Conductive silicone compositions containing carboxylic acid functional polyorganosiloxane thixotropic agents

A carboxylic acid-functional polyorganosiloxane is used to enhance the thixotropic index of filled silicone compositions, addressing the challenge of balancing conductivity and processability by increasing low shear viscosity, thus facilitating stable application and extrusion.

JP2024543145AActive Publication Date: 2024-11-19DOW SILICONES CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024531203
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-02
Filing Date
2022-10-17
Publication Date
2024-11-19
Estimated Expiration
2042-10-17

AI Technical Summary

Technical Problem

Filled silicone compositions face a challenge in balancing high conductive properties with maintainable processability, as increasing filler content enhances conductivity but increases viscosity, making application difficult.

Method used

Incorporation of a carboxylic acid-functional linear polyorganosiloxane as a thixotropic agent to preferentially increase low shear viscosity, thereby enhancing the thixotropic index of the composition.

Benefits of technology

The solution effectively increases the thixotropic index by 50% or more, ensuring stable application and extrusion while maintaining low viscosity under shear.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543145000001
    Figure 2024543145000001
  • Figure 2024543145000002
    Figure 2024543145000002
  • Figure 2024543145000003
    Figure 2024543145000003
Patent Text Reader

Abstract

1. A composition comprising filler particles dispersed in a matrix material, the matrix material comprising: (a) from 0.01 to 1.50 weight percent of a first polyorganosiloxane, the first polyorganosiloxane being a linear polyorganosiloxane having an average of two or more carboxylic acid groups per molecule; and (b) from 5 to 30 weight percent of a second polyorganosiloxane that does not contain carboxylic acid groups, the second polyorganosiloxane being a liquid at 25 degrees Celsius and a pressure of 101 megapascals, the filler particles being present in a concentration in the range of from 15 to 78 volume percent based on the volume of the composition, the weight percent values ​​being based on the weight of the composition, and the composition not comprising at least one of an aliphatic diol and a silicone polyether.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to conductive silicone compositions containing a carboxylic acid functional siloxane thixotropic agent.

[0002] Introduction Filled silicone compositions include fillers dispersed in a matrix material that includes a polysiloxane component. Filled silicone compositions are used in many applications, including conductive silicone compositions, such as thermally conductive materials and electrically conductive materials. The fillers in conductive silicone compositions help to enhance the conductive properties of the composition. Thermally conductive silicone compositions typically contain thermally conductive fillers, and electrically conductive silicone compositions typically contain electrically conductive fillers. The fillers are often present in concentrations of 15 volume percent (vol%) or more, and can be present in concentrations up to 80 volume% or even more, based on the volume of the filled silicone composition. Increasing the amount of electrically conductive filler can increase the conductive properties of the silicone composition, but it also typically increases the viscosity of the filled silicone composition, which can make it difficult to apply the silicone composition to a substrate (poor processability). As a result, there has been a tension between maximizing the conductive properties of the silicone composition and maintaining the processability of the silicone composition.

[0003] Although it is desirable to have high processability by having a low viscosity under high shear, it is often also desirable to have a high viscosity under low or no shear to maintain the shape and position in which it is placed (i.e., physical stability). Shear-thinning compositions have a relatively high viscosity under low or no shear to provide composition stability, while exhibiting a relatively low viscosity under shear to allow flow during application. As a result, shear-thinning compositions can be easily applied by relatively high shear methods such as extrusion, yet maintain physical stability once applied. There are ways to introduce shear-thinning properties into filled silicone compositions. However, the challenge is to identify a way to induce shear-thinning behavior in filled silicone compositions while still achieving a sufficiently low viscosity under shear to allow extrusion of the composition. Many methods of increasing shear-thinning properties often result in reduced extrusion / flow under shear. Shear-thinning behavior is often characterized by the "thixotropic index" of a composition, which is the ratio of the viscosity at low shear conditions divided by the viscosity at high shear conditions. Increasing the thixotropic index corresponds to increasing the shear thinning properties of the composition.

[0004] The thixotropic index can be increased by increasing the low shear viscosity, decreasing the high shear viscosity, or a combination of both. However, it may be desirable to preferentially increase the low shear viscosity versus decreasing the high shear viscosity. Increasing the low shear viscosity improves physical stability and compositional stability (settling of fillers from the composition) after application or during storage. When these features are most important, for example in vertical applications where the composition must not drip or sag, it is desirable to increase the low shear viscosity as much as possible. Changing the high shear viscosity up or down can have undesirable effects on the method of deposition or extrusion of the composition, so it may be desirable to minimize the change in high shear viscosity.

[0005] It is an object of the present invention to identify an additive for a filled silicone composition that preferentially increases the low shear viscosity of the filled silicone composition relative to its high shear viscosity in order to increase the thixotropic index of the filled silicone composition. More specifically, it is an object of the present invention to identify an additive for a filled silicone composition containing 15 to 80 volume percent filler, based on the volume of the filled silicone composition, that preferentially increases the maximum viscosity of the composition relative to the minimum viscosity while increasing the thixotropic index of the composition, and that has a viscosity of less than 200 Pascal when measured by a strain sweep method over a strain amplitude range of 0.01 percent (%) to 300% as described hereinafter. * seconds (Pa * s) or less, preferably 100 Pa * The objective is to identify an additive that achieves a minimum viscosity of no greater than 0.05 wt. s. It is even more desirable if the additive is also capable of increasing the thixotropic index of the filled silicone composition by preferably 50% or more, preferably 75% or more, and most preferably 100% or more. Summary of the Invention

[0006] The present invention provides a solution to the problem of identifying an additive for a filled silicone composition that preferentially increases the low shear viscosity of the silicone composition relative to its high shear viscosity in order to increase the thixotropic index of the composition. The additive of the present invention acts as a thixotropic agent for a filled silicone composition containing 15 to 80 volume percent filler that increases the thixotropic index of the filled silicone composition, preferentially increasing the maximum viscosity relative to the minimum viscosity of the filled silicone composition, and has a viscosity of less than 200 Pascal when measured by a strain sweep method over a strain amplitude range of 0.01 percent (%) to 300%, as described below in this specification. * seconds (Pa * s) or less, and even 100Pa * The additive can simultaneously increase the thixotropic index of the filled silicone composition by even 50% or more, preferably by 75% or more, and most preferably by 100% or more.

