Expandable Protective Coating

A two-part intumescent coating composition forms a closed-cell foam to address incomplete coverage and weight issues of traditional coatings, offering lightweight, effective protection and ease of rework for electronic substrates.

JP2024542505AActive Publication Date: 2024-11-15H K WENTWORTH LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024529991
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-03
Filing Date
2022-12-02
Publication Date
2024-11-15
Estimated Expiration
2042-12-02

AI Technical Summary

Technical Problem

Existing protective coatings for electronic substrates, such as conformal coatings and potting materials, struggle with incomplete coverage of features, weight, and difficulty in removal, making them impractical for complete protection and rework of electronic assemblies.

Method used

A two-part intumescent protective coating composition that expands into a closed-cell foam, comprising Part A with a polyol component, foaming catalyst, and optionally a gel catalyst, and Part B with an isocyanate-functional material, providing complete coverage and encapsulation of features while being lightweight and resistant to thermal shock, humidity, and condensation.

Benefits of technology

The coating achieves superior coverage of electronic substrates, reducing weight by up to 94% compared to traditional methods, maintains insulation and protection against harsh environments, and allows for easy rework of electronic assemblies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024542505000001_ABST
    Figure 2024542505000001_ABST
Patent Text Reader

Abstract

The present disclosure relates to a two-part coating composition comprising Part A including: (a) a polyol component including at least one of a difunctional polyol, a trifunctional polyol, and a tetrafunctional polyol, (b) a blowing catalyst, (c) optionally a gel catalyst, and d) water, and Part B including an isocyanate-functional material that is an isocyanate prepolymer having an isocyanate functionality of at least 2, preferably having a functionality greater than 2 and less than 3. The coating composition produced an expanded closed cell foam coating that provides protection for electronic substrates operating in harsh environments.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] FIELD OF THE DISCLOSURE This disclosure relates generally to expandable protective coating materials and methods of using the expandable protective coating materials to coat one or more surfaces of a substrate. [Background technology]

[0002] Protective coatings are used in a variety of applications to provide resistance to thermal shock, high temperatures, and relative humidity, as well as to protect against condensation and submersion. In many applications, it is desirable to protect the surfaces of substrates, including surfaces that contain one or more features, from the environment and damage. These substrates contain electronic assemblies where it is desirable to protect and / or encapsulate features contained thereon.

[0003] Electrical circuits are typically implemented on supporting substrates, such as printed circuit boards (PCBs) and printed wiring boards (PWBs), that have suitable electrical properties including dielectric strength, power factor, insulating properties, etc. The supporting substrate also exhibits physical properties required for a given application, such as tensile strength and tear resistance.

[0004] The design, construction, and manufacture of electrical circuit systems also takes into consideration environmental use. The humidity and / or temperature of the environment in which the electrical circuitry operates can have significant significance to the design. In many environments, the circuit specifications require a protective enclosure, and both the electrical and physical characteristics of the protective enclosure are considered in relation to the environmental conditions that will be encountered, including the extreme fluctuations in conditions that may occur.

[0005] Common protective coatings for electronic assemblies include, but are not limited to, potting materials, other encapsulating resins, and conformal coatings.

[0006] One of the main purposes of potting materials is to provide protection and support for sensitive electronic devices in environments that include exposure to chemicals, high humidity, vibration, and temperature extremes. Although these potting materials have provided good results, they are often very heavy; that is, the potting materials used to fill the devices or assemblies are often very thick, which may be a disadvantage for certain applications. The potting work is also not easily re-pouring (i.e., soft enough to be cut to facilitate removal for inspection and / or repair of the filled parts). One example of a potting material for filling electronic devices or assemblies is described in U.S. Patent No. 8,614,266 to Li et al., the subject matter of which is incorporated herein by reference in its entirety.

[0007] By encapsulating the entire surface of the electronic board, the encapsulation resin provides complete insulation for the unit, combining good electrical properties with mechanical protection. These resins are generally two-component systems in which the resin (part A) is mixed with a precise amount of a hardener (part B) to initiate a chemical reaction that results in a cross-linked polymer. Encapsulation resins are described, for example, in U.S. Patent Application Publication No. 2016 / 0322283 to McMahon et al., the subject matter of which is incorporated herein by reference in its entirety.

[0008] Potting materials and encapsulating resins provide a high level of protection for electronic substrates such as printed circuit boards (PCBs). These resins can be applied at thicknesses of about 0.5 mm or more and are generally quite thick. An increase in thickness leads to a significant increase in weight. On the other hand, the increased thickness provides greater protection against chemical attack, especially in the case of prolonged immersion. In addition, the resins can provide excellent protection against physical impacts, since the bulk of the resin can help dissipate forces across the electronic substrate. The use of dark colored resins can also completely hide the PCB, which can allow for some security of the design. However, these resins can also be difficult to remove, making rework of the PCB infeasible, as removal can result in destruction of the PCB.

[0009] Conformal coatings, on the other hand, are typically applied as very thin coatings to provide the maximum level of protection possible while using the thinnest amount of material to minimize heat trapping and added weight. Conformal coatings may be applied at thicknesses ranging from about 25 to 250 micrometers dry film thickness, for example, resulting in minimal weight gain to the assembly. Conformal coatings protect electronic boards (e.g., PCBs) and their components from the environment and corrosion. The material is applied to the board after it is assembled, so it "conforms" to the shape of the board and its components. Conformal coatings can cover the entire circuit board (if desired), protecting both the board and its components, including component leads, solder joints, exposed wiring, and other areas of exposed metal. The thin coating protects the metal from corrosion, as well as shielding the entire board from spray, moisture, fungus, dust, and other contamination from harsh environments. Conformal coatings can also help to extend the operating life of the PCB by helping to prevent damage from thermal and mechanical stresses, as well as rough handling.

[0010] Conformal coatings are typically non-conductive dielectric materials that can increase the dielectric strength between traces and other metal conductors, reducing the surface area required for the circuit, allowing for smaller, denser PCB layouts. There are different types of conformal coating materials or chemicals used depending on the specific needs of the electronic board. Some of the more commonly used conformal coatings include acrylic resins, silicone resins, urethane resins, and epoxy resins. An example of a conformal coating can be found in U.S. Pat. No. 4,300,184 to Colla, the subject matter of which is incorporated herein by reference in its entirety, which describes a water-free coating material containing fumed silica powder and a single-component urethane coating formulation, a process that removes all air bubbles from the formulation. WO 03 / 013199 to Glatkowski et al. describes a conformal coating that provides shielding against electromagnetic interference and contains carbon nanotubes.

[0011] Most conformal coatings are single-component systems that have long usable life, low curing or drying temperatures, and short drying times. Being one-part solutions, they are obviously easier to process and apply. However, most single-component coatings are solvent-based in order to modify their viscosity for application purposes. Conformal coatings can be applied manually in a variety of ways, including brushing, spraying, and dipping.

[0012] Two-component polyurethane coatings can also be used that combine the protection and properties of resins with the ease of application of conformal coatings, but are solvent-free and offer environmental benefits. These coatings can provide excellent coverage, and their flexibility provides protection for delicate parts. Two-component coatings provide excellent mechanical properties and abrasion resistance, but because they are two-component, they require more complex application equipment than one-component coatings. These two-component coatings can also be more difficult to remove, making repairs to the board very difficult.

[0013] A significant problem with conformal coatings is that it is difficult to effectively cover interconnect protruding pin-like circuit elements on a PCB or PWB, as these elements may remain at least partially exposed when using conformal coatings. In such cases, a potting material may be required in addition to the conformal coating to embed the circuitry and completely encapsulate the tiny protrusions and irregularities, which adds significant weight.

[0014] Low hardness, low modulus compounded resin systems have been proposed to fill the gap between the thick encapsulation resin and potting material and the thin dielectric conformal coating. These resins are designed to provide mechanical structural support while providing vibration damping and reducing overall resin weight and cost. Examples of these coatings can be found in U.S. Pat. Nos. 9,832,902 and 9,699,917 (both to Jordan, Jr. et al.), the subject matter of each of which is incorporated herein by reference in its entirety. However, these coatings still suffer from the same problem of insufficient coverage of features.

[0015] As seen in Figure 1, typical conformal coatings have difficulty completely covering features on electronic substrates and may leave edges of such features uncovered, resulting in incomplete protection. On the other hand, as shown in Figure 2, potting materials are very dense materials that provide protection for the features but add weight to the final product.

[0016] As an alternative to conformal coatings and encapsulating and potting resins, electronic substrates may be partially coated or microencapsulated with epoxy resins, however, these methods are typically used only in specific areas or to coat selected components.

[0017] It can thus be seen that a need remains for improved protective coatings that can provide superior protection of one or more surfaces of substrates, particularly substrates that include protruding circuit elements and other protruding features that can be difficult to completely cover or coat.

[0018] A variety of biliquid foam compositions have been developed that exhibit desirable properties.

