the protrusions 31b to have a surface roughness (Ra) of 0.05 to 0.3 μm, particularly 0.08 to 0.2 μm. Here, the surface roughness (Ra) of the protrusions 31b may be defined as the surface roughness (Ra) of the outer surface of the protrusions 31b other than the flat portion 31a.
[0030] On the other hand, the ratio of the height (b) of each protrusion 31b to the length (a) of the base of the protrusion 31b may be in the range of 0.4 to 1.5 (b / a), particularly 0.6 to 1.2 (b / a). When the ratio (b / a) is within the above-defined range, the adhesion between the metal foil 30 and the insulating base 20 can be enhanced.
[0031] The flat portion 31a of the protrusion 31 is a flat surface at the upper end of the protruding portion 31. The flat portion 31a may be the upper surface of the protruding portion 31b having a truncated cone shape or a truncated polygonal pyramid shape. Specifically, the flat portion 31a may have a circular, elliptical or polygonal shape. Fine irregularities may be densely formed to provide a flat surface that can be considered to be included within the range of the flat portion 31a.
[0032] In each of the projections 31, the ratio of the length (c) of the flat portion 31a to the length (a) of the base of the protruding portion 31b may be in the range of 0.1 to 0.7 (c / a), particularly 0.2 to 0.6 (c / a). When the ratio (c / a) is within the above-defined range, the adhesion between the metal foil 30 and the insulating base 20 can be enhanced. The length (c) of the flat portion 31a refers to the maximum length in the plane of the flat portion 31a.
[0033] Considering the adhesion between the metal foil 30 and the insulating base 20, the resolution of the circuit pattern, etc., the unit area (1 μm 2 The number of protrusions 31 per unit area may be 25 or less, particularly 5 to 20, and more particularly 7 to 15.
[0034] The metal foil 30 including one or more protrusions 31 may be formed by electroless plating. Specifically, after forming the metal foil 30 by forming a metal seed foil by electroless plating, crystal grains grow continuously on the metal seed foil to form a plurality of protrusions 31 on the surface. By electroless plating, the metal foil 30 has a smaller thickness, a smaller surface roughness, and a larger porosity than electroplating. The metal foil 30 formed by electroless plating can be efficiently introduced into a process for forming a circuit pattern on a substrate.
[0035] The composition of the electroless plating solution used to form the metal foil 30 is not particularly limited, but may include a metal ion source and a nitrogen compound.
[0036] The metal ion source may specifically be a copper ion source selected from the group consisting of copper sulfate, copper chloride, copper nitrate, copper hydroxide, copper sulfamate and mixtures thereof. The metal ion source may be present in a concentration of 0.5 to 300 g / L, in particular 100 to 200 g / L.
[0037] The nitrogen compound diffuses the metal ions to form a plurality of protrusions 31 on the surface of the metal seed foil formed by the metal ion source. Specifically, the nitrogen compound may be selected from the group consisting of purine, adenine, guanine, hypoxanthine, xanthine, pyridazine, methylpiperidine, 1,2-di-(2-pyridyl)ethylene, 1,2-di-(pyridyl)ethylene, 2,2'-dipyridylamine, 2,2'-bipyridyl, 2,2'-bipyrimidine, 6,6'-dimethyl-2,2'-dipyridyl, di-2-furyl ketone, N,N,N',N'-tetraethylenediamine, 1,8-naphthyridine, 1,6-naphthyridine, terpyridine, and mixtures thereof. The nitrogen compound may be present in a concentration of 0.01 to 10 g / L, particularly 0.05 to 1 g / L.
[0038] The electroless plating solution may further include one or more additives selected from the group consisting of a chelating agent, a pH adjuster, and a reducing agent.
[0039] Specifically, the chelating agent may be selected from the group consisting of tartaric acid, citric acid, acetic acid, malic acid, malonic acid, ascorbic acid, oxalic acid, lactic acid, succinic acid, sodium potassium tartrate, dipotassium tartrate, hydantoin, 1-methylhydantoin, 1,3-dimethylhydantoin, 5,5-dimethylhydantoin, nitrilotriacetic acid, triethanolamine, ethylenediaminetetraacetic acid, tetrasodium ethylenediaminetetraacetate, N-hydroxyethylenediaminetriacetate, pentahydroxypropyldiethylenetriamine, and mixtures thereof. The chelating agent may be present in a concentration of 0.5 to 600 g / L, specifically 300 to 450 g / L.
