Sustainable Polyethylene Laminates for Packaging
The polyethylene laminate film with a differential seal initiation temperature and specific ethylene polymer compositions addresses the issues of stiffness and heat resistance, enabling high-speed packaging operations and recyclability without additional barrier coatings.
Patent Information
- Application Number
- JP2024530515
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-23
- Filing Date
- 2022-11-22
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-11-22
AI Technical Summary
Conventional polyethylene laminates lack sufficient stiffness and heat resistance, making them unsuitable for high-speed packaging operations and requiring additional barrier coatings, which complicates recycling and increases costs.
A polyethylene laminate film comprising a printed film with specific ethylene polymer compositions and a sealant film, designed to have a differential seal initiation temperature and excellent mechanical properties, allowing high-speed operation without additional barrier coatings.
The laminate film achieves improved heat resistance, mechanical properties, and barrier performance, enabling smooth operation on high-speed packaging machines while being fully recyclable and maintaining good optical properties.
Smart Images

Figure 2024542519000016 
Figure 2024542519000017 
Figure 2024542519000018
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyethylene laminate film comprising a print film and a sealant film.Furthermore, the present invention relates to an article comprising the polyethylene laminate film, and the use of the polyethylene laminate film in packaging applications.The present invention also relates to a sealant film and its use in packaging applications. [Background technology]
[0002] Laminate films are widely used in packaging applications. Conventional flexible packaging laminates include different polymer families, e.g. polyester (e.g. PET), polyamide or oriented polypropylene (e.g. BOPP) as the printing film and polyethylene (PE) as the sealant film. Laminates are generally employed in the packaging industry to meet multifunctional requirements from different films, i.e. sufficient toughness-related properties of the sealant film to ensure package integrity without distortion or rupture, and stiffness- and barrier-related properties of the substrate film to ensure improved shelf life and subsequent handling and manipulation of the packaged goods, especially during packaging in form-fill-seal (FFS) machines. Besides good sealing performance, a balanced behavior of impact strength (e.g. dart impact) and mechanical properties (e.g. stiffness, tensile strength) as well as good aesthetic performance (e.g. in terms of gloss and transparency) are desired for the sealant film. The substrate is laminated with a polyethylene sealant film to provide good stiffness, heat resistance, optical and barrier properties.
[0003] Recently, there has been a growing trend to laminate polyethylene sealant films to substrates also made of polyethylene, providing a “pure” polyethylene solution. These laminates, based on a single class of resin, can be easily recycled by conventional methods, improving sustainability and reducing production costs by using cheaper polyethylene polymers. However, replacing conventional substrates with polyethylene substrates has been difficult, as the polyethylene substrate lacks stiffness and has poor heat resistance, which may not be adequate to withstand the faster packaging speeds on vertical form-fill-seal (VFFS) lines and the higher temperatures of the top sealing jaws. “Pure” polyethylene solutions usually tend to have poor stiffness, heat resistance and barrier performance, making them difficult to use on a variety of FFS machines and in a variety of end applications. It is a big challenge to produce a complete PE laminate with the necessary properties to run smoothly on high-speed VFFS packaging machines, where higher heat resistance is essential to avoid problems with the film sticking to the sealing jaws. Thus, although "pure" polyethylene laminates are known, there remains a need to further improve the performance of such laminates, particularly when the substrate is produced as an unoriented PE film.
[0004] WO 2018 / 187438 describes a laminate structure for packaging comprising a sealant film and a layered printed film having a thickness of 15 microns to 30 microns. The middle layer of the printed film has a density of 0.950 to 0.965 g / cm 3 and a melt index (I2) of 0.1 to 20 g / 10 min. The inner and outer layers are both 0.925 to 0.965 g / cm3 and contain at least 90% by weight of high density polyethylene (HDPE). 3 The film contains a linear low density polyethylene (LLDPE) having a density of 1000 .mu.m. No details regarding the SIT, optical properties, or mechanical properties are disclosed in this publication, either for the printed film or the laminate structure. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Application Publication No. 2018 / 187438 Summary of the Invention [Problem to be solved by the invention]
[0006] It is therefore an object of the present invention to provide a polyethylene laminate film, preferably produced from a conventional non-oriented blown film (blowing film) or cast film, which exhibits excellent performance in high speed VFFS operations by having good or even improved heat resistance and mechanical properties and at the same time exhibits excellent sealing performance.
[0007] It is a further object of the present invention to provide a polyethylene laminate film having good barrier properties, preferably without the use of additional barrier coating (e.g. metallization) procedures, which are required for the intended use of the laminate film, especially in packaging applications where moisture barrier is important.
[0008] It is a further object of the present invention to provide a polyethylene laminate film having good optical properties (eg gloss and haze) while also meeting the aesthetic requirements set forth in films for packaging applications.
[0009] Finally, it is an object of the present invention to provide a polyethylene laminate film containing printed film having the properties (mechanical properties and heat resistance) required for high speed printing operations and subsequent performance on the packaging line. [Means for solving the problem]
[0010] These combinations of objects are achieved by the present invention, which comprises a polyethylene laminate film having an inner surface and an outer surface, a) A printed film comprising an outer layer E, a core layer F and an inner layer G, the inner layer G forming the outer surface of the laminate film, the inner layer G having a compressive strength of 920 to 935 kg / m 3 a printed film made of an inner layer G composition including a component AG that is an ethylene copolymer having a density of 0.5 to 2.0 g / 10 min and a melt flow rate (MFR2) measured in accordance with ISO 1133; and b) a sealant film comprising an outer layer A, a core layer B and an inner layer C, said inner layer C forming said inner surface of said laminate film, said inner layer C being made of an inner layer C composition comprising at least one ethylene polymer; Including, The outer layer A of the sealant film is laminated to the outer layer E of the printing film, A polyethylene laminate film is provided, wherein the seal initiation temperature (SIT) at 5N of the outer surface of the laminate film is at least 10°C higher than the seal initiation temperature at 5N of the inner surface of the laminate film, the seal initiation temperature being measured according to ASTM F 2029 and ASTM F 88.
[0011] The present invention is based on the discovery that such a polyethylene laminate film can be provided by the combination of a printed film and a sealant film, where the inner layer of the printed film comprises a specially selected ethylene polymer and the heat resistance properties of the outer layer of the laminate film are specially tailored.
[0012] The combination of the print film and the inner layer of the sealant film in the polyethylene laminate film of the present invention achieves the above object.
[0013] The difference in seal initiation temperature between the two outer faces of the laminated film is at least 10°C and the very good mechanical properties allow the laminated film to be run at packaging speeds of 50-80 pouches / min while achieving excellent sealing behavior without problems of sticking to the jaws at the sealing bar of the VFFS line.
[0014] This laminate film achieves excellent barrier properties without the need for barrier coatings or metallization and can be used without recyclability issues in the majority of packaging applications where moisture barrier is most critical.
[0015] Although it is very difficult to increase the heat resistance of a polyethylene film while maintaining good optical properties, this laminate film also features relatively high gloss and low haze. Thus, the polyethylene laminate film of the present invention has all the properties desired for a laminate film used in packaging applications.
[0016] Furthermore, the printed film of the laminate film can be easily run on a high speed printing press. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 shows the structure of one embodiment of the laminate film of the present invention. [Diagram 2] FIG. 2 shows the sealing initiation temperature of sealant films. [Diagram 3] FIG. 3 shows the seal initiation temperature of printed film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] In the present invention, the polyethylene laminate film comprises or consists of a sealant film and a printing film.
[0019] Printing Film <Structure> The expression "printed film" refers to a film that includes a layer that can be used in a printing operation (such as a high speed printing process). The film can be a non-printed film or a printed film.
[0020] The printed film of the present invention comprises or consists of several layers, at least an outer layer E, a core layer F and an inner layer G. The core layer F is the outer layer, i.e. located between the outer layer E and the inner layer G. Preferably, the outer layer E of the printed film is a printable or printed layer, i.e. printing can be carried out on the outer layer E of the printed film, preferably after a surface treatment (corona treatment).
[0021] The printed film also functions as a substrate (film) and contributes to the mechanical and / or optical properties of the laminate film. Thus, in this disclosure, the terms "printed film" and "substrate film" or "substrate" are used interchangeably. When laminated to the sealant film, the inner layer G forms the outer surface of the laminate film.
[0022] In one embodiment, the printed film consists of an outer layer E, a core layer F, and an inner layer G. In another embodiment, the printed film includes one or more additional intermediate (or subskin) layers Y.
[0023] In certain embodiments, the printed film further comprises one or more intermediate layers Y between the core layer F and the inner layer G, and between the core layer F and the outer layer E, for example in the 5 layer film structure E / Y1 / F / Y2 / G or the 7 layer film structure E / Y1 / Y1 / F / Y2 / Y2 / G. Preferably, the printed film comprises up to 9 layers, more preferably up to 7 layers.
[0024] When present, the intermediate layer Y preferably comprises or consists of a composition similar to that of the adjacent layer. Thus, the intermediate layer Y may be either the composition of the core layer F, or the composition of the adjacent inner layer G or the adjacent outer layer E.
[0025] Preferably, the printed film has a thickness of 15 to 40 μm, more preferably 20 to 38 μm, and most preferably 22 to 35 μm.
[0026] Preferably, the core layer F has a thickness of 30-80% of the total printed film thickness, more preferably 35-75%, and most preferably 40-70%.
[0027] The outer layer E and / or the inner layer G each preferably have a thickness of 10-35%, more preferably 15-30%, for example 25% of the total film thickness. In a five-layer film structure E / Y1 / F / Y2 / G, the inner layer G and / or the outer layer E each preferably have a thickness of 5-25%, more preferably 7.5-20% of the total printed film thickness.
[0028] Preferably, the printing film is a "polyethylene film", i.e. a film comprising or consisting of at least one ethylene polymer, which may be a homopolymer or a copolymer of ethylene. Preferably, the polyolefin film comprises at least 90% by weight, more preferably at least 95% by weight, most preferably at least 98% by weight, based on the total weight of the polyethylene film. Preferably, the polyethylene film comprises 90-100% by weight, more preferably 95-100% by weight, most preferably 98-100% by weight, based on the total weight of the polyethylene film. Most preferably, the polyethylene film consists exclusively of ethylene polymer. Preferably, the ethylene polymer comprises or consists of either an ethylene homopolymer and / or a copolymer of ethylene and propylene and / or an α-olefin having 4-10 carbon atoms. Preferably, the polyethylene film does not comprise a non-polyolefin polymer, more preferably does not comprise a non-polyethylene polymer. Particularly preferred, the polyethylene film does not comprise a polyester or polyamide polymer. The use of polyethylene film allows for a fully recyclable and sustainable packaging structure to be provided.
[0029] Generally, print films are provided as oriented or unoriented films. Oriented films are those that are "stretched" after production. Oriented films are usually stretched in the machine direction (MD) and / or transverse direction (TD) by more than 300%, preferably more than 500%. Films stretched in the machine direction are often called "MDO" films. Films stretched in two directions are called "biaxially oriented polyethylene" (BOPE). Unoriented films are blown or cast films, which are not intentionally stretched (preferably more than 200%) after film production by any suitable means, i.e., by subsequent heating and / or the use of rollers during film production.
[0030] Preferably, the printed film is a non-oriented film. Preferably, the printed film is produced on a standard blown and / or cast film line through a standard film machinery system (nip rollers or take-off rollers and winders) without the use of a stretching device.
[0031] As understood within the meaning of the present disclosure, the print film and its respective layer compositions for layer preparation can also contain additives such as stabilizers, processing aids and / or pigments. Examples of such additives include antioxidants, UV stabilizers, acid scavengers, nucleating agents, antiblocking agents, slip agents, etc., as well as polymer processing agents (PPAs). The additives may be present in some or only one layer of the film, with the same or different contents. The additives may be added to each layer composition during the preparation of the composition, or may already be included in any of the polymers used to prepare the respective layer composition.
[0032] Generally, each additive may be present in an amount of 0-5000 ppm based on the total weight of the respective layer composition used to prepare the layer of the film. The additives are generally available from a number of suppliers and are included in the composition as a single additive or as a mixture of two or more additives. Such compositions may generally be present in the layer composition in an amount of 0-5 wt %, based on the weight of the respective layer composition used to prepare the layer of the film.
[0033] Generally, within the meaning of the present disclosure, percentages (%) are understood to be percentages by weight (wt %), unless otherwise specified.