[0019] British Patent No. 1496922 describes a foam composition comprising polyol A, polyisocyanate M (a blend of TDI and polymeric isocyanate), water, and catalysts N (triethylenediamine in dipropylene glycol), P (bis(2-dimethylamine ether) ether), R (amine catalyst), and S (dibutyltin dilaurate).

[0020] US Patent Application Publication No. 2013 / 0225706 describes a foam composition in which a first part comprises a trifunctional polyol, a chain extender, water, an amine catalyst in dipropylene glycol, and a tin catalyst. A second part consists of polymeric MDI.

[0021] U.S. Patent Application Publication No. 2009 / 0247659 describes a two-component foam composition comprising Part A and Part B, where Part A consists of polymeric MDI and Part B comprises an aromatic polyester polyol, an oxypropylated polyether triol, a tertiary amine catalyst, a potassium octoate catalyst, and water.

[0022] China Patent No. 112552474 describes a two-liquid foam composition in which a first part comprises a glycerin-based polyether polyol, a propylene glycol-based polyether polymer, an amine catalyst (N,N-dimethylcyclohexylamine), a tin catalyst (dibutyltin dilaurate), and water, and a second part comprises a polymethylene polyphenyl polyisocyanate.

[0023] China Patent No. 106750095 describes a two-component composition that includes a glycine-based polyol, a triethylenediamine catalyst, a dibutyltin laurate catalyst, and polymeric MDI. The isocyanate remains separate from the mixture containing the other ingredients, and the two are combined at the time of use.

[0024] New coating formulations that are lightweight and provide complete coverage and / or encapsulation of circuit elements and other features are highly desirable. Summary of the Invention

[0025] It is an object of the present invention to provide an improved protective coating composition.

[0026] It is another object of the present invention to provide a protective coating composition that provides excellent coating of features mounted on electronic substrates.

[0027] It is another object of the present invention to provide a method for coating or encapsulating features on an electronic substrate.

[0028] It is another object of the present invention to provide a coating composition that produces a protective coating that is low stress.

[0029] Another object of the present invention is to provide a protective coating that has a reduced weight compared to prior art coatings.

[0030] It is another object of the present invention to provide a coating that is electrically insulating.

[0031] Another object of the present invention is to provide a coating that is resistant to thermal shock, high temperatures, and relative humidity.

[0032] It is yet another object of the present invention to provide a coating that provides protection from condensation and submersion.

[0033] It is yet another object of the present invention to provide a coating that provides flame retardancy.

[0034] It is yet another object of the present invention to provide an aesthetically pleasing coating.

[0035] It is yet another object of the present invention to provide a coating that can be bonded to a topcoat layer to provide additional protection.

[0036] It is yet another object of the present invention to provide a coating having a low viscosity.

[0037] To that end, in one aspect, the present invention generally provides a two-part protective coating composition comprising: a) Part A, a. a polyol component comprising at least one of a difunctional polyol and a trifunctional polyol; b. Blowing catalyst; c. optionally, a gel catalyst; d. optionally, at least one flame retardant; and e. water; and b) Part B, an isocyanate-functional material having an isocyanate functionality of at least 2, preferably the isocyanate-functional material is an isocyanate prepolymer, the isocyanate prepolymer having a functionality of greater than 2 and less than 3; and and optionally a part B comprising at least a flame retardant; A two-part protective coating composition in which a flame retardant must be present in at least one of Part A and Part B.

[0038] The two-part protective coating compositions described herein can be mixed and applied to one or more surfaces of a substrate to produce a lightweight, closed-cell foam protective coating that can protect the surface from environmental, chemical and moisture attack, thermal shock, and the like, and provide flame retardancy.

[0039] In a second aspect, the invention generally relates to a method of applying a protective coating to one or more surfaces of a substrate, the method comprising: a) mixing a two-component coating composition, the two-component coating composition comprising: i) Part A, a. a polyol component comprising at least one of a difunctional polyol, a trifunctional polyol, and a tetrafunctional polyol; b. Blowing catalyst; c. optionally, a gel catalyst; d. optionally, at least one flame retardant; and e. water; and ii) Part B, an isocyanate-functional material having an isocyanate functionality of at least 2, preferably the isocyanate-functional material is an isocyanate prepolymer having a functionality of greater than 2 and less than 3; and and optionally, a part B comprising at least one flame retardant; To prepare a liquid coating composition, at least one flame retardant must be present in at least one of Part A and Part B; b) applying the liquid coating composition to a substrate and expanding the liquid coating composition into a closed cell foam coating.

[0040] In a third aspect, the invention generally relates to an electronic substrate assembly comprising a printed circuit board, the printed circuit board including a base support and a plurality of electrical circuit components extending outwardly from a surface of the attached base support and electrically connected to an electrical circuit, wherein a closed-cell foam protective coating is applied to at least a portion of a surface of the electronic substrate assembly including the plurality of electrical circuit components, the closed-cell protective coating comprising the two-part coating composition of the first aspect of the invention, Part A and Part B being in mixed form in the closed-cell protective coating, and / or the closed-cell protective coating being applied by the method of the second aspect of the invention.

[0041] Additional advantageous features, functionality, and applications of the disclosed systems and methods of the present disclosure will become apparent from the following description, particularly when read in conjunction with the accompanying drawings. [Brief description of the drawings]

[0042] Features and aspects of the embodiments are described below with reference to the accompanying drawings, in which elements are not necessarily drawn to scale and in certain figures, parts may be exaggerated or removed for clarity.

[0043] Exemplary embodiments of the present disclosure are further described with reference to the accompanying drawings, in which it is noted that the various features, steps, and combinations of features / steps described below and illustrated in the figures can be arranged and organized differently to result in embodiments that are still within the scope of the present disclosure.

[0044] The invention will now be described with reference to the following drawings: [Figure 1] 1 shows a cross-sectional view of a prior art conformal coating on a feature of an electronic substrate. [Diagram 2] 1 shows a diagram of an electronic substrate having features coated with a prior art resin potting material. [Diagram 3] 1 shows diagrams of three different electronic assemblies coated with the expanded protective coating of the present invention. [Figure 4] 1 shows the results of measuring the surface insulation resistance of the composition of Example 1. [Diagram 5] 1 shows a diagram of an electronic assembly coated with an expanded protective coating of the present invention, the coating being subjected to a thermal shock test. [Figure 6] 4 shows the results of measuring the surface insulation resistance of the composition of Comparative Example 1. [Figure 7] 1 shows a diagram of an electronic assembly partially coated with a protective coating of the present invention. [Figure 8] 8 shows a diagram of the electronic assembly of FIG. 7 further coated with a topcoat over the top of the protective coating layer. [Figure 9] 1 shows a comparison of electronic assemblies coated with the composition of Example 1 and the composition of Comparative Example 1 after 1000 hours at 85° C. / 85% RH. [Figure 10] 1 shows a graph demonstrating the weight savings of the coating composition of the present invention compared to prior art encapsulating coatings. [Figure 11] FIG. 1 shows a diagram of a substrate coated with a foam coating of the present invention with or without a topcoat layer. [Figure 12] 1 shows a graph illustrating the improvement in water absorption achieved by overcoating a foam with a topcoat layer. [Figure 13] 1 shows a graph of the electrical insulation properties of a coating according to the present invention after immersion at 50° C. for one week.

[0045] Also, although not every element may be labeled in every figure, all elements having the same reference number indicate similar or identical parts. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0046] The present invention generally relates to an expandable liquid coating composition having specific performance characteristics for producing an expanded protective coating that can coat and / or encapsulate features of a substrate, including an electronic substrate, including micro-projections and irregularities. The electronic substrate may be a surface mounted electronic device that contains one or more circuit elements. In addition, the protective coating may be designed to protect the electronic substrate from harsh environments, including exposure to chemicals, high humidity, vibration, and temperature extremes over extended periods of time. The protective coating may also be designed to provide improved flame retardancy.

[0047] The present invention provides a liquid-applied elastomeric coating composition that expands into a closed-cell foam coating and can be used to provide a protective coating for electronic assemblies and other substrates. In addition, the coating composition can be used in the process of repairing or modifying electronic substrates such as PCBs or PCWs, since the repaired or modified circuit boards can be easily overcoated using the coating compositions and processes detailed herein.

[0048] Thus, the present invention provides an expandable protective coating that can be applied to printed circuit systems and other electronic substrates, such as substrates containing small irregularities and protrusions that require protection. The expandable coating composition is applied as a liquid and expands rapidly to form an expanded closed cell foam protective coating.

[0049] It should be understood that the disclosed embodiments are merely illustrative of the present disclosure, which may be embodied in various forms. Thus, the details disclosed herein with reference to exemplary assembly / manufacturing methods and associated processes / techniques of assembly and use should not be construed as limiting, but merely as a basis for teaching those skilled in the art how to make and use the advantageous assemblies / systems described herein.