[0040] Specifically, the pH adjuster may be selected from the group consisting of sodium hydroxide, potassium hydroxide, lithium hydroxide, and mixtures thereof. The pH adjuster can adjust the pH of the electroless plating solution to 8 or more, particularly 10 to 14, and more particularly 11 to 13.5.
[0041] Specifically, the reducing agent may be selected from the group consisting of formaldehyde, sodium hypophosphite, sodium hydroxymethanesulfinate, glyoxylic acid, borohydride, dimethylamine borane, and mixtures thereof. The reducing agent may be present in a concentration of 1 to 20 g / L, particularly 5 to 20 g / L.
[0042] The conditions for electroless plating for forming the metal foil 30 may be appropriately adjusted depending on the thickness of the metal foil 30. Specifically, the electroless plating temperature may be 20 to 60° C., particularly 30 to 40° C., and the electroless plating time may be 2 to 30 minutes, particularly 5 to 20 minutes.
[0043] The thickness of the metal foil 30 formed by electroless plating may be 5 μm or less, particularly 0.1 to 1.2 μm. If the thickness of the metal foil 30 is 5 μm or less, the response ability of forming a microcircuit pattern (controlling the line / space (L / S) to 10 to 15 μm) can be enhanced.
[0044] The surface roughness (Rz) of the metal foil 30 is 0.05 to 1.5 μm, preferably 0.05 to 1.0 μm, and more preferably 0.05 to 0.4 μm. As described above, the surface roughness of the metal foil is transferred to the surface of the insulating base. As a result, the surface area of the insulating base is increased, and sufficient adhesion is ensured. If sufficient adhesion is not ensured, the subsequent process may not proceed, or separation or peeling may occur during pattern formation. Furthermore, since the surface roughness of the metal foil used in the present invention is lower than that of the metal foil used in the previous invention, the transmission loss due to the skin depth is small, which is more advantageous for 5G communication using high frequencies.
[0045] There is no particular limitation on the composition of the metal foil 30. Specifically, the metal may be selected from the group consisting of copper, silver, gold, nickel, aluminum, and mixtures thereof.
[0046] In order to bond the metal foil 30 to the insulating base 20, the metal foil 30 is placed on the insulating base 20 so that the multiple protrusions 31 present on the metal foil 30 face the insulating base 20. That is, the surface of the metal foil 30 on which the multiple protrusions 31 are present is bonded to the insulating base 20. This can ensure strong adhesion between the metal foil 30 and the insulating base 20.
[0047] The plurality of protrusions formed on the surface of the metal foil are bonded to the surface of the insulating base so that the surface roughness of the metal foil can be transferred to the insulating base. As described above, the metal foil may be laminated by pressing under a certain pressure. In this process, the surface roughness of the metal foil can be transferred to the surface of the insulating base.
[0048] Specifically, as a result of this transfer, the insulating base may have the same surface roughness as the metal foil, and the surface roughness per unit area (μm 2 ) 2-100 particles / μm, especially 5-20 particles / μm 2 , and especially 7 to 15 particles / μm 2 The holes can ensure high adhesive strength of the insulating base.
[0049] As mentioned above, a metal foil may be directly attached to the surface of the substrate to form holes. Alternatively, a primer may be attached to the surface of the metal foil, the metal foil with the primer attached may be attached to the surface of the substrate, and the metal foil may be removed to roughen the substrate. That is, a primer attached to the metal foil may be used to roughen the surface of the substrate. If a metal foil cannot be used to roughen the surface of the substrate, the use of a primer may be selected. Any material that can be attached to the surface of the substrate and transfer the roughness of the metal foil may be used for the primer. For the subsequent process, the use of a polymer resin is more preferred (see FIG. 8).
[0050] The present invention uses a process for forming a circuit pattern, such as a semi-additive process (SAP) or a modified semi-additive process (mSAP), to form a circuit pattern on a substrate, and is characterized in that a metal foil having specific surface characteristics is bonded to the substrate before forming a via hole, unlike the conventional technique of forming a via hole in the substrate and then performing electroless plating or sputtering to form a seed layer for electroplating on the surface of the substrate and in the via hole. The features of the present invention will be described in detail with reference to the drawings.
[0051] A method for forming a circuit pattern on a substrate according to one embodiment of the present invention includes preparing a substrate having a metal base bonded to an insulating base (step (a)), bonding a metal foil having one or more flat-topped protrusions onto the insulating base (step (b)), forming one or more via holes penetrating the insulating base and the metal foil (step (c)), forming seed portions on the inner walls of the via holes (step (d)), disposing a dry film on the metal foil and patterning the dry film (step (e)), and electroplating the via holes exposed by the patterning to form a circuit pattern (step (f)).