[0034] <Composition> Each of the print film layers is made of a composition that includes at least one polymer (e.g., polyethylene) component. If the composition includes multiple polymer components, it is a blend of these components. Additional compounds (polymer processing aids, antiblock agents, slip agents, and other additives) may be present in the composition.
[0035] Inner layer G The inner layer G is made of an inner layer G composition that contains components that contribute, inter alia, to the heat resistance and optical properties of the film. In addition, this layer also imparts mechanical properties to the film.
[0036] When laminated to a sealant film, the inner layer G forms the outer surface of the laminate film. Good optical properties are important for this layer since the printing films used in the laminate film are typically reverse printed on the outer layer.
[0037] The choice of ethylene polymer for the inner layer produces a printing film that is ideal for high speed printing operations, especially printing speeds above 200m / min.
[0038] Ingredient AG The inner layer G of the printed film is 920-935kg / m 3and a melt flow rate (MFR2) of 0.5 to 2.0 g / 10 min, as measured in accordance with ISO 1133.
[0039] In general, ethylene polymers can be unimodal or multimodal, e.g., bimodal. By "modality" of a polymer is meant the structure of the molecular weight distribution of the polymer, i.e., the appearance of the curve showing the number of molecules as a function of molecular weight. If the curve shows one maximum, the polymer is called "unimodal", if the curve shows a very broad maximum or two or more maxima and the polymer consists of two or more fractions, the polymer is called "bimodal", "multimodal", etc. For example, if a polymer is produced in a sequential multistage process using reactors connected in series, with different conditions in each reactor, the polymer fractions produced in the different reactors will each have their own molecular weight distribution and weight average molecular weight. When the molecular weight distribution curve of such a polymer is recorded, the individual curves from these fractions are superimposed on the molecular weight distribution curve of the entire resulting polymer product, usually resulting in a curve with two or more distinct maxima.
[0040] In the production of unimodal ethylene polymers, ethylene polymers are produced in a reactor under certain conditions with respect to monomer composition, hydrogen gas pressure, temperature, pressure, etc. As comonomers, other olefins having up to 12 carbon atoms, such as α-olefins having 3 to 12 carbon atoms, e.g., propene, 1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-decene, etc., are commonly used in the copolymerization of ethylene.
[0041] For example, in the production of bimodal ethylene polymers, a first ethylene polymer is produced in a first reactor under certain conditions with respect to monomer composition, hydrogen gas pressure, temperature, pressure, etc. After polymerization in the first reactor, the reaction mixture containing the produced polymer is fed to a second reactor where further polymerization takes place under different conditions. Typically, a first polymer with a high melt flow rate (low molecular weight) and moderate or low comonomer loading or no comonomer loading is produced in the first reactor, while a second polymer with a low melt flow rate (high molecular weight) and high comonomer loading is produced in the second reactor. The resulting final product consists of an intimate mixture of polymers from the two reactors, whose different molecular weight distribution curves form a molecular weight distribution curve with a broad maximum or two maximum values. That is, the final product is a bimodal polymer mixture.
[0042] Preferably, component AG is a multimodal ethylene copolymer, more preferably a bimodal ethylene copolymer, even more preferably a copolymer of ethylene and at least two different C4-C 12 It is a copolymer with an α-olefin monomer, i.e. a terpolymer.
[0043] Preferably, the multimodal terpolymer comprises or consists of a multimodal polymer of ethylene and at least two different comonomers selected from α-olefins having 4 to 10 carbon atoms and has a ratio MFR of 13 to 30. 21 / Has MFR2 and MWD ≤6.
[0044] Such multimodal ethylene terpolymers are disclosed, for example, in WO 2016 / 083208. For the definitions (such as the "modalities" of the polymers) and for the preparation of these ethylene terpolymers, reference is made to WO 2016 / 083208. Furthermore, all embodiments and preferred embodiments of ethylene terpolymers having the required density as described in WO 2016 / 083208 are also preferred embodiments of the multimodal ethylene terpolymers of component AG according to the present invention, whether or not they are explicitly described herein.
[0045] The multimodal ethylene terpolymer preferably has an MFR2 in the range of 0.5 to 2.5 g / 10 min, particularly preferably 1.0 to 1.8 g / 10 min. Preferably, the multimodal ethylene terpolymer has an MFR2 in the range of 922 to 933 kg / m 3 , more preferably 923 to 930 kg / m 3 The multimodal ethylene terpolymer preferably has a specific MFR of 13 to 30, more preferably 15 to 25. 21 / Has MFR2.
[0046] The at least two α-olefin comonomers having 4 to 10 carbon atoms of the multimodal ethylene terpolymer are preferably 1-butene and 1-hexene. Preferably, the total amount of comonomers present in the multimodal ethylene terpolymer is 0.5 to 10 mol%, preferably 1.0 to 8 mol%, more preferably 1.0 to 5 mol%, more preferably 1.1 to 4.0 mol%.
[0047] The multimodal ethylene terpolymer, which is preferably a bimodal terpolymer, preferably comprises or consists of an ethylene polymer component (A1) and an ethylene polymer component (B1), the ethylene polymer component (A1) having a higher MFR2 than the ethylene polymer component (B1).
[0048] More preferably, the ethylene polymer component (A1) has an MFR2 of 1 to 50 g / 10 min, preferably 1 to 40 g / 10 min, more preferably 1 to 30 g / 10 min, more preferably 2 to 20 g / 10 min, more preferably 2 to 15 g / 10 min, and even more preferably 2 to 10 g / 10 min.
[0049] The ratio of MFR2 of the ethylene polymer component (A1) to MFR2 of the ethylene polymer component (B1) is 2-50, preferably 5-40, more preferably 10-30, even more preferably 10-25, and even more preferably 11-25.
[0050] Preferably, the ethylene polymer component (A1) contains a comonomer different from the ethylene polymer component (B1). Preferably, the ethylene polymer component (A1) has a smaller amount (mol%) of comonomer than the ethylene polymer component (B1), more preferably the ratio of the amount (mol%) of α-olefin comonomer having 4 to 10 carbon atoms present in the ethylene polymer component (A1) to the amount (mol%) of at least two α-olefin comonomers having 4 to 10 carbon atoms in the final multimodal polymer of ethylene is 0.2 to 0.6, preferably 0.25 to 0.5.
[0051] Preferably, the α-olefin comonomer having 4 to 10 carbon atoms of the ethylene polymer component (A1) is 1-butene and the α-olefin comonomer having 4 to 10 carbon atoms of the ethylene polymer component (B1) is 1-hexene. Particularly preferred, the bimodal terpolymer is prepared in two or more polymerization stages, in which a lower α-olefin comonomer (e.g. 1-butene) is introduced by slurry polymerization in a loop reactor and a higher α-olefin comonomer (1-hexene) is introduced by gas phase polymerization in a gas phase reactor.
[0052] Preferably, the ethylene polymer component (A1) has a density different from, and preferably higher than, the ethylene polymer component (B1). The density of the ethylene polymer component (A1) is preferably 925 to 950 kg / m 3, more preferably 930 to 945 kg / m 3 It is.
[0053] Preferably, the multimodal ethylene terpolymer comprises ethylene polymer component (A1) in an amount of 30-70 wt%, preferably 40-60 wt%, more preferably 35-50 wt%, more preferably 40-50 wt%, and ethylene polymer component (B1) in an amount of 70-30 wt%, preferably 60-40 wt%, more preferably 65-50 wt%, more preferably 60-50 wt%, based on the total amount of ethylene polymers (100 wt%).
[0054] Most preferably, the multimodal ethylene terpolymer is composed of the ethylene polymer components (A1) and (B1) as homopolymer components. Thus, the ratio of the ethylene polymer component (A1) to the ethylene polymer component (B1) is (30-70):(70-30), preferably (40-60):(60-40), more preferably (35-50):(65-50), and more preferably (40-50):(60-50).
[0055] In a particularly preferred embodiment, the multimodal terpolymer is a bimodal terpolymer, i.e. comprising a low molecular weight component and a high molecular weight component, and has a MFR2 of 1.0 to 1.8 g / 10 min, and / or a MFR5 of 2.8 to 4.5 g / 10 min, and / or a MFR of 20 to 36 g / 10 min. 21 , and / or 925-929 kg / m 3 and / or a molecular weight distribution (M w / M n ), and / or M between 15 and 25 kg / mol n , and / or M between 70 and 125 kg / mol w , and / or MFR between 15 and 25 21 / MFR2 ratio (FRR 21 / 2 ), and / or MFR of 6-9 21 / MFR5 ratio (FRR 21 / 5 All molecular weight parameters are determined by GPC conventional methods using standard calibrations, as detailed below.
[0056] As the AG component, the resin Anteo™ FK2715 from Borealis or Borouge can be used.
[0057] Preferably, component AG is present in the inner layer G composition in an amount of 40 to 80 weight percent, more preferably 50 to 75 weight percent, and most preferably 55 to 70 weight percent, based on the total weight of the inner layer G composition.
[0058] In addition to component AG, the inner layer G composition may include further components different from component AG.
[0059] Ingredients BG1 and BG2 The inner layer G composition may further include components BG1 and / or BG2.
[0060] Preferably, component BG1 is 915 to 930 kg / m 3 and a melt flow rate (MFR2) of 0.05 to 1.0 g / 10 min, measured in accordance with ISO 1133.
[0061] Such LLDPEs are well known in the art and are usually prepared by a catalytic polymerization process. The LLDPE of component BG1 is preferably a multimodal LLDPE, more preferably a bimodal LLDPE. Such multimodal LLDPEs and their preparation are described, for example, in the referenced WO 2004 / 000933, pages 9-12.
[0062] The LLDPE of component BG1 is preferably 920 to 928 kg / m 3 , more preferably 920 to 925 kg / m 3 has a density of
[0063] Preferably, the LLDPE of component BG1 is an ethylene copolymer. The comonomer may be an α-olefin having 4 to 12 carbon atoms, such as 1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-decene. More preferably, the LLDPE is a copolymer of ethylene and 1-butene or 1-hexene, most preferably a copolymer of ethylene and 1-butene.
[0064] Preferably, the total amount of comonomers present in the LLDPE of component BG1 is from 2.0 to 6.0 mol %, more preferably from 2.5 to 5.5 mol %, and most preferably from 3.0 to 5.2 mol %.
[0065] Preferably, the LLDPE of component BG1 has a MFR2 of 0.1 to 0.5 g / 10 min, more preferably 0.15 to 0.4 g / 10 min, and most preferably 0.20 to 0.30 g / 10 min.
[0066] Component BG1 preferably has a lower density and / or a lower melt flow rate (MFR2) than component AG.
[0067] In a particularly preferred embodiment, the LLDPE of component BG1 has an MFR2 of 0.20 to 0.30 g / 10 min and / or an MFR5 of 0.80 to 1.2 g / 10 min and / or an MFR of 18 to 26 g / 10 min. 21 , and / or 920-925 kg / m 3 and / or a molecular weight distribution (MWD) between 10 and 24 and / or a M between 10 and 15 kg / mol n , and / or M between 150 and 250 kg / mol w , and / or MFR between 80 and 110 21 / MFR2 ratio (FRR 21 / 2 ), and / or MFR of 18-26 21 / MFR5 ratio (FRR 21 / 5 All molecular weight parameters are determined by GPC conventional methods using standard calibrations, as detailed below.
[0068] As LLDPE for component BG1, resins Borstar FB2230 or FB2235 from Borealis or Borouge can be used.
[0069] Preferably, component BG2 is 950 to 970 kg / m 3 and a melt flow rate (MFR2) of 0.2 to 2.0 g / 10 min, measured in accordance with ISO 1133.
[0070] HDPE is well known in the art and is typically produced by a catalyzed polymerization process.
[0071] The HDPE of component BG2 is preferably a multimodal HDPE, more preferably a bimodal HDPE.
[0072] The HDPE of component BG2 is preferably 955 to 968 kg / m 3 , more preferably 958 to 965 kg / m 3 Such multimodal HDPE and its production are described, for example, in the referenced International Application Publication No. WO 2020 / 109289, pages 19-28.
[0073] Preferably, the HDPE is a copolymer. An ethylene copolymer is a polymer containing ethylene monomer and one or more comonomers. The comonomer may be an α-olefin having 4 to 12 carbon atoms, such as 1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-decene. More preferably, the HDPE is a copolymer of ethylene and 1-butene, 1-hexene or 1-octene, most preferably a copolymer of ethylene and 1-butene.
[0074] Preferably, the total amount of comonomers present in HDPE is from 0.0 to 0.40 mol %, more preferably from 0.01 to 0.30 mol %, and most preferably from 0.02 to 0.20 mol %.
