2-heat forming forging process for large crank throws
The two-heat forming forging process for large crank throws addresses inefficiencies in conventional methods by using multiple anvil molds and forging processes to enhance forging ratio and internal quality, achieving efficient and cost-effective production.
Patent Information
- Application Number
- JP2024529594
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-01-20
- Filing Date
- 2022-08-02
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-08-02
AI Technical Summary
Conventional forging processes for large crank throws are complex, costly, and inefficient, requiring multiple heats, high equipment demands, and result in low yield and poor internal quality, with issues like chipping and folding.
A two-heat forming forging process that sets the shape and parameters of a 2-web body with a protruding base in the first heat, followed by determining the shape and parameters of the journal in the second heat, using multiple anvil molds and forging processes to achieve the desired form in a single hit.
The process increases the forging ratio, improves internal quality, reduces material wastage, and lowers production costs by utilizing multiple upsetting and stretching processes, achieving efficient and cost-effective forging of large crank throws.
Smart Images

Figure 2024543095000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to crank throw forgings, particularly to a two-heat form-forging process for large crank throws, and is in the field of forging technology. In particular, the present disclosure relates to assembled crank throw forging preforms, and in particular to a forging process for large assembled crank throw preforms. The present disclosure also relates to forging of large crank throws, particularly to a forging process for the journal portion of large crank throws. The present disclosure also relates to a form-forging process for crank throws.
[0002] (CROSS REFERENCE TO RELATED APPLICATIONS) This disclosure relates to a Chinese application filed with the National Intellectual Property Office of the People's Republic of China on January 20, 2022, having application number 202210066376.7 and entitled "Two-heat forming forging process for large crank throws", a Chinese application filed with the National Intellectual Property Office of the People's Republic of China on January 20, 2022, having application number 202210065615.7 and entitled "Forging process for crank throw preforms", a Chinese application filed with the National Intellectual Property Office of the People's Republic of China on January 20, 2022, having application number 202210065615.7 and entitled "Forging process for crank throw preforms", Priority is claimed based on a Chinese application filed with the State Intellectual Property Office, bearing application number 202210065671.0 and entitled "Forging process for journal of large crank throw", and a Chinese application filed with the State Intellectual Property Office on January 20, 2022, bearing application number 202210066077.3 and entitled "Shaping forging process for crank throw", the entire contents of which are incorporated herein by reference. [Background technology]
[0003] The crankshaft is a main component used for converting between the rotary motion and reciprocating motion of the machine, and the crank throw is an important element of the crankshaft. The crankshaft functions to convert between the rotary motion and reciprocating motion of the machine, and the crank throw of the large crankshaft is required to have sufficient rigidity, strength, and impact load resistance because the force it receives is large and complex. In order to meet the above performance requirements, it is common to select a forged crank throw for the large assembled crankshaft, and the production process of the forged crank throw is relatively complicated, requiring multiple steps, multiple heats, and multiple replacements of the anvil mold. The journal is the part of the crank throw that connects with the connecting rod, and the forging process is the most complicated, and a columnar forging material close to the net shape of the journal is forged by integral forging at one end of both webs of the crank throw.
[0004] Commonly used forging processes include full mold forging, die forging and bending forging. Die forging requires tens of thousands of tons of forging machines and expensive dies, and the quality of the forgings is not ideal. Bending forging has good metal flow and shaping, is easy to operate, and does not require high requirements for equipment, but has a large number of heats, increases material consumption and energy consumption, and even the most advanced manufacturers at home and abroad need 5 to 7 heats to complete the forging, and the cold work allowance of the forgings is very large. The traditional methods for forging crank throws are die forging and free forging. These two methods not only have high production costs and low production efficiency, but also require forging machines of tens of thousands of tons and expensive dies, and the yield of the forgings is very low, they cannot meet the forging ratio requirements, the crystal grains of the internal structure of the forgings are coarse and the quality is insufficient, and the forgings often have chipping and folding defects. Summary of the Invention [Problem to be solved by the invention]
[0005] The inventors have carried out simulation calculations and scientific analysis of the above problems, and have found that the forging process of the conventional crank throw is outdated, the installation of the die is not rational, and the replacement method of the anvil die is not scientific, so there is a need to scientifically design and improve the forging process. [Means for solving the problem]
[0006] The present disclosure has devised a two-heat forming forging process for large crank throws, which sets the shape and parameters of a two-web body with a protrusion base in the first heat, sets the shape, parameters and bending parameters of the two webs and the intermediate state of the journal in the second heat, and uses a die forging process to achieve the purpose of forging a large crank throw forging in two heats.
