Reinforced Polyamide

By blending polyamide with an impact modifier and low viscosity siloxane-based polymer, the impact strength and flow properties of reinforced nylon compositions are enhanced, addressing the limitations of existing technologies and enabling the production of lightweight, high-strength articles.

JP2024543352APending Publication Date: 2024-11-21DOW GLOBAL TECHNOLOGIES LLC +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024527109
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-11-15
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing reinforced nylon compositions face challenges in achieving improved impact strength, particularly at low temperatures, while maintaining flow properties and avoiding increased costs, with existing impact modifiers like maleic anhydride grafted polyolefin elastomers leading to irreversible imide bonding and reduced flow properties.

Method used

Incorporating a blend of polyamide, an impact modifier, and a low viscosity siloxane-based polymer, such as polydimethylsiloxane (PDMS), to enhance impact strength and flow properties without significantly increasing costs.

Benefits of technology

The reinforced polyamide compositions exhibit a significant improvement in impact strength, up to 100% enhancement at room temperature and below, with maintained or improved flexural modulus, and reduced capillary viscosity, enabling the production of lightweight articles with thinner walls.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543352000001
    Figure 2024543352000001
  • Figure 2024543352000002
    Figure 2024543352000002
  • Figure 2024543352000003
    Figure 2024543352000003
Patent Text Reader

Abstract

A reinforced polyamide composition comprising: (a) at least one polyamide; (b) at least one toughening agent component; and (c) a 1 mm thick reinforced polyamide composition having good impact strength. 2 / s~100,000mm 2 and at least one siloxane-based component having a viscosity of about 100 / s; a method for producing the reinforced polyamide composition; and articles made from the reinforced polyamide composition.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to reinforced polyamide compositions, more particularly, the present invention relates to reinforced polyamide compositions comprising a blend of a polyamide, an impact modifier, and a siloxane-based polymer that imparts improved impact strength and flow properties to the reinforced polyamide composition. [Background technology]

[0002] Nylon is a generic name for a family of synthetic thermoplastic polymers composed of polyamides. Polyamides (PA) are repeating units linked by amide bonds. Nylon is a well-known synthetic thermoplastic polymer based on aliphatic or semi-aromatic polyamides in which at least 85% by weight of the amide linkages (-CO-NH-) are directly bonded to two aliphatic groups.

[0003] Synthetic processed nylon (or PA) is a plastic with excellent mechanical properties, solvent resistance, abrasion resistance, etc., and nylon materials can be melt processed into various fibers, films, or shapes to form articles / products and parts for use in various applications. For example, reinforced nylon composites can be used in applications such as automotive applications, industrial machinery applications, consumer applications, and electronic applications. There is a continuing need to improve the impact strength of reinforced nylon at both room temperature and below room temperature, especially in the automotive field. However, nylon has low notched impact strength, and in particular, nylon exhibits the disadvantage of low toughness in low temperature environments, which limits the further use of nylon in industry. Therefore, the industry is constantly seeking ways to make the impact strength performance of reinforced nylon better (increase or improve).

[0004] Typically, the impact strength performance (or impact resistance) of reinforced nylon is increased by adding an impact modifier (IM) agent or additive to the reinforced nylon. Adding impact modifier materials to reinforced nylon is one way to improve the impact strength of reinforced nylon at both room temperature and below room temperature, especially in the automotive field. Furthermore, more efficient impact modifiers are needed to allow for further reduction in the weight of articles made from reinforced nylon, as they can improve the stiffness / toughness / flow balance of reinforced nylon and reduce the costs associated with the manufacture of reinforced nylon and articles made therefrom.

[0005] So far, the main impact modifier (IM) used in reinforced nylon has been maleic anhydride grafted polyolefin elastomer. Usually, maleic anhydride (MAH) is grafted onto the backbone of polyolefin elastomer (POE) to enhance the compatibility between POE and nylon through the reaction between the anhydride groups grafted on POE and the amine end groups in nylon, as shown in the following general chemical reaction scheme (Scheme (I)):

[0006] [ka]

[0007] MAH-grafted POE provides the required good compatibility properties between non-polar polyolefins and highly polar nylons. However, the reaction causes irreversible imide bonds, which significantly reduces the flow properties of the resulting nylon / POE blend compositions.