[0050] As used herein, "a," "an," and "the" refer to both the singular and the plural, unless the context clearly dictates otherwise.

[0051] As used herein, the term "about" refers to a measurable value of a parameter, amount, duration, etc., and is meant to include no more than + / -15% variation, preferably no more than + / -10% variation, more preferably no more than + / -5% variation, even more preferably no more than + / -1% variation, and even more preferably no more than + / -0.1% variation of and from the specifically recited value, so long as such variations are appropriate to practice the invention described herein. It is further to be understood that the values ​​to which the modifier "about" refers are themselves specifically disclosed herein.

[0052] As used herein, spatially relative terms such as "beneath," "below," "lower," "above," "upper," "front," and "back" are used for ease of explanation to describe the relationship of one element or feature to another element or feature. It is further understood that the terms "front" and "back" are not intended to be limiting and are intended to be interchangeable where appropriate.

[0053] As used herein, the terms "comprise(s)" and / or "comprising" specify the presence of stated features, integers, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components, and / or groups thereof.

[0054] When ASTM or other standards are referenced herein, the standards are expected to be the most current standards as of the filing of this application, unless otherwise specified.

[0055] As used herein, the term "polyol" refers to an organic compound that contains multiple hydroxyl groups.

[0056] In one aspect, the invention generally relates to a two-component coating composition, the two-component coating composition comprising: a) Part A, a. a polyol component comprising at least one of a difunctional polyol, a trifunctional polyol, and a tetrafunctional polyol; b. Blowing catalyst; c. optionally, a gel catalyst; d. optionally, one or more additives selected from the group consisting of foam stabilizers, copolymers, inert inorganic fillers or extenders, colorants, antioxidants, UV stabilizers, and flame retardants; and e. water; and b) Part B, and Part B comprising an isocyanate-functional material, the isocyanate-functional material being an isocyanate prepolymer having an isocyanate functionality of at least 2, preferably greater than 2 and less than 3.

[0057] In one aspect, the invention generally relates to a two-component coating composition, the two-component coating composition comprising: c) In Part A, a. a polyol component comprising at least one of a difunctional polyol, a trifunctional polyol, and a tetrafunctional polyol; b. Blowing catalyst; c. optionally, a gel catalyst; d. optionally, at least one flame retardant; and e. water; and d) Part B, an isocyanate-functional material, the isocyanate prepolymer having an isocyanate functionality of at least 2, preferably greater than 2 and less than 3; and and optionally, a part B comprising at least one flame retardant; At least one flame retardant must be present in at least one of Part A and Part B of the two-part coating composition.

[0058] The polyol component of Part A includes at least one of a difunctional polyol, a trifunctional polyol, and a tetrafunctional polyol, and may include additional polyols capable of reacting with isocyanate groups. Examples of such polyols include glycols, i.e., diols containing 1,2 dihydroxy groups, such as ethylene glycol or propylene glycol and its derivatives, polypropylene glycol, polytetramethylene ether glycol, and glycerol or glycerin and its derivatives. In one embodiment, the polyol of the polyol component has a molecular weight of less than about 2000, more preferably less than about 1,000, more preferably less than about 600, more preferably a weight average molecular weight of about 300 to about 600 Daltons.

[0059] In some embodiments, the polyol is an asymmetric diol having 3 to 20 carbon atoms, more preferably 4 to 12 carbon atoms, and most preferably 5 to 10 carbon atoms. Examples of such asymmetric diols include, but are not limited to, 2-ethyl-1,3-hexanediol, 1,2-propanediol, 1,3-butanediol, 2,2,4-trimethyl-1,3-pentanediol, 1,12-octadecanediol, 1,2-hexanediol, 1,2-octanediol, and 1,2-decanediol. Other examples of polyols include tetrols such as pentaerythritol. The polyol can also be a polyether polyol prepared from either ethylene oxide and / or propylene oxide, optionally reacted with another polyol (e.g., glycol or glycerol).

[0060] Suitable polyols include polyether polyols, polyester polyols, polymer polyols comprising a dispersion of polymer particles in a continuous polyol phase, and other polyhydroxy-containing compounds. Preferred polyols include, by way of example and not limitation, poly(tetramethylene oxide) polymers, copolymers of tetramethylene oxide and ethylene oxide, and polymers and copolymers of propylene oxide.

[0061] In one embodiment, the polyol component includes at least one of a difunctional polyol, a trifunctional polyol, and a tetrafunctional polyol. In one embodiment, the polyol component includes two or more of a difunctional polyol, a trifunctional polyol, and a tetrafunctional polyol.

[0062] In one embodiment, the difunctional polyol is selected from the group consisting of polyethylene glycol, polypropylene glycol, polycaprolactone, polybutadiene, polyester, polyether, polyfarnesene, ethylene glycol dimerate, and combinations of two or more of the foregoing. Preferably, the difunctional polyol is a hydrophobic polyol selected from the group consisting of polybutadiene, polyfarnesene, and ethylene glycol dimerate.

[0063] In one embodiment, the trifunctional polyol is selected from the group consisting of polyethylene glycol, polypropylene glycol, polycaprolactone, polybutadiene, polyester, polyether, polyfarnesene, ethylene glycol dimerate, and combinations of two or more of the foregoing. In one embodiment, the trifunctional polyol comprises castor oil (i.e., ricinoleic acid triglyceride), a renewable raw material that is widely available commercially. Derivatives of castor oil, including any polyol derived from castor oil, including hydrolysis products, ethoxylation products, transesterification products, or esterification products, or polyamide products, can also be used in the practice of the present invention. Another example of a suitable trifunctional polyol is cashew nut liquid (CNSL)-based polyol.

[0064] In one embodiment, the polyol component comprises 0-99.99 wt%, more preferably 0.1-99.9 wt%, preferably 30-70 wt%, more preferably 45-55 wt% of a difunctional polyol, and / or 0.0-99.99 wt%, more preferably 0.1-99.9 wt%, preferably 30-70 wt%, more preferably 45-55 wt% of a trifunctional polyol, and / or 0.0-99.99 wt%, more preferably 0.1-99.9 wt%, preferably 30-70 wt%, more preferably 45-55 wt% of a tetrafunctional polyol.

[0065] In one embodiment, the water content of part A is in the range of 0.05 to 10% by weight, more preferably 0.1 to 9% by weight, more preferably 0.5 to 8% by weight, or optionally in the range of 3 to 7% by weight, or optionally in the range of 4.5 to 5.5% by weight.

[0066] Part A also includes one or more catalysts. In one embodiment, the catalyst includes a blend of a blowing catalyst and a gel catalyst to control the reaction rates of the gel and blow reactions. In another embodiment, the catalyst includes one or more blowing catalysts. In another embodiment, a single catalyst is used as both the blowing catalyst and the gel catalyst.

[0067] The blow / foam catalyst preferentially catalyzes the reaction between water and an isocyanate source to produce carbon dioxide. In one embodiment, the blow catalyst comprises an amine catalyst, such as, for example, a triol catalyst, a tetrapolyol catalyst, and a tertiary amine catalyst. Further examples of suitable catalysts include various alkylamines, aliphatic amines, aromatic amines, alkyl ethers, and alkyl thiol ethers, such as those based on bismuth or tin, including bismuth octoate, bismuth laurate, and other similar compounds. Other catalysts include tin catalysts, such as stannous octoate, dibutyltin dioctoate, and dibutyltin dilaurate.

[0068] Suitable amine catalysts include, but are not limited to, aliphatic amines, alicyclic amines, aromatic amines, alcohol amines, or one of their ammonium compounds. Examples of aliphatic amines include, but are not limited to, triethylenediamine, N,N,N,N-tetramethylalkylenediamine, N,N,N,N-pentamethyldiethylenetriamine, triethylamine, N,N-dimethylbenzylamine, N,N-dimethylhexadecylamine, and N,N-dimethylbutylamine, among others. Examples of alicyclic amines include, but are not limited to, triethylenediamine, N-ethylmorpholine, N-methylmorpholine, N,N-diethylpiperazine, N-diethyl-2-methylpiperazine, N,N-bis-(α-hydroxypropyl)-2-methylpiperazine, and N-hydroxypropyldimethylmorpholine, among others. Examples of aromatic amines include, but are not limited to, pyridine, N,N-dimethylpyridine, among others.

[0069] Commercially available amine catalysts that can be used in the compositions described herein include bis(2-dimethylaminoethyl)ether (available from Momentive Performance Materials under the trade name NIAX A-1), triethylenediamine dipropylene glycol solution (available from Momentive Performance Materials under the trade name NIAX A-33), tertiary gel amine (available from Momentive Performance Materials under the trade name NIAX Catalyst EF-600), and tertiary amine (available from Momentive Performance Materials under the trade name NIAX Catalyst EF-700). Other similar amine catalysts are known to those skilled in the art and can be used in the compositions of the present invention.