[0007] Specifically, the present disclosure provides a forging process for crank slope preforms, which sets the shape and parameters of the crank slope preforms, sets an automatically changing anvil die, and uses a forging process that repeats upsetting and stretching to achieve forging in one hit. The present disclosure provides a forging process for the journals of large crank throws, which uses multiple different special anvil dies, and performs multiple forging presses on the forgings at multiple angles and with multiple changes of anvil dies to gradually form the journal part, thereby minimizing the cold work allowance of the journal part and making the forging process quicker. The present disclosure provides a forming forging process for crank throws, which sets the shape and parameters of the forgings, and achieves journal forming, process forming, bending, crimping, and finish forging in one hit, thereby achieving the purpose of reducing the number of hits and increasing the forging ratio.
[0008] The present disclosure provides the following technical solution: A two-heat forming forging process for a large crank throw, using a forging machine, an anvil mold, and an operation device, the anvil mold includes an upper anvil, a lower mold, a core mold, and an upper mold, the lower mold includes a small flat anvil, a large flat anvil, a double-edge press groove mold, a convex mold, a trapezoidal mold, and a concave mold, the upper mold includes an upsetting plate, an exchange anvil mold, and an overlaying folding mold, the operation device includes a work table and a manipulator, the work table includes a horizontal work table and a vertical work table, and the manipulator is a first manipulator. and a second manipulator, the upper anvil is connected to the forging machine, the convex die and the double edge press groove die respectively form fixed hinges with the large flat anvil, the exchange anvil die includes a concave exchange anvil die and an arc-shaped exchange anvil die, there are a plurality of core dies, different core dies have different thicknesses at both ends, the lower die is disposed on the horizontal work table and can move together with the horizontal work table, the first manipulator is configured to clamp the forging, and the second manipulator is configured to clamp the core die or the upper die, The two-heat forming forging process for this large crank throw includes the following steps: 1st heat: Forging a preform having a two-web body with a protrusion in the middle, The two web bodies are set to have a length L, a width b, and a height h1, and the protrusion base has a height h2 and a width b, so that the total height of the preform is: h=h1+h2; Step 1: Select a billet according to the weight requirements of the crank throw forging, and heat it to a predetermined forging temperature; Step 2: The billet heated in step 1 is placed between the upper anvil and the small flat anvil to elongate the billet. Step 3: The forging stretched in step 2 is placed upright on a vertical work table, and the second manipulator clamps the upsetting plate and places it between the forging and the upper anvil, upsetting the forging to 1 / 2 of its original length; Step 4: The forging upset in step 3 is stretched to have a cross section of (3b / 4) x (3b / 4); Step 5: Place the forging stretched in step 4 on a vertical workbench and set the forging to 1 / 2 of its original length. Step 6: The forging made in step 5 is stretched to have a cross section of b × b. Step 7: Place the middle part of the forging from step 6 above the double edge press groove, and forge parallel left and right grooves below the forging; Step 8: The forged product having the left and right grooves in step 7 is turned upside down by 180° and placed on a large flat anvil for forging. The left part of the left groove and the right part of the right groove are forged into a two-web body having a width of b, a height of h1, and a length of L, respectively, and the part between the left groove and the right groove is forged into a protruding base having a height of h2 and a width of b, thereby producing a two-web body preform; 2nd heat: Forging 2. Set the transition shape, parameters and bending parameters of the web body and journal; 1. Journal forging Step 9: Heat the forging from step 8 to the forging temperature. Step 10: The heated preform is placed on a large flat anvil, and the two webs are pressed thinly and stretched to the required dimensions of the forging. Step 11: The first manipulator clamps the preform and places the middle part of the preform of step 10 above the convex mold, then repeatedly rotates it 180 degrees to forge, moves left and right to forge, and forges it by changing the position multiple times to roughly forge the two sides