[0008] To date, many efforts have been made to improve the impact strength of reinforced nylon, including, for example, optimizing the MAH graft ratio of IM, lowering the Tg of POE, and / or providing crosslinks in POE. Most of the efforts involve designing the MAH-grafted POE (also abbreviated as "POE-g-MAH") component, such as improving the MAH level grafted onto POE. However, the aforementioned industry efforts to optimize both the impact strength and flow performance of reinforced nylon compositions have met with limited success.

[0009] For example, U.S. Patent No. 9,056,982(B2) and U.S. Patent No. 9,388,312 refer to a thermoplastic composition in pellet or solid form comprising 50 weight percent to 99 weight percent of nylon 6.6 resin, 1 weight percent to 50 weight percent of a polymeric performance improver, and 0.01 weight percent to 25 weight percent of a silicone additive, wherein the silicone additive comprises an ultra-high molecular weight siloxane polymer that cannot be considered either a gel or an oil, and the siloxane polymer is not functionalized and is non-reactive with polyamide.

[0010] US Patent Publication No. 20140316041 (corresponding to WO 2014176143(A1)) refers to the use of ultra-high molecular weight polydimethylsiloxane (PDMS) as a toughening agent in thermoplastic or thermosetting resin systems. The resin systems described in the above reference encompass a wide variety of polymers and polyamides. Precipitated and fumed silica are also blended into PDMS. The loading of PDMS is high, ranging from 20% to 80% by weight in the compositions disclosed in the above reference. Such high loading of PDMS can be detrimental to resin systems using PDMS due to poor compatibility between high polarity polyamides and low polarity PDMS.

[0011] China Patent No. 110437611(A) refers to reinforced nylon composites with ultra-low temperature resistance. The composites described in the above reference require amino- or epoxy-terminated PDMS as a toughening agent, in addition to glass fibers, lubricants, and other additives. No polyolefin elastomers useful as toughening agents are mentioned. In addition, the above reference requires high loadings of toughening agents (e.g., 5% to 12% by weight based on the total formulation).

[0012] China Patent No. 102964822(A) mentions that nylon is reinforced by using vinyl-PDMS with at least two vinyl groups as the reinforcement agent for nylon. Hydrogen silicone oil is also used as a cross-linking agent. Vinyl groups must be present in the PDMS to be cross-linked with hydrogen silicone oil.

[0013] CN111117223(A) refers to an automotive bearing material made from a nylon composite containing recycled nylon, where the second component polymer of parts 1-10 uses ultra-high molecular weight (Mw) PDMS with ultra-high Mw PE, PU, ​​ethylene-propylene copolymer, etc. The objective disclosed in CN111117223(A) is to reduce water adsorption of the nylon composite. CN111117223(A) does not mention improving impact strength or flowability or using PDMS to improve impact strength or flowability.

[0014] In view of the limitations regarding impact strength offered by known reinforced nylon compositions, it would be desirable to further improve the impact strength of reinforced nylon, especially at low temperatures, such as below -30°C, without adversely affecting other properties of the reinforced nylon, such as the flowability of the reinforced nylon, and without significantly increasing the manufacturing cost of the reinforced nylon.

[0015] It would further be desirable to provide new reinforced nylon compounds, materials or compositions having improved properties, such as increased toughness, by blending the appropriate components to form improved reinforced nylon compositions. Summary of the Invention

[0016] In one broad embodiment, the present invention relates to a reinforced polyamide composition comprising a blend of (a) at least one polyamide (e.g., a nylon compound), (b) at least one impact modifier, and (c) at least one liquid, low viscosity siloxane-based polymer to form a reinforced nylon composition such that the reinforced polyamide composition has improved impact strength properties.

[0017] In another embodiment, the reinforced polyamide composition of the present invention comprises component (a), which is at least one polyamide having a concentration of 50% to 98.99% by weight, component (b), which is at least one impact modifier composition having a concentration of 1% to 50% by weight, and component (c), which is at least one liquid, low viscosity siloxane-based polymer having a concentration of 0.01% to 10% by weight, based on the total weight of the reinforced polyamide composition.