[0070] The amine catalyst is used in the composition in an appropriate amount to control the reaction during the synthesis of the polyurethane foam. In one embodiment, the amine catalyst is used in an amount of about 0.01 to about 5 weight percent of Part A, preferably about 0.5 to about 2.5 weight percent, and more preferably about 0.75 to about 1.25 weight percent of Part A.

[0071] The gel catalyst promotes the gelling reaction and traps the produced carbon dioxide in the polymer matrix, resulting in a closed-cell foam protective coating. In one embodiment, the gel catalyst comprises an organometallic catalyst, which may be, for example, a tin, bismuth, or potassium-based catalyst. Examples of these organometallic catalysts include, for example, tin catalysts such as dialkyltin dialkanoates, stannous octoate, dibutyltin dilaurate, dibutyltin diacetate, zinc neodecanoate, bismuth neodecanoate and neodecanoic acid blends, iron acetylacetonate, potassium acetate catalysts, potassium octoate catalysts, stannous octoate catalysts, and bismuth-based gelling catalysts, by way of example and not limitation. One example of a commercially available organotin catalyst is available from EVONIK under the trade name Kosmos 16. In another embodiment, the gel catalyst is a gel amine catalyst, such as NIAX A33 or NIAX EF600, available from Momentive Performance Materials Inc.

[0072] In one embodiment, the gel catalyst is used in an amount of about 0.01 to about 5% by weight of Part A, preferably about 0.05 to about 0.5% by weight, and more preferably about 0.1 to about 0.3% by weight of Part A.

[0073] The total amount of catalyst in Part A (i.e., the total "polyol side" composition) can vary depending in part on the method by which the expandable coating composition is applied. For example, in spray coating applications, the total amount of catalyst present may range from greater than 0 percent to less than 1 percent by weight of the total "polyol side" composition, optionally but preferably including gel catalyst levels of 0.2 percent to 0.8 percent of the total "polyol side" composition, and blow catalyst levels of 0.2 percent to 0.8 percent of the total "polyol side" composition. On the other hand, for dispensing operations, the preferred gel catalyst levels are 0.02 percent to 0.25 percent of the total "polyol side", and the preferred blow catalyst levels are 0.02 percent to 0.25 percent of the total "polyol side" composition.

[0074] As mentioned above, Part B of the coating composition comprises an isocyanate-functional material having an isocyanate functionality of at least 2. In one embodiment, the isocyanate-functional material comprises an isocyanate prepolymer having an average functionality greater than 2 and less than 3.

[0075] In one embodiment, the isocyanate prepolymer is the reaction product between diphenylmethane 4,4' diisocyanate and (ad) / or diphenylmethane 2,2'-diisocyanate, and / or diphenylmethane 2,4'-diisocyanate (MDI) with adipic acid, 2-methyl-1,3-propanediol, and trimethylolpropane based polyester polyols.

[0076] In one embodiment, the polyisocyanate used to prepare the prepolymer of the polyurethane composition may be any compound having at least two isocyanate moieties, such as 1,5-naphthylene diisocyanate, 4,4'-diphenylmethane diisocyanate (4,4'-MDI), 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyl diisocyanate, dialkyldiphenylmethane diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, toluene diisocyanate, butane-1,4-diisocyanate, hexamethylene diisocyanate, isopropylene diisocyanate, naphthylene diisocyanate, 1,5-naph ... Diisocyanates include, for example, 4,4'-MDI, methylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, cyclohexane-1,4-diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, lysine diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, methyl-cyclohexane diisocyanate, m-tetramethylxylylene diisocyanate, 2,4,6-triisopropylbenzene diisocyanate, isopropylidenebis(4-cyclohexylisocyanate), and mixtures thereof. A preferred diisocyanate mixture includes a mixture of 4,4'-MDI and 2,4-MDI.

[0077] The polyisocyanate used to prepare the prepolymer can also be, for example, a polyisocyanate prepared by reacting a diisocyanate with a diisocyanate-reactive compound such as a polyol (e.g., a diol) or a polyamine (e.g., a diamine). Exemplary polyisocyanates used to prepare the prepolymer include the polymeric form of MDI. The polyisocyanate used to prepare the prepolymer can also be a carbodiimide-modified diisocyanate (e.g., a carbodiimide-modified MDI).

[0078] As mentioned above, the polyisocyanates generally have an average functionality of from about 2 to about 3, more preferably from 2.1 to 3, more preferably from 2.1 to 2.9, more preferably from 2.3 to 2.8, and most preferably from 2.5 to 2.7.

[0079] In one embodiment, the isocyanate prepolymer comprises an MDI trimer, such as a solvent-free product based on 4,4'-diphenylmethane diisocyanate (MDI) with an average functionality of 2.7, commercially available from BASF under the trade name Lupranat® M20S. What is important in this embodiment is that the isocyanate prepolymer reacts sufficiently quickly with the water and polyol components. By "sufficiently quickly" we mean that the isocyanate prepolymer reacts with the water and polyol components in less than 10 minutes, preferably less than 8 minutes, preferably less than 7 minutes, preferably less than 6 minutes, preferably less than 5 minutes, preferably less than 4 minutes, and most preferably less than 3 minutes to produce an expanded closed-cell foam protective coating. The balance between carbon dioxide generation and polymerization is important and must be complementary. Polymerization must proceed quickly to capture carbon dioxide as it is generated. If carbon dioxide generation is faster than polymerization, the foam will collapse. In a preferred embodiment, once carbon dioxide generation begins, polymerization must also begin.

[0080] In another embodiment, the formulation is optimized for delayed reaction.

[0081] In one embodiment, a chain extender may also be included in Part A of the composition to provide tailoring properties. Chain extenders are typically low molecular weight diols or diamines that react with diisocyanates to build polyurethane molecular weight and increase hard segment block length. Examples of suitable low molecular weight chain extenders include aliphatic, araliphatic, aromatic and / or cycloaliphatic compounds, more preferably difunctional compounds, such as diamines and / or alkanes having 2 to 10 carbon atoms in the alkylene radical, such as 1,2-ethylenediol, 1,4-butanediol, 1,6-hexanediol, 1,3-propanediol, and / or dialkylene-, trialkylene-, tetraalkylene-, pentaalkylene-, hexaalkylene-, heptaalkylene-, octaalkylene-, non-alkylene, and decaalkylene-glycols having 2 to 8 carbon atoms in the alkylene moiety, the corresponding oligopropylene glycols and / or propylene glycols. Other examples of suitable chain extenders include, but are not limited to, 1,4-butanediamine, ethylenediamine, diaminopropane, cyclohexanediphenylalanine, among others. Combinations of two or more of the foregoing can be used. The concentration of the chain extender in Part A, if used, can be in the range of about 2 to about 20% by weight, more preferably about 5 to 15% by weight.

[0082] In one embodiment, the protective coating composition includes a flame retardant. If used, the flame retardant may include, for example, aluminum hydroxide trihydrate (ATH), a phosphorus-containing polyol, or a microencapsulated ammonium polyphosphate. Alternatively or in addition, the flame retardant may include a component that is solid at room temperature. Suitable flame retardant materials that are solid at room temperature have a typical average particle size of 50 to 500 micrometers, more preferably 100 to 400 micrometers, more preferably 90 to 350 micrometers. In one embodiment, the solid flame retardant component is made from expandable flake graphite, a commercially available product of which is available under the trade name GrafGuard (manufactured by NEOGRAF Solutions, Ohio, USA). In one embodiment, the flame retardant includes ATH and expandable flake graphite.

[0083] The solid flame retardant component may be present in at least one of the reactive components (i.e., either Part A or Part B). In one embodiment, the solid flame retardant component is present in at least one of the reactive components at a weight percent of greater than 0 percent to less than 70 percent based on the total weight of the components. In some embodiments, the flame retardant component may be present in both the first component (Part A) and the second component (Part B). Further, the solid flame retardant component may be present in the cured protective coating composition at a weight percent of 5 percent to 50 percent, more preferably about 10 percent to about 40 percent, or about 20 percent to about 35 percent, or about 25 percent to about 30 percent, based on the total weight of the cured composition.

[0084] In one embodiment where the two-part coating composition is formulated for spray application, the solid flame retardant has a particle size in the range of 80 to 100 micrometers, more preferably in the range of about 85 to about 95 micrometers. In one embodiment where the two-part coating composition is formulated for dispensing application, the solid flame retardant has a particle size in the range of about 60 to about 180 micrometers, preferably about 70 to 160 micrometers, or even about 90 to about 150 micrometers. The flame retardant may be added to Part A of the composition at a concentration in the range of about 10 to about 30% by weight, more preferably about 15 to about 20% by weight.