of the journal; Step 12: The preform of step 11 is placed on a trapezoidal mold so that the protrusion base faces upward, and the concave exchange anvil mold is clamped by the second manipulator and placed on the preform, and the lower surface of the journal is roughly forged at the bottom surface of the two web bodies facing the protrusion base; Step 13: The two side surfaces and the lower surface of the journal of step 11 and step 12 are placed in a convex mold, and then repeatedly inverted and moved left and right to alternately forge the two side surfaces, the lower surface and the connection portion of the journal, so as to forge it close to the journal shape; Step 14: Place the journal of the preform from Step 13 in a concave shape, repeatedly invert it to change the angle of the forging press, press down the head portion of the protruding base with the upper anvil, such that the head portion of the protruding base is formed as the upper surface of a polygonal journal by the forging press, and the two side surfaces and the lower surface of the journal are formed as semi-cylindrical bodies by the forging press. Step 15: Alternately arrange the journals forged in Step 14 in convex and concave shapes, use an uneven anvil and an arc-shaped exchange anvil type as the upper anvil, forge the journals at multiple angles to forge the cylindrical material of the journals. 2. Bending Step 16: Place the lower surface of the cylindrical journal in a concave shape, clamp the covering and bending die with the second manipulator and cover and arrange it on the upper surfaces of the two webs of the two-web body, press down with the upper anvil, and bend the preform to a predetermined angle to form a "herringbone" shape. 3. Press Fitting Step 17: Place the "herringbone" preform on a large flat anvil, insert the core die with the largest difference in thickness at both ends into the opening of the preform with the second manipulator, press down with the upper anvil, press fit the two legs of the "herringbone" shape, bring the two legs of the preform closer, turn it upside down and press and forge it so that the two legs of the preform contact the core die. Step 18: Exchange the core dies in the order of the largest difference in thickness at both ends, repeat the operation in Step 17 so that the two webs of the two-web body contact the core die, invert the preform and perform forging, and finish forging the outside of the two-web body to forge the crank handle of the crank throw. 4. Stretching the Head Portion Step 19: Synchronously rotate the core die and the preform in a press-fitted state and place them on a large flat anvil, forge the head portion of the protruding base and stretch it to form a crank throw head portion in the shape of a frustum of a square pyramid. 5. Finishing Step 20: Place the preform from Step 19 on a large flat anvil or a small flat anvil and finish the crank throw to the predetermined dimensions of the finished product.
[0009] Preferably, the first manipulator is a left manipulator and the second manipulator is a right manipulator.
[0010] Preferably, in step 2, the billet is stretched to 1.2 to 1.7 times its original length.
[0011] Preferably, in step 3, the rectangular forging is upset to 1 / 2±20% of its original length.
[0012] Preferably, in step 4, the forging is stretched into a rectangular blank having a cross section of 3b / 4(1±5%)×3b / 4(1±5%).
[0013] Preferably, in step 5, the forging is upset to 1 / 2±10% of the original length.
[0014] Preferably, in step 6, the forging is stretched to have a cross section of b(1+0~5%) x b(1+0~5%).
[0015] Preferably, the convex shape is an arc shape.
[0016] Preferably, the diameter of the journal in the vertical direction of the preform is within ±5% of the diameter of the finished product.
[0017] Preferably, the concave surface of the concave replacement anvil mould is adapted to mate with the convex surface of the preform. Effect of the Invention
[0018] In the present disclosure, the shape and parameters of a forged preform having a protrusion base and two web bodies are set in the first heat, and multiple upsetting and stretching processes are used to complete the forging of the preform. In the second heat, the shape and parameters of a forged product in an intermediate state in multiple processes are set, and a forging press is used in which the product is repeatedly rotated and moved left and right at different angles, and a forging press is used in which the anvil mold is repeatedly replaced, and a covered bending mold with an arc-shaped pressing surface is used to perform rotational pressing and bending, and multiple core molds are used to perform multiple pressings, so that the forging is gradually formed, and the forming forging of the crank throw is achieved.