[0018] In yet another embodiment, the present invention includes a method for preparing the above reinforced polyamide composition exhibiting improved impact strength properties (eg, at least a 10% increase).

[0019] In yet another embodiment, the present invention includes a method for producing the above reinforced nylon composition having improved impact strength properties.

[0020] In still yet another embodiment, the present invention includes articles made with the above reinforced polyamide compositions having improved impact strength properties.

[0021] In one or more other embodiments, the invention includes articles made using the reinforced nylon compositions described above, and methods for making the articles.

[0022] Additional features and advantages of embodiments of the invention are set forth in the detailed description that follows, and in part will be readily apparent to those skilled in the art from the description, or may be learned by practicing the embodiments described herein, including the detailed description and claims. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Temperatures herein are in degrees Celsius (°C).

[0024] "Room temperature (RT)" and / or "ambient temperature" herein means a temperature between 20°C and 26°C, unless otherwise specified.

[0025] An "elastomer" is a polymer that has viscoelastic properties (i.e., both viscous and elastic), weak intermolecular forces, generally a low Young's modulus, and a high strain at break compared to other materials. The IUPAC (International Union of Pure and Applied Chemistry) defines the term "elastomer" as "a polymer exhibiting rubber-like elasticity."

[0026] A "polymer" is a polymeric compound prepared by polymerizing monomers of the same or different types. Thus, the generic term polymer encompasses the terms "homopolymer" (used to refer to a polymer prepared from only one type of monomer, with the understanding that trace amounts of impurities may be incorporated into the polymer structure), and "interpolymer", which includes copolymers (used to refer to a polymer prepared from two different types of monomers), terpolymers (used to refer to a polymer prepared from three different types of monomers), and polymers prepared from more than three different types of monomers. Trace amounts of impurities, such as catalyst residues, may be incorporated in and / or within the polymer. It also encompasses all forms of copolymers, such as random, block, etc. Although polymers are often referred to as "made with" one or more specific monomers, "based on" a specific monomer or type of monomer, "containing" a specific monomer content, etc., it should be noted that in this context, the term "monomer" is understood to refer to the polymerized residue of a specific monomer, and not to the non-polymerized species. Generally, polymers are referred to herein in terms of "units" which are the polymerized form of the corresponding monomers.

[0027] The term "composition" refers to a mixture of materials that make up the composition, as well as reaction products and decomposition products formed from the materials of the composition.

[0028] By "nylon polymer composition" herein is meant a combination, mixture, or blend of at least one pure nylon polymer with at least one or more other components, such as elastomers, glass fibers, small molecule additives, etc. The types of blends used to blend the materials are generally, but are not limited to, proceeded by twin screw extrusion or immersion.

[0029] As used herein, "impact modifier" refers to an additive that is added to increase the flexibility, toughness, and impact strength of various plastic resins to meet the physical property requirements of hard parts.

[0030] The terms "impact toughness," "impact strength," and "impact resistance," as used herein with respect to nylon compositions, refer to the performance property of impact strength of a nylon composition as evaluated by the impact method set forth in CHARPY, ISO 179. The above terms may be used interchangeably.

[0031] "Room temperature (RT) impact strength" in reference to a nylon composition, as used herein, means the impact strength value of the nylon composition tested under room temperature conditions.

[0032] The terms "comprising," "including," "having," and their derivatives are not intended to exclude the presence of any additional components, steps, or procedures, whether or not they are specifically disclosed herein. For the avoidance of doubt, all compositions claimed through the use of the term "comprising" may include any additional additives, adjuvants, or compounds, whether polymeric or not, unless specifically stated to the contrary. In contrast, the term "consisting essentially of" excludes from the scope of any succeeding description any other component, step, or procedure, except those that are not essential to operability. The term "consisting of" excludes any component, step, or procedure not expressly delineated or listed. The term "or" refers to the listed members individually and in any combination, unless otherwise specified. The use of the singular includes the use of the plural, and vice versa.

[0033] Numerical ranges disclosed herein include all values ​​between the lower limit and the upper limit (inclusive). Ranges containing explicit values ​​(e.g., ranges 1, or 2, or 3-5, or 6, or 7) include any subranges between any two explicit values ​​(e.g., the range 1-7 above includes the subranges 1-2, 2-6, 5-7, 3-7, 5-6, etc.).