[0085] An advantage of using expandable graphite in the expandable compositions described herein is that the formulations do not contain halogenated materials. In addition, the use of expandable graphite as a flame retardant also does not adversely affect electrical properties, unlike phosphorus-based polyols, which are known to be susceptible to hydrolysis and give unacceptable electrical performance in high temperature / high humidity environments. In addition, compositions containing expandable graphite also meet UL94 V-0 requirements at low loads. In one embodiment, the expandable graphite is present in the composition at a concentration ranging from 5 to 30% by weight, more preferably 10 to 20% by weight, which is less than 0.2 g / cm. 3 The concentration is sufficient to pass the UL94 V-0 test at a foam density of 100%. Thus, compositions containing flame retardants such as expandable graphite could pass the UL94 V-0 test without significantly affecting the foam density or adversely affecting the foam's electrical insulating properties. Also, low density foams are still achievable compared to compositions using ATH as a flame retardant. Some grades also impart a desirable thixotropic rheology.

[0086] The protective coating compositions of the present invention may also optionally, but preferably, include inert inorganic fillers or extenders such as talc, calcium carbonate, silica, wollastonite, aluminum hydroxide, clays such as kaolin, calcium sulfate fibers, mica, glass beads, and nanomaterials such as nanographene, nanofibers, and nanoparticles. Other inert inorganic fillers are known to those skilled in the art.

[0087] The protective coating composition may also optionally, but preferably, include a colorant, such as a dye or pigment, to impart a particular color to the coating material. These colorants are selected to avoid any chemical incompatibilities between the chemistry of the protective coating composition and the chemistry of the colorant, and are used in an amount to provide the desired color in the resulting expanded closed cell protective coating.

[0088] The protective coating composition may also optionally, but preferably, include an antioxidant or UV stabilizer, examples of which include, but are not limited to, amine-based and phenolic antioxidants, commercially available from BASF under the trade names Irganox® 1035, Irganox® L135, and Irganox® PS800FL.

[0089] In one embodiment, the protective coating composition includes a non-reactive diluent. One example of a suitable non-reactive diluent is a polyalphaolefin (PAO), which may be an oligomer of an α-olefin. PAOs are generally high purity hydrocarbons with paraffinic structure and a high degree of side branching, which may include irregular or regular branching. PAOs may include oligomers or low molecular weight polymers of branched and / or linear alpha olefins. Suitable olefins include, but are not limited to, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, and blends thereof. Useful PAOs include certain grades of Synfluid® available from Chevron Phillips Chemical Company, such as Synfluid® PAO 8.

[0090] In one embodiment, the substrate coated with the composition described herein is an electrical circuit assembly comprising a base support and a plurality of electrical circuit components extending outwardly from an attached surface of the base support and electrically connected to the electrical circuit. The substrate is coated with a thin layer of the coating composition as defined and described in detail herein, which expands to form a closed cell foam coating.

[0091] In one embodiment, the base support comprises a printed circuit board assembly including a support base or substrate on which a conductor pattern of highly conductive material is attached to define interconnect circuit conductors. Various electrical components, such as resistors, transistors, etc., are attached to the board and connected to the conductors. The components may also have terminals that may pass through board openings with electrical solder connections. The soldered connections and terminals define sharp projections or asperities that extend outside the board and components.

[0092] The coating composition of the present invention can be prepared by mixing all of the components of Part A together and then mixing Part A with Part B. As one skilled in the art would understand, Part A and Part B can be combined or mixed in any manner acceptable for forming such a polymer resin system. Such methods include, but are not limited to, hand mixing, static mixing, dynamic mixing, or impingement mixing. It is further noted that the individual parts of the multi-part system can be added in any order (e.g., Part A can be mixed with Part B, or vice versa).

[0093] In one embodiment, it is preferred to mix Part A with Part B at or just before the coating composition is contacted with the surface of the substrate. In other words, once Part A is mixed with Part B, the coating composition should be applied or otherwise contacted with the surface to be coated within less than 120 seconds, preferably less than 90 seconds, more preferably less than 60 seconds, more preferably less than 45 seconds, more preferably less than 30 seconds, and most preferably less than 20 seconds. In one embodiment, Part A and Part B are mixed using a static mixer and applied to the surface of the substrate. In another embodiment, Part A and Part B are sprayed together to provide the desired mixture.

[0094] In addition, as described herein, the coating composition may be optimized to enhance its compatibility with a particular coating method. For example, in one embodiment, the coating composition may be optimized for spray coating. In another embodiment, the coating composition may be optimized for coating a substrate by dispensing. The table below provides examples of suitable Part A formulations for the two-part composition of the present invention, which can be mixed with the appropriate Part B, as further demonstrated in the examples.

[0095] An exemplary Part A formulation of a two-part composition that has been optimized for spray coating includes the following:

[0096] [Table 1]

[0097] Exemplary Part A formulations of two-part compositions that are optimized for dispensing include the following:

[0098] [Table 2] 1 Capa products are available from Ingevity 2NIAX products are available from Momentive Performance Materials Inc.

[0099] Unlike formulations optimized for spray coating, it was observed that in compositions optimized for dispensing, density (volume x expansion) appears to be affected by the concentration of blowing agent and not by the catalyst.

[0100] The thickness of the coating composition applied is controlled so that the volume expansion is within the desired level. The coating generally expands preferentially in the Z direction due to the production of carbon dioxide. That is, in one embodiment, the volume expansion in the Z direction (i.e., perpendicular to the surface of the substrate) is controlled to less than 25 times, preferably 8 times to 20 times, and more preferably about 10 times to about 15 times. For example, in one embodiment, the coating is applied at a thickness of about 300 micrometers, which results in a volume expansion of 10 times. On the other hand, a thicker coating may result in a volume expansion of 25 times or more, which may result in less desirable results. Based thereon, the coating is applied as a liquid at a thickness that will produce an expanded closed cell foam protective coating of the desired thickness.

[0101] In one embodiment, the coating composition is optimized so that the foaming reaction occurs in less than 10 minutes, preferably less than 5 minutes, and more preferably less than 4 minutes at room temperature until the foamed coating is tack-free. In one embodiment, the foaming reaction begins within 5-30 seconds of application.

[0102] In another embodiment, the composition is formulated to delay the onset of foaming and facilitate the application process. For example, in one embodiment, the blowing catalyst may be microencapsulated in a water-soluble shell and incorporated into Part B. The water-soluble shell can take 5-10 minutes to dissolve and release the blowing catalyst (which can be controlled by the thickness and solubility of the cell wall), resulting in the onset of foaming and polymerization. In another embodiment, the composition may be formulated to delay the onset of foaming by optimizing by varying the catalyst and by varying the concentrations of the catalyst and / or other components to control the rate of onset of foaming and thus delay the onset.

[0103] In one embodiment, delayed foam generation using the compositions described herein is achieved by using a low viscosity and slower gel to allow for better flow around the parts.

[0104] As shown in Figure 10, weight savings of over 85% are achieved by using an expanded foam coating composition overcoated with a protective top cat layer compared to a solid epoxy compound. In addition, it can be seen that the weight contribution of the thin top coat is negligible. Furthermore, the application of the expanded foam layer does not slow down production time, since the expanded foam coating layer is tack-free in less than 5 minutes and can be overcoated after about 2 minutes, or about 2.5 minutes, or about 3 minutes.

[0105] 11 shows an electronic component containing a cavity filled with a foam composition according to the present invention compared to a cavity filled with a foam composition and then thinly overcoated (i.e., 500 micrometers or 1 mm of protective coating). All three materials were subjected to thermal shock testing from -40°C to +85°C for 1000 cycles, and all materials passed the thermal shock test without cracking or loss of adhesion.

[0106] Figure 12 shows a graph illustrating the improvement in water absorption achieved by the topcoat. As shown in Figure 12, the expanded foam coating without a coating appeared to reach a saturation level of about 6.5%. In contrast, the expanded foam coating with the topcoat layer showed improved saturation levels, with the presence of 1 mm of topcoat on the expanded foam layer resulting in the same level of water absorption as a solid epoxy potting compound (i.e., ER2188).

[0107] Further, Figure 13 shows the electrical insulation (50V) under immersion at 50°C for 1 week. As seen in Figure 13, water absorption does not result in poor surface insulation resistance (SIR) in the expanded foam. In addition, it was found that the expanded foam in combination with a 0.5mm topcoat layer provides exemplary SIR and low water absorption.

[0108] In one embodiment, the coating composition is optimized for ease of application to complex circuit board designs, however, there is a trade-off between cream time / rise time / tack-free time and volumetric height expansion.

[0109] In one embodiment, the intumescent coating composition is formulated for latent foaming, where the coating composition is formulated to remain in an unexpanded state until foaming is initiated by an external force, such as UV light, microwaves, heat, or other external initiation source. As noted above, in one embodiment, the intumescent coating composition may be formulated to delay the onset of foaming, and the time to foaming may be optimized to be at least about 3 minutes, or at least about 5 minutes, or at least about 8 minutes.