[0019] The forging process of the crank slope preform according to the present disclosure utilizes multiple upsetting and stretching processes to increase the forging ratio and improve the internal quality of the forging, so that the forging is gradually formed and the forging of the crank slope preform can be achieved in one hit, thereby achieving the objectives of the simplest forging process, the least material loss, and the lowest production cost.
[0020] The forging process of the journal of the large crank throw disclosed herein uses a number of different special anvil dies, which are repeatedly rotated and moved left and right at different angles to forge and press, and the different anvil dies are repeatedly replaced to forge and press the journal, thereby achieving the objectives of good forming degree of the journal material, small machining allowance, short forging time, small material consumption, and low production cost.
[0021] The crank throw forming forging process disclosed herein uses a number of different special anvil dies, which are moved left and right and rotated repeatedly to change the angle of the forging press, and different anvil dies are repeatedly used to perform the forging press, so as to gradually form the journal. By installing a covered folding die between the forging and the upper anvil, not only can the anvil die be quickly replaced, but also the arc-shaped pressing surface of the folding die is used to allow the two web bodies of the forging to form rolling pressing between the die during the bending process, so that the crank throw forging can be continuously bent with a relatively small pressing force and a relatively short pressing distance, and a relatively large crank throw forging can be bent with a forging machine with a relatively small pressure, achieving forging formation in one hit.
[0022] The present disclosure provides a forging process that achieves the shape forging and bending forging of crank throw forgings with a relatively small force and a relatively short forging press distance, and realizes the forging of relatively large crank throw forgings by a forging machine with a relatively small pressure. The present invention has the characteristics of a large forging ratio, good forming degree, small machining allowance, short forging time, small material consumption, and low production cost. [Brief description of the drawings]
[0023] [Figure 1] FIG. 13 is a schematic diagram of the initial state in step 2. [Diagram 2] FIG. 13 is a schematic diagram of the end state in step 2. [Diagram 3] FIG. 13 is a schematic diagram of the initial state in step 3. [Figure 4] FIG. 13 is a schematic diagram of the end state in step 3. [Diagram 5] FIG. 13 is a schematic diagram of the initial state in step 4. [Figure 6] FIG. 13 is a schematic diagram of the end state in step 4. [Figure 7] FIG. 13 is a schematic diagram of the initial state in step 5. [Figure 8] FIG. 13 is a schematic diagram of the end state in step 5. [Figure 9]FIG. 13 is a schematic diagram of the initial state in step 6. [Figure 10] FIG. 13 is a schematic diagram of the end state in step 6. [Figure 11] Schematic diagram of step 7. [Figure 12] FIG. 13 is a schematic diagram of the initial state in step 8. [Figure 13] FIG. 13 is a schematic diagram of the end state in step 8. [Figure 14] FIG. [Figure 15] FIG. [Figure 16] FIG. 1 is a schematic diagram of step 10. [Figure 17] FIG. 2 is a front view of the initial state of forging in step 11. [Figure 18] FIG. 18 is a left side view of FIG. 17. [Figure 19] FIG. 18 is a left side view of the workpiece in FIG. 17 in a 180° inverted state. [Figure 20] FIG. 2 is a schematic diagram of the initial state of forging in step 12. [Figure 21] 1 is a schematic diagram of the final state of forging in step 12. FIG. [Figure 22] 1 is a schematic diagram of the forging state seen from a certain direction in step 13. FIG. [Figure 23] 13 is a schematic diagram of the forging state seen from another direction in step 13. FIG. [Figure 24] FIG. 14 is a schematic diagram of step 14. [Diagram 25] FIG. 13 is a schematic diagram of the forging state between the upper anvil and the convex die in step 15. [Figure 26] FIG. 13 is a schematic diagram of the forging state between the upper anvil and the convex die in step 15. [Figure 27] FIG. 13 is a schematic diagram of the forging state between the upper anvil and the convex die in step 15. [Figure 28] FIG. 13 is a schematic diagram of the forging state of the concave exchange anvil die and the concave die in step 15. [Figure 29]FIG. 13 is a schematic diagram of the forging state of the concave exchange anvil die and the concave die in step 15. [Diagram 30] FIG. 13 is a schematic diagram of the forging state of the concave exchange anvil die and the concave die in step 15. [Diagram 31] FIG. 1 is a schematic diagram of the initial state of forging in step 16. [Diagram 32] 1 is a schematic diagram of the forging end state in step 16. FIG. [Diagram 33] FIG. 13 is a schematic diagram of the initial state of forging in step 17. [Diagram 34] 1 is a schematic diagram of the final state of forging in step 17. FIG. [Diagram 35] FIG. 2 is a schematic diagram of the forging state in step 18. [Diagram 36] FIG. 13 is a schematic diagram of the state in which the head portion of the crank throw is forged in step 19. [Figure 37] FIG. 36 is a schematic diagram showing the state in which the forged product shown in FIG. 35 is rotated 90° to forge the head portion of the crank throw. [Figure 38] FIG. 13 is a schematic diagram showing the finish forging of the crank handle with the core die attached in step 20. [Figure 39] FIG. 13 is a schematic diagram showing the finish forging of the crank handle with the core die attached in step 20. [Diagram 40] FIG. 13 is a schematic diagram showing the finish forging of the crank handle with the core die removed in step 20. [Diagram 41] FIG. 13 is a schematic diagram showing the finish forging of the crank handle with the core die removed in step 20. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] The present disclosure will now be further described with reference to the drawings.