[0034] As used throughout this specification, the following abbreviations have the following meanings unless the context clearly dictates otherwise: "=" means "equal to" or "equal to", "<" means "less than", ">" means "greater than", "≦" means "less than or equal to", "≧" means "greater than or equal to", "@" means "at", μm = microns, g = grams, mg = milligrams, mW / m·K = milliwatts·Kelvin per meter, L = liters, mL = milliliters, g / mL = grams per milliliter, g / L = grams per liter, g / 10min = grams per 10 minutes, kg / m 3 = kilograms per cubic meter, ppm = parts per million by weight, pbw = parts by weight, rpm = revolutions per minute, m = meter, mm = millimeter, cm = centimeter, μm = micrometer, mm 2 / s = millimeters per second, min = minutes, s = seconds, ms = milliseconds, hr = hours, Pa = pascals, MPa = megapascals, Pa·s = pascal seconds, mPa·s = millipascal seconds, g / mol = grams per mole, g / eq = grams per equivalent, mg KOH / g = milligrams of potassium hydroxide per gram, Mn = number average molecular weight, Mw = weight average molecular weight, pts = parts by weight, 1 / s or second -1 = reciprocal of seconds [s -1 ], °C = degrees Celsius, mmHg = millimeters of mercury, psig = pounds per square inch, kPa = kilopascals, % = percent, vol% = volume percent, mol% = mole percent, and wt% = weight percent.

[0035] Unless otherwise specified, all percentages, parts, ratios, and other amounts are defined by weight. For example, all percentages set forth herein are weight percentages (wt %) unless otherwise indicated.

[0036] Specific embodiments of the present invention are described herein below. These embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the inventive subject matter to those skilled in the art.

[0037] In general, the present invention comprises reinforced polyamide (e.g., nylon) blends or compositions useful for producing nylon articles / products or parts for a variety of applications, particularly those applications requiring the nylon composition to have increased impact strength and flow properties.

[0038] In a broad embodiment, the reinforced polyamide composition of the present invention comprises a blend or mixture of (a) at least one polyamide (e.g., a nylon compound), (b) at least one toughening agent component, and (c) at least one liquid, low viscosity siloxane-based polymer to form a reinforced nylon composition such that the impact strength properties of the reinforced polyamide composition are improved.

[0039] The polyamide compound of the nylon composition, component (a), is a polymer containing repeating amide groups (R-CO-NH-R') as an integral part of the polymer backbone. The polyamide compound useful in the present invention may include one or more polyamide compounds. Suitable polyamide resins that can be used in the present invention include any polyamide known in the art. Polyamides useful in the present invention include, but are not limited to, for example, aliphatic, semi-crystalline, aromatic, semi-aromatic nylon resins, and mixtures thereof. Nylon resins are essentially those prepared from starting materials of lactams or diamines, aliphatic, semi-aromatic or aromatic dicarboxylic acids, and mixtures thereof. Suitable lactams useful in the present invention include, for example, caprolactam, laurolactam, and mixtures thereof. Suitable amines useful in the present invention include, for example, tetramethylenediamine; hexamethylenediamine (HMD); 2-methylpentamethylene-diamine; undecamethylenediamine; dodecamethylenediamine; 2.2.4-(2,4,4-trimethyl-hexamethylenediamine; 5-methylnonaethylenediamine; metaxylylenediamine (MXD); paraxylylenediamine; 2-methyl-1,5-pentamethylenediamine (MPMD); and mixtures thereof. Suitable dicarboxylic acids useful in the present invention include, for example, adipic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid (DDDA), terephthalic acid (TPA), isophthalic acid (IPA), 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid, 5-sodium-sulfoisophthalic acid, hexahydroterephthalic acid, hexahydroisophthalic acid, and mixtures thereof.