[0110] In one embodiment, the coating composition may be constrained to create an aesthetically pleasing housing with a completely closed surface. For example, the foam may be constrained by placing a board in the housing to limit the expansion space of the foam. That is, in some embodiments, it is advantageous to constrain the foam during expansion to tailor the properties of the foam surface. In one embodiment, the coatings described herein may be constrained, for example, when an electronic board is placed in the housing. In this case, the foamable coating can only expand within the limited confines of the housing. The coating is otherwise free to expand naturally until the expansion reaction is complete. In one embodiment, the coating may expand preferentially in the Z direction due to the carbon dioxide produced.

[0111] The protective foam coatings described herein preferably provide an insulation resistance (insulation at a combination of high temperature and high humidity) of at least 100 MOhm at 85C / 85%RH. In addition, the protective foam coatings are also formulated to withstand at least 1000 thermal shock cycles from -40 to +130°C.

[0112] The volume resistivity and surface resistivity of the protective foam coating are preferably at least about 10 11 It is measured in ohms-cm (volume) or ohms / square (surface). If the value is below this level, the product does not provide sufficient protection.

[0113] It is preferred that the water absorption of the protective closed cell foam coating is as low as possible, in one embodiment the water absorption has values ​​that perform comparably to typical resin systems, exhibiting less than 1% w / w water absorption after 14 days of immersion.

[0114] The protective closed cell foam coating preferably exhibits an elongation at break (%) of at least 10%, preferably in the range of 10-100%, more preferably 20-80%, and most preferably about 40-60%.

[0115] In one embodiment, a topcoat can be applied to the foamed coating, which can be aesthetic or functional in nature and can modify the properties of the foamed coating. For example, a hard, chemically resistant coating can be applied over the foamed coating to provide abrasion and chemical resistance. Alternatively, a conductive coating can be applied to provide RF shielding functionality. In this case, the foam acts as an electrical insulating layer to prevent shorting of components of a circuit board or other electronic substrate. In yet another embodiment, the foamed coating can be overcoated with a thin layer of encapsulating resin. That is, once the foamed coating is formed on the surface of the electronic substrate, a thin layer of encapsulating resin can be applied. The thin layer of encapsulating resin can have a thickness of more than 0 mm and less than 5 mm, preferably less than 4 mm, more preferably less than 3 mm, more preferably less than 2 mm, more preferably less than 1 mm, more preferably less than 0.5 mm.

[0116] Figure 7 shows a diagram of an electronic assembly partially coated with a protective coating of the present invention. The coating of the present invention may also include a topcoat applied over the swollen protective coating, as shown in Figure 8.

[0117] The topcoat material may be added to improve abrasion resistance, solvent resistance, and / or electrical conductivity to act as a Faraday cage for RF shielding. It is believed that the protective coatings described herein can be used in combination with a topcoat that provides improved electrical conductivity to replace or significantly strengthen the housings of electronic devices.

[0118] In one embodiment, the topcoat comprises a hard, chemically resistant coating that can provide abrasion and chemical resistance, hi another embodiment, the topcoat comprises a conductive coating that can provide RF shielding functionality, and the foam acts as an electrical insulating layer to prevent shorting or changes in behavior of electronic substrates (e.g., PCBs).

[0119] In one embodiment, the topcoat comprises a hydrophobic formulation that can also provide improved water resistance. Many of these functions are normally handled by the metal or polymer housing, which adds significant weight. The use of a protective coating in combination with a topcoat layer can provide the same or similar level of protection as the metal or polymer housing, while substantially reducing the overall weight.

[0120] The ability to use a foamed coating in combination with a very thin layer of encapsulating resin provides a weight reduction of at least 75%, preferably at least 80%, and more preferably at least 85%, compared to an electronic substrate coated with only the encapsulating resin.

[0121] The inventors of the present invention have found that the expanded protective coatings described herein provide greater than about 90%, or greater than 92%, or even greater than 94% weight reduction compared to the same volume of potting material or encapsulating resin. In addition, the expanded protective coatings provide greater than about 10%, or greater than 12%, or even greater than 14% weight reduction compared to conformal coatings and also provide more complete coverage. That is, the expanded protective coatings of the present invention provide complete coverage and / or encapsulation of features, including vertical features, of electronic substrates due to the vertical expansion of the material during foaming.

[0122] The present invention provides a coating layer that effectively solves the application speed problem, provides sufficient coverage of all of the features contained on the electronic substrate, and can provide protection against typical harsh environments.

[0123] The invention will now be discussed with reference to the following non-limiting examples. EXAMPLES

[0124] The swelled protective coating was subjected to the following tests, as described below.

[0125] Condensation testing was carried out using surface insulation resistance (SIR) measurements to predict circuit reliability according to procedures developed by the National Physical Laboratory (UK).

[0126] Water vapor permeability testing was performed according to ASTM D1653 using the wet cup method (ie, Payne Cup).

[0127] Thermal shock was evaluated to measure resistance to damage due to sudden extreme temperature changes (i.e., -40°C to 130°C) over a short period of time.

[0128] A gravimetric water immersion test was performed according to a modified version of ASTM C272 to test foam on soldermask coated epoxy laminate to simulate a circuit board construction.

[0129] Volume resistivity and surface resistivity of the swollen protective coatings were performed according to ASTM D-257.

[0130] Flame retardancy was evaluated by the UL94 vertical flame test method, Standard for Tests for Flammability of Plastic Materials for Parts in Devices and Appliances. Within this standard, materials are subjected to various flame tests to ascertain their performance in flammable conditions. The UL94 V flammability method evaluates both the burn time and afterglow time after repeated flame application and dripping of flame specimens in a vertical flame test.

[0131] To achieve the UL94 V-0 standard, the sample must meet the following criteria 1) to 5). 1) Burning combustion does not persist for more than 10 seconds after application of a controlled flame. 2) The total flame burning time of the five samples does not exceed 50 seconds. 3) None of the samples burn to the mounting clamps by either flame or glowing heat. 4) None of the samples drip burning particles that would result in ignition of the cotton wool beneath them. 5) The sample does not exhibit red-hot burning for more than 30 seconds after the second controlled flame is removed.

[0132] Tensile properties were evaluated according to ASTM-D-638.

[0133] Example 1: The compositions were prepared as follows.

[0134] [Table 3]

[0135] The ingredients of Part A were mixed together thoroughly, then Part A and Part B were mixed in a ratio of 1.44:1 (w / w), and the composition was coated to a thickness of 300 micrometers onto the surface of an electronic substrate containing several vertical features. The coating expanded 10 times to a height of 3 mm within 4 minutes, completely covering / encapsulating the vertical features, as shown in FIG. 3.

[0136] The material from Example 1 was applied to an IPC B-24 test coupon (dipped tin and bare copper finish) at the same mix ratio (1.44:1 w / w), foamed, cured, and cured at room temperature for 24 hours, then placed in a humidity chamber and ramped to 85°C / 85%RH while the SIR was measured every 20 minutes at 50V bias. Notably, the insulation resistance of this foam remains above the typical industry acceptance standard of 100MΩ (8logΩ) throughout the 1000 hour test. At the end of the test, the coating still adhered well and showed no signs of reversion or delamination, indicating that the material is likely to provide excellent protection in high humidity conditions. The results are shown in Figure 4.

[0137] Example 2: The compositions were prepared as follows.

[0138] [Table 4]

[0139] The ingredients of Part A were mixed together thoroughly, then Part A and Part B were mixed in a ratio of 1.04:1 (w / w) and the composition was then coated onto an automotive test board, which was coated with 300 μm of the liquid coating composition and allowed to expand to a cured and swollen protective coating of 3 mm.

[0140] The coated assembly was then subjected to 1000 thermal shock cycles as described above and showed no evidence of cracking, as shown in Figure 5. There was some sign of discoloration but no sign of cracking, there was no noticeable embrittlement and the expanded protective coating remained flexible and spongy.

[0141] It should also be noted that, if desired, colorants can be added to the composition, as discussed above, to offset discoloration.

[0142] Example 3: The compositions were prepared as follows.

[0143] [Table 5]

[0144] The ingredients of Part A were mixed thoroughly. Part A was mixed with Part B in a 1.6:1 (w / w) ratio and coated onto a pre-weighed (4 dp) IPC B24 test board. After 24 hours, the coated board was weighed to 4 decimal places and then placed in DI water for 14 days. After 14 days, the coated assembly was removed, excess water was removed, and the "dry" assembly was immediately re-weighed to determine the % water absorption of the coating as shown below.

[0145] [Table 6]

[0146] The percentage of water absorption can be calculated as follows: 100 x 0.0372 / 4.0338 = 0.92%

[0147] Example 4: The compositions were prepared as follows.

[0148] [Table 7]

[0149] The ingredients of Part A were mixed thoroughly, then Part A and Part B were mixed in a ratio of 1.32:1 (w / w) and approximately 0.5 mL was dispensed into a mold (13 mm x 127 mm x 3 mm) used to make 3 mm thick samples for UL94 V-0 vertical flame test. After 1 hour, the samples were removed from the mold and then left overnight before flame testing. Flame samples were prepared in the same manner from a similar non-flame retardant coating of Example 2. The results are shown below.