[0075] Preferably, the HDPE of component BG2 has a MFR2 of 0.25 to 1.8 g / 10 min, more preferably 0.3 to 1.5 g / 10 min, even more preferably 0.4 to 1 g / 10 min, and most preferably 0.5 to 0.9 g / 10 min.
[0076] In a particularly preferred embodiment, the HDPE of component BG2 has an MFR2 of 0.5 to 0.9 g / 10 min and / or an MFR5 of 2.0 to 3.5 g / 10 min and / or an MFR of 30 to 50 g / 10 min. 21 , and / or 958-965 kg / m 3 and / or a molecular weight distribution (MWD) of 10-15 and / or a M of 7-12 kg / mol n , and / or M between 100 and 165 kg / mol w , and / or MFR between 50 and 75 21 / MFR2 ratio (FRR 21 / 2), and / or MFR between 10 and 25 21 / MFR5 ratio (FRR 21 / 5 All molecular weight parameters are determined by GPC conventional methods using standard calibrations, as detailed below.
[0077] As the HDPE of component BG2, the resin Borstar FB5600 manufactured by Borouge can be used.
[0078] Preferably, components BG1 and / or BG2 are present in the inner layer G composition in an amount of 15 to 45 weight percent, more preferably 20 to 40 weight percent, based on the total weight of the inner layer G composition.
[0079] Ingredient CG The inner layer G composition may further comprise component CG. Preferably, component CG is a low density ethylene polymer (LDPE), more preferably 918 kg / m 3 ~928kg / m 3 and a melt flow rate (MFR2) measured in accordance with ISO 1133 in the range of 1.5 to 2.5 g / 10 min.
[0080] LDPE is well known in the art and is usually manufactured in a high pressure process carried out in a tubular reactor or autoclave.
[0081] LDPE and its production are described, for example, on page 9, line 29 to page 12, line 6 of the referenced WO 2017 / 055174.
[0082] The LDPE of the component CG is preferably 918 to 928 kg / m 3 , more preferably 919 to 927 kg / m 3 , and most preferably 920 to 925 kg / m 3 has a density of
[0083] Preferably, the LDPE of component CG has an MFR2 of 1.6 to 2.4 g / 10 min.
[0084] In a particularly preferred embodiment, the LDPE of component CG has an MFR2 of 1.6 to 2.4 and / or a molecular weight of 920 to 925 kg / m 3 and / or MWD between 5.5 and 9, and / or M between 12 and 18 kg / mol n , and / or M between 80 and 130 kg / mol w All molecular weight parameters are measured by GPC viscosimetry using standard calibrations, as further detailed below.
[0085] As LDPE for component CG, resins FT6230 or FT6236 from Borealis or Borouge can be used.
[0086] Preferably, component CG is present in the inner layer G composition in an amount of from 5 to 15 weight percent, more preferably from 7 to 13 weight percent, based on the total weight of the inner layer G composition.
[0087] In one embodiment, the inner layer G composition comprises or consists of components AG and BG1, and optionally CG, in any of the above embodiments.
[0088] In another embodiment, the inner layer G composition comprises or consists of components AG and BG2, and optionally CG, in any of the above embodiments.
[0089] In a further embodiment, the inner layer G composition comprises or consists of components AG, BG1 and BG2, and optionally CG, in any of the above embodiments.
[0090] In a preferred embodiment, the inner layer G composition comprises, or consists of, component AG in an amount of 50-75 wt.%, either one of components BG1 or BG2 in an amount of 25-40 wt.%, and optionally component CG in an amount of 0-15 wt.%, based on the total weight of the inner layer G composition.
[0091] In general, component AG is responsible for the relatively high seal initiation temperature and good optical properties of the printed film. Components BG1 and BG2 further contribute to the high seal initiation temperature without affecting the optical properties of the printed film.
[0092] Core layer F The core layer F composition of the printing film is made of a core layer F which contains components that contribute to the film stiffness required in particular for the film extrusion process and also for printing operations, especially high speed printing operations.
[0093] Ingredient AF The core layer F composition can include component AF. Preferably, component AF is a high density ethylene polymer (HDPE), preferably having a viscosity of 950 to 970 kg / m, as described for component BG2 of the inner layer G composition. 3 and a melt flow rate (MFR2) in the range of 0.2-2.0 g / 10 min, measured in accordance with ISO 1133.
[0094] All embodiments described for component BG2 are embodiments for component AF. Component AF can be independently selected from any one of these embodiments, and the selected embodiment can be the same or different for AF and BG2.
[0095] Preferably, component AF is present in the core layer F composition in an amount of up to 90 wt.%, preferably from 50 to 90 wt.%, more preferably from 60 to 88 wt.%, and most preferably from 70 to 87 wt.%, based on the total weight of the core layer F composition.
[0096] Component AF imparts high stiffness to the printed film.
[0097] Ingredient BF The core layer F composition can include component BF. Preferably, component BF is an ethylene copolymer, preferably having a viscosity of 920 to 935 kg / m, as described for component AG of the inner layer G composition. 3 and a melt flow rate (MFR2) of 0.5 to 2.0 g / 10 min measured in accordance with ISO 1133.
[0098] All embodiments described for component AG are also embodiments for component BF. Component BF can be independently selected from any one of these embodiments, and the selected embodiment can be the same or different for BF and AG.
[0099] Preferably, component BF is present in the core layer F composition in an amount of 5 to 40 weight percent, more preferably 10 to 35 weight percent, based on the total weight of the core layer F composition.
[0100] In one embodiment, the core layer F is made of a core layer F composition comprising or consisting of components AF and BF, selected from any one of the above embodiments.
[0101] In a preferred embodiment, component AF is present in the core layer F composition in an amount of 50 to 90 wt.%, more preferably 70 to 87 wt.%, and component BF is present in the core layer F composition in an amount of 10 to 50 wt.%, preferably 13 to 30 wt.%, based on the total weight of the core layer F composition.
[0102] outer layer E The outer layer E of the printed film is made of an outer layer E composition that includes components that contribute to the heat resistance, mechanical properties, and optical properties of the film. The outer layer E is preferably a printing layer of the film or a printable layer of the film. In the laminate film, the outer layer E can be disposed between the core layer F and the outer layer A of the sealant film.
[0103] Ingredient AE The outer layer E composition can include component AE. Preferably, component AE is an ethylene copolymer, preferably having a viscosity of 920 to 935 kg / m, as described for component AG of the inner layer G composition. 3 and a melt flow rate (MFR2) in the range of 0.5-2.0 g / 10 min, measured in accordance with ISO 1133.
[0104] All embodiments described for component AG are also embodiments for component AE. Component AE can be independently selected from any one of these embodiments, and the selected embodiment can be the same or different for AE and AG.
[0105] In one embodiment, components AE and AG, and optionally BF, are identical.
[0106] Preferably, component AE is present in the outer layer E composition in an amount of 40 to 80 weight percent, more preferably 50 to 75 weight percent, and most preferably 55 to 70 weight percent, based on the total weight of the outer layer E composition.
[0107] Ingredient BE The outer layer E composition can include component BE. Preferably, component BE is a linear low density ethylene polymer (LLDPE), more preferably having a viscosity of 915 to 930 kg / m, as described for component BG1 of the inner layer G composition. 3 and a melt flow rate (MFR2) of 0.05 to 1.0 g / 10 min measured in accordance with ISO 1133.
[0108] All embodiments described for component BG1 are embodiments for component BE. Component BE can be independently selected from any one of these embodiments, and the selected embodiment can be the same or different for BE and BG1.
[0109] Preferably, component BE is present in the outer layer E composition in an amount of from 15 to 40 weight percent, more preferably from 20 to 40 weight percent, based on the total weight of the outer layer E composition.
[0110] Ingredients CE The outer layer E composition can include component CE. Preferably, component CE is a low density ethylene polymer (LDPE), preferably having a viscosity of 918 kg / m, as described for component CG of the inner layer G composition. 3 ~928kg / m 3 and melt flow rates (MFR2) in the range of 1.5-2.5 g / 10 min, measured according to ISO 1133.
[0111] All embodiments described for component CG are also embodiments for component CE. Component CE can be independently selected from any one of these embodiments, and the selected embodiment can be the same or different for CE and CG.
[0112] Preferably, component CE is present in the outer layer E composition in an amount of from 5 to 15 weight percent, more preferably from 7 to 13 weight percent, based on the total weight of the outer layer E composition.
[0113] In one embodiment, the outer layer E composition comprises or consists of components AE and BE, and optionally CE, in any of the above embodiments.
[0114] In one embodiment, the outer layer E composition comprises or consists of the same polymeric components as the inner layer G composition (eg, AG, BG1 and optionally CG).
[0115] In a preferred embodiment, the outer layer E composition comprises or consists of component AE in an amount of 50-75 wt.%, component BE in an amount of 25-40 wt.%, and optionally component CE in an amount of 0-15 wt.%, based on the total weight of the outer layer E composition.
[0116] <Characteristics> The printed film is characterized by a high stiffness (e.g. tensile modulus of 500-1000 MPa), high heat resistance (e.g. SIT of 110-120°C) together with good optical properties (haze and gloss). This is achieved in particular by using component AG in the printed film. Components BG1 and / or BG2 also contribute to the improvement of the properties, in particular the high stiffness and / or SIT, without sacrificing the optical properties (i.e. gloss and haze) of the printed film.
[0117] Sealant Film <Structure> The expression "sealant film" refers to a film that includes a sealing layer, which is a layer that promotes adhesion to other films, layers, or articles.
[0118] The sealant film of the present invention comprises or consists of several layers, which are at least an outer layer A, a core layer B and an inner layer C. The core layer B is located on the outside, i.e. between the outer layer A and the inner layer C, and preferably the inner layer C is the sealing layer. When laminated to a printing film, the inner layer C forms the inner surface of the laminate film.
[0119] In one embodiment, the sealant film consists of an outer layer A, a core layer B, and an inner layer C. In another embodiment, the sealant film comprises one or more additional intermediate (or subskin) layers X.
[0120] In certain embodiments, the sealant film further comprises one or more intermediate layers X between the core layer B and the inner layer C, and the core layer B and the outer layer A, for example in a 5-layer film structure A / X1 / B / X2 / C or a 7-layer film structure A / X1 / X1 / B / X2 / X2 / C. Preferably, the sealant film comprises up to 9 layers, more preferably up to 7 layers.
[0121] When present, the intermediate layer X preferably comprises or consists of a composition similar to that of the adjacent layer, which may be either the composition of the core layer B, or the composition of the adjacent inner layer C or the adjacent outer layer A.
[0122] Preferably, the sealant film has a thickness of 35 to 120 μm, more preferably 40 to 110 μm, and most preferably 40 to 100 μm.
[0123] In the sealant film, the core layer B preferably has a thickness of 30 to 80%, more preferably 35 to 75%, and most preferably 40 to 70% of the total thickness of the sealant film.
[0124] The outer layer A and / or the inner layer C each preferably have a thickness of 10-35%, preferably 15-30%, for example 25% of the total thickness of the sealant film. In the five-layer film structure A / X1 / B / X2 / C, the inner layer C and / or the outer layer A each preferably have a thickness of 5-20%, more preferably 7.5-15% of the total thickness of the sealant film.
[0125] Preferably, the sealant film is a "polyethylene film" as defined above for the printing film.
[0126] The sealant film and the compositions of each layer for preparing the layers thereof may contain additives of the same types and amounts as those described for the printing film.
[0127] Preferably, the sealant film is a non-oriented film, orientation being as defined above for the printed film.
[0128] <Composition> Each of the sealant film layers is made of a composition that includes at least one polymer (e.g., polyethylene) component. If the composition includes multiple polymer components, it is a blend of these components. Additional compounds (additives such as polymer processing aids, antiblock agents, or slip agents) may be present in the composition.
[0129] Inner layer C The inner layer C is made of an inner layer C composition that includes components that contribute, among other things, to the heat sealability and optical properties of the film. The inner layer C composition includes at least one ethylene-based polymer. When laminated to a printed film, the inner layer C forms the inner surface of the laminate film. The inner layer C of the sealant film is preferably a sealing layer.
[0130] Component AC Preferably, the inner layer C of the sealant film has a compressive strength of 915 to 925 kg / m 3 and a melt flow rate (MFR2) of 0.5 to 2.0 g / 10 min measured in accordance with ISO 1133.
[0131] The density of component AC is preferably at least 3 kg / m higher than the density of component AG. 3 , more preferably at least 5 kg / m 3 low.