[0040] In the present invention, nylon homopolymers or copolymers derived from these starting materials are used either alone or in mixtures.Specific examples of polyamide resins that are desirable for use in the compositions of the present invention include the following: (nylon 6); polyundecaneamide (nylon 11); polylauramide (nylon 12); polyhexamethylene adipamide (nylon 66); polytetramethylene adipamide (nylon 46); polyhexamethylene sebacamide (nylon 610); polyhexamethylene dodecamide (nylon 612); polyhexamethylene terephthalamide (6T); polyhexamethylene isoterephthalamide (61); 2-methylpentamethylene terephthalamide (nylon DT); 2-methylpentamethylene isophthalamide (DI); polyhexamethylene terephthalamide / polycapramide copolymer (nylon 6T / 6); polyhexamethylene terephthalamide / polydodecanamide copolymer (nylon 6T / 12); polyhexamethylene adipamide / polyhexamethylene terephthalamide copolymer (nylon 66 / 6T); polyhexamethylene adipamide / polyhexamethylene isophthalamide copolymer (nylon 66 / 61); polyhexamethylene adipamide Polyhexamethylene adipamide / polyhexamethylene isophthalamide f-polycapramide copolymer (nylon 66 / 61 / 6); Polyhexamethylene adipamide / polyhexamethylene terephthalamide / -polyhexamethylene isophthalamide copolymer (nylon 66 / 6T / 61); Polyhexamethylene terephthalamide / polyhexamethylene isophthalamide copolymer (nylon 6T / 61); Polyhexamethylene terephthalamide / poly(2-methylpentamethylene) terephthalamide copolymer (nylon 6T / M5T); Polyhex polyhexamethylene terephthalamide f-polyhexamethylene sebacamide / polycapramide copolymer (nylon 6T / 610 / 6); polyhexamethylene terephthalamide / polydodecanamide / polyhexamethylene adipamide copolymer (nylon 6T / 12 / 66); polyhexamethylene terephthalamide / polydodecanamide / -polyhexamethylene isophthalamide copolymer (nylon 6T / 12 / 61); poly m-xylylene adipamide (nylon MXD6); and mixtures and copolymers of any of the above compounds.

[0041] In some preferred embodiments, the polyamide component, component (a), can be any polyamide for which impact strength is desired. For example, the polyamide component may be selected from the group consisting of: (ai) nylon-6; (aii) nylon-4,6; (aiii) nylon-6,6; (aiv) nylon-6,10; (av) nylon-6,9; (avi) nylon-6,12; (avii) nylon-7; (aviii) nylon-10; (aix) nylon-10,10; (ax) nylon-11; (axi) nylon-12; (axii) nylon-12.12; (aviii) 6T-12T; (axiv) 6I-12I; (axv) polyamides formed from 2-methylpentamethylenediamine and / or hexamethylenediamine and one or more acids selected from the group consisting of adipic acid, isophthalic acid, and terephthalic acid; (axvi) blends and / or copolymers of such nylons and polyamides; and (axvii) mixtures thereof.

[0042] In other preferred embodiments, the polyamide may be selected from the group consisting of nylon 6 (a polycaprolactam made from self-polymerizing caprolactam), nylon 6,6 (a hexamethylenediamine-adipic acid condensation product, which is a long chain synthetic polyamide with repeating amide groups in the polymer backbone), nylon 4, nylon 11, nylon 6,10; and combinations thereof.

[0043] In yet other preferred embodiments, the polyamide compounds useful in the present invention include nylon 6; nylon 6,6; and mixtures thereof.

[0044] In some embodiments, the polyamide component, component (a), can be selected from commercially available compounds, such as Ultramid series products (available from BASF). In other embodiments, some examples of commercially available polyamide compounds useful in the present invention can include, for example, Zytel 7304 NC010 (available from Dupont), PA6-YH800 (available from Yueyang Baling Shihua Chemical & Synthetic Fiber Co. Ltd.), and mixtures thereof.

[0045] The concentration of the polyamide component, component (a), can be 50% by weight to 98.99% by weight in one embodiment, 70% by weight to 92% by weight in another embodiment, and 75% by weight to 90% by weight in yet another embodiment.

[0046] The toughening agent component (b) (or impact modifier component) useful in the compositions of the present invention may be selected, for example, from maleic anhydride grafted polyolefin elastomers; amine or carboxylic acid functionalized polyolefins; ionomers comprising metal salts of carboxylic acid functionalized polyolefins; and mixtures thereof.