[0007] The present invention is the result of the discovery that carboxylic acid functional linear polyorganosiloxanes having an average of two or more carboxylic acid groups per molecule can act as thixotropic agents in filled silicone compositions to accomplish the above objectives.

[0008] In a first aspect, the invention is a composition comprising filler particles dispersed in a matrix material, the matrix material comprising: (a) from 0.01 to 1.50 weight percent of a first polyorganosiloxane, the first polyorganosiloxane being a linear polyorganosiloxane having an average of two or more carboxylic acid groups per molecule; and (b) from 5 to 30 weight percent of a second polyorganosiloxane that does not contain carboxylic acid groups, the second polyorganosiloxane being liquid at 25 degrees Celsius and a pressure of 101 megapascals; the filler particles are present in a concentration in the range of from 15 to 78 volume percent based on the volume of the composition, the weight percent values ​​being based on the weight of the composition, and the composition does not contain at least one of an aliphatic diol and a silicone polyether.

[0009] The compositions of the present invention are useful, for example, as filled conductive polysiloxane compositions, such as thermally conductive polysiloxane compositions and / or conductive polysiloxane compositions. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Test methods refer to the test method most recent to the priority date of this document unless a date is given with the test method number. References to test methods contain both a reference to the testing institute and the test method number. The following test method abbreviations and identifiers apply herein: ASTM refers to ASTM International Methods, EN refers to European Norm, DIN refers to Deutsches Institut fur Normung, ISO refers to the International Organization for Standards, and UL refers to the Underwriters Laboratory.

[0011] Products identified by trade names refer to compositions available under those trade names as of the priority date of this document.

[0012] "Plurality" means two or more. "And / or" means "and, or alternatively." All ranges are inclusive of the endpoints unless otherwise indicated.

[0013] "Hydrocarbyl" refers to a univalent group formed by removing a hydrogen atom from a hydrocarbon, and includes alkyl and aryl groups.

[0014] "Alkyl" refers to a hydrocarbon radical that can be obtained by removing a hydrogen atom from an alkane. An alkyl can be straight-chained or branched.

[0015] "Aryl" refers to a radical that may be obtained by removing a hydrogen atom from an aromatic hydrocarbon.

[0016] The "maximum viscosity", "minimum viscosity", and "thixotropy index" of a composition are measured according to the following oscillatory shear strain amplitude sweep ("strain sweep") method. Prepare circular parallel serrated plates (e.g., part number 401978.901, from TA Instruments, New Castle, DE, USA) with a diameter of 25 millimeters (mm). Place the sample composition on one plate and press the other plate against the sample composition until the plates are parallel to each other, the gap spacing between the plates is 1.0 mm, the sample composition is in thermal contact with both plates, and the gap spacing between the plates is filled. Using an ARES-G2 strain-controlled rheometer (TA Instruments, New Castle, DE, USA), perform a logarithmic sweep of strain amplitude from 0.01 percent (%) to 300% with 20 sampling points per decade using an angular frequency of 10 radians per second at 23 degrees Celsius (°C). The strain amplitude is expressed as a function of percent oscillatory strain amplitude in Pascals. * seconds (Pa * The complex viscosity at 100°C is recorded. The "maximum viscosity" is 0.1 microNewtons. * "Minimum Viscosity" is the highest complex viscosity recorded above an oscillatory torque amplitude of 1.5 metric tons (or equivalently, above an oscillatory stress amplitude threshold of 0.0326 Pascals). "Minimum Viscosity" is the lowest complex viscosity recorded above the same threshold.

[0017] "Thixotropy index" is the ratio of maximum viscosity to minimum viscosity. The compositions of the present invention achieve a thixotropy index of 5 or more, even 10 or more, 20 or more, 30 or more, 40 or more, 50 or more, 60 or more, 70 or more, 80 or more, 90 or more, 100 or more, even 150 or more, 200 or more, 250 or more, or even 300 or more, while still achieving a viscosity of 100 Pa. * s or less, even 75Pa * s or less, 50Pa * s or less, 25Pa * s or less, even 10Pa * A minimum viscosity of 0.15 or less can be achieved.

[0018] 29 Si, 13 C, and 1H nuclear magnetic resonance spectroscopy is used to determine the composition and average number of siloxane units in polysiloxanes (see, for example, The Analytical Chemistry of Silicones, Smith, A. Lee, ed., John Wiley & Sons: New York, 1991, p. 347ff).

[0019] The compositions of the present invention include filler particles dispersed (distributed) in a matrix material, the matrix material including a first polyorganosiloxane and a second polyorganosiloxane.

[0020] The first polyorganosiloxane contains an average of two or more carboxylic acid groups per molecule. In the broadest scope, the first polyorganosiloxane can be of any structure or shape, including linear, branched, cyclic, or a combination of linear and cyclic, known as a "dumbbell" structure. The dumbbell structure can have the following chemical structure:

[0021] [ka] In the formula, R d is independently selected in each occurrence from the group of hydrocarbyls having 1 to 12 carbon atoms and carboxylic acid functionalized hydrocarbyls; R e and R g is independently selected in each occurrence from hydrocarbyl having 1 to 8 carbon atoms; R f is independently in each occurrence selected from oxygen and a divalent hydrocarbon having 1 to 12 carbon atoms; subscript m is independently in each occurrence a value in the range of 2 to 4, and subscript n is independently in each occurrence a value in the range of 5 to 150; provided that at least a carboxylic acid group is present per molecule.