[0132] LLDPE is well known in the art and is produced by a catalytic polymerization process.
[0133] Preferably, component AC is a multimodal ethylene copolymer, more preferably a bimodal ethylene copolymer, even more preferably a copolymer of ethylene and at least two different C4-C 12It is a copolymer with an α-olefin monomer, i.e. a terpolymer.
[0134] Preferably, the ethylene copolymer has a specific MFR of 13 to 30. 21 / Has MFR2 and / or MWD ≤6.
[0135] Preferably, the ethylene copolymer comprises or consists of a multimodal polymer of ethylene and one or more comonomers selected from α-olefins having 4 to 10 carbon atoms and has a specific MFR of 13 to 30. 21 / MFR2, and MWD ≤6.
[0136] Such multimodal ethylene copolymers are disclosed, for example, in WO 2016 / 083208.
[0137] The multimodal ethylene copolymer preferably has a MFR2 of 0.6 to 2.0 g / 10 min, particularly preferably 1.2 to 1.8 g / 10 min.
[0138] Preferably, the multimodal ethylene copolymer has a viscosity of 910 to 925 kg / m 3 , more preferably 913 to 922 kg / m 3 and particularly preferably 915 to 920 kg / m 3 It is.
[0139] The multimodal ethylene copolymer preferably has a specific MFR of 13 to 30, even more preferably 15 to 25. 21 / Has MFR2.
[0140] Multimodal ethylene copolymers preferably have an MWD of 6 or less, usually greater than 1, more preferably 3-5.
[0141] The α-olefin comonomers having 4 to 10 carbon atoms of the multimodal ethylene copolymers are preferably 1-butene and / or 1-hexene.
[0142] Preferably, the total amount of comonomers present in the multimodal ethylene copolymer is from 0.5 to 10 mol %, preferably from 1 to 8 mol %, more preferably from 1 to 5 mol %, even more preferably from 1.5 to 5 mol %, and most preferably from 2.5 to 4 mol %.
[0143] In a preferred embodiment, the multimodal ethylene copolymer is a bimodal copolymer, i.e., comprising a low molecular weight component and a high molecular weight component, and has a MFR2 of 1.2 to 1.8 g / 10 min, and / or a MFR5 of 3.0 to 5.0 g / 10 min, and / or a MFR of 20 to 40 g / 10 min. 21 , and / or 916-920 kg / m 3 and / or a molecular weight distribution (MWD) of 3-5 and / or a M of 15-25 kg / mol n , and / or M between 80 and 115 kg / mol w , and / or MFR between 15 and 25 21 / MFR2 ratio (FRR 21 / 2 ), and / or MFR of 6-9 21 / MFR5 ratio (FRR 21 / 5 ).
[0144] In a further preferred embodiment, the ethylene copolymer of component AC comprises or consists of an ethylene terpolymer, more preferably a multimodal ethylene terpolymer (II).
[0145] Preferably, the multimodal ethylene terpolymer (II) has a viscosity of 910 kg / m 3 ~925kg / m 3 and MFR2 of 0.5-2.0 g / 10 min.
[0146] The multimodal ethylene terpolymer (II) preferably comprises or consists of a multimodal polymer of ethylene and at least two different comonomers selected from α-olefins having 4 to 10 carbon atoms and has a specific MFR of 13 to 30. 21 / MFR2, and MWD ≤5.
[0147] Such multimodal ethylene terpolymers are disclosed, for example, in WO 2016 / 083208. For the definition of these ethylene terpolymers (e.g., the "modality" of the polymer) and the method of production, reference is made to WO 2016 / 083208. Furthermore, 3 All embodiments and preferred embodiments of ethylene terpolymers as described in WO 2016 / 083208, having a density in the range of 0.1 to 1.0, are also preferred embodiments of multimodal ethylene terpolymers (II) in the present disclosure, whether or not explicitly described herein.
[0148] The multimodal ethylene terpolymer (II) preferably has a MFR2 of 0.6 to 2.0 g / 10 min, particularly preferably 1.2 to 1.8 g / 10 min.
[0149] Preferably, the multimodal ethylene terpolymer (II) has a melting point of 910 to 925 kg / m 3 , more preferably 913 to 922 kg / m 3 and particularly preferably 915 to 920 kg / m 3 It is.
[0150] The multimodal ethylene terpolymer (II) preferably has a specific MFR of 13 to 30, more preferably 15 to 25. 21 / Has MFR2.
[0151] The at least two α-olefin comonomers having 4 to 10 carbon atoms of the multimodal ethylene terpolymer (II) are preferably 1-butene and 1-hexene.
[0152] Preferably, the total amount of comonomers present in the multimodal ethylene terpolymer (II) is from 0.5 to 10 mol %, more preferably from 1 to 8 mol %, even more preferably from 1 to 5 mol %, still more preferably from 1.5 to 5 mol %, and most preferably from 2.5 to 4 mol %.
[0153] The multimodal ethylene terpolymer (II), which is preferably a bimodal terpolymer, preferably comprises or consists of an ethylene polymer component (A1) and an ethylene polymer component (B1), the ethylene polymer component (A1) having a higher MFR2 than the ethylene polymer component (B1).
[0154] Preferably, the ethylene polymer component (A1) has a MFR2 of from 1 to 50 g / 10 min, more preferably from 1 to 40 g / 10 min, even more preferably from 1 to 30 g / 10 min, even more preferably from 2 to 20 g / 10 min, even more preferably from 2 to 15 g / 10 min, and most preferably from 2 to 10 g / 10 min.
[0155] The ratio of MFR2 of the ethylene polymer component (A1) to MFR2 of the ethylene polymer component (B1) is 2-50, preferably 5-40, more preferably 10-30, even more preferably 10-25, and most preferably 11-25.
[0156] Preferably, the ethylene polymer component (A1) comprises a comonomer different from the ethylene polymer component (B1).
[0157] Preferably, the ethylene polymer component (A1) has a lower amount (mol %) of comonomer than the ethylene polymer component (B1), more preferably the ratio of the amount (mol %) of α-olefin comonomer having 4 to 10 carbon atoms present in the ethylene polymer component (A1) to the amount (mol %) of the at least two α-olefin comonomers having 4 to 10 carbon atoms in the final multimodal ethylene terpolymer is 0.10 to 0.60, preferably 0.15 to 0.50.
[0158] Preferably, the α-olefin comonomer having 4 to 10 carbon atoms of the ethylene polymer component (A1) is 1-butene and the α-olefin comonomer having 4 to 10 carbon atoms of the ethylene polymer component (B1) is 1-hexene.
[0159] Preferably, the ethylene polymer component (A1) has a density different from, and preferably higher than, the density of the ethylene polymer component (B1).
[0160] The density of the ethylene polymer component (A1) is preferably 925 to 950 kg / m 3 , more preferably 930 to 945 kg / m 3 It is.
[0161] Preferably, the multimodal ethylene terpolymer (II) comprises an ethylene polymer component (A1) in an amount of 30 to 70 wt%, more preferably 40 to 60 wt%, even more preferably 35 to 50 wt%, still more preferably 40 to 50 wt%, based on the total amount (100 wt%) of the multimodal ethylene terpolymer (II); and an ethylene polymer component (B) in an amount of 70 to 30 wt%, more preferably 60 to 40 wt%, even more preferably 50 to 65 wt%, even more preferably 50 to 60 wt%, based on the total amount (100 wt%) of the multimodal ethylene terpolymer (II).
[0162] Most preferably, the multimodal ethylene terpolymer (II) is composed of the ethylene polymer components (A1) and (B1) as homopolymer components. Thus, the ratio of the ethylene polymer component (A1) to the ethylene-based polymer component (B1) is (30-70):(70-30), preferably (40-60):(60-40), more preferably (35-50):(65-50), and even more preferably (40-50):(50-60).
[0163] In a particularly preferred embodiment, the multimodal ethylene terpolymer (II) is a bimodal terpolymer, i.e. comprising a low molecular weight component and a high molecular weight component, and has a MFR2 of 1.2 to 1.8 g / 10 min, and / or a MFR5 of 3.0 to 5.0 g / 10 min, and / or a MFR of 20 to 40 g / 10 min. 21 , and / or 915-920 kg / m 3 and / or a molecular weight distribution (MWD) between 3.0 and 5.0, and / or a M between 15 and 25 kg / mol. n , and / or M between 80 and 115 kg / mol w, and / or MFR between 15 and 25 21 / MFR2 ratio (FRR 21 / 2 ), and / or MFR of 6-9 21 / MFR5 ratio (FRR 21 / 5 ).
[0164] Also preferred as multimodal ethylene terpolymers (II) are commercial products such as Anteo™, in particular Anteo™ FK1828 or Anteo™ FK1820, from Borealis or Borouge, which have the properties required here.
[0165] Preferably, component AC is present in the inner layer C composition in an amount of 50 to 95 weight percent, more preferably 60 to 90 weight percent, and most preferably 70 to 85 weight percent, based on the total weight of the inner layer C composition.
[0166] Component AC is particularly suitable for imparting a low seal initiation temperature to the sealant film while maintaining good optical properties.
[0167] Ingredient BC The inner layer C composition may include component BC. Preferably, component BC is a low density ethylene polymer (LDPE), and preferably has a viscosity of 918 to 928 kg / m, similar to component CG of the inner layer G composition. 3 and a melt flow rate (MFR2) of 1.5 to 2.5 g / 10 min measured in accordance with ISO 1133.
[0168] All embodiments described for component CG are embodiments of component BC. Component BC can be independently selected from any one of these embodiments, and the selected embodiment can be the same or different for BC and CG.
[0169] Preferably, component BC is present in the inner layer C composition in an amount of 5 to 50 weight percent, more preferably 10 to 30 weight percent, based on the total weight of the inner layer C composition.
[0170] In one embodiment, the inner layer C composition comprises or consists of components AC and BC in any of the above embodiments.
[0171] In a preferred embodiment, the inner layer C composition comprises or consists of component AC in an amount of 50 to 95 wt%, preferably 70 to 85 wt%, and component BC in an amount of 5 to 50 wt%, preferably 15 to 30 wt%, based on the total weight of the inner layer C composition.
[0172] Core layer B The core layer B of the sealant film comprises a core layer B composition that includes components that contribute, among other things, to the film's stiffness and other mechanical properties such as dart impact and tear resistance.
[0173] Ingredient A-B The core layer B composition may comprise component AB. Preferably, component AB is a medium density ethylene polymer (MDPE), preferably 925 to 945 kg / m 3 and has a melt flow rate (MFR2) of 0.05 to 0.50 g / 10 min, measured in accordance with ISO 1133.
[0174] Such MDPE is also well known in the art and is typically produced by a catalyzed polymerization process.
[0175] The MDPE of component AB is preferably a multimodal MDPE, more preferably a bimodal MDPE. Such multimodal MDPE and its preparation are described, for example, in the referenced WO 2017 / 021389, pages 8 to 10.
[0176] Preferably, the MDPE of component AB is 930 to 940 kg / m 3 , more preferably 932 to 938 kg / m 3 Preferably, the density of component AB is higher than that of component AC.
[0177] Preferably, the MDPE of component AB is an ethylene copolymer. The comonomer may be an α-olefin having 4 to 12 carbon atoms, such as 1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-decene. More preferably, the MDPE is a copolymer of ethylene and 1-butene or 1-hexene, most preferably a copolymer of ethylene and 1-butene.
[0178] Preferably, the total amount of comonomers present in the MDPE of component AB is from 1.0 to 4.0 mol %, more preferably from 1.5 to 3.5 mol %, and most preferably from 2.0 to 3.2 mol %.
[0179] Preferably, the MDPE of component AB has a MFR2 of 0.06 to 0.35 g / 10 min, more preferably 0.08 to 0.30 g / 10 min, most preferably 0.10 to 0.20 g / 10 min.
[0180] Preferably, the MDPE of component AB has a MFR5 of 0.35 to 1.20 g / 10 min, more preferably 0.37 to 1.00 g / 10 min, most preferably 0.40 to 0.80 g / 10 min.
[0181] In a particularly preferred embodiment, the MDPE of component AB has an MFR2 of 0.10 to 0.20 g / 10 min and / or an MFR5 of 0.40 to 0.80 g / 10 min and / or an MFR of 10 to 20 g / 10 min. 21 , and / or 932-938 kg / m 3 and / or a molecular weight distribution (MWD) of 15-35 and / or a M of 8-12 kg / mol. n , and / or M between 150 and 280 kg / mol w , and / or MFR between 80 and 150 21 / MFR2 ratio (FRR 21 / 2 ), and / or MFR of 20-30 21 / MFR5 ratio (FRR 21 / 5 All molecular weight parameters are determined by GPC conventional methods using standard calibrations, as detailed below.