[0047] In some embodiments, the toughener component, component (b), is selected from the group consisting of, for example, (bi) at least one polymer consisting essentially of at least one polymerized unsaturated monomer selected from the class consisting of polymerized ethylene, at least one polymerized α-olefin having from 3 carbon atoms to 12 carbon atoms, and branched, linear, and cyclic compounds having from 4 carbon atoms to 14 carbon atoms; (bii) unsaturated monomers selected from the class consisting of α,β ethylenically unsaturated dicarboxylic acids having from 3 carbon atoms to 8 carbon atoms and derivatives thereof selected from the class consisting of monoesters of alcohols having from 1 carbon atom to 29 carbon atoms, anhydrides of dicarboxylic acids, metal salts of dicarboxylic acids, and monoesters of said dicarboxylic acids having from 0% to 100% of the carboxylic acid groups ionized by neutralization with a metal ion; and (biii) a mixture of the above components (bi) and (bii).

[0048] In some embodiments, the toughening agent component (also referred to as "impact modifier"; component (b)) comprises maleic anhydride functionalized elastomeric ethylene copolymers, maleic anhydride functionalized ethylene, alpha-olefin copolymers, terpolymers of ethylene, acrylic esters and maleic anhydride, maleic anhydride (MAH) grafted polyolefin elastomers (POE), and combinations thereof. In one preferred embodiment, the toughening agent component, component (b), is maleic anhydride grafted polyolefin elastomer (POE-g-MAH).

[0049] In some embodiments, the toughener component can be selected from commercially available compounds such as, but not limited to, Exxelor series products (available from ExxonMobil); Tafmer series products (available from Mitsui Chemicals, Inc.); and mixtures thereof.

[0050] The toughening agent component (b) may be further characterized as having a predetermined MAH graft ratio, melt index, molecular weight, molecular weight distribution, and / or branching before the toughening agent component is mixed with the nylon component (a) and the PDMS component (c). For example, the toughening agent component has an MAH graft ratio of 0.1 to 5 in one embodiment, 0.2 to 2.0 in another embodiment, and 0.3 to 1.0 in yet another embodiment. For example, the impact modifier has a density of 0.8 g / cc to 0.95 g / cc in one embodiment, 0.83 g / cc to 0.93 g / cc in another embodiment, and 0.85 g / cc to 0.92 g / cc in yet another embodiment.

[0051] The concentration of the toughening (impact modifier) ​​compound, component (b), used to prepare the nylon composition of the present invention includes, for example, from 1 wt % to 50 wt % in one embodiment, from 8 wt % to 35 wt % in another embodiment, and from 10 wt % to 25 wt % in yet another embodiment, based on the weight of the nylon composition.

[0052] In some embodiments, the siloxane-based component, component (c), can include, for example, disiloxanes, trisiloxanes, polydimethylsiloxanes (PDMS), and mixtures thereof.

[0053] In one embodiment, the siloxane-based component is PDMS. Several types of PDMS, including carbinol-functionalized PDMS, carboxyl-functionalized PDMS, amino-functionalized PDMS, and non-functionalized PDMS, have been found to be useful in the present invention, i.e., the above selected types of PDMS provide significant improvements in the impact strength of reinforced nylon. In some embodiments, the PDMS may contain one or more functional groups, such as carbon groups, including hydroxyl, amino, epoxy, carboxyl, mercapto groups, and mixtures thereof. In some embodiments, the functional groups in the polydimethylsiloxane are at the end of the polydimethylsiloxane chain or on the side of the polydimethylsiloxane chain. Examples of suitable non-functionalized PDMS useful in the present invention include any one or more of the XIAMETER™ PMX-200 series products manufactured by The DOW Chemical Company.

[0054] PDMS with different molecular weights (Mw; as determined by viscosity) have also been found to provide improved impact strength for reinforced nylon compositions. Amino-functionalized PDMS also provide additional benefits related to flow properties, such as reduced capillary viscosity.

