Method for producing hot strip made of fine-grained steel material

Rapid cooling of hot strips post-rolling addresses inefficiencies in existing methods by enabling direct use of fine-grained steel strips with optimized texture and mechanical properties, eliminating the need for additional annealing.

JP2024543075AInactive Publication Date: 2024-11-19SMS GROUP GMBH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024527813
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-17
Filing Date
2022-11-17
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for producing fine-grained steel strips are inefficient and require additional annealing processes due to slow cooling in coil form, which hinders immediate tissue state achievement.

Method used

A method involving rapid cooling of hot strips after the last rolling pass, with a cooling rate of ≥600K/(s·mm) and a thickness of <1.5mm to 1.75mm, below the transformation temperature, followed by immediate winding into coils, using water or gas additives to control cooling, and a control system to optimize texture and mechanical properties.

Benefits of technology

Enables direct use of hot-rolled steel sheets with optimized texture and mechanical properties without subsequent heat treatment, reducing production costs and improving grain size control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543075000001_ABST
    Figure 2024543075000001_ABST
Patent Text Reader

Abstract

The present invention is a method for determining the thickness d WB ≦1.75mm and average ferrite grain size g s It relates to a method for producing hot strip made of fine-grained steel material with grain size ≦5 μm. The previously necessary heat treatment of the hot strip to adjust the mechanical properties is avoided by an optimized rolling and cooling strategy.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention is a method for determining the thickness d WB ≦1.75mm, average ferrite grain size g s The present invention relates to a method for producing hot strip made of fine grain steel having a grain size of ≦5 μm. [Background technology]

[0002] Fine-grained steel strips are usually produced in a multi-stage process: first, a hot strip is produced from a slab by means of multiple hot deformations and then wound into a coil. The hot strip thus produced is then heat treated and / or cold rolled, whereby the thickness, the structure and the desired mechanical properties of the strip are adjusted. However, there is a demand from the consumer side to make the known multi-stage process more cost-effective and simpler. One possibility is to adjust the thickness of the strip as well as its structure for a possible end use already after hot rolling.

[0003] Slabs, especially thin slabs, are made of a material with a thickness of d WB It is known from the prior art to roll hot strip <1.5 mm. For this purpose, slabs or thin slabs are heated to the material-specific deformation temperature and rolled to strip steel in a hot strip mill with a series of reduction passes. The hot strip is then coiled into coils. The structure of the hot strip, and therefore the mechanical properties, are adjusted by the cooling conditions after hot deformation and cooling of the hot strip in coil form.

[0004] A disadvantage of this known method is that cooling in coil form is slow due to the tight winding of the ribbon, so that a usable texture is not achieved immediately, but only has to be produced or adjusted by a subsequent additional annealing treatment. Summary of the Invention [Problem to be solved by the invention]

[0005] It is therefore an object of the present invention to further develop the known method for producing fine-grained steel products, in such a way that the hot-rolled steel sheet can be directly used not only with regard to its thickness but also with regard to its structure. [Means for solving the problem]

[0006] The object of the present invention is achieved by a method having the features of claim 1 as well as by a hot strip having the features of claim 10 or claim 11. The hot strip made of fine-grained steel material is subjected to at least the following processing steps: heating the raw product, in particular a slab or a thin slab, to a deformation temperature; hot rolling the crude product in a hot strip mill with more than two reduction passes, in particular more than five reduction passes, into a steel strip; · winding the hot strip into a coil; Manufactured by.

[0007] The hot strip is cooled, in particular by compact cooling, after the last reduction pass before being coiled to the hot rolling temperature T W Therefore, the temperature T is lower than the transformation temperature of the steel. H Cool to transformation temperature T H is the temperature at which austenite decomposition begins. H can be read from the average chemical analysis and the associated ZTU or ZTA diagram. Alternatively, the transformation temperature T H During solidification, the segregation of chemical elements may cause local deviations in the chemical analysis, so the transformation temperatures T H may need to be further adjusted, which may shift the local decomposition temperature to a higher or lower local transformation temperature. H is the transformation temperature T H The time t is adjusted so that the core and transition regions of the slab are given preferential consideration.

[0008] The cooling of hot strip by rapid cooling is R ≧600K / (s·mm), more preferably a R Relative cooling rate a ≥ 800K / (s·mm) R Additionally, the cooling of the hot strip by rapid cooling is started after the last reduction pass within a period of t≦0.2 seconds, more preferably t≦0.1 seconds.