[0182] As MDPE for component AB, the resin Borstar FB1350 from Borealis or Borouge can be used.
[0183] Preferably, component AB is present in the core layer B composition in an amount of 35 to 80 weight percent, more preferably 40 to 75 weight percent, and most preferably 50 to 70 weight percent, based on the total weight of the core layer B composition.
[0184] The component AB especially imparts high rigidity to the core layer B.
[0185] Ingredient BB The core layer B composition may include component BB. Preferably, component BB is a linear low density ethylene polymer (LLDPE) and preferably has a viscosity of 915 to 925 kg / m, similar to component AC of the inner layer C composition. 3 and a melt flow rate (MFR2) of 0.5 to 2.0 g / 10 min measured in accordance with ISO 1133.
[0186] All embodiments described for component AC are also embodiments for component BB. Component BB can be independently selected from any one of these embodiments, and the selected embodiment can be the same or different for BB and AC.
[0187] Preferably, component BB is present in the core layer B composition in an amount of 15 to 45 weight percent, more preferably 20 to 40 weight percent, based on the total weight of the core layer B composition.
[0188] Particularly in combination with component AB, component BB contributes good stiffness as well as high dart impact properties to the sealant film.
[0189] Ingredient CB The core layer composition can include component CB. Preferably, component CB is a low density ethylene polymer (LDPE), preferably having a viscosity of 918 to 928 kg / m, as described for component CG of the inner layer G composition. 3and a melt flow rate (MFR2) of 1.5 to 2.5 g / 10 min, measured in accordance with ISO 1133.
[0190] All embodiments described for component CG are embodiments of component CB. Component CB can be independently selected from any one of these embodiments, and the selected embodiment can be the same or different for CB and CG.
[0191] Preferably, component CB is present in the core layer B composition in an amount of 5 to 15 weight percent, more preferably 7 to 13 weight percent, based on the total weight of the inner layer B composition.
[0192] In one embodiment, the core layer B composition comprises or consists of components AB and BB, and optionally CB, in any one of the above-mentioned embodiments.
[0193] In a preferred embodiment, the core layer B composition comprises or consists of component AB in an amount of 50-75 wt.%, component BB in an amount of 25-40 wt.%, and optionally component CE in an amount of 0-15 wt.%, based on the total weight of the core layer B composition.
[0194] outer layer A The outer layer A of the sealant film comprises an outer layer A composition including one or more components. In a laminate film, the outer layer A may be disposed between the core layer B and the outer layer E of the printed film and contributes to the mechanical and optical properties of the film.
[0195] Ingredient AA The outer layer composition can include component AA. Preferably, component AA is a linear low density ethylene polymer (LLDPE), preferably having a viscosity of 915 to 930 kg / m, as described for component BG1 of the inner layer G composition. 3 and a melt flow rate (MFR2) of 0.05 to 1.0 g / 10 min measured in accordance with ISO 1133.
[0196] All embodiments described for component BG1 are embodiments of component AA. Component AA can be independently selected from any one of these embodiments, and the selected embodiment can be the same or different for AA and BG1.
[0197] Preferably, component AA is present in the outer layer A composition in an amount of from 25 to 55 weight percent, more preferably from 30 to 50 weight percent, based on the total weight of the outer layer A composition.
[0198] Ingredient B.A. The outer layer composition may include component BA. Preferably, component BA is a linear low density ethylene polymer (LLDPE) and preferably has a viscosity of 915 to 925 kg / m, similar to component AC of the inner layer C composition. 3 and a melt flow rate (MFR2) of 0.5 to 2.0 g / 10 min measured in accordance with ISO 1133.
[0199] All embodiments described for component AC are also embodiments for component BA. Component BA can be independently selected from any one of these embodiments, and the selected embodiment can be the same or different for BA and AC.
[0200] Preferably, component BA is present in the outer layer A composition in an amount of 25 to 55 weight percent, more preferably 30 to 50 weight percent, based on the total weight of the outer layer A composition.
[0201] Ingredient CA The outer layer A composition can include component CA. Preferably, component CA is a low density ethylene polymer (LDPE), preferably having a viscosity of 918 kg / m, as described for component CG of the inner layer G composition. 3 ~928kg / m 3 and a melt flow rate (MFR2) in the range of 1.5-2.5 g / 10 min, measured according to ISO 1133.
[0202] All embodiments described for component CG are embodiments of component CA. Component CA can be independently selected from any one of these embodiments, and the selected embodiment can be the same or different for CA and CG.
[0203] Preferably, component CA is present in the outer layer A composition in an amount of from 5 to 35 weight percent, more preferably from 10 to 30 weight percent, based on the total weight of the outer layer A composition.
[0204] In one embodiment, the outer layer A composition comprises or consists of components AA and BA, and optionally CA, in any of the above embodiments.
[0205] In a preferred embodiment, the outer layer A composition comprises or consists of component AA in an amount of 30-50 wt.%, component BA in an amount of 30-50 wt.%, and optionally component CA in an amount of 0-30 wt.%, based on the total weight of the outer layer A composition.
[0206] Specific Embodiments of the Sealant Film The present invention also relates to a sealant film. In a particular embodiment, the present invention relates to a sealant film comprising an outer layer A, a core layer B and an inner layer C, wherein the inner layer C is a) 915-925kg / m 3 and a melt flow rate (MFR2) of 0.5 to 2.0 g / 10 min, as measured in accordance with ISO 1133; and b) 918-928kg / m 3 and a melt flow rate (MFR2) of 1.5 to 2.5 g / 10 min measured according to ISO 1133, in an amount of preferably 10 to 30 wt %, based on the total weight of the inner layer C composition; and The following criteria: c) The core layer B has a thickness of 925 to 945 kg / m 3and a melt flow rate (MFR2) of 0.05 to 0.50 g / 10 min, measured according to ISO 1133, in an amount of preferably 40 to 75 wt. %, based on the total weight of the core layer B composition; and d) The outer layer A has a compressive strength of 915 to 930 kg / m 3 and a melt flow rate (MFR2) of 0.05 to 1.0 g / 10 min, measured according to ISO 1133, in an amount of preferably 30 to 50 wt. %, based on the total weight of the outer layer A composition. At least one of the following is satisfied.
[0207] In one embodiment, criterion c) is met. In another embodiment, criterion d) is met. In yet a further embodiment, both criteria c) and d) are met.
[0208] Preferably, component AC is present in the inner layer C composition in an amount of 50 to 95 weight percent, more preferably 60 to 90 weight percent, and most preferably 70 to 85 weight percent, based on the total weight of the inner layer C composition.
[0209] Components AC, BC, AB and AA can be selected from any one of the embodiments described above.
[0210] The inner layer C composition, in any one of the embodiments described above, can further include component CC.
[0211] The core layer B composition and the outer layer A composition may include additional components, as described above for particular layers of the sealant film.
[0212] <Characteristics> The sealant film is characterized by a relatively high stiffness (i.e., tensile modulus of 300-500 MPa) for a sealant film, high drop impact (i.e., high DDI) and other tensile properties. The sealant film exhibits excellent sealing behavior due to lower seal initiation temperature and hot tack temperature (e.g., SIT below 95°C). These properties can be achieved by the use of component AC in the sealant film and further improved by the presence of component BC in the inner layer C. Also, the presence of components AA and AB in the respective other layers A and B of the sealant film (even more so with components BA and BB) further contributed to the excellent properties of the sealant film.
[0213] Preferably, the sealant film has a seal initiation temperature (SIT) at 5N of less than 100°C, preferably less than 95°C, when measured at the inner layer C of the sealant film. Preferably, the film has a seal initiation temperature (SIT) at 5N of 80 to 100°C, preferably 85 to 95°C, when measured at the inner layer C of the sealant film. The seal initiation temperature (SIT) at 5N is measured according to ASTM F 2029 and ASTM F 88.
[0214] Preferably, the sealant film has a machine direction (MD) tensile modulus (1% secant modulus) of 280 MPa to 600 MPa, preferably 300 MPa to 500 MPa. The machine direction (MD) tensile modulus (1% secant modulus) is measured according to ASTM D882.
[0215] Preferably, the sealant film has a haze value of less than 12%, more preferably less than 10%. Preferably, the sealant film has a haze value of 3 to 12%, more preferably 5 to 10%. The haze value is measured according to ASTM D1003 as an index of film transparency, and this value indicates good transparency.
[0216] Preferably, the sealant film has a gloss value of at least 80, more preferably at least 90. Preferably, the sealant film has a gloss value of 80 to 140, more preferably 90 to 130. The gloss value (GU) is measured at 60 degrees according to ISO 2813 on the inner layer C or on the outer layer A, preferably on the inner layer C.
[0217] Preferably, the sealant film has a Dart Drop Impact (DDI) of at least 200g, more preferably at least 210g. Preferably, the sealant film has a Dart Drop Impact (DDI) of 200-600g, more preferably 210-550g. The Dart Drop Impact (DDI) is measured according to ASTM D1709 "Method A" on a sealant film having a thickness of preferably 35-120μm, more preferably 40-110μm, most preferably 40-100μm.
[0218] Polyethylene Laminate Film <Structure> In the present invention, the polyethylene laminate film comprises or consists of the sealant film and the printing film of any of the above-mentioned embodiments laminated together.
[0219] The laminate film includes an inner surface and an outer surface, with an inner layer of printed film G forming the outer surface of the laminate film and an inner layer of sealant film C forming the inner surface of the laminate film.
[0220] In a laminate film, the print film and the sealant film are connected via their respective outer layers E and A, which form the middle layer of the laminate film. In other words, the outer layer A of the sealant film is laminated to the outer layer E of the print film.
[0221] The connection, i.e., lamination of the printed and sealant films to one another, can be effected by conventional lamination equipment using conventional lamination methods, such as adhesive lamination, including both solvent-based and solventless adhesive lamination using conventional commercially available adhesives. The adhesive can be applied to the sealant and / or printed film by any suitable method, including, for example, the use of a laminating machine, gravure coating, roll coating, wire rod coating, spray coating, and the like. The film surface to which the adhesive is applied can be corona treated to increase the surface energy and provide sufficient wetting for the adhesive components.
[0222] Lamination can alternatively be performed as a sandwich lamination without the use of adhesive, with or without a melt web between the films. Such melt web can be any conventional polyethylene-based melt web material, such as LDPE. Lamination can also be performed by extrusion coating techniques. All of these lamination methods are well known in the art and described in the literature.
[0223] Preferably, lamination is performed using an adhesive (such as a solventless adhesive), which may form a layer between layer E and layer A (eg, adhesive layer D in FIG. 1).
[0224] Preferably, the adhesive has a density of 1.0 g / m 2 to 3.5 g / m 2 , more preferably 1.2 g / m 2 ~2.5g / m 2 The weight of the
[0225] Preferably, the adhesive (or adhesive layer) comprises less than 5% by weight of the total weight of the laminate film. The percentage of adhesive usually depends on the total weight of the laminate film, which correlates with the thickness of the laminate film. For example, a laminate film of about 75 μm preferably comprises a maximum of 4% by weight of adhesive, based on the total weight of the laminate film, and a laminate film of about 130 μm preferably comprises a maximum of 3% by weight of adhesive, based on the total weight of the laminate film.
[0226] Preferably, the laminate film has a thickness of 50 to 160 μm, more preferably 55 to 145 μm, and most preferably 60 to 130 μm.
[0227] The laminate film is a "polyethylene film" as defined above for the printing film. The use of polyethylene film provides a fully recyclable and sustainable packaging structure. It is therefore particularly preferred that both the printing film and the sealant film are polyethylene films, which are composed of at least 90% by weight, more preferably at least 95% by weight, and most preferably at least 98% by weight of ethylene polymers (including ethylene homopolymers and ethylene and one or more C3-C6 polymers), based on the total weight of the respective films. 12 Preferably, neither the print film nor the sealant film contains a non-polyolefin polymer, such as, for example, a polyester or polyamide. The laminate film may contain a non-polyolefin polymer in the adhesive layer (e.g., a polyurethane adhesive), but this preferably constitutes less than 5 wt. % of the total weight of the laminate film.
[0228] The substrate film is typically reverse printed, i.e. printing is done on the outer layer E of the substrate film which is then laminated with the outer layer A of the sealant film as depicted in FIG. 1, with the outer layers E and A forming the core / middle layer of the laminate film.