[0055] In some embodiments, the siloxane-based component (PDMS) used in the present invention can be selected from commercially available compounds such as XIAMETER™ PMX-200 (available from The Dow Chemical Company); KF series products (available from SHIN-ETSU Co. Ltd.); and mixtures thereof. In one embodiment, the non-functionalized PDMS useful in the present invention includes commercially available products available from The Dow Chemical Company. In another embodiment, the functionalized PDMS useful in the present invention is commercially available products available from SHIN-ETSU Co. Ltd. Without being limited thereto, the PDMS is used in liquid form as opposed to solid or pellet form.

[0056] In some embodiments, the viscosity of the siloxane-based component is in one typical embodiment 1 mm2 / s~100,000mm 2 / s, in another embodiment 3 mm 2 / s~90,000mm 2 / s, and in yet another embodiment, 5 mm 2 / s~80,000mm 2 / s.

[0057] The concentration of the siloxane-based component, component (c), can be from 0.01% to 10% by weight in one embodiment, from 0.1% to 8% by weight in another embodiment, and from 0.2% to 5% by weight in yet another embodiment, based on the nylon composition.

[0058] In some embodiments, the reinforced polyamide composition of the present invention may further comprise one or more optional components, additives or other pharmaceutical compounds, if desired. Optional compounds, component (d), useful in the reinforced polyamide composition of the present invention may include, for example, fillers, lubricants, plasticizers, pigments, dyes, antioxidants, stabilizers, nucleating agents, flame retardants, blowing agents, and mixtures thereof.

[0059] Generally, the concentration of the optional compounds when used in the reinforced polyamide composition includes, for example, from 0 wt. % to 50 wt. % in one embodiment, from 0.01 wt. % to 50 wt. % in another embodiment, from 0.1 wt. % to 40 wt. % in yet another embodiment, and from 0.1 wt. % to 30 wt. % in yet another embodiment.

[0060] In one typical embodiment, the reinforced nylon composition comprises: (a) at least one polyamide (e.g., a nylon compound); (b) at least one toughening agent component; and (c) 1 mm 2 / s~100,000mm 2 The nylon composition may be prepared by combining, blending, or mixing the nylon composition with at least one liquid, low viscosity siloxane-based polymer having a viscosity of about 100 / s. The resulting mixture forms a reinforced nylon composition that exhibits improved impact strength properties.

[0061] As an illustration of one embodiment of the present invention, and not by way of limitation, a general method for making the reinforced nylon composition of the present invention comprises mixing, combining or blending (a) at least one polyamide at a concentration of 50% to 98.99% by weight based on the weight of the reinforced nylon composition; (b) at least one toughening agent at a concentration of 1% to 50% by weight based on the weight of the reinforced nylon composition; (c) at least one siloxane-based polymer at a concentration of 0.01% to 10% by weight based on the weight of the reinforced nylon composition; and (d) any optional components, optionally at a concentration of less than 50% by weight based on the weight of the reinforced nylon composition.

[0062] In some embodiments, the method of the present invention for preparing a reinforced polyamide composition exhibiting improved toughness comprises melt mixing, in one step, component (a), which is a polyamide, component (b), which is a toughening agent, and component (c), which is a siloxane-based polymer, at a predetermined temperature and for a predetermined time. The one-step melt mixing process can be carried out at a melt temperature of 200°C or higher in one embodiment, 200°C to 350°C in another embodiment, 220°C to 320°C in another embodiment, and 250°C to 300°C in yet another embodiment. The duration of the one-step melt mixing process can be greater than 20 seconds in one embodiment, 20 seconds to 10 minutes in another embodiment, and 30 seconds to 5 minutes in yet another embodiment. In one embodiment, the above melt mixing one-step process can be carried out in at least one extruder, such as a conventional twin-screw (at least two screws) extruder.

[0063] In another embodiment, the method of the present invention for preparing a reinforced polyamide composition exhibiting high flow and toughness can include at least two steps: (I) a first step of mixing at least two components: (α) the above-mentioned toughening agent component (b), such as POE-g-MAH; and (β) the above-mentioned siloxane-based polymer component (c), such as PDMS, at a predetermined temperature and for a predetermined time to form a blended composite component (i.e., to form a toughening agent / siloxane-based polymer mixture); and (II) a second step of melt mixing (γ) the above-mentioned polyamide component (a), and (δ) the blended composite component from step (I) to form a reinforced polyamide composition.