[0022] Desirably, the first polyorganosiloxane is a linear polyorganosiloxane. The carboxylic acid groups can be terminal or pendant (pendant meaning located along the polymer chain other than at the end of the chain) or a combination of terminal and pendant. Linear polyorganosiloxanes are those having the formula R″3SiO 1 / 2 ("M") and R"2SiO 2 / 2 ("D") siloxane units, wherein R" is a monovalent organic or substituted organic group bonded to a silicon atom, and each O of the siloxane unit may be selected from 1 / 2 and O 2 / 2 refers to an oxygen atom shared with another silicon atom of another siloxane unit. A linear polyorganosiloxane has no more than two, preferably no more than one, R″SiO 3 / 2 ("T") and SiO 4 / 2 ("Q") siloxane units. Desirably, the first polyorganosiloxane has one or more carboxylic acid groups at each end of the linear polyorganosiloxane as the terminal carboxylic acid group(s).

[0023] The first polyorganosiloxane has the chemical structure (I): HOOC-R'-R2SiO-[R2SiO] n -SiR2-R'-COOH (I). During the ceremony, R' is independently selected in each occurrence from the group of divalent hydrocarbons having 1 or more carbon atoms, and can have 2 or more, 3 or more, 4 or more, 5 or more, 6 or more, 7 or more, 8 or more, or even 9 or more carbon atoms, while typically having 12 or less carbon atoms, and can have 10 or less, 9 or less, 8 or less, 6 or less, 5 or less, 4 or less, 3 or less, or even 2 or less carbon atoms. For example, R' can be -[CH2]9- in one or all occurrences.

[0024] R is independently in each occurrence selected from the group of hydrocarbyls having 1 or more, 2 or more, 3 or more, 4 or more, 5 or more, 6 or more, or even 7 or more carbon atoms, and typically has 8 or less carbon atoms, and can have 7 or less, 6 or less, 5 or less, 4 or less, 3 or less, or even 2 or less carbon atoms. For example, R can be selected from methyl and phenyl groups.

[0025] The subscript n is the average number of [R2SiO] groups in the first polyorganosiloxane and has a value of 5 or more, and can have a value of 10 or more, 20 or more, 30 or more, 40 or more, 50 or more, 60 or more, 70 or more, 80 or more, 90 or more, or even 100 or more, while typically having a value of 150 or less, 140 or less, 130 or less, 120 or less, 110 or less, or even 100 or less.

[0026] The concentration of the first polyorganosiloxane in the composition is desirably 0.01 weight percent (wt%) or more, and can include 0.02 wt% or more, 0.04 wt% or more, 0.06 wt% or more, 0.08 wt% or more, 0.10 wt% or more, 0.25 wt% or more, 0.50 wt% or more, 0.75 wt% or more, 1.00 wt% or more, 1.25 wt% or more, and at the same time, is typically 1.50 wt% or less, 1.40 wt% or less, 1.30 wt% or less, 1.20 wt% or less, 1.10 wt% or less, 1.00 wt% or less, 0.8 wt% or less, 0.60 wt% or less, 0.40 wt% or less, 0.20 wt% or less, 0.10 wt% or less, or even 0.08 wt% or less.

[0027] The matrix material further comprises a second polyorganosiloxane that does not contain carboxylic acid groups. The second polyorganosiloxane is liquid at 25 degrees Celsius (°C) and a pressure of 1010 megapascals (MPa). "Liquid" means that the material will conform to the shape of its container.

[0028] The second polyorganosiloxane may be a linear polyorganosiloxane. For example, the second polyorganosiloxane may have the average chemical structure (II): R a R”2SiO-[R2SiO] m -OR”2R a (II). During the ceremony, R” and R a is independently selected at each occurrence from hydrocarbyl groups having preferably 1 or more and at the same time 8 or less, 6 or less, 4 or less, or even 3 or less, or 2 or less carbon atoms. R″ can be an alkyl group, while R a can be an alkenyl group, such as a vinyl group. For example, each R a may be a vinyl group and each R″ may be selected from a methyl group or a phenyl group.

[0029] The subscript "m" is the average number of R2SiO units per molecule and is generally a value of 40 or more, and can be 50 or more, 60 or more, even 70 or more, 80 or more, 100 or more, 125 or more, 150 or more, 175 or more, or even 200 or more, while typically being 800 or less, and can be 600 or less, 400 or less, 200 or less, 150 or less, 100 or less, 80 or less, 60 or less, or even 50 or less, or 45 or less.

[0030] The second polyorganosiloxane is typically present in a concentration of 5% by weight or more, preferably 6% by weight or more, and may be 8% by weight or more, 10% by weight or more, 12% by weight or more, 14% by weight or more, 16% by weight or more, 18% by weight or more, 20% by weight or more, 22% by weight or more, 24% by weight or more, 26% by weight or more, or even 28% by weight or more, and at the same time, typically 30% by weight or less, 29% by weight or less, 27% by weight or less, 25% by weight or less, 23% by weight or less, 21% by weight or less, 19% by weight or less, 17% by weight or less, 15% by weight or less, 13% by weight or less, 9% by weight or less, or even 7% by weight or less, based on the weight of the composition.

[0031] The matrix material can include a third polyorganosiloxane that is different from the first and second polyorganosiloxanes. The third polyorganosiloxane can include two or more silylhydride groups. For example, the matrix material can include a first polyorganosiloxane and a second polyorganosiloxane having vinyl functional groups (e.g., each R a is vinyl), and a third polyorganosiloxane having a plurality of silyl hydride (SiH) groups.

[0032] The composition further comprises filler particles dispersed in the matrix material, the filler particles being present in a concentration of 15 volume percent (vol%) or more, 20 volume% or more, 25 volume% or more, 30 volume% or more, 35 volume% or more, 40 volume% or more, 45 volume% or more, 50 volume% or more, 55 volume% or more, 60 volume% or more, 65 volume% or more, 70 volume% or more, or even 75 volume% or more, based on the volume of the composition, while being present in a concentration of about 78 volume% or less, or 75 volume% or less, 74 volume% or less, 70 volume% or less, 65 volume% or less, 60 volume% or less, 55 volume% or less, 50 volume% or less, 45 volume% or less, 40 volume% or less, 35 volume% or less, or even 30 volume% or less.