[0009] The combination of features of the present invention, namely the cooling rate, the thickness of the hot strip, and the temperature T below the transformation temperature of pearlite, bainite and / or martensite, H The combination of cooling to thickness d WB <1.5mm from 300MPa to 400MPa and thickness d WB ≧1.5 mm and ≦1.75 mm produces hot strip having said yield point of 400 MPa to 500 MPa.

[0010] Preferred embodiments of the method are described in claims 2 to 9 which refer to claim 1. W to transformation temperature T H Cooling of the hot strip to a temperature below preferably takes place within a distance of ≦6 m, preferably ≦4 m, after the last reduction pass. The earlier the rapid cooling begins after the last reduction pass, the better the grain growth due to the rapid cooling according to the invention can be reduced or prevented. In this case, attention must be paid to the suppression of undesired grain growth, especially in fine-grained steels.

[0011] Transformation temperature T HCooling to a temperature below 1000° C. is preferably carried out using water as a coolant. Water is a standardized coolant, which is easy to transport and can be easily provided in terms of process engineering. The cooling water used may also contain additives that modify the cooling properties of the water. Gases, especially air, are also understood as additives to the cooling water in the sense of the present invention. In this case, it is irrelevant whether the gas is used to transport the cooling water or to atomize the cooling water, for example after or with a spray nozzle. Additives in the sense of the present invention can also be chemicals suitable for modifying the boiling point or other physical or chemical properties of the cooling water.

[0012] During cooling, V ≥ 0.002 m for the mass flow rate of the hot strip 3 / kg, preferably V≧0.004m 3 It is preferred to set a relative water volume flow rate of 100 / kg / min, in which range sufficient water for the desired cooling effect is provided without overtaxing the water management of the hot strip mill.

[0013] A control or regulation system with at least one process model determines the setpoint of the cooling rate before the last reduction pass and / or adapts it during the hot deformation of the hot strip. Said process model then simulates, preferably online, the evolution of the structure during the hot rolling process on the basis of chemical analyses of the hot strip to be rolled and other process parameters. In the sense of the present invention, process parameters are understood to mean all process parameters which are directly or indirectly related to the production of hot strip in a hot strip mill. Direct process parameters are, for example, the rolling speed, slab temperature, chemical analyses or pass reductions, and indirect process parameters are, for example, the age of the rollers, the cooling water composition or the state of the equipment. Simulation models which simulate the structure on the basis of chemical analyses and known temperature profiles are known from the state of the art. The control and regulation system of the rolling mill determines the possible temperature profile of the hot strip on the basis of existing set reference values ​​or actual values ​​with the aid of known temperature models. This is preferably done periodically during the ongoing process. Likewise, the actual structure of the hot strip is periodically simulated by the structure model from these temperature profiles. If the actual structure deviates from the target structure, set criteria, such as the cooling intensity at different points in the rolling mill or the pass reduction, are adapted by a control or regulation system.

[0014] Furthermore, the process model uses optimization algorithms to determine set points for the cooling rate to be adjusted so that the target structure, especially the ferrite grain size, is achieved. Such control or adjustment improves the control of the mechanical properties of the finished hot strip by targeted adjustment of the structure development during the hot rolling process. With the aid of the process model, the control system can better compensate and optimize for possible variations.

[0015] Preferably, the texture sensor determines the texture composition of the hot strip, and the process model takes into account the measured actual texture composition when determining the cooling rate set point. The use of texture sensors at certain points in the hot strip mill not only makes it possible to determine the texture evolution based on chemical analysis, but also to take into account the actual state of the texture when predicting the texture evolution. This makes the cooling rate set point determination more accurate and less skewed.

[0016] The hot strip preferably consists of a steel having the following analyses: C: 0.05% to 0.20%, preferably 0.05% to 0.10% Si: 0.01% to 0.50%, preferably 0.05% to 0.20% Mn: 0.30% to 2.20%, preferably 0.40% to 1.80% Al: 0.015% to 0.075%, preferably 0.015% to 0.035% N: 0.000% to 0.050%, preferably 0.001% to 0.025% Nb: 0.00% to 0.10%, preferably 0.01% to 0.06% Ti: 0.00% to 0.12%, preferably 0.01% to 0.10% V: 0.00% to 0.10%, preferably 0.01% to 0.06% Mo: 0.00% to 0.35%, preferably 0.01% to 0.10% Ca: 0.005% to 0.035%, preferably 0.005% to 0.025% The balance is Fe, as well as impurities unavoidable during production.

[0017] Such steels are particularly suitable due to their transformation behavior and fundamental mechanical properties.