[0229] <Characteristics> The laminate film of the present invention has improved mechanical properties along with good optical properties and excellent barrier properties. The improved heat resistance allows the laminate film to run smoothly on high-speed VFFS machines. In general, a higher SIT of the print film than the sealant film is desired to avoid sealing jaw sticking problems in subsequent use on the VFFS line, which is highly correlated with delta SIT (also called the SIT difference between the laminate inner surface and the laminate outer surface).
[0230] The compositions of the inner layers G and C of the print film and sealant film are selected so that the seal initiation temperature (SIT) at 5N of the outer surface of the laminate film is at least 10°C, preferably at least 11°C, and more preferably at least 12°C higher than the seal initiation temperature at 5N of the inner surface of the laminate film, the seal initiation temperature being measured in accordance with ASTM F 2029 and ASTM F 88.
[0231] Preferably, the seal initiation temperature (SIT) at 5N of the outer surface of the laminate film is 10 to 30°C, more preferably 12 to 25°C, higher than the seal initiation temperature at 5N of the inner surface of the laminate film.
[0232] This temperature difference between the two outer layers of the laminate film allows the laminate film to run at packaging speeds of 50 to 80 bags per minute without having problems sticking to the jaws of the seal bar on a VFFS line.
[0233] Preferably, the outer surface of the laminate film has a seal initiation temperature (SIT) at 5N, measured at the outer surface (i.e., inner layer G) of the laminate film of at least 105° C., preferably at least 110° C. Preferably, the film has a seal initiation temperature (SIT) at 5N, measured at the outer surface (i.e., inner layer G) of the laminate film of from 105 to 125° C., preferably from 110 to 125° C. The seal initiation temperature (SIT) at 5N is measured according to ASTM F 2029 and ASTM F 88.
[0234] Preferably, the inner surface of the laminate film has a seal initiation temperature (SIT) at 5N measured at the inner surface of the laminate film (i.e. inner layer C) of less than 110° C., preferably less than 105° C. Preferably, the film has a seal initiation temperature (SIT) at 5N measured at the inner surface of the laminate film (i.e. inner layer C) of 80-110° C., preferably 85-105° C., even more preferably 85-100° C. The seal initiation temperature (SIT) at 5N is measured according to ASTM F 2029 and ASTM F 88.
[0235] It should be noted that any of the above ranges for the seal initiation temperature at 5N (SIT) of the inner surface of the laminate film can be combined with any of the above ranges for the seal initiation temperature at 5N (SIT) of the outer surface of the laminate film.
[0236] A further important parameter in measuring the stiffness of a film is the tensile strength / 1% secant modulus. The secant modulus is a measure of the strength properties in the elastic region of the film and represents the actual deformation at a selected point on the stress-strain curve. As a result, the secant modulus provides valuable insight into the stiffness and resistance to elongation in use, or how prone the film is to stretch during subsequent printing and packaging operations such as form-fill-and-seal (FFS) machines and / or under normal operating tensions in packaging. Stiffness is therefore very important for polyethylene films.
[0237] The laminate film preferably has a tensile modulus in the machine direction (MD) (1% secant modulus) of 400 MPa to 800 MPa, preferably 400 MPa to 600 MPa. The tensile modulus in the machine direction (MD) (1% secant modulus) is measured according to ASTM D882.
[0238] The sealant film preferably has a tensile modulus in the machine direction (MD) (1% secant modulus) of 280 MPa to 600 MPa, preferably 300 MPa to 500 MPa. The tensile modulus in the machine direction (MD) (1% secant modulus) is measured according to ASTM D882.
[0239] Preferably, the printed film has a tensile modulus in the machine direction (MD) (1% secant modulus) of 500 MPa to 1000 MPa, preferably 600 MPa to 800 MPa. The tensile modulus in the machine direction (MD) (1% secant modulus) is measured according to ASTM D882.
[0240] It has been found that improved laminate film performance for high speed FFS packaging can be achieved by using a high stiffness (e.g. 400-600 MPa) polyethylene laminate film made from the developed sealant film having excellent stiffness (e.g. 300-500 MPa) and low SIT (e.g. less than 95°C) and laminating it with a printing film having excellent heat resistance (high SIT) and good optical properties (i.e. haze and gloss) (e.g. 500-1000 MPa).
[0241] The haze value of the laminate film is preferably less than 12%, more preferably less than 10%. The haze value of the laminate film is preferably 3 to 12%, more preferably 5 to 10%. The haze value is measured according to ASTM D003 as a scale indicating the transparency of the film, and this value indicates good transparency.
[0242] Preferably, either or both of the print film and the sealant film have a haze value of less than 12%, more preferably less than 10%. Preferably, either or both of the print film and the sealant film have a haze value of 3 to 12%, more preferably 5 to 10%. The haze value is measured according to ASTM D1003 as a scale indicating the transparency of the film, and this value indicates good transparency.
[0243] Preferably, the laminate film has a gloss value of at least 80, more preferably at least 90. Preferably, the film has a gloss value of 80 to 140, more preferably 90 to 130. The gloss value (GU) is measured at 60° according to ISO 2813 on the inner layer C or G, preferably on the inner layer G which is the outer surface of the laminate film.
[0244] Preferably, either or both of the print film and the sealant film have a gloss value of at least 80, more preferably at least 90. Preferably, either or both of the print film and the sealant film have a gloss value of 80 to 140, more preferably 90 to 130. The gloss value (GU) is measured at 60° according to ISO 2813 on the respective inner layer C / G or outer layer A / E, preferably on the inner layers G and / or C.
[0245] Excellent barrier (e.g. 4.0 g / m 2 / day) was obtained for the laminate film without the use of a barrier coating or metallization. Thus, the laminate film of the present invention has good barrier properties primarily in those cases where a moisture barrier is most important.
[0246] Preferably, the laminate film is 5 g / m 2 / day or less, preferably 4.5g / m 2 / day or less. Preferably, the laminate film has a water vapor transmission rate (WVTR) of 1 to 4 g / m 2 / day, more preferably 1.5-4.5g / m 2 / day. The water vapor transmission rate (WVTR) is measured at 37.8°C and 90% RH according to ASTM F-1249.
[0247] Preferably, the laminate film has a thickness of 2000 cm 3 / m 2 / day or less, preferably 1800cm 3 / m 2 / day or less. Preferably, the laminate film has an oxygen transmission rate (OTR) of 600 to 2000 cm 3 / m 2 / day, more preferably 800-1800 cm 3 / m 2 / day. Oxygen transmission rate (OTR) is measured at 23°C and 0% RH according to ISO15105-2.
[0248] Further properties of the laminate film are as follows: The laminate film preferably has a tensile modulus in the transverse direction (TD) (1% secant modulus) of 500 MPa to 1200 MPa, more preferably 550 MPa to 1000 MPa. The tensile modulus in the transverse direction (TD) (1% secant modulus) is measured according to ASTM D882.
[0249] Preferably, the laminate film has a tensile breaking stress in the machine direction (MD) of 40 to 80 MPa, more preferably 45 to 70 MPa. Preferably, the laminate film has a tensile breaking stress in the transverse direction (TD) of 25 to 60 MPa, more preferably 27 to 50 MPa.
[0250] Preferably, the laminate film has an elongation at break in the machine direction (MD) of 350 to 700%, more preferably 400 to 650%, and preferably, the laminate film has an elongation at break in the transverse direction (TD) of 450 to 900%, more preferably 500 to 800%.
[0251] The parameters tensile stress at break and elongation at break are measured according to ISO 527-3.
[0252] Preferably, the laminate film has a machine direction (MD) tear strength (Elmendorf) of 2.0 to 15.0 N, more preferably 2.2 to 10.0 N. Preferably, the laminate film has a transverse direction (TD) tear strength (Elmendorf) of 20.0 to 50.0 N, more preferably 23.0 to 45.0 N. The tear strength (Elmendorf) is measured according to ASTM D 1922.
[0253] Preferably, the laminate film has a Dart Drop Impact (DDI) of at least 200g, more preferably at least 210g. Preferably, the laminate film has a Dart Drop Impact (DDI) of 200-600g, more preferably 210-550g. The Dart Drop Impact (DDI) is measured according to ASTM D1709 "Method A" on a laminate film having a thickness of preferably 50-160μm, more preferably 55-145μm, most preferably 60-130μm.
[0254] Preferably, the laminate film has a coefficient of friction less than 0.60, more preferably less than 0.50. Preferably, the laminate film has a coefficient of friction between 0.10 and 0.50, more preferably between 0.15 and 0.48. The coefficient of friction is measured according to ISO 8295 under dynamic conditions (in / in or out / out).
[0255] In one embodiment, the seal initiation temperature (SIT) of the film at 5N on the outer surface of the laminate film, measured according to ASTM F 2029 and ASTM F 88, is 10-30°C higher than the seal initiation temperature at 5N on the inner surface of the laminate film, the inner layer G has a gloss value measured at 60° according to ISO 2813 of at least 80, and optionally a tensile modulus in the machine direction (MD) (1% secant modulus) measured according to ASTM D882 of 400 MPa to 800 MPa.
[0256] <Preparation> Both the sealant film and the printing film of the laminate film are generally prepared by conventional methods for the preparation of multilayer films, where the layers of the film are coextruded.
[0257] The different polymeric components contained in any layer of the film are usually intimately mixed prior to layer formation, for example using a twin-screw extruder, preferably a counter-rotating or co-rotating extruder, and the blend is then converted into a coextruded film.
[0258] The films can be produced by blown film or cast film processes. To produce such multilayer films, for example, at least two polymer melt streams are typically extruded simultaneously (i.e., coextruded) through a multichannel tubular, annular, or circular die, blown with air (or a combination of gases), expanded, and / or cooled to form a tube that forms the film. The production of blown films is a well-known process.
[0259] Blown (co)extrusion can be carried out at a temperature ranging from 150°C to 230°C, more preferably 160°C to 225°C, followed by cooling with a blown gas (typically air) at a temperature of 10°C to 40°C, more preferably 12°C to 16°C, to obtain a frost line height of 0.5 to 4 times the die diameter, more preferably 1 to 2 times.
[0260] The blow-up ratio (BUR) should generally be in the range of 1.5 to 3.5, preferably 2.0 to 3.0, and more preferably 2.1 to 2.8.
[0261] Since the sealant film and the printing film are preferably non-oriented films, it is preferable that they are not subjected to a stretching step in consideration of the possibility of orientation.
[0262] The laminate film is prepared from the sealant and the printed film by a lamination process as described above.
[0263] <Items and Use> The present invention also relates to articles comprising the polyethylene laminate film of the present invention. Preferred articles are packaging articles such as pouches, such as stand-up pouches, sachets, bags, sachets, lamitubes, and the like.
[0264] The present invention further relates to the use of the polyethylene laminate film of the present invention for packaging molded articles, in particular for use in (vertical) form-fill-seal packaging techniques or for forming pouches such as stand-up pouches, sachets, bags, sachets, lamitubes, etc.
[0265] Specific articles and applications are heavy duty shipping bags, detergent pouches, and articles and applications for packaging various food products such as rice, wheat, cereals, flour, food grains, pet food, etc., and non-food products such as detergents / soap powders, building materials, chemicals, etc.
[0266] Any one of the embodiments of the present invention described herein can be combined with one or more of these embodiments. In particular, any embodiment described for the polyethylene laminate film of the present invention can be applied to the use of the polyethylene laminate film or molded article.
[0267] Furthermore, the present invention relates to a molded article comprising the sealant film, as described above for the laminate film, and to the use of the sealant film for packaging of a molded article.
[0268] In the following the invention will be further explained by means of examples with reference to the drawings.
[0269] <Measurement and Judgment Method> The following definitions of terms and methods of determination apply to the above general description of the invention and the following examples, unless otherwise defined.
[0270] a) Measurement of Melt Flow Rate (MFR) Melt flow rate (MFR) is measured according to ISO 1133 and is expressed in g / 10 min. The higher the melt flow rate, the lower the viscosity of the polymer. MFR is measured for polyethylene at 190°C under loads of 2.16 kg (MFR2), 5.00 kg (MFR5), and 21.6 kg (MFR 21 ) is measured.
[0271] The quantity FRR (Flow Ratio) is an index of molecular weight distribution and indicates the ratio of flow rates at different loads. Thus, FRR 21 / 5 is MFR 21 / Indicates the value of MFR5.
[0272] b) Density The density of the polymer is measured according to ISO 1183-1:2004 (method A) on compression moulded specimens prepared according to ISO 17855-2 and is expressed in kg / m 3 As shown in the figure.