[0033] The filler particles can be thermally conductive fillers, electrically conductive fillers, non-conductive fillers, or any combination of these types of fillers. Desirably, the filler particles are any one or any combination of two or more selected from thermally conductive fillers and electrically conductive fillers.

[0034] Thermally conductive fillers include metal particles, such as aluminum, silver, and copper particles; metal-coated particles, including any type of particle coated with a metal, such as aluminum, silver, and copper; inorganic particles, such as boron nitride, aluminum oxide, zinc oxide, magnesium oxide, aluminum nitride, and aluminum trihydrate; and carbonaceous materials, such as carbon nanotubes, graphene, and carbon fibers.

[0035] Conductive fillers include metal particles, such as particles of silver, gold, platinum, palladium, nickel, copper, and alloys thereof; any type of particle coated with a metal, such as silver, gold, platinum, palladium, nickel, copper, and alloys thereof; as well as carbon black, carbon fibers, carbon nanotubes, and graphene.

[0036] The filler particles typically have an average particle size of 0.05 micrometers (μm) or more, 0.1 μm or more, 0.2 μm or more, 0.5 μm or more, 1.0 μm or more, 2.0 μm or more, 3.0 μm or more, 5.0 μm or more, 10 μm or more, 20 μm or more, 30 μm or more, 40 μm or more, 50 μm or more, and preferably 60 μm or more, 70 μm or more, 80 μm or more, 90 μm or more. The average particle size may be equal to or greater than 250 μm, equal to or less than 200 μm, equal to or less than 150 μm, equal to or less than 100 μm, equal to or less than 90 μm, equal to or less than 80 μm, equal to or less than 70 μm, equal to or less than 60 μm, equal to or less than 50 μm, equal to or less than 40 μm, equal to or less than 30 μm, equal to or less than 20 μm, equal to or less than 10 μm, equal to or less than 5.0 μm, or even equal to or less than 3.0 μm, or equal to or less than 1.0 μm. The average particle size is measured as the volume-weighted median (Dv50) of the particle size distribution of the polyorganosiloxane using a Mastersizer™ 3000 laser diffraction particle size analyzer manufactured by Malvern Instruments.

[0037] In the broadest scope, the filler particles can be of any shape, including any combination of any one or more of the following shapes: spherical, polyhedral, platelet, rod-like, or irregularly shaped (e.g., "crushed").

[0038] The composition can, and typically does, include a combination of filler particles of different types and / or sizes, for example, the composition can include a collection of two or more, or even three or more, different filler particles that differ in composition and / or shape and / or size.

[0039] The composition of the present invention may or may not further include a filler treating agent as part of the matrix material. Filler treating agents are typically desirable to improve the dispersion of fillers in the matrix material by reducing filler agglomeration and filler-filler interactions. Filler treating agents can also improve the wet-out of the filler surface by the matrix material, reduce the viscosity of the composition, and cap reactive groups on the filler surface to prevent reactions with the filler that may reduce the shelf life of the composition. Desirably, the treating agent is a trialkoxy-functional silicone and / or silane. The treating agent can include or consist of one or both of alkyltrialkoxysilanes and monotrialkoxysiloxy-terminated diorganopolysiloxanes.

[0040] Examples of suitable alkyltrialkoxysilanes have the general formula: 1 )(R 2 O)3Si, where R 1 is desirably alkyl having 1 or more carbon atoms, and can have 2 or more, 3 or more, 4 or more, 5 or more, 6 or more, 7 or more, 8 or more, 9 or more, 10 or more, 11 or more, 12 or more, 13 or more, 14 or more, 15 or more, or even 16 or more carbon atoms, while typically having an average of 18 or less carbon atoms per molecule, and can have 17 or less, 16 or less, 15 or less, 14 or less, 13 or less, 12 or less, 11 or less, or even 10 or less carbon atoms; R 2is preferably an alkyl having 1 or more, 2 or more, 3 or more, 4 or more, 5 or more, or even 6 or more carbon atoms, while typically containing 10 or less, 9 or less, 8 or less, 7 or less, 6 or less, 5 or less, 4 or less, 3 or less, or even 2 or less carbon atoms. Desirably, the alkyltrialkoxysilane is an alkyltrimethoxysilane having the alkyl group described above. Examples of suitable alkyltrialkoxysilanes are n-decyltrimethoxysilane and methyltrimethoxysilane. The concentration of alkyltrialkoxysilane in the composition may be, based on the weight of the composition, generally 0 wt.% or more, 0.05 wt.% or more, 0.10 wt.% or more, 0.20 wt.% or more, 0.22 wt.% or more, or 0.24 wt.% or more, and at the same time, generally 0.75 wt.% or less, 0.50 wt.% or less, 0.40 wt.% or less, or 0.30 wt.% or less, preferably 0.28 wt.% or less, 0.26 wt.% or less, or 0.24 wt.% or less, and may be 0.22 wt.% or less.

[0041] Examples of suitable monotrialkoxysiloxy-terminated diorganopolysiloxanes generally have the following chemical structure (III): R3SiO-(R2SiO) h -[(CH2) e ((CH3)2SiO) f ] g -(CH2) e -Si(OR 2 ) 3(III), In the formula, R and R 2are each, independently at each occurrence, as defined above; subscript h is the average number of (RSiO) units per molecule, typically having a value of 10 or more, 15 or more, 20 or more, 25 or more, or even 30 or more, and simultaneously about 150 or less, 140 or less, 130 or less, 120 or less, 110 or less, 100 or less, 90 or less, 80 or less, 70 or less, 60 or less, 50 or less, 45 or less, 40 or less, 35 or less, or even 30 or less; and subscript e is the average number of CH the subscript f typically has a value of 0 or more, 1 or more, 2 or more, 3 or more, and at the same time is usually 4 or less, 3 or less, or even 2 or less; the subscript g typically has a value of 0 or more, 1 or more, 2 or more, 3 or more, and at the same time is about 6 or less, 5 or less, 4 or less, 3 or less, or even 2 or less; and the subscript g typically has a value of 0 or more, 1 or more, 2 or more, 3 or more, 4 or more, and at the same time is about 6 or less, 5 or less, 4 or less, or even 3 or less.