[0025] Forging the first heat First, a billet is placed in a heating furnace and heated to a forging temperature. A 16-ton billet is used as the billet.
[0026] As shown in Figures 1 and 2, the heated forging 4 is clamped by the first manipulator 2 and placed between the upper anvil 1 and the small anvil 3, so that the length and cross-section of the forging 4 meet the aspect ratio requirements, and preferably the forging 4 is stretched to 1.5 times its original length.
[0027] As shown in Figures 3 and 4, the stretched forging 4 is placed upright on a vertical work table, and the second manipulator 2' clamps the upsetting plate 5 and places it between the forging and the upper anvil 1, and the forging 4 is upset to half its original length.
[0028] As shown in Figures 5 and 6, the forging 4 is placed on a flat anvil 3 and elongated to a cross section of (3b / 4) x (3b / 4), preferably, the forging 4 is placed on a flat anvil 3 and elongated to a cross section of 900 mm x 900 mm and a length of 2500 mm.
[0029] As shown in Figures 7 and 8, the actions of Figures 3 and 4 are repeated to upset the forging 4 to half its original length, preferably by placing the forging 4 on a flat anvil 3 and upsetting the forging 4 to a length of 1250 mm.
[0030] As shown in Figures 9 and 10, the operations of Figures 5 and 6 are repeated to elongate the forging 4 having a cross section of b x b, and preferably the forging 4 is elongated by the upper anvil 1 and the small anvil 3 to a cross section of 1200 mm x 1200 mm and a length of 1400 mm.
[0031] As shown in Figure 11, the middle portion of the forging 4 is placed above a double edge press groove 6, and parallel left and right grooves are forged into the lower portion of the forging 4. Preferably, a double edge press groove 11 is used instead of the lower anvil, and parallel left and right grooves are forged into the lower portion of the blank 11.
[0032] As shown in Figures 12 and 13, the forging 4 having the left and right grooves is turned upside down by 180° and placed on a large flat anvil 8. The left portion of the left groove and the right portion of the right groove are forged into a two-web body having a width of b, a height of h1, and a length of L, and the portion between the left and right grooves is forged into a protruding base having a height of h2 and a width of b, thereby producing a two-web preform 7.
[0033] 14 and 15 are front and plan views, respectively, of the preform.
[0034] 2nd heat forging The second heat forging is carried out based on the preform obtained in the first heat forging, and the shape of the preform is a two-web body having protruding pedestals.
[0035] The preform is again heated to the forging temperature.
[0036] As shown in FIG. 16, a heated preform 7 is placed on a large flat anvil 8 and pressed down by an upper anvil 1 to thinly press and stretch the two webs, and is finished to a predetermined dimension.
[0037] As shown in Figures 17 to 19, the preform 7 is clamped by the first manipulator 2 and the central part of the preform 7 is positioned above the convex mold 9, and the preform 7 is repeatedly rotated 180° and forged, forged while moving left and right, and forged in different positions multiple times to roughly forge the two side surfaces of the journal.