[0018] The Al / N ratio is preferably between 1 and 10, preferably between 1 and 8. Such an adjusted Al / N ratio reduces both edge cracking as the slab solidifies and the susceptibility to edge cracking during the first deformation pass in the rolling mill.

[0019] The hot strip temperature of the hot strip, prior to the last reduction pass before rapid cooling, is preferably at least 50° C., more preferably at least 30° C. and up to 100° C. higher than the Ae3 temperature of the alloy of the hot strip, thereby ensuring that the formation of ferrite in the hot strip occurs only at the start of rapid cooling and that the more deformable austenite is present during deformation of the hot strip in the rolling mill stand.

[0020] Furthermore, the object of the present invention is achieved by a hot strip produced by the method according to any one of claims 1 to 9. The finished hot strip is WB Hot strip thickness of <1.5 mm, preferably 1.2 mm, and tensile strength R of 300 to 400 mPA m And yield point R ≧ 340mPA e Furthermore, the subject of the present invention is a hot strip produced by the method according to any one of claims 1 to 7, comprising: WB Hot strip thickness of ≦1.75 mm, preferably <1.4 mm, and tensile strength R of 400 to 500 mPA m And R e With a yield point of ≧340 mPA, this is eliminated by hot stripping.

[0021] The detailed description of the invention is accompanied by three drawings. [Brief description of the drawings]

[0022] [Figure 1] Casting and rolling plant example [Diagram 2] Example temperature profile of hot strip made of fine grain material during processing [Diagram 3]Degree of deformation during the process [Figure 4] a) Conventional structure of fine-grained steel, b) Structure using the method of the invention The invention will now be explained in more detail with reference to the drawings, in which identical technical elements are provided with the same reference numbers in all figures.

[0023] FIG. 1 shows the schematic structure of a casting and rolling plant for the production of hot strip. The continuous casting plant 1 produces slabs or thin slabs from the liquid melt. In the first furnace 2, the slabs are heated to the temperature before the first pass in the roughing mill 3. Between the roughing mill 3 and the finishing mill stand 5 there is another soaking furnace 4. After the last finishing mill stand 4, 5 a compact cooling system 6 according to the invention is arranged. It can provide sufficient cooling liquid to adjust the desired cooling rate of the strip. After cooling the strip is wound onto reels 6 into coils.

[0024] FIG. 2 shows a diagram with the temperature progression a of the hot strip from the first pass in the roughing mill stand to the winding up of the coil on a reel. Starting from a pass temperature of, for example, 1,120° C., the hot strip is rolled in stages to a thickness of ≦1.6 mm. Without further influences, the temperature progression occurs, for example, according to curve a. The furnace between the roughing mill stand and the first pass in the finishing mill stand does not heat the rough strip, but rather serves to homogenize the temperature between the core and the outer layer of the rough strip. After the last deformation step in the last finishing mill stand, the finished hot strip is cooled by compact cooling to a temperature of ≦520° C. Then cooling to a reel temperature of, for example, 150° C. is carried out by laminar cooling.

[0025] [Table 1] Table 1 gives an example of an analysis of a fine-grained material. The technically possible deformations in the individual reduction passes at this analysis, as well as the example actual deformations, are shown in FIG. 3. It is clear here that deformation can essentially take place in the first four mill stands. Thereafter, the possible deformations decrease, which has an advantageous effect on the tolerances of the finished hot strip. This allows the method to adjust and maintain the fine grain from the very beginning of deformation.

[0026] 4a) and b) show the respective textured surfaces of the rolled hot strips. Both hot strips consist of the same alloy, i.e. they are rolled from a single batch of slabs. Figure a) shows the textured surface of a conventionally produced hot strip. Figure b) shows the textured surface of a hot strip produced according to the invention, where both hot strips were wound into coils after hot rolling. Comparing the textured surfaces, it is evident that the method according to the invention produces a significantly finer grain immediately after hot rolling. The average grain size is 5.5 μm in figure a) and 4.4 μm in figure b). The structure shown in figure b) allows the direct use of the hot strip without further subsequent heat treatment. [Explanation of symbols] 1. Continuous casting plant 2 furnace 3 Roughing Mill 4 Furnace 5 Finishing Rolling Mill Stand 6 Compact Cooling 7 Reels