[0042] Desirably, the monotrialkoxysiloxy-terminated diorganopolysiloxane has the general molecular structure (IV): (CH3)3SiO-((CH3)2SiO) t -Si(OR 2 ) 3(IV). One particularly preferred trialkoxysiloxy-terminated diorganopolysiloxane is R 2 is equal to methyl, and the subscript t is equal to a value of 130 or less, preferably 120 or less, preferably 110 or less, more preferably 110 or less or 100 or less, 90 or less, 80 or less, 70 or less, 60 or less, 50 or less, 40 or less, or 30 or less, and simultaneously greater than 20, preferably greater than 30, to form a terminal trimethoxy-functionalized silicon atom.

[0043] The concentration of monotrialkoxysiloxy-terminated diorganosiloxane is typically 0 wt% or more, 0.10 wt% or more, 0.20 wt% or more, 0.30 wt% or more, 0.40 wt% or more, 0.50 wt% or more, 0.75 wt% or more, or even 1.0 wt% or more or 2.0 wt% or more, while being about 3.0 wt% or less, 2.0 wt% or less, 1.20 wt% or less, 1.15 wt% or less, or even 1.10 wt% or less, based on the weight of the composition.

[0044] The composition may further comprise any one or any combination of a number of additional components (or none). Examples of such additional components include cure inhibitors, cure catalysts, crosslinkers, antioxidant stabilizers, pigments, viscosity modifiers, silica fillers, and spacer additives. For the avoidance of doubt, the composition may not comprise any one or any combination or more of such additional components. For example, the composition may not comprise silica fillers. "Silica fillers" refers to solid particulates containing silica, including natural silica (such as crystalline quartz, ground quartz, and diatomaceous silica), and synthetic silica (fumed silica, fused silica, silica gel, and precipitated silica). Additionally or alternatively, the composition of the present invention may not comprise polyether and / or silanol-functional polydimethylsiloxane.

[0045] Examples of cure inhibitors include 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclotetrasiloxane, 1-ethynyl-1-cyclohexanol, 2-phenyl-3-butyn-2-ol, 2-methyl-3-butyn-2-ol, fumarate, maleate, and methyl(tris(1,1-dimethyl-2-propynyloxy))silane. When present, the inhibitor is typically present at a concentration of 0.0001% by weight or more, 0.001% by weight or more, based on the weight of the composition, and at the same time, generally at a concentration of 5% by weight or less, or even 1% by weight or less, or even 0.5% by weight or less.

[0046] The curing catalyst may include, for example, a hydrosilylation curing catalyst, such as a platinum-based catalyst, such as Karstedt's catalyst and / or Speier's catalyst (H2PtCl6).

[0047] The crosslinker comprises a siloxane having an average of two or more silylhydride (SiH) functional groups per molecule, and includes the third polyorganosiloxane described herein above.

[0048] When present, antioxidants may be included at a concentration typically between 0.001 and 1% by weight of the composition. Antioxidants may be present alone or in combination with stabilizers. Antioxidants include phenolic antioxidants and stabilizers include organophosphorus derivatives.

[0049] Examples of pigments include carbon black, graphite, titanium dioxide, and copper phthalocyanine. When present, pigments tend to be present at a concentration of 0.0001 to 1% by weight based on the weight of the composition.

[0050] The spacer additive is a non-thermally conductive filler with an average particle size ranging from 50 to 250 micrometers. Examples of spacers include glass and polymer beads.

[0051] The composition may be free of any one of hydroxyl-functional polysiloxanes, particularly terminal silanol (Si-OH) functional polysiloxanes; hydroxyl-functional hydrocarbons, such as aliphatic diols; and silicone polyethers, or any combination of two or more.

[0052] Thermally conductive composition The composition of the present invention can include a thermally conductive composition. As the thermally conductive composition, the filler particles are present in a concentration of preferably 40% by volume or more, 50% by volume or more, 60% by volume or more, or even 70% by volume or more, based on the volume of the composition, and at the same time, the filler particles are present in a concentration of generally less than 78% by volume, preferably 74% by volume or less, and 70% by volume or less, 60% by volume or less, or even 50% by volume or less.

[0053] When the thermally conductive filler is present in a concentration in the range of 40 to 70% by volume, based on the volume of the composition, the first polyorganosiloxane is desirably present in a concentration of 0.01% by weight or more, and may be 0.05% by weight or more, 0.10% by weight or more, 0.15% by weight or more, 0.20% by weight or more, 0.40% by weight or more, 0.60% by weight or more, 0.80% by weight or more, 1.00% by weight or more, 1.2% by weight or more, or even 1.4% by weight or more, while typically 1.5% by weight or less, 1.3% by weight or less, 1.1% by weight or less, 1.0% by weight or less, 0.8% by weight or less, 0.6% by weight or less, 0.4% by weight or less, 0.2% by weight or less, or even 0.1% by weight or less, based on the weight of the composition.

[0054] When the thermally conductive filler is present at a concentration in the range of more than 70% by volume and less than 78% by volume, typically in the range of 70 to 74% by volume, based on the volume of the composition, the first polyorganosiloxane is desirably present at a concentration of 0.01% by weight or more, and may be 0.05% by weight or more, 0.10% by weight or more, 0.15% by weight or more, 0.20% by weight or more, 0.25% by weight or more, 0.30% by weight or more, or even 0.40% by weight or more, while typically 0.5% by weight or less, 0.4% by weight or less, 0.3% by weight or less, 0.2% by weight or less, 0.1% by weight or less, or even 0.075% by weight or less, based on the weight of the composition.