[0038] As shown in Figures 20 and 21, the preform 7 is placed in the trapezoidal mold 11 with the protrusion base facing upward, and the concave exchange anvil mold 10 is clamped by the second manipulator 2' and placed on the preform 7, and the lower surface of the journal is roughly forged at the bottom surfaces of the two web bodies facing the protrusion base.
[0039] As shown in FIGS. 22 and 23, place the two side surfaces and the lower surface of the journal on the convex mold 9, clamp the preform 7 with the second manipulator 2' and repeatedly invert it, move it left and right to alternately forge the two side surfaces, the lower surface and the connecting part of the journal, and forge the two side surfaces, the lower surface and the connecting part of the journal to be close to the journal shape. Preferably, at the same time, forge and press with the upper anvil 1 to make the protruding platform polygonal.
[0040] As shown in FIG. 24, place the journal in the preform 7 on the concave mold 12, repeatedly invert the preform 7 with the second manipulator 2' to change the angle of the forging press, press down the head part of the protruding platform with the upper anvil, and forge and press to form the head part of the protruding platform as the upper surface of the polygonal journal, and forge and press to form the two side surfaces and the lower surface of the journal as semi-cylindrical bodies.
[0041] As shown in FIGS. 25 to 30, place the journal between the upper anvil 1 and the convex mold 9, between the upper anvil 1 and the concave mold 12, between the arc-shaped exchange anvil mold 13 and the convex mold 9, and between the arc-shaped exchange anvil mold 13 and the concave mold 12, and forge the journal at multiple angles to forge it into a cylindrical journal.
[0042] As shown in FIGS. 31 and 32, place the lower surface of the journal on the concave mold 12, clamp the covering and bending mold 14 with the second manipulator 2' and place it on the upper surfaces of the two webs of the two-web body, press it down with the upper anvil 1, and bend the preform 7 to a predetermined angle to form a "herringbone" shape.
[0043] As shown in FIGS. 33 and 34, place the preform 7 horizontally on the flat anvil 8 with the second manipulator 2', insert the core mold 15 with the largest difference in thickness at both ends into the opening of the preform 7 with the first manipulator 2, press the two webs together, turn it upside down and further forge and press the two webs so that the two webs are in contact with the core mold.
[0044] As shown in Figure 35, the first manipulator 2 is used to replace the core dies 15 in the order of the largest difference in thickness between the two ends, and the operations of Figures 33 and 34 are repeated so that the two webs are further brought into contact with the core dies, the forging is reversed and forged, and the outside of the two-web body is finish forged to forge the crank handle of the crank throw, preferably into two parallel crank handles.
[0045] As shown in Fig. 36, the core mold 15 and preform 7 are rotated in a pressed state, and the head portion of the projection is placed on the large flat anvil 8 and forged. The preform 7 in the state shown in Fig. 36 is rotated 90° as shown in Fig. 37, and the upper end portion of the journal is further forged and stretched to form a crank throw head portion in the shape of a quadrangular pyramid.
[0046] As shown in Fig. 38, the preform 7 is placed on a large flat anvil 8, and the crank shank is finished. Alternatively, the preform 7 is placed on a small flat anvil 3, and the crank shank is finished. As shown in Fig. 39, the core mold 15 and the preform 7 are inverted in the pressed state, and the side of the crank shank is finished.
[0047] As shown in Figure 40, the preform 7 is rotated and the crank shank is placed on the large flat anvil 8 and the crank throw is finish forged to the desired dimensions. Alternatively, the preform 7 is rotated and the crank shank is placed on the small flat anvil 3 and the crank throw is top-finish forged to the desired dimensions. As shown in Figure 41, the forging is rotated 90° to finish the sides of the crank shank and finish forging the crank throw. [Industrial Applicability]
[0048] This disclosure relates to a two-heat forming forging process for a large crank throw. A forging machine, an anvil mold, and an operating device are used. In the first heat, the shape and parameters of a forging preform having a protrusion base and two web bodies are set, and multiple upsetting and stretching processes are used to complete the forging of the preform. In the second heat, the shape and parameters of the intermediate forging in multiple steps are set, and a forging press by repeatedly rotating and moving left and right at different angles and a forging press by repeatedly replacing anvil molds are used, and a covered bending mold with an arc-shaped pressing surface is used to perform rotational pressing and bending, and multiple core molds are used to perform multiple pressings, so that the forging is gradually formed, and the forming forging of the crank throw is achieved. This disclosure provides a forging process that achieves forming forging and bending forging of a crank throw forging with a relatively small force and a relatively short forging press distance, and realizes forging of a relatively large crank throw forging by a forging machine with a relatively small pressure. The present invention has the characteristics of large forging ratio, good forming degree, short forging time, small material consumption, and low production cost.