[0052] In step (a), a substrate is prepared in which a metal base 10 is bonded to an insulating base 20. In step (b), a metal foil 30 having one or more protrusions and a flat upper end is bonded onto the insulating base 20. Steps (a) and (b) are the same as those described above, and detailed descriptions thereof will be omitted.
[0053] In step (c), one or more via holes H are formed in the substrate in which the metal base 10 is bonded to the insulating base 20. The via holes H penetrate the metal foil 30 and the insulating base 20, but not the metal base 10. The via holes H can be formed by any suitable method generally known in the art, such as drilling or laser processing. After forming the via holes (H), the method of the present invention may further include roughening the inner walls of the via holes (H) (desmearing, for example, plasma desmearing) and / or removing impurities (for example, ash) present on the surface of the metal foil 30 or in the via holes H.
[0054] In step (d), a seed portion is formed on the inner wall of the via hole H. The seed portion 40 allows for subsequent plating or filling of the via hole H by electroplating. The seed portion 40 may be formed using a conductive material. The seed portion 40 may be formed by coating the inner wall of the via hole H with a conductive resin composition or by electroless plating with an electroless plating solution. The conductive resin composition may include a conductive resin generally known in the art, and the electroless plating solution may include a copper ion source and be generally known in the art.
[0055] In step (e), the dry film 50 is patterned according to a desired circuit pattern. Specifically, the dry film 50 is patterned by placing the dry film 50 on the metal foil 30, exposing the dry film 50, and developing the dry film 50 to form the desired circuit pattern. The exposure and development of the dry film 50 may be performed by any suitable process commonly known in the art.
[0056] In step (f), the surface of the metal foil 30 exposed by the patterning and the via holes H are electroplated to form a circuit pattern. The composition of the electroplating solution used for electroplating is not particularly limited, and may include a metal ion source, a strong acid, a halogen ion source, a brightener, a leveling agent, and a carrier.
[0057] The source of metal ions may be a source of copper ions, specifically copper sulfate pentahydrate.
[0058] The strong acid may be selected from the group consisting of sulfuric acid, hydrochloric acid, methanesulfonic acid, ethanesulfonic acid, propanesulfonic acid, trifluoromethanesulfonic acid, sulfonic acid, hydrobromic acid, fluoroboric acid, and mixtures thereof.
[0059] The source of halogen ions may be a source of chloride ions, specifically hydrochloric acid.
[0060] The brightening agent may be selected from the group consisting of bis(3-sulfopropyl)disulfide (sodium salt), 3-mercapto-1-propanesulfonic acid (sodium salt), 3-amino-1-propanesulfonic acid, O-ethyl-S-(3-sulfopropyl)dithiocarbonate (sodium salt), 3-(2-benzthiazolyl-1-thio)-1-propanesulfonic acid (sodium salt), N,N-dimethyldithiocarbamic acid-(3-sulfopropyl)ester (sodium salt) and mixtures thereof.
[0061] The carrier may be a material commonly known in the art. Specifically, the carrier may be made of metal or polymer resin. The carrier made of metal can effectively discharge static electricity generated during storage and transportation of the metal foil. The carrier made of polymer resin is easily separated from the metal foil. Therefore, the material for the carrier can be appropriately selected according to each process and user's choice.
[0062] Electroplating of the exposed surfaces of metal foil 30 and via holes H with an electroplating solution minimizes the formation of defects such as voids and ensures uniformity and reliability of the final circuit pattern.
[0063] The method may further include, after step (f), peeling off the patterned dry film 50, and etching the remaining portion of the metal foil 30 exposed by the peeling off of the dry film 50 with an etching composition to form a desired circuit pattern on the substrate (step (g)). The etching composition may be any of those commonly known in the art.
[0064] A further embodiment of the present invention provides a method for forming a circuit pattern on a substrate, which includes the steps of: preparing a substrate in which a metal base is bonded to an insulating base (step (a')), bonding a metal foil having one or more flat-topped protrusions on the insulating base (step (b')), peeling off the metal foil having a surface roughness formed by the protrusions to transfer the surface roughness of the metal foil to the insulating base (step (c')), forming one or more via holes penetrating the insulating base (step (d')), forming seed portions on the surface of the insulating base having the via holes and on the inner walls of the via holes (step (e')), disposing a dry film on the insulating base on which the seed portions are formed, patterning the dry film (step (f')), and electroplating the via holes exposed by the patterning to form a circuit pattern (step (g')).