[0273] c) GPC 1) Conventional GPC method Molecular weight average (M z , M w and M. n ), molecular weight distribution (MWD), and polydispersity index PDI=M w / M n (In the formula, M n is the number average molecular weight, M w The breadth, expressed as the weight average molecular weight (Mw), was determined by gel permeation chromatography (GPC) according to ISO 16014-1:2003, ISO 16014-2:2003, ISO 16014-4:2003 and ASTM D 6474-12 using the following equation:
number
number
number
[0274] Fixed elution interval ΔVi During, A i , M i are the elution volumes V i is the chromatographic peak slice area related to the molecular weight (MW) of the polyolefin, and N is equal to the number of data points obtained from the chromatogram between the integration limits.
[0275] A high-temperature GPC system equipped with an infrared (IR) detector (IR4 or IR5 from PolymerChar, Valencia, Spain) or a differential refractometer (RI) from Agilent Technologies, and equipped with three Agilent-PLgel Olexis columns and one Agilent-PLgel Olexis Guard column was used. 1,2,4-Trichlorobenzene (TCB) stabilized with 250 mg / L 2,6-ditertbutyl-4-methyl-phenol was used as the mobile phase. The chromatographic system was operated at a column temperature of 160 °C, detector temperature of 160 °C, and a constant flow rate of 1 mL / min. 200 μL of sample solution was injected per analysis. Data collection was performed using either Agilent Cirrus software version 3.3 or PolymerChar GPC-IR control software.
[0276] The column set was calibrated with 19 narrow MWD polystyrene (PS) standards ranging from 0.5 kg / mol to 11500 kg / mol. The PS standards were dissolved at room temperature for several hours. Conversion of the polystyrene peak molecular weights to polyolefin molecular weights was performed using the Mark Houwink equation and the following Mark Houwink constants:
number
[0277] A third order polynomial fit was used to fit the calibration data.
[0278] All samples were prepared in a concentration range around 1 mg / mL, and PE was dissolved in freshly distilled TCB stabilized with 250 ppm Irgafos 168 at 160 °C for 3 h with continuous gentle rocking.
[0279] 2)GPC viscosity method Molecular weight average of LDPE (M z , M w , M n The molecular weight average (Mw, Mn), molecular weight distribution (MWD), and polydispersity index PDI=Mw / Mn (where M n is the number average molecular weight, M w The breadth, expressed as the weight average molecular weight (MWD), was measured by gel permeation chromatography (GPC) according to ISO 16014-4 2019. A PL 220 (Polymer Laboratories) GPC equipped with an IR4 infrared detector and an online four-capillary bridge viscometer (PL-BV 400-HT) was used. Three Olexis columns and one Olexis Guard column from Polymer Laboratories were used as stationary phase, and 1,2,4-trichlorobenzene (TCB, stabilized with 250 mg / L 2,6-ditertbutyl-4-methyl-phenol) as mobile phase at 160 °C and a constant flow rate of 1 mL / min was applied. 200 μL of sample solution was injected per analysis. The detector constant and interdetector delay volume of the corresponding viscometer were measured using a narrow PS standard (MWD = 1.01) with a molar mass of 132900 g / mol and an intrinsic viscosity of 0.4789 dl / g. The detector constant for the IR4 detector is NIST1475a, and dn / dc is 0.094 cm 3 Measured as / g.
[0280] The column set was calibrated using universal calibration (according to ISO 16014-2:2019) with at least 15 narrow MWD polystyrene (PS) standards ranging from 0.5 kg / mol to 11600 kg / mol. The intrinsic viscosities of the relevant PS standards were determined from the corresponding concentrations (IR4), the online viscometer signal, and the measured polystyrene detector constant. For low molecular weight PS with molar masses below 3000 g / mol, the initial weighed concentration is used due to end group effects in the IR detector.
[0281] The molecular weight (M2) of the sample in each chromatographic slice using the universal calibration method can be calculated by the following correlation:
number
[0282] All data processing and calculations were performed using Cirrus Multi-Offline SEC-Software version 3.2 (Polymer Laboratories, a Varian inc. Company).
[0283] All samples were prepared by dissolving 5.0–9.0 mg of polymer in 8 mL (160 °C) stabilized TCB (same as the mobile phase) and running the solution at up to 160 °C with continuous gentle rocking for 2.5 h for PP and up to 3 h for PE.
[0284] d) Comonomer Content Comonomer content was determined as described on pages 31-34 of WO 2019 / 081611.
[0285] e) Mechanical properties Tensile modulus and tensile stress at break The tensile properties of the films were measured at 23°C according to ISO 527-3 using type 2 specimens with blown films as shown below: Tensile modulus in the machine direction (MD) and transverse direction (TD) were measured as 1% secant modulus according to ASTM D882 at a test speed of 500 mm / min and a gauge length of 50 mm.
[0286] Tensile stress at break was measured according to ISO 527-3, specimen type 2, with a gauge length of 50 mm and a test speed of 500 mm / min. Film samples were prepared as described in the Examples section below.
[0287] Elongation at break The elongation at break in the machine direction (MD) and transverse direction (TD) was measured according to ISO 527-3 on films of the indicated thicknesses produced as described in the Examples section below.
[0288] Dirt drop impact Dart Drop Impact (DDI) was measured according to "Method A" of ASTM D1709 on films of the indicated thicknesses prepared as described in the Examples section below.
[0289] f) Optical properties Gloss, clarity and haze, as measures of the optical appearance of a film, were measured in accordance with ISO 2813 (gloss) and ASTM D1003 (haze and clarity) on films of the indicated thicknesses prepared as described in the Examples section below.
[0290] The gloss of the outer and inner layers was measured at a 60° angle according to ISO 2813. As per ISO 2813, the BYK-Gardner Micro-TRI-Gloss Meter allows three measurement angles (20°, 60°, 85°) and the gloss value at 60° is recorded and reported as Gloss Units (GU). Thus, the gloss is measured on both surfaces of the film and judged separately.
[0291] g) Friction coefficient The coefficient of friction under dynamic conditions, both in / in and out / out, was measured according to ISO 8295.
[0292] h) Seal Initiation Temperature (SIT) In principle, a heat seal is formed by bonding two films (polymers) in a manner that forces them into firm contact while at least partially molten. The test method also covers an evaluation section after the heat sealing process has been carried out. The force required to separate the specimens containing the seal is measured using a UTM (also to identify the mode of specimen failure). Specimens were selected with a film sealing surface produced as described in the "Examples" below, according to the ASTM F 2029; ASTM F 88 standards. A minimum of five specimens must be used for each sealing temperature for the test. The term "seal initiation temperature" (SIT) is defined as "seal initiation temperature at 5N" and refers to the temperature at which a seal with a strength of 5N is formed after cooling. The temperature at which a heat seal is formed immediately after the sealing operation (seal time 1.0 s for film thicknesses less than 65 microns, sealing pressure 3 bar, seal time 1.5 s for film thicknesses 65 microns and above), the strength of the heat seal is measured at specific time intervals (at least 24 hours after the sealing cycle is completed, when the seal is cooled to ambient temperature and reaches maximum strength).
[0293] i) Hot tack temperature This test method is a procedure to measure the temperature required for a film sample to reach a specified seal strength under a specified seal time and pressure according to the ASTM F 1921 standard. Thus, the hot tack test measures the heat seal strength of a film immediately after sealing, before cooling to ambient conditions. The test required film specimens over 25 mm wide and 250 mm long for each seal temperature. According to ASTM F 1921, the hot tack temperature (°C) was measured at a force of 1 N under the following conditions: sealing pressure of 3 bar, dwell / seal time of 1 second, cooling / delay time of 100 milliseconds (release), and test / peel speed of 200 mm / second. For thicknesses of 65 microns and above, similar test conditions with a dwell / seal time of 1.5 seconds are used.
[0294] j) Water vapor transmission rate (WVTR) The water vapor transmission rate of the films produced in the Examples below was measured according to the ASTM F-1249 standard. Water vapor transmission rate (WVTR) tests are performed at 37.8° C. and 90% relative humidity (RH) according to ASTM F1249:2006 and / or ISO 15106-2:2003.
[0295] k)Oxygen transmission rate (OTR) The oxygen barrier property, i.e. oxygen transmission rate, was measured on blown films prepared as follows: The specimens were mounted as a sealed semi-barrier between two chambers at ambient atmospheric pressure. One chamber was slowly purged with a nitrogen flow at a given temperature and relative humidity, while the other chamber was purged with an oxygen flow at the same temperature and relative humidity as the nitrogen flow. As oxygen gas permeated the film and entered the nitrogen carrier gas, it was carried to a coulometric detector where it produced an electric current whose magnitude was proportional to the amount of oxygen flowing into the detector per unit time. The oxygen transmission rate (OTR) test was performed according to ISO 15105-2 at 23 °C and 0% relative humidity using 10 sccm of N2 and O2 (99.5%) gases, with a film surface area of 50 cm. 2 It will be carried out.
[0296] l) Thickness The film thickness was measured according to ISO 4593. EXAMPLES
[0297] A sealant film and a printed film were produced, each having a three-layer structure consisting of a core layer, an inner layer, and an outer layer. Example IE1 represents a sealant film of the laminate of the present invention, and Example CE1 is a comparative sealant film. Examples IE2 and IE3 represent printed films of the laminate of the present invention, and CE2 is a comparative printed film. The thickness of each sealant film is 45 μm, and the thickness of each printed film is 27 μm. The thickness of the core layer of each film is 50% of the total thickness of each film, and the thickness of each outer layer (i.e., the inner layer and the outer layer) is 25% of the total thickness of each film.
[0298] All of the inventive and comparative examples are non-oriented films (by definition). Details of the inventive and comparative examples are summarized below: Laminate films were produced using these sealants and printed films: Invention Laminate 1 (IE4) includes IE1 sealant film and IE2 printing film; Invention Laminate 2 (IE5) comprises an IE1 sealant film and an IE3 printing film; and The comparative laminate (CE3) contains the CE1 sealant film and the CE2 printed film.
[0299] Further film details are shown in Table 1.
[0300] [Table 1]
[0301] The polymers used in the preparation of the inventive and comparative films are listed below.
[0302] [Table 2]
[0303] experiment Because no special stretching equipment was used in the film preparation, the film was produced on a standard blown and / or cast film line with standard film machinery systems (nip rollers or take-off rollers and winders) and can be called an "unoriented film." The film can be formed by any suitable method of blown and / or cast film processes, and the materials forming each layer can be coextruded through a coextrusion feedblock and die assembly, resulting in a film with three or more layers that are adhered together but differ in composition.
[0304] The polyethylene blends used for the printed film layers described above can be produced by suitable conventional multilayer film extrusion lines, preferably at temperatures of 150-230°C, more preferably 160-225°C. The conventional blown film production techniques used in this respect are known in principle and available to those skilled in the art. Typically, the individual film layers are coextruded at temperatures of 160-225°C and cooled by blowing air at temperatures of 12-16°C, resulting in a frost line height of 1-2 times the die diameter.
[0305] The blown films were produced on a Polyrema (Reifenhauser, blown film line with internal bubble cooling system) with a production rate of 150 kg / hr and a cooling air temperature of 12–16° C. Details are shown in Table 3.
[0306] [Table 3]
[0307] Tables 4 and 5 show the blown film line temperature profiles, i.e., the melt temperatures and respective melt pressures used for the different layers in the blown film extruder, for the sealant film and the printed film, respectively. The films were produced using a standard co-extruder for polyethylene, however, slightly different process conditions were used for each film to optimize film aesthetics and achieve consistent film production.
[0308] [Table 4]
[0309] [Table 5]
[0310] Table 6 shows the temperature profile of the blown film line, i.e., the temperatures used for the different layers of the blown film extruder at different locations on the blown film line.
[0311] [Table 6]
[0312] Rotogravure Printing Process All printed films in Table 1 were printed on a BOBST Rotomec 4003, 10-color rotogravure press. The rewinder tension was optimized to run the 27 μm PE film, with a tension of 4-6 bar for smooth operation. The unwinder tension was kept very close to the rewind tension of 4-6 bar and adjusted when reverse printing at (high) speeds above 200 meters / min.
[0313] Laminate Preparation After rotogravure printing, the reverse-printed printed substrate film and the sealant film were laminated using a solvent-free adhesive system manufactured by Henkel. Lamination was performed using a solvent-free laminator manufactured by Nordmeccanica at a running speed of 250 m / min and an adhesive concentration of 1.7 g / m. 2 So I went.