[0049] It should be noted that the two-heat forming and forging process for large crank throws according to the present disclosure can be implemented and used in various industrial applications, such as in the forging field. [Explanation of symbols]
[0050] 1 Upper anvil 2 First manipulator 2′ Second manipulator 3 Kodaira Anvil 4 Forgings 5 Upset Plate 6 Double edge press groove mold 7 Preform 8. Ohira Anvil 9 Convex 10 Concave exchange anvil type 11 Trapezoid 12 Concave 13 Lower arc type 14 Covered folding type 15 Core Type
Claims
1. A two-heat forming forging process for large crank throws, comprising: A forging machine, an anvil mold, and an operating device are used, the anvil mold includes an upper anvil, a lower mold, a core mold, and an upper mold, the lower mold includes a small flat anvil, a large flat anvil, a double edge press groove mold, a convex mold, a trapezoidal mold, and a concave mold, the upper mold includes an upsetting plate, an exchange anvil mold, and an overlaying folding mold, the operating device includes a work table and a manipulator, the work table includes a horizontal work table and a vertical work table, the manipulator includes a first manipulator and a second manipulator, and the upper an anvil is connected to the forging machine, the convex die and the double edge press groove die respectively form fixed hinges with the large flat anvil, the exchange anvil die includes a concave exchange anvil die and an arc-shaped exchange anvil die, there are a plurality of core dies, different core dies have different thicknesses at both ends, the lower die is disposed on the horizontal work table and can move together with the horizontal work table, the first manipulator is configured to clamp the forging, and the second manipulator is configured to clamp the core die or the upper die, The two-heat forming forging process of the large crank throw includes the following steps: First heat: A preform having two webs with a protrusion in the middle is forged. The two web bodies have a length L, a width b and a height h. 1 The projection base is set to have a height of h 2 and the width is b, the total height of the preform is: h = h 1 +h 2 and Step 1: Select a billet according to the weight requirements of the crank throw forging and heat it to a predetermined forging temperature; Step 2: The billet heated in step 1 is placed between the upper anvil and the small flat anvil to elongate the billet; Step 3: The forging stretched in step 2 is placed upright on the vertical work table, and the second manipulator clamps the upsetting plate and places it between the forging and the upper anvil, upsetting the forging to 1 / 2 of its original length; Step 4: The forging upset in step 3 is stretched to have a cross section of (3b / 4) x (3b / 4); Step 5: Place the forging stretched in step 4 upright on the vertical work table and set the forging to 1 / 2 of its original length; Step 6: The forging upset in step 5 is stretched to have a cross section of b x b; Step 7: Place the middle part of the forging stretched in step 6 above the double edge press groove, and forge parallel left and right grooves below the forging; Step 8: The forging having the left and right grooves in step 7 is turned upside down by 180° and placed on a large flat anvil for forging. The left part of the left groove and the right part of the right groove are forged to have a width b and a height h, respectively. 1 The forging is performed to form a two-web body having a length of L, and the part between the left and right grooves has a height of h. 2 and forging the web into a protruding base having a width b, thereby producing a two-web preform. Second Heat: Forging Set the transition shapes, parameters, and bending parameters of the two web bodies and the journal, Step 9: Heat the preform of Step 8 to the forging temperature, Step 10: Place the heated preform on the flat anvil, press and stretch the two web bodies thinly, and finish to the predetermined dimensions, Step 11: Clamp the preform with the first manipulator, place the middle part of the preform of Step 10 above the convex part, repeatedly invert it 180 degrees for forging, forge while moving left and right, change the position multiple times for forging, and rough forge the two side surfaces of the journal, Step 12: Place the preform in the trapezoidal mold so that the protruding platform of the preform of Step 11 faces upward, clamp the concave exchange anvil mold with the second manipulator and mount it around the preform, and rough forge the lower