[0065] 4, a substrate in which a metal base 10 is bonded to an insulating base 20 is prepared (step (a')), and a metal foil 30 is bonded onto the insulating base 20 (step (b')). Steps (a') and (b') are the same as those described above, and detailed descriptions thereof will be omitted.
[0066] In step (c'), the surface roughness of the metal foil 30 is transferred to the insulating base 20. Specifically, the metal foil 30, which has a surface roughness formed by one or more protrusions 31 and is joined to the insulating base 20, is peeled off from the insulating base 20. As a result, the surface roughness of the metal foil 30 is transferred to the surface of the insulating base 20, and the surface of the insulating base 20 is roughened. The metal foil 30 may be peeled off by copper etching, which is a common method used to peel off metal foils, specifically by using a copper etching solution, or by half etching. By transferring the surface roughness of the metal foil 30, the surface of the insulating base 20 is roughened to the same degree as above, 2 to 100 particles / μm. 2 This allows the formation of holes.
[0067] By forming surface roughness on the insulating base 20 with the metal foil 30, adhesion between the seed portion formed on the insulating base 20 and the insulating base for subsequent electroplating can be increased, thereby increasing the possibility of forming a microcircuit pattern.
[0068] In step (d'), one or more via holes H are formed in the substrate including the insulating base 20 having a rough surface. The via holes H penetrate the insulating base 20, not the metal base 10. The via holes H can be formed by any suitable method generally known in the art, such as drilling or laser processing. After forming the via holes (H), the method of the present invention may further include roughening the inner walls of the via holes (H) (desmearing, for example, plasma desmearing) and / or removing impurities (for example, ash) present on the surface of the insulating base 20 or in the via holes H.
[0069] In step (e'), a seed portion 40 is formed on the surface of the insulating base 20 and the inner wall of the via hole H. The seed portion 40 enables plating or filling of the via hole H by subsequent electroplating to plate the surface of the insulating base 20. The seed portion 40 may be formed using a conductive material. The seed portion 40 may be formed by electroless plating using an electroless plating solution. The electroless plating solution may include a copper ion source and may be one commonly known in the art.
[0070] In step (f'), the dry film 50 is patterned according to a desired circuit pattern. Specifically, the dry film 50 is patterned by placing the dry film 50 on the insulating base 20 on which the seed portion 40 is formed, exposing the dry film 50, and developing the dry film 50 to form the desired circuit pattern. The exposure and development of the dry film 50 may be performed by any suitable process generally known in the art.
[0071] In step (g'), the surface of the seed portion 40 exposed by the patterning and the via hole H are electroplated to form a circuit pattern. The composition of the electroplating solution used for electroplating is not particularly limited, and may include a metal ion source, a strong acid, a halogen ion source, a brightener, a leveling agent, and a carrier. The composition of the electroplating solution is the same as that described above, and a detailed description thereof will be omitted.
[0072] The method may further include, after step (g'), peeling off the patterned dry film 50, and etching the remaining portion of the seed portion 40 exposed by the peeling off of the dry film 50 with an etching composition to form a desired circuit pattern on the substrate (step (h')). The etching composition may be any of those commonly known in the art.
[0073] As described above, the present invention uses a metal foil having a specific surface structure, and therefore, unlike the conventional technology that uses electroless plating or sputtering to form a circuit pattern on a substrate, high adhesive strength (bonding strength) to an insulating base is ensured, and the circuit pattern can be formed on the substrate in a simple and economical manner. The use of the metal foil enables the formation of a microcircuit pattern, and can increase the uniformity and reliability of the circuit pattern, which contributes to the manufacture of boards that require the transmission of high-frequency signals (e.g., circuit boards applied to 5G devices).
[0074] The present invention will be described in more detail with reference to the following examples. However, these examples are provided for illustrative purposes and do not serve to limit the scope of the present invention. It will be apparent to those skilled in the art that various modifications and variations can be made without departing from the scope and spirit of the present invention.
[0075] [Preparation Example 1] The laminate of the Cu foil carrier and the release layer (consisting of an alloy layer of nickel and molybdenum and an organic layer of sodium mercaptobenzotriazole) was placed in an electroless plating bath. As a result of the electroless plating, a metal foil (copper foil) with a thickness of 1 μm was formed on the release layer. For the electroless plating, 190-200 g / L of a metal ion source (CuSO 4 5H 2 An electroless plating solution containing 0.01-0.1 g / L of a nitrogen compound (guanine), 405-420 g / L of a chelating agent (potassium sodium tartrate), a pH adjuster (NaOH), and a reducing agent (28% formaldehyde) was used. Electroless plating was performed at 30°C for 10 minutes.