[0150] [Table 8]

[0151] The non-flame retardant formulation of Example 2 burned completely and failed UV94V, while the flame retardant formulation of Example 4 met the UL94 V-0 standard.

[0152] Example 5: The compositions were prepared as follows. Part A:

[0153] [Table 9] 1 Capa products are available from Ingevity 2 NIAX products are available from Momentive Performance Materials Inc.

[0154] Part B was a 50:50 blend of Ongronat 2100 (available from BorsodChem), a polymeric MDI with an average functionality of 2.6-2.7, and Desmodur E23, a solvent-free aromatic polyisocyanate prepolymer based on diphenylmethane diisocyanate.

[0155] The ingredients of Part A were mixed thoroughly, then Part A and Part B were mixed in a ratio of 1.32:1 (w / w). Approximately 0.5 mL was dispensed into a mold used to prepare 10 mm thick samples for UL94 V-0 vertical burn testing. As described above, 20% expandable graphite was mixed into the polyol side of the two-part composition to provide an expanded protective coating containing 10.5% expandable graphite by weight.

[0156] After 1 hour the samples were removed from the mould and then left overnight before being flame tested. Flame samples were prepared in the same manner from a similar non-flame retardant coating of Example 2. The results are shown below.

[0157] [Table 10]

[0158] As can be seen from this table, all samples from this example pass the UV94 V-0 vertical burn test.

[0159] Example 6: The compositions were prepared as follows. Part A:

[0160] [Table 11] 1 Capa products are available from Ingevity 2 NIAX products are available from Momentive Performance Materials Inc.

[0161] Part B was the same as in Example 5. The ingredients of Part A were mixed thoroughly, then Part A and Part B were mixed in a ratio of 1.32:1 (w / w). Approximately 0.5 mL was dispensed into a mold used to prepare 15 mm thick samples for UL94V-0 vertical burn testing. As described above, 40% expandable graphite was mixed into the polyol side of the two-part composition to provide an expanded protective coating containing 23% expandable graphite by weight.

[0162] After 1 hour the samples were removed from the mould and then left overnight before being flame tested. Flame samples were prepared in the same manner from a similar non-flame retardant coating of Example 2. The results are shown below.

[0163] [Table 12]

[0164] Comparative Example 1: The compositions were prepared as follows.

[0165] [Table 13]

[0166] The ingredients of Part A were mixed thoroughly, then Part A and Part B were combined in a ratio of 1.90:1 (w / w) and dispensed onto IPC-B24 test coupons (both immersion tin and bare copper finishes), foamed, cured, and cured for 24 hours, then placed in a humidity chamber and ramped to 85°C / 85%RH while the SIR was measured every 20 minutes at 50V bias for approximately 1000 hours. The recorded insulation resistance values ​​are shown below. Notably, the insulation resistance quickly dropped below the industry accepted value of 100MΩ (8 logΩ) and continued to trend downward, suggesting that the material is a poor moisture barrier and protective coating. Upon removal from the chamber, Comparative Foam #1 showed a significant reduction in signs of reversion in terms of volume, area of ​​delamination, and sticky surface compared to Foam Example #1, which was essentially unchanged after 1000 hours of exposure at 85°C / 85%RH. The results are shown in Figure 6.

[0167] Figure 9 shows a comparison after 1000 hours at 85°C / 85% RH between an electronic assembly coated with the composition of Example 1 and an electronic assembly coated with the composition of Comparative Example 1. As can be seen in Figure 9, the composition of Example 1 provided a coated that provided good protection of the electronic assembly, while the coating produced according to the composition of Comparative Example 1 deteriorated and provided an insufficient moisture barrier and protective coating.

[0168] Although the present disclosure has been described with reference to exemplary implementations, the present disclosure is not limited by or to such exemplary implementations, but rather, various modifications, improvements, and / or alternative implementations may be employed without departing from the spirit or scope of the present disclosure.

[0169] In addition, although the invention has been described as providing an expanded protective coating on an electronic substrate, there are other applications in which an expanded coating that is lightweight and strong and provides electrical insulation, thermal insulation, and / or barrier properties is beneficial, and thus, electronic substrates are believed to be but one exemplary application of the protective coatings described herein, either alone or in combination with a suitable topcoat over the expanded coating layer.

Claims

1. A two-component coating composition, comprising: a) Part A, a. a polyol component comprising at least one of a difunctional polyol, a trifunctional polyol, and a tetrafunctional polyol; b. a blowing catalyst; c. optionally, a gel catalyst; d. optionally, at least one flame retardant; and e. Water; and b) Part B, a. an isocyanate-functional material having an isocyanate functionality of at least 2, preferably the isocyanate-functional material is an isocyanate prepolymer having a functionality of greater than 2 and less than 3; and b. Part B optionally comprising at least one flame retardant; A two-part coating composition, wherein the flame retardant must be present in at least one of Part A and Part B.

2. 2. The two-component coating composition of claim 1, wherein the difunctional polyol is present and is selected from the group consisting of polyethylene glycol, polypropylene glycol, polycaprolactone, polybutadiene, polyester, polyether, polyfarnesene, ethylene glycol dimerate, and combinations of two or more of the foregoing.

3. 3. The two-component coating composition of claim 2, wherein the difunctional polyol comprises a hydrophobic polyol selected from the group consisting of polybutadiene, polyfarnesene, and ethylene glycol dimerate.

4. 4. The two-component coating composition of any one of claims 1 to 3, wherein the trifunctional polyol is present and is selected from the group consisting of polyethylene glycol, polypropylene glycol, polycaprolactone, polybutadiene, polyester, polyether, polyfarnesene, ethylene glycol dimerate, and combinations of two or more of the foregoing.

5. The two-part coating composition of claim 4, wherein the trifunctional polyol comprises castor oil.

6. The two-component coating composition of any one of claims 1 to 5, wherein the polyol component comprises 0.1 to 99.9 wt% of the difunctional polyol.

7. The two-component coating composition of claim 6, wherein said polyol component comprises 30 to 70 weight percent of said difunctional polyol.

8. The two-component coating composition of claim 7, wherein said polyol component comprises 45 to 55 weight percent of said difunctional polyol.

9. The two-component coating composition of any one of claims 1 to 8, wherein the polyol component comprises 0.1 to 99.9 wt% of the trifunctional polyol.

10. The two-component coating composition of claim 9, wherein the polyol component comprises 30 to 70 weight percent of the difunctional polyol.

11. The two-component coating composition of claim 10, wherein said polyol component comprises 45 to 55 weight percent of said trifunctional polyol.

12. The two-component coating composition of any one of claims 1 to 11, wherein the polyol component comprises 0.1 to 99.9 wt% of the tetrafunctional polyol.

13. The two-component coating composition of claim 12, wherein the polyol component comprises 30 to 70 weight percent of the tetrafunctional polyol.

14. The two-component coating composition of claim 13, wherein said polyol component comprises 45 to 55 weight percent of said tetrafunctional polyol.

15. The two-component coating composition of any one of claims 1 to 14, wherein the tetrafunctional polyol comprises pentaerythritol.

16. The two-component coating composition according to any one of claims 1 to 15, wherein the water content of part A is in the range of 0.05 to 10 wt.

17. The two-component coating composition of claim 16, wherein the water content of Part A is in the range of 0.1 to 9 wt %.

18. 18. The two-component coating composition of claim 17, wherein the water content of Part A is in the range of 0.5 to 8 wt.%.

19. 20. The two-component coating composition of claim 18, wherein the water content of Part A is in the range of 3 to 7 wt.%.

20. 20. The two-component coating composition of claim 19, wherein the water content of Part A is in the range of 4.5 to 5.5 wt.%.

21. The two-component coating composition according to any one of claims 1 to 20, wherein the blowing catalyst is an amine catalyst.

22. 22. The two-component coating composition of claim 21, wherein the blowing catalyst is a tertiary amine catalyst.

23. 23. The two-component coating composition of claim 21 or 22, wherein the amine catalyst is selected from the group consisting of one of an aliphatic amine, a cycloaliphatic amine, an aromatic amine, an alcohol amine or an ammonium compound thereof, triethylenediamine, N,N,N,N-tetramethylalkylenediamine, N,N,N,N-pentamethyldiethylenetriamine, triethylamine, N,N-dimethylbenzylamine, N,N-dimethylhexadecylamine, N,N-dimethylbutylamine, triethylenediamine, N-ethylmorpholine, N-methylmorpholine, N,N-diethylpiperazine, N-diethyl-2-methylpiperazine, N,N-bis-(α-hydroxypropyl)-2-methylpiperazine, N-hydroxypropyldimethylmorpholine, pyridine, N,N-dimethylpyridine, and combinations of two or more of the foregoing.