surface of the journal on the bottom surface of the two web bodies facing the protruding platform, Step 13: Place the two side surfaces and the lower surface of the journal of Steps 11 and 12 on the convex part, repeatedly invert them, move left and right to alternately forge the two side surfaces, the lower surface and the connection part of the journal, and forge it to be close to the journal shape, Step 14: Place the journal of the preform of Step 13 in the concave mold, repeatedly invert it to change the angle of the forging press, press down the head part of the protruding platform with the upper anvil, the head part of the protruding platform is formed as the upper surface of the polygonal journal by the forging press, and the two side surfaces and the lower surface of the journal are formed as semi-cylindrical bodies by the forging press, Step 15: Place the journal forged in Step 14 alternately in the convex and concave molds, use the non-flat anvil as the upper anvil and the arc-shaped exchange anvil mold, forge the journal at multiple angles, and forge the cylindrical material of the journal, Step 16: Place the lower surface of the cylindrical journal in the concave mold, clamp the covering and bending mold with the second manipulator and cover and place it on the upper surfaces of the two webs of the two web bodies, and the preform is bent to a predetermined angle to form a "herringbone" shape, Step 17: Place the "V"-shaped preform on the flat anvil, insert the core mold with the largest difference in thickness at both ends into the opening of the preform using the second manipulator, press together the two legs of the "V"-shaped preform, bring the two legs of the preform closer, turn it upside down and press and forge it so that the two legs of the preform contact the core mold. Step 18: Replace the core mold in the order of the decreasing difference in thickness at both ends, repeat the operation in Step 17 so that the two webs of the two web bodies contact the core mold, turn the preform over and perform forging, finish-forge the outside of the two web bodies to forge the crank handle of the crankshaft. Step 19: Synchronously rotate the core mold and the preform in a pressed state, forge the head part of the boss and stretch it into a square pyramid-shaped crankshaft head part. Step 20: Place the preform in Step 19 on the flat anvil or the small flat anvil and finish the crankshaft to a predetermined dimension. Characterized in that it is a two-heat forming forging process for a large crankshaft.
2. The first manipulator is a left manipulator and the second manipulator is a right manipulator. Characterized in that it is the two-heat forming forging process for a large crankshaft according to Claim 1.
3. In Step 2, stretch the billet to 1.2 to 1.7 times its original length. Characterized in that it is the two-heat forming forging process for a large crankshaft according to Claim 1 or 2.
4. In Step 3, position the rectangular forging at 1 / 2 ± 20% of its original length. Characterized in that it is the two-heat forming forging process for a large crankshaft according to any one of Claims 1 to 3.
5. In Step 4, stretch the forging into a rectangular material with a cross-section of 3b / 4(1 ± 5%) × 3b / 4(1 ± 5%). Characterized in that it is the two-heat forming forging process for a large crankshaft according to any one of Claims 1 to 4.
6. In Step 5, position the forging at 1 / 2 ± 10% of its original length. Characterized in that it is the forging process for a crankshaft preform according to any one of Claims 1 to 5.
7. In Step 6, stretch the forging into one with a cross-section of b(1 + 0 to 5%) × b(1 + 0 to 5%). A forging process for a crank slope preform according to any one of claims 1 to 6.
8. The convex shape is an arc shape. The two-heat forming forging process for large crank throws according to any one of claims 1 to 7.
9. The vertical diameter of the journal preform is within ±5% of the diameter of the finished product. The two-heat forming forging process for large crank throws according to any one of claims 1 to 8.
10. The concave surface of the concave exchange anvil mold is configured to mate with the convex surface of the preform. The two-heat forming forging process for large crank throws according to any one of claims 1 to 9.
Citation Information
Patent Citations
Combined anvil die and process for forging large crank throw
CN113926973A
Method of producing crank throw
JP1977111863A
Forging method and dies of crank throw using theunbended preform
KR1020020072859A