[0055] The thermally conductive composition desirably includes a filler treating agent as described above.

[0056] One desirable second polyorganosiloxane for use in the thermally conductive composition of the present invention has terminal vinyl functionality and an average degree of polymerization in the range of 40 to 800 (i.e., each R is methyl and each R a is vinyl and m is in the range of 40 to 800.

[0057] conductive composition The composition of the present invention can be a conductive composition.As a conductive composition, filler particles are preferably present in a concentration of 5% by volume or more, can be 10% by volume or more, 15% by volume or more, 20% by volume or more, or even 25% by volume or more, and at the same time, typically present in a concentration of 55% by volume or less, even 50% by volume or less, 45% by volume or less, 40% by volume or less, 35% by volume or less, 30% by volume or less, 25% by volume or less, 20% by volume or less, 15% by volume or less, 10% by volume or less, or even 8% by volume or less based on the volume of the composition.

[0058] When the composition is a conductive composition, the first polyorganosiloxane is desirably present in a concentration of 0.1 wt.% or more, 0.2 wt.% or more, 0.3 wt.% or more, 0.4 wt.% or more, 0.5 wt.% or more, 0.6 wt.% or more, 0.7 wt.% or more, 0.8 wt.% or more, 0.9 wt.% or more, 1.0 wt.% or more, 1.1 wt.% or more, 1.2 wt.% or more, 1.3 wt.% or more, or even 1.4 wt.% or more, based on the weight of the composition, while typically present in a concentration of 1.5 wt.% or less, 1.4 wt.% or less, 1.3 wt.% or less, 1.2 wt.% or less, 1.1 wt.% or less, 1.0 wt.% or less, 0.9 wt.% or less, 0.8 wt.% or less, 0.7 wt.% or less, 0.6 wt.% or less, or even 0.5 wt.% or less. The second polyorganosiloxane has terminal vinyl functionality and an average degree of polymerization in the range of 140 to 800 (i.e., each R is methyl and each R a It is also desirable that the polydimethylsiloxane has a chemical structure (II)) in which R is vinyl and m is within the range of 140 to 800.

[0059] The conductive composition desirably further comprises a silylhydride-functional polydimethylsiloxane crosslinker and a platinum-based hydrosilylation catalyst. Examples of suitable platinum-based hydrosilylation catalysts include any one or combination of two or more selected from the group consisting of platinum(0)-1,3-divinyl-1,1,3,3-tetramethyldisiloxane (Karstedt's catalyst), HPtCl, di-μ-carbonyldi-π-cyclopentadienyldinickel, platinum-carbonyl complexes, platinum-divinyltetramethyldisiloxane complexes, platinum cyclovinylmethylsiloxane complexes, platinum acetylacetonate (acac), platinum black, chloroplatinic acid, platinum compounds such as chloroplatinic acid hexahydrate, reaction products of chloroplatinic acid with monohydric alcohols, platinum bis(ethylacetoacetate), platinum bis(acetylacetonate), platinum dichloride, and complexes of these platinum compounds with olefins or low molecular weight organopolysiloxanes, or platinum compounds microencapsulated in a matrix or in a core-shell structure. The hydrosilylation catalyst may be part of a solution containing complexes of platinum with low molecular weight organopolysiloxanes, including 1,3-diethenyl-1,1,3,3-tetramethyldisiloxane complexes with platinum. These complexes may be microencapsulated in a resin matrix. The catalyst may be 1,3-diethenyl-1,1,3,3-tetramethyldisiloxane complexes with platinum. EXAMPLES

[0060] Table 1 identifies the materials for use in preparing the samples described herein.

[0061] [Table 1-1]

[0062] [Table 1-2] DOWSIL is a trademark of The Dow Chemical Company. SYL-OFF is a trademark of Dow Corning Corporation.

[0063] Thermally conductive composition samples - Part I Base Thermally Conductive Composition First, a base thermally conductive composition (TC) is prepared, and then samples are prepared by mixing the conductive composition with the first polyorganosiloxane component. Five base thermally conductive compositions (TC-1 to TC-5) are prepared according to the formulations in Table 2 and the following procedure: Add the second polyorganosiloxane 1, the filler treatment, and filler 3 to a 100 milliliter (mL) polypropylene cup, place the cup in a Flacktek Speedmixer, and mix at 2000 revolutions per minute (RPM) for 20 seconds. Then add filler 2 and mix again at 2000 RPM for 30 seconds, followed by adding filler 1 and mixing at 2000 RPM for 30 seconds. The resulting mixture is transferred to an aluminum pan and heated to 150 degrees Celsius (°C) under a vacuum of 3.066 megapascals (23 torr) pressure for 1 hour.

[0064] [Table 2] * Wt%2 is the weight percent of matrix material in the composition.

[0065] Thermally conductive composition The first (1 st ) Prepare thermally conductive composition samples using the base thermally conductive composition of Table 2 by adding polyorganosiloxane.

[0066] 0.1%, 0.5%, and 1.5% by weight st For samples containing polyorganosiloxane, 20 grams (g) of the base thermally conductive composition and the specified amount of 1 stPrepare thermally conductive composition samples in 40 milliliter (mL) polypropylene cups by adding 0.02 g of polyorganosiloxane for every 0.1 wt% specified in Table 2 (e.g., 0.02 g for 0.1 wt%, 0.10 g for 0.5 wt%, 0.30 g for 1.5 wt%). st Polyorganosiloxane is used.

[0067] 0.01% by weight and 0.05% by weight st For samples containing polyorganosiloxane, 100 g of the base thermally conductive composition and 0.01 g (for 0.01 wt%) or 0.05 g (for 0.05 wt%) of st Thermally conductive composition samples are prepared in 100 mL polypropylene cups by adding the polyorganosiloxane.

[0068] The samples are mixed using a Flacktek Speedmixer, mixing at 1500 revolutions per minute (RPM) for 20 seconds to obtain the sample thermally conductive composition.