Claims

1. Thickness d WB and g s In the manufacture of hot strip made of fine-grained steel having an average ferrite grain size of ≦5 μm, the hot strip manufactured has a thickness d<1.5 mm. WB When the thickness d is 1.5 mm or more and ≦1.75 mm, the yield point is 300 MPa to 400 MPa. WB and having a yield point of 400 MPa to 500 MPa, and at least the following steps: - heating the raw product, in particular a slab or a thin slab, to a deformation temperature; - hot rolling the raw product in a hot strip mill with more than two reduction passes, in particular more than five reduction passes, to obtain WB < 1.5 mm thickness, or d WB obtaining a hot strip having a thickness of ≧1.5 mm and ≦1.75 mm; - winding the hot strip into a coil; A manufacturing method in which - after the last reduction pass before being coiled, the hot strip is cooled rapidly, in particular by compact cooling, to the hot rolling temperature T W from a temperature T below the transformation temperature of the hard phase, in particular pearlite, bainite and / or martensite H and - a R ≧600K / (s·mm), preferably a R Relative cooling rate a ≧800K / (s·mm) R cooling the hot strip by quenching with; said cooling of the hot strip by rapid cooling begins within a period of ≦0.2 s, preferably ≦0.1 s, after the last reduction pass; The method according to claim 1,

2. Hot rolling temperature T W From the above, the transformation temperature T H2. The method according to claim 1, characterized in that the cooling of the hot strip to a temperature of less than 100° C. is performed within a distance of ≦6 m, preferably ≦4 m after the last reduction pass.

3. Transformation temperature T H 3. The method according to claim 1 or 2, characterized in that the cooling to a temperature below is carried out using water as the coolant.

4. During cooling, V ≥ 0.002 m for the mass flow rate of the hot strip 3 / kg, preferably V≧0.004m 3 4. The method according to claim 3, characterized in that the relative water volume flow rate of 1 / kg is adjusted.

5. - a control or regulation involving a process model defines a set point for the cooling rate before the last reduction pass and / or adjusts during the hot deformation; and - a process model simulating the evolution of the structure during the hot rolling process based on the chemical analysis of the hot strip and other process parameters; and - the process model uses an optimization algorithm to determine cooling rate settings such that the target structure, in particular the ferrite grain size, is achieved; The method according to any one of claims 1 to 4, characterized in that

6. a texture sensor determines the texture composition of the hot strip; and - the process model takes into account the actual measured composition of the structure when determining the cooling rate setpoint; The method according to claim 5, characterized in that

7. Hot strips had the following analysis: C: 0.05% to 0.20%, preferably 0.05% to 0.10% Si: 0.01% to 0.50%, preferably 0.05% to 0.20% Mn: 0.30% to 2.20%, preferably 0.40% to 1.80% Al: 0.015% to 0.075%, preferably 0.015% to 0.035% N: 0.000% to 0.050%, preferably 0.001% to 0.025% Nb: 0.00% to 0.10%, preferably 0.01% to 0.06% Ti: 0.00% to 0.12%, preferably 0.01% to 0.10% V: 0.00% to 0.10%, preferably 0.01% to 0.06% Mo: 0.00% to 0.35%, preferably 0.01% to 0.10% Ca: 0.005% to 0.035%, preferably 0.005% to 0.025% The balance is Fe and unavoidable impurities during production. The method according to any one of claims 1 to 6, characterized in that the steel material has a

8. 8. A method according to claim 7, characterized in that the Al / N ratio is between 1 and 10, preferably between 1 and 8.

9. 9. The method according to any one of claims 1 to 8, characterized in that the hot strip temperature of the hot strip before the last reduction pass before rapid cooling is at least 50°C, preferably at least 30°C and up to 100°C higher than the Ae3 temperature of the alloy of the hot strip.

10. A hot strip produced by the method according to any one of claims 1 to 9, - the hot strip is WB having a hot strip thickness of < 1.5 mm, preferably ≦ 1.2 mm; and - Tensile strength R from 300 MPa to 400 MPa m , and a yield point R of ≧340 MPa e having The hot strip,

11. A hot strip produced by the method according to any one of claims 1 to 9, - the hot strip is WB having a hot strip thickness of ≦1.75 mm, preferably ≦1.4 mm; and - Tensile strength R from 400 MPa to 500 MPa m , and a yield point R of ≧340 MPa e having The hot strip,

Citation Information

Patent Citations

  • Method for producing hot rolled steel sheet

    JP2004143503A

  • Hot rolled steel sheet and its production method

    JP2008189978A

  • Hot rolled steel sheet and production method therefor

    JP2016211047A

  • Hot rolled steel sheet, cold rolled steel sheet and process for producing the same

    WO2007015541A1

  • Process for producing hot-rolled steel sheet having fine ferrite structure and hot-rolled steel sheet

    WO2008096394A1