24. The two-component coating composition of any one of claims 1 to 23, wherein the gel catalyst is an organometallic catalyst or an amine catalyst.

25. 25. The two-part coating composition of claim 24, wherein the organometallic catalyst is selected from the group consisting of dialkyltin dialkanoates, stannous octoate, dibutyltin dilaurate, dibutyltin diacetate, zinc neodecanoate, a blend of bismuth neodecanoate and neodecanoic acid, iron acetylacetonate, potassium acetate catalysts, potassium octoate catalysts, stannous octoate catalysts, bismuth based gelling catalysts, and combinations of the foregoing.

26. 25. The two-part coating composition of claim 24, wherein the amine catalyst is a gel amine catalyst.

27. The two-part coating composition of any one of claims 1 to 26, wherein Part A further comprises a chain extender.

28. 28. The two-component coating composition of claim 27, wherein the chain extender comprises a diol or diamine selected from the group consisting of aliphatic, araliphatic, aromatic and / or cycloaliphatic compounds, optionally having a low molecular weight.

29. 29. The two-component coating composition of claim 28, wherein the chain extender comprises a difunctional compound selected from diamines and / or alkanediols having 2 to 10 carbon atoms in the alkylene radical.

30. 30. The two-component coating composition according to any one of claims 27 to 29, wherein the chain extender is selected from the group consisting of 1,2-ethylenediol, 1,4-butanediol, 1,6-hexanediol, 1,3-propanediol, and / or dialkylene-, trialkylene-, tetraalkylene-, pentaalkylene-, hexaalkylene-, heptaalkylene-, octaalkylene-, non-alkylene, and decaalkylene-glycols having 2 to 8 carbon atoms in the alkylene portion, the corresponding oligopropylene glycols and / or propylene glycols.

31. The two-component coating composition of any one of claims 1 to 30, wherein Part A further comprises an inert inorganic filler or extender.

32. 32. The two-component coating composition of claim 31 , wherein the inert inorganic filler or extender is selected from the group consisting of talc, calcium carbonate, silica, wollastonite, aluminum hydroxide, kaolin, clay, calcium sulfate fibers, mica, glass beads, and nanomaterials such as nanographene, nanofibers, and nanoparticles.

33. 33. The two-component coating composition of any one of the preceding claims, wherein the flame retardant is selected from the group consisting of aluminum hydroxide trihydrate, phosphorus-containing polyols, microencapsulated ammonium polyphosphate, solid flame retardants, and combinations of the foregoing.

34. 34. The two-component coating composition of claim 33, wherein the flame retardant is a solid at room temperature, and the solid flame retardant has a typical average particle size of 50 to 500 micrometers.

35. The two-component coating composition of claim 34, wherein the solid flame retardant has a typical average particle size of 100 to 400 micrometers.

36. The two-component coating composition of claim 34, wherein the solid flame retardant has a typical average particle size of 90 to 350 micrometers.

37. The two-component coating composition of any one of claims 33 to 36, wherein the solid flame retardant comprises expandable graphite.

38. 38. The two-component coating composition of any one of claims 33 to 37, wherein the flame retardant comprises a combination of aluminum hydroxide trihydrate and expandable graphite.

39. 1. A method of applying a protective coating to one or more surfaces of a substrate, the method comprising: c) mixing a two-component coating composition, the two-component coating composition comprising: i) Part A, a. a polyol component comprising at least one of a difunctional polyol, a trifunctional polyol, and a tetrafunctional polyol; b. a blowing catalyst; c. optionally, a gel catalyst; d. optionally, at least one flame retardant; and e. Water; and ii) Part B, an isocyanate-functional material having an isocyanate functionality of at least 2, preferably said isocyanate-functional material being an isocyanate prepolymer having a functionality of greater than 2 and less than 3; and and Part B optionally comprising at least one flame retardant; To prepare a liquid coating composition, the at least one flame retardant must be present in at least one of Part A and Part B; d) applying the liquid coating composition to a substrate and expanding the liquid coating composition into a closed cell foam coating.

40. 40. The method of claim 39, wherein the liquid coating composition expands in volume vertically from the surface of the substrate by a factor less than 25 times the applied thickness of the liquid coating composition to form an expanded closed cell foam coating.

41. 41. The method of claim 40, wherein the liquid coating composition expands in volume vertically from the surface of the substrate by a factor of 8 to 20 times the applied thickness of the liquid coating composition to form the expanded closed cell foam coating.

42. 42. The method of claim 41 , wherein the liquid coating composition expands in volume vertically from the surface of the substrate by a factor of about 10 to about 15 times the applied thickness of the liquid coating composition to form the expanded closed cell foam coating.

43. A method according to any one of claims 39 to 42, wherein the foaming reaction occurs in less than 10 minutes to produce a tack-free coating.

44. 44. The method of claim 43, wherein the foaming reaction occurs in less than 5 minutes to produce a tack-free coating.

45. 45. The method of claim 44, wherein the foaming reaction occurs in less than 4 minutes to produce a tack-free coating.

46. The method of any one of claims 39 to 45, wherein the liquid coating composition is applied by spraying.

47. The method of any one of claims 39 to 45, wherein the liquid coating composition is applied by dispensing.

48. The method according to any one of claims 39 to 47, wherein the substrate is an electronic substrate comprising at least one of irregularities and protrusions, and the expanded coating composition encapsulates at least one of the irregularities and protrusions.

49. The method of any one of claims 39 to 48, further comprising applying a topcoat layer over the expanded closed cell foam coating layer.

50. 50. The method of claim 49, wherein the topcoat layer has a thickness greater than 0 mm and less than 5 mm.

51. 51. The method of claim 50, wherein the topcoat layer has a thickness of less than 4 mm.

52. 52. The method of claim 51, wherein the topcoat layer has a thickness of less than 3 mm.

53. 53. The method of claim 52, wherein the topcoat layer has a thickness of less than 2 mm.

54. 54. The method of claim 53, wherein the topcoat layer has a thickness of less than 1 mm.

55. 55. The method of claim 54, wherein the topcoat layer has a thickness of less than 0.5 mm.

56. The method of any one of claims 49 to 55, wherein the topcoat layer is selected from the group consisting of a chemical resistant coating, a hydrophobic coating, a microencapsulated resin, and combinations of the foregoing.

57. 57. The method of any one of claims 39 to 56, wherein the expanded closed cell foam coating layer is flame retardant and capable of passing a UL94 V-0 vertical burn test.

58. The method of any one of claims 39 to 57, wherein the liquid coating composition is constrained in at least one direction to limit the expansion space of the foam.

59. The method of any one of claims 39 to 58, wherein the liquid coating composition is optimized to delay the foaming reaction.

60. The method according to any one of claims 39 to 59, wherein the blowing catalyst is microencapsulated.

61. 61. An electronic board assembly comprising a printed circuit board, the printed circuit board including a base support and a plurality of electrical circuit components extending outwardly from a surface of the attached base support and electrically connected to an electrical circuit, a closed cell foam protective coating applied to at least a portion of a surface of the electronic board assembly including the plurality of electrical circuit components, the closed cell protective coating comprising the two-part coating composition of any one of claims 1 to 38, Part A and Part B being in mixed form in the closed cell protective coating, and / or the closed cell protective coating being applied by the method of any one of claims 39 to 60.

62. 62. The electronic board assembly of claim 61, wherein the protective coating is capable of passing a UL94 V-0 vertical burn test.

63. 63. The electronic substrate assembly of claim 61 or 62, further comprising a topcoat layer over the closed cell protective coating.

64. 64. The electronic substrate assembly of claim 63, wherein the topcoat layer has a thickness greater than 0 mm and less than 5 mm.

65. 65. The electronic substrate assembly of claim 64, wherein the topcoat layer has a thickness of less than 4 mm.

66. 66. The electronic substrate assembly of claim 65, wherein the topcoat layer has a thickness of less than 3 mm.

67. 67. The electronic substrate assembly of claim 66, wherein the topcoat layer has a thickness of less than 2 mm.

68. 68. The electronic substrate assembly of claim 67, wherein the topcoat layer has a thickness of less than 1 mm.

69. 69. The electronic substrate assembly of claim 68, wherein the topcoat layer has a thickness of less than 0.5 mm.

70. 70. The electronic substrate assembly of any one of claims 63 to 69, wherein the topcoat layer is selected from the group consisting of a chemically resistant coating, a hydrophobic coating, a microencapsulated resin, and combinations of the foregoing.

Citation Information

Patent Citations

  • Urethane resin composition and preparation of moisture-proof insulated packaged circuit board

    JP1991028218A

  • Circuit component incorporating module

    JP2004103998A

  • Phosphorus flame retardants and their uses

    JP2012511089A

  • Formulated resin compositions for flood coating electronic circuit assemblies

    JP2017524794A

  • Low TVOC flame-retardant polyurethane spray foam system

    WO2021013478A1