[0069] The formulations of the thermally conductive composition samples are in Table 3 along with the properties of the thermally conductive compositions, which are sorted by the volume percent of filler in the composition. As previously described herein, the strain sweep method is used to characterize the maximum viscosity, minimum viscosity and thixotropy index.

[0070] [Table 3] 1 Minimum viscosity is 200Pa * s, the thixotropic index increases, and the maximum viscosity increases more than the minimum viscosity for the corresponding reference composition, the sample passes. 2 Minimum viscosity is 200Pa * The sample was rejected because it exceeded the maximum amount of s. 3 The sample was rejected because it became a non-flowable mixture and the viscosity could not be measured.

[0071] Samples of Thermally Conductive Compositions-Part II (High Viscosity / High Degree of Polymerization Secondary Polyorganosiloxanes) Base thermally conductive composition TC-6 (Reference 6) is prepared by mixing together 12.24 g of second polyorganosiloxane 2, 1.9 g of second polyorganosiloxane 3, 0.47 g of filler treatment 1, 62.88 g of filler 1, and 22.51 g of filler 3 in a polypropylene cup in a Flacktek speedmixer at 2500 RPM for 20 seconds. The mixture is heated at 150° C. for 1 hour under a vacuum of 3.066 megapascals (23 Torr) pressure to obtain Reference 6. TC-6 is 71% filled by volume.

[0072] Sample 21 is prepared by combining 20 g of Reference 6 with 0.02 g of the first polyorganosiloxane 1. Sample 21 contains 0.1 wt % of the first polyorganosiloxane 1.

[0073] The maximum and minimum viscosities and the thixotropy index of Reference 6 and Sample 21 are measured. The results are in Table 4.

[0074] [Table 4] 1 Minimum viscosity is 200Pa * s, the thixotropic index increases, and the maximum viscosity increases more than the minimum viscosity for the corresponding reference composition, the sample passes.

[0075] Thermally conductive composition samples - Part III (samples without aluminum trihydrate) Prepare Reference 7 in a 1 gallon Baker Perkins Sigma Blade Mixer. Add 827g of second polyorganosiloxane 4, 40g of filler treatment 1, 40g of filler treatment 2, and 1229g of filler 5 and mix for 5 minutes. Scrape chamber walls with a spatula, add 5242g of filler 4 and mix for 5 minutes. Scrape chamber walls with a spatula, add 2621g of filler 2 and mix for 5 minutes. Scrape chamber walls, then mix for an additional 5 minutes. Vacuum to 25 Torr and mix for 30 minutes. Heat to 135°C, mix for 60 minutes, then cool to obtain Reference 7. The concentration of filler is 70% by volume of the composition.

[0076] Prepare Sample 22 by adding 100 g of Reference 7 to a Flacktek 100Max polypropylene cup, then add 0.05 g of the first Polyorganosiloxane 1. Mix in a Flacktek speedmixer at 2500 RPM for 20 seconds, followed by 1000 RPM for 10 seconds.

[0077] Prepare Sample 23 by adding 100 g of Reference 7 to a Flacktek 100Max polypropylene cup, then adding 0.10 g of the first Polyorganosiloxane 1. Mix in a Flacktek speedmixer at 2500 RPM for 20 seconds, followed by 1000 RPM for 10 seconds.

[0078] Determine the maximum and minimum viscosities and thixotropy indices of Reference 7 and Samples 22 and 23. The results are in Table 5.

[0079] [Table 5] 1 Minimum viscosity is 200Pa * s, the thixotropic index increases, and the maximum viscosity increases more than the minimum viscosity for the corresponding reference composition, the sample passes.

[0080] Thermally conductive composition samples - Part IV (samples containing methyltrimethoxysilane treatment) Prepare Reference 8 by adding 0.88 g of the second polyorganosiloxane 1 and 0.84 g of filler treatment 3 to a 100 mL polypropylene cup, placing the cup in a Flacktek speedmixer, and mixing at 2000 RPM for 20 seconds. Add 41.64 g of filler 6, mix at 2000 RPM for 30 seconds, then add 41.64 g of filler 7, mix at 2500 RPM for 20 seconds. Mix by hand, then mix again at 2500 RPM for 20 seconds. Transfer the resulting mixture to an aluminum pan and heat to 10° C. under vacuum at a pressure of 3.066 megapascals (23 torr) for 1 hour to obtain Reference 8.

[0081] Prepare sample 24 by mixing 30 g of reference 8 with 0.03 g of first polyorganosiloxane 1 at 1000 RPM for 20 seconds, followed by hand mixing, then mixing at 1000 RPM for 20 seconds, and hand mixing again. Leave at 25 °C for 2 days before characterization.

[0082] Sample 25 is prepared similarly to Sample 4, except that First Polyorganosiloxane 2 is used instead of First Polyorganosiloxane 1.

[0083] The maximum and minimum viscosities and thixotropy indexes are measured for Reference 8 and Samples 24 and 25. The results are in Table 6.

[0084] [Table 6] 1 Minimum viscosity is 200Pa * s, the thixotropic index increases, and the maximum viscosity increases more than the minimum viscosity for the corresponding reference composition, the sample passes.

[0085] Curable Conductive Composition Samples - Part I Table 7 presents the formulations of the curable conductive composition samples in Part I (References 9, 10 and Samples 26-33 and Samples C and D). The samples are prepared as follows.

[0086] First, prepare a catalyst / inhibitor solution by adding 7.89 g of platinum catalyst 1 and 12.25 g of the second polyorganosiloxane 2 in a polypropylene cup and mixing for 30 seconds at 2000 RPM using a FlackTeck speedmixer. Add 12.11 g of inhibitor 1 and mix for 30 seconds at 2000 RPM.

[0087] Then prepare the masterbatch by adding 92.91g of the second Polyorganosiloxane 3 to a polypropylene cup, then add 5.071g of the catalyst / inhibitor solution. Mix at 2000 RPM for 30 seconds. Add 2.03g of Si-H Polysiloxane and mix at 2000 RPM for 30 seconds. This is "Masterbatch 1".