[0314] VFFS packaging trial The vertical form-fill-seal (VFFS) machine used to manufacture the flexible pouches was a poly heat seal (PHS) machine manufactured by Pace packaging (Model-Pace P250 4S). The operating parameters are shown in Table 7.
[0315] [Table 7]
[0316] Film characteristics The laminate films were tested for several properties, including barrier properties, mechanical strength, optical properties, etc. The results are shown in Table 8 and discussed in terms of the properties of the sealant film and the printed film.
[0317] [Table 8]
[0318] The properties of the sealant and printed film of the laminate are given below.
[0319] [Table 9]
[0320] As can be seen from Table 9, the IE1 sealant film has improved mechanical properties (tensile modulus, tensile strength, tensile break stress, dart drop impact, tear resistance) as well as optical properties (haze and gloss) over the comparative sample CE1.
[0321] The high 1% secant modulus (300-500 MPa) shown in Table 9 indicates that the IE1 sealant film has improved stiffening capability over the CE1 sealant film, implying that the IE1 film requires more energy input to deform the film to the same relative extent, which is more suitable for the manufactured laminate film.
[0322] Both the tensile properties and Dart Drop Impact (DDI) of the IE1 sealant film are significantly higher along with good optical properties, and these results are generally designed to maintain the high mechanical performance of the laminate film.
[0323] The coefficient of friction (COF) of both outer layers was measured under dynamic conditions and was found to be less than 0.5, making it suitable for further processing, lamination and FFS operations.
[0324] The IE1 sealant film exhibits a 30% to 40% reduction in water vapor transmission rate (WVTR), demonstrating superior moisture barrier performance to the CE1 film.
[0325] The sealing behavior of IE1 sealant film is shown in Figure 2 by low seal initiation temperature and low hot tack temperature, i.e., seal initiation temperature at 5N is about 95°C or less, and hot tack seal initiation temperature at 1N is about 90°C or less, which reflects the performance of seal integrity. Since the low SIT of the sealing layer is just essential to create the SIT or heat resistance difference between the sealing layer and the top layer of the printed film, the sealing behavior of IE1 sealant film can improve the performance of the whole laminate film, which brings advantages during packaging operation on VFFS machines (faster packaging speed while the film is used for VFFS packaging application).
[0326] Once the sealant film was laminated with the substrate, the SIT of the sealing layer C of the laminate increased to a slightly higher temperature (close to 100°C) because the total thickness of the laminate was thicker than that of a single sealant film.
[0327] Therefore, the IE1 sealing layer has improved sealing properties over the CE1 sealing layer, which means less energy is required to create a seal of the same strength. This is highly beneficial while using the film in packaging line operations at packaging speeds of 50-80 pouches / min.
[0328] [Table 10]
[0329] Referring to Table 10, a higher tensile modulus (1% secant modulus) and also a higher tensile strength were obtained for the IE2 and IE3 printed films compared to the comparative CE2 printed film. The film properties obtained using the described formulations show that the 1% (MD) secant modulus for the IE2 and IE3 printed films is in the range of 620-660 MPa, indicating high stiffness, which not only improves the overall stiffness of the laminate film but also provides a superior body that meets the requirements of high speed printing operations, thus facilitating the running of the laminate film at faster wrapping speeds.
[0330] For IE2 and IE3 printed films, good optical properties (haze and gloss) as well as improved barrier performance (WVTR and OTR) are reported.
[0331] The seal initiation temperatures at 5N of the inner layers of IE2 and IE3 are increased compared to the CE2 sample.
[0332] FIG. 3 shows that the polyethylene substrate of the present invention has improved heat resistance (compared to the CE2 sample, the seal initiation temperature at 5N of the inner layers of IE2 and IE3 is increased, ranging from 110 to 120°C), which helps to produce a higher delta SIT (ΔSIT). Delta SIT (ΔSIT) is calculated as the difference between the seal initiation temperature (SIT) of the print film layer G and the sealant film layer C. Thus, IE2 and IE3 films can withstand the high temperature of the top vertical seal bar of the FFS packaging machine and produce a high delta SIT (between the outer laminate surface and the inner laminate surface).
Claims
1. A polyethylene laminate film having an inner surface and an outer surface, a) A printed film comprising an outer layer E, a core layer F and an inner layer G, the inner layer G forming the outer surface of the laminate film, the inner layer G having a strength of 920 to 935 kg / m 3 and a melt flow rate (MFR) of 0.5 to 2.0 g / 10 min measured according to ISO 1133 2 a printed film made of an inner layer G composition comprising component AG, which is an ethylene copolymer having b) a sealant film comprising an outer layer A, a core layer B and an inner layer C, said inner layer C forming said inner surface of said laminate film, said inner layer C being made of an inner layer C composition comprising at least one ethylene polymer; Including, The outer layer A of the sealant film is laminated to the outer layer E of the printing film, A polyethylene laminate film, wherein the seal initiation temperature (SIT) at 5N of the outer surface of the laminate film is at least 10°C higher than the seal initiation temperature at 5N of the inner surface of the laminate film, the seal initiation temperature being measured according to ASTM F 2029 and ASTM F 88.
2. The inner layer C composition has a viscosity of 915 to 925 kg / m 3 and a melt flow rate (MFR) of 0.5 to 2.0 g / 10 min measured according to ISO 1133 2 2. The polyethylene laminate film of claim 1, comprising a component AC that is a linear low density ethylene polymer having
3. The inner layer G composition of the printed film comprises component AG in an amount of 50 to 75 wt. % based on the total weight of the inner layer G composition; and / or the inner layer C composition of the sealant film comprises component AG in an amount of 915 to 925 kg / m 3 and a melt flow rate (MFR) of 0.5 to 2.0 g / 10 min measured according to ISO 1133 23. The polyethylene laminate film according to claim 1, further comprising a component AC, which is a linear low density ethylene polymer having a molecular weight of 100 to 2000, in an amount of preferably 60 to 90% by weight based on the total weight of the inner layer C composition, and the density of the component AC is lower than the density of the component AG.
4. The inner layer G composition of the printed film has a viscosity of 915 to 930 kg / m 3 and a melt flow rate (MFR) of 0.05 to 1.0 g / 10 min measured according to ISO 1133 2 Component BG1, a linear low density ethylene polymer having a viscosity of 950 to 970 kg / m 3 and a melt flow rate (MFR) of 0.2 to 2.0 g / 10 min measured according to ISO 1133 2 4. The polyethylene laminate film of claim 3, further comprising a component BG2 which is a high density ethylene polymer having a molecular weight of 15 to 45% by weight of either or each of the components BG1 and BG2, based on the total weight of the inner layer G composition.
5. Any or all of the components AC, AG and BG2 are bimodal ethylene copolymers, preferably any or both of the components AC and AG are ethylene and at least two different C 4 -C 12 The polyethylene laminate film according to claim 3 or 4, which is a copolymer with an α-olefin monomer.
6. The inner layer C composition of the sealant film has a viscosity of 918 to 928 kg / m 3 and a melt flow rate (MFR) of 1.5 to 2.5 g / 10 min measured according to ISO 1133 2 6. The polyethylene laminate film according to claim 3, further comprising a component BC which is a low density polyethylene having a molecular weight of 10 to 30% by weight based on the total weight of the inner layer C composition.
7. The core layer F of the printed film has a resistance of 950 to 970 kg / m 3 and a melt flow rate (MFR) of 0.2 to 2.0 g / 10 min measured according to ISO 1133 2 7. The polyethylene laminate film according to claim 1, made of a core layer F composition comprising component AF, a high density ethylene polymer having a molecular weight of 1000 to 2000, preferably in an amount of up to 90% by weight, based on the total weight of the core layer F composition.
8. The core layer F composition of the printed film has a viscosity of 920 to 935 kg / m 3 and a melt flow rate (MFR) of 0.5 to 2.0 g / 10 min measured according to ISO 1133 2 8. The polyethylene laminate film of claim 7, further comprising a component BF which is an ethylene copolymer having the formula:
9. The core layer B of the sealant film has a strength of 925 to 945 kg / m 3 and a melt flow rate (MFR) of 0.05 to 0.50 g / 10 min measured according to ISO 1133 2 ), preferably in an amount of 40 to 75 wt. %, based on the total weight of the core layer B composition; and / or 915 to 925 kg / m 3 and a melt flow rate (MFR) of 0.5 to 2.0 g / 10 min measured according to ISO 1133 2 9. The polyethylene laminate film according to any one of claims 1 to 8, which is made of a core B layer composition comprising component BB, which is a linear low density ethylene polymer having a molecular weight of 100 to 2000, preferably in an amount of 20 to 40 wt%, based on the total weight of the core layer B composition.
10. The outer layer A of the sealant film has a resistance of 915 to 930 kg / m 3 and a melt flow rate (MFR) of 0.05 to 1.0 g / 10 min measured according to ISO 1133 2 Component AA is a linear low density ethylene polymer having a viscosity of 915 to 925 kg / m 3 and a melt flow rate (MFR) of 0.5 to 2.0 g / 10 min measured according to ISO 1133 2 10. The polyethylene laminate film of claim 1, wherein the outer layer A composition comprises a component BA, which is a linear low density ethylene polymer having a molecular weight of 100 to 2000, and preferably comprises either or each of components AA and BA in an amount of 30 to 50 wt. %, based on the total weight of the outer layer A composition.
11. The following criteria: a) the laminate film and / or the sealant film and / or the printing film have a haze value, measured according to ASTM D1003, of less than 12%; b) said laminate film and / or said sealant film and / or said printing film have a gloss value of at least 80 measured at 60° on said respective inner layer C / G or outer layer A / E according to ISO 2813; c) the sealant film has a machine direction (MD) tensile modulus (1% secant) of 280 to 500 MPa, and / or the print film has a machine direction tensile modulus of 500 to 1000 MPa, and / or the laminate film has a machine direction tensile modulus of 400 to 800 MPa, measured according to ASTM D882; and d) The laminate film has a film thickness of 5 g / m2 measured at 37.8°C and 90% RH according to ASTM F-1249. 2 / day or less, and optionally has a water vapor transmission rate (WVTR) of 2000 cm3 measured at 23°C and 0% RH in accordance with ISO 15105-2. 3 / m 2 / d or less of oxygen transmission rate (OTR); The polyethylene laminate film according to any one of claims 1 to 10, which satisfies one or more of the following requirements.
12. The polyethylene laminate film according to any one of claims 1 to 12, wherein the printed film has a thickness of 15 to 40 μm, the sealant film has a thickness of 35 to 120 μm, each of the printed film and the sealant film comprises up to 7 layers, is manufactured by a blown film or cast film process, is preferably a non-oriented film, and optionally the laminate film comprises an adhesive layer between the outer layer A of the sealant film and the outer layer E of the printed film.
13. A sealant film comprising an outer layer A, a core layer B and an inner layer C, The inner layer C is a) 915-925kg / m 3 and a melt flow rate (MFR) of 0.5 to 2.0 g / 10 min measured according to ISO 1133 2 Component AC, a linear low density ethylene polymer having b) 918-928kg / m 3 and a melt flow rate (MFR) of 1.5 to 2.5 g / 10 min measured according to ISO 1133 2 ), preferably in an amount of 10 to 30 wt % based on the total weight of the inner layer C composition; The following criteria: c) The core layer B has a compressive strength of 925 to 945 kg / m 3 and a melt flow rate (MFR) of 0.05 to 0.50 g / 10 min measured according to ISO 1133 2 ), preferably in an amount of 40 to 75 wt. % based on the total weight of the core layer B composition; and d) The outer layer A has a compressive strength of 915 to 930 kg / m 3 and a melt flow rate (MFR) of 0.05 to 1.0 g / 10 min, measured according to ISO 1133. 2Component AA is a linear low density ethylene polymer having a molecular weight of 100 to 2000, preferably in an amount of 30 to 50 wt %, based on the total weight of the outer layer A composition; A sealant film that satisfies at least one of the above requirements.
14. A molded article comprising the polyethylene laminate film according to any one of claims 1 to 12 or the sealant film according to claim 13.
15. Use of the polyethylene laminate film according to any one of claims 1 to 12 or the sealant film according to claim 13 for packaging an article.
Citation Information
Patent Citations
Packaging method and laminate film
JP2002193318A
Packaging method, coexttrusion laminated film, and square-bottomed bag
JP2004059088A
Polyethylene laminate for use in flexible packaging materials
JP2020515441A
Polyethylene laminate for use in flexible packaging materials
JP2020526409A
Multilayer polyethylene laminates and films for use in flexible packaging materials
JP2020526412A