[0076] [Experimental Example 1] The surface and cross section of the metal foil formed in Preparation Example 1 were analyzed with a scanning electron microscope (SEM) and a cross section polisher (CP), respectively. The results are shown in FIGS.
[0077] 5 and 6, on the surface of the metal foil prepared in Preparation Example 1, a plurality of protrusions having flat upper ends were formed.
[0078] [Example 1] The method as claimed in claim 9 and illustrated in FIG. 1 was used to form a circuit pattern.
[0079] [Experimental Example 2] When the circuit pattern was formed in Example 1, the metal foil of Preparation Example 1 was bonded to an insulating base and then peeled off, so that the surface roughness of the metal foil was transferred to the insulating base. The surface of the insulating base was then analyzed by a scanning electron microscope (SEM). The SEM image is shown in FIG. 7.
[0080] Referring to FIG. 7, the surface of the insulating base was roughened to correspond to the surface structure of the metal foil.
[0081] [Experimental Example 3] Nanotus Cu foil Nanotus Cu foil was laminated onto a 100 × 100 mm test piece (ABF GL-103, Ajinomoto).
[0082] Cu foil was heated to 100°C and 5 kg / m 2 The laminate was laminated for 60 seconds at a temperature of 100°C and a pressure of 5 kg / m 2 The laminate was post-laminated at 100° C. for 60 seconds and cured at 130° C. for 30 minutes and 165° C. for 30 minutes.
[0083] After lamination, the carrier copper foil was removed and copper electroplating (20 μm) was performed with Nanotus Cu.
[0084] The adhesive strength was evaluated under the following conditions: peel test area 10 mm, test speed 50 mm / min, and angle 90°.
[0085] [Table 1]
Claims
1. A method for forming a circuit pattern on a substrate, comprising: preparing a substrate having a metal base bonded to an insulating base; bonding a metal foil having one or more flat-topped protrusions onto the insulating base; and transferring the surface roughness of the metal foil to the insulating base.
2. 2. The method of claim 1, wherein the metal foil is bonded onto the insulating base such that the flat-topped projections face a surface of the insulating base.
3. The method of claim 1 , wherein each of the flat-topped protrusions includes a protruding portion having a frusto-conical or frusto-pyramidal shape and a flat portion formed at an upper end of the protruding portion.
4. The method of claim 3 , wherein the protrusions have a plurality of microprojections formed on a surface thereof.
5. The method of claim 1, wherein the surface roughness (Rz) of the metal foil is 0.05 to 1.5 μm.
6. The method of claim 1 , wherein the metal foil has a thickness of 5 μm or less.
7. The method of claim 1 , wherein the metal foil is formed by electroless plating.
8. Unit area (μm 2 2. The method of claim 1, wherein 2 to 100 holes per inch are formed in the surface of the insulating base to which the roughness is transferred.
9. 1. A method for forming a circuit pattern on a substrate, comprising: preparing a substrate having a metal base bonded to an insulating base; bonding a metal foil having one or more flat-topped protrusions onto the insulating base; forming one or more via holes penetrating the insulating base and the metal foil; forming seed portions on inner walls of the via holes; disposing a dry film on the metal foil, patterning the dry film, and electroplating the via holes exposed by patterning to form a circuit pattern.
10. 1. A method for forming a circuit pattern on a substrate, comprising: preparing a substrate having a metal base bonded to an insulating base; bonding a metal foil having one or more flat-topped protrusions on the insulating base; peeling off the metal foil having a surface roughness formed by the protrusions to transfer the surface roughness of the metal foil to the insulating base; forming one or more via holes penetrating the insulating base; forming seed portions on a surface of the insulating base having the via holes and on inner walls of the via holes; placing a dry film on the insulating base on which the seed portions are formed, patterning the dry film; and electroplating the via holes exposed by patterning to form a circuit pattern.
Citation Information
Patent Citations
Production method of structure
JP2006219752A
Method for manufacturing transferred structure, and mother die for use in the same
JP2010087500A
Printed circuit board and manufacturing method for the same
JP2012109526A
Roughened copper foil, copper foil provided with carrier, copper-clad laminated sheet, and printed wiring board
WO2016158775A1
Roughened copper foil, copper foil with carrier, copper-clad multi-layer board, and printed wiring board
WO2019188712A1