[0088] Weigh the specified amount of Filler 8 from Table 7 into a polypropylene cup (total batch size 20.00 g) and add the specified amount of Masterbatch 1 and mix for 30 seconds at 2000 RPM. Add the specified amount of First Polyorganosiloxane 1 or First Polyorganosiloxane 2 and mix for 30 seconds at 2000 RPM to obtain the final curable conductive composition sample.

[0089] [Table 7]

[0090] Curable Conductive Composition Samples - Part II (Curable Compositions) The curable conductive composition samples of Part II (References 11 and 12 and Samples 34 and 35) are prepared in the following manner.

[0091] First, prepare a catalyst / inhibitor solution by adding 7.89 g of platinum catalyst 1 and 12.25 g of the second polyorganosiloxane 2 in a polypropylene cup and mixing for 30 seconds at 2000 RPM using a FlackTeck speedmixer. Add 12.11 g of inhibitor 1 and mix for 30 seconds at 2000 RPM.

[0092] Reference 11: Add 24.00g of Filler 8 and 5.28g of the second Polyorganosiloxane 4 to a polypropylene cup and mix at 2000 RPM for 30 seconds. Add 0.31g of catalyst / inhibitor solution and mix at 2000 RPM for 30 seconds. Add 0.42g of Si-H polysiloxane and mix at 2000 RPM for 30 seconds.

[0093] Reference 12: Prepare the same as Reference 11, except use 24.01 g of filler 8, 0.16 g of Si-H polysiloxane, 0.32 g of catalyst / inhibitor solution, and 5.53 g of second polyorganosiloxane 5 (instead of second polyorganosiloxane 4).

[0094] Sample 34: Prepare similarly to Reference 11, except use 5.00g of the second polyorganosiloxane 4 and 0.40g of the Si-H polysiloxane, and mix in 0.30g of the first polyorganosiloxane 1 at 2000 RPM for 30 seconds after adding all other ingredients.

[0095] Sample 35: Prepare similarly to Reference 12, except use 5.25g of the second Polyorganosiloxane 5 and 0.31g of the catalyst / inhibitor solution, and mix in 0.30g of the first Polyorganosiloxane 1 at 2000 RPM for 30 seconds after adding all other ingredients.

[0096] Table 8 shows the characterization results of the conductive composition samples.

[0097] [Table 8] 1 Minimum viscosity is 200Pa * s, the thixotropic index increases, and the maximum viscosity increases more than the minimum viscosity for the corresponding reference composition, the sample passes. 2 The sample failed because it did not result in an increase in the thixotropic index.

Claims

1. 1. A composition comprising filler particles dispersed in a matrix material, the matrix material comprising: (a) 0.01 to 1.50 weight percent of a first polyorganosiloxane, the first polyorganosiloxane being a linear polyorganosiloxane having an average of two or more carboxylic acid groups per molecule; (b) 5 to 30 weight percent of a second polyorganosiloxane that is free of carboxylic acid groups, the second polyorganosiloxane being a liquid at 25 degrees Celsius and a pressure of 101 megapascals; The filler particles are present in a concentration in the range of greater than or equal to 15 volume percent and less than 78 volume percent, based on the volume of the composition, the weight percent values ​​being based on the weight of the composition, and the composition does not include at least one of an aliphatic diol and a silicone polyether.

2. The first polyorganosiloxane has an average chemical structure (I): HOOC-R’-R 2 SiO-[R 2 SiO] n -SiR 2 -R’-COOH (I) 2. The composition of claim 1, having the formula:

3. Each R' is -[CH 2 ] 9 -, each R is methyl, and subscript n is a value within the range of 8 to 130.

4. The second polyorganosiloxane has an average chemical structure (II): R a R” 2 SiO-[R 2 SiO] m -OR” 2 R a (II) wherein each R″ and R a is independently at each occurrence selected from the group of hydrocarbyls having 1 to 8 carbon atoms, and subscript m is a value in the range of 40 to 800.

5. The composition of claim 4 , wherein the matrix material further comprises a third polysiloxane containing two or more silyl hydride groups.

6. the filler particles comprise thermally conductive filler particles in a concentration ranging from 40 to 74 volume percent based on the volume of the composition; i. when the thermally conductive filler is present in a concentration in the range of 40 to 70 volume percent based on the volume of the composition, the first polyorganosiloxane is present in a concentration in the range of 0.01 weight percent to less than 1.5 weight percent based on the weight of the composition; and ii. The composition according to any one of claims 1 to 5, wherein the thermally conductive filler is present at a concentration of more than 70 volume percent and at the same time 74 volume percent based on the volume of the composition, the first polyorganosiloxane is present at a concentration in the range of 0.01 weight percent to 0.5 weight percent based on the weight of the composition.

7. The composition of claim 6 further comprising a filler treating agent selected from trialkoxy-functional silicones and silanes.

8. The composition of any one of claims 1 to 5, wherein the filler particles comprise conductive filler particles present in a concentration in the range of 5 to 55 volume percent based on the volume of the composition, and the first polyorganosiloxane is present in a concentration in the range of 0.1 to 1.5 weight percent, based on the weight of the composition.

9. 9. The composition of claim 8, wherein the second polyorganosiloxane contains at least two vinyl groups per molecule, and the composition further comprises a hydride silyl-functional polydimethylsiloxane crosslinker and a platinum-based hydrosilylation catalyst.

10. The composition according to any one of claims 1 to 9, wherein the composition does not comprise any one of an aliphatic diol, a silicone polyether, and a Si-OH terminated polysiloxane, or any combination of two or more thereof.

Citation Information

Patent Citations

  • Self-repairing organosilicone resin and preparation method thereof

    CN109320723A

  • Heat-conductive silicone grease composition

    JP2009221310A

  • Gel composition and cosmetic preparation

    WO2009025146A1