[0064] The first mixing step (I) can be carried out, for example, by immersing or blending components (b) and (c) together, and then mixing the immersed or blended components, for example, using at least one twin-screw extruder. When the immersion method is used for the first mixing step (I), the temperature of the first mixing step (I) can be less than 60°C in one embodiment, 0°C to 60°C in another embodiment, and 10°C to 55°C in yet another embodiment. When the immersion method is used, the time of the first mixing step (I) can be more than 1 hour in one embodiment, 1 hour to 48 hours in another embodiment, and 2 hours to 24 hours in yet another embodiment.

[0065] When the blending method is used in the first melt-mixing step (I), the first melt-mixing step (I) can be carried out at a temperature of more than 100° C. in one embodiment, from 100° C. to 200° C. in another embodiment, and from 120° C. to 180° C. in yet another embodiment. When the blending method is used, the time for the first mixing step (I) can be more than 1 second in one embodiment, from 20 seconds to 10 minutes in another embodiment, and from 30 seconds to 5 minutes in yet another embodiment.

[0066] When the immersion method is used for the first mixing step (I), the temperature of the second melt mixing step (II) may be more than 200°C in one embodiment, 230°C to 350°C in another embodiment, and 250°C to 300°C in yet another embodiment. The time of the melt mixing second step (II) may be more than 1 second in one embodiment, 20 seconds to 10 minutes in another embodiment, and 30 seconds to 5 minutes in yet another embodiment. In one embodiment, the above melt mixing second step (II) may be carried out in at least one extruder, such as a conventional twin screw (at least two screws) extruder.

[0067] When a compounding method is used for the first mixing step (I), the melt mixing step (II) can be carried out at a temperature and for a time that can be the same as the first mixing step (I).

[0068] In another embodiment, a method for preparing a reinforced polyamide composition exhibiting high toughness can include at least three steps: (A) a first step of melt mixing at least two components: (α) at ​​least one toughening agent component (b), such as POE-g-MAH; and (β) at least one siloxane-based component, such as a siloxane-based polymer, such as PDMS, to form a toughening agent / siloxane-based polymer mixture; (B) a second step of pelletizing the toughening agent / siloxane-based polymer mixture from step (A) to form a plurality of composite pellets; and (C) a third step of melt mixing at least two components: (γ) at least one polyamide; and (ε) a plurality of composite pellets from step (B) to form a reinforced polyamide composition. In one embodiment, the third step (C) of melt mixing can be carried out in at least one extruder, such as a conventional twin-screw (at least two screws) extruder.

[0069] The temperature of the first melt-mixing step (A) may be less than 200° C. in one embodiment, 100° C. to 200° C. in another embodiment, and 120° C. to 180° C. in yet another embodiment. The mixing time of the first melt-mixing step (A) may be more than 1 second in one embodiment, 20 seconds to 10 minutes in another embodiment, and 30 seconds to 5 minutes in yet another embodiment.

[0070] The pelletizing step (B) is carried out using conventional equipment such as a strand cutter to cut the resin exiting the extruder into pellets of a desired size.

[0071] The temperature of the third melt-mixing step (C) may be, in one embodiment, above 200° C., in another embodiment, from 230° C. to 350° C., and in yet another embodiment, from 250° C. to 300° C. The time of the third melt-mixing step (C) may be, in one embodiment, above 1 second, in another embodiment, from 20 seconds to 10 minutes, and in yet another embodiment, from 30 seconds to 5 minutes.

[0072] The embodiments of the inventive process for preparing a reinforced polyamide composition and its steps as described above can be carried out by conventional equipment known to those skilled in the art, for example, mixing of the components to form a uniform or homogeneous mixture can be carried out by known blenders or mixers such as twin screw extruders, BUSS kneaders, batch mixers, and the like.

[0073] As discussed above, the reinforced polyamide composition of the present invention comprises (a) at least one polyamide (e.g., a nylon compound); (b) at least one toughening agent component (e.g., POE-g-MAH); and (c) 1 mm 2 / s~100,000mm 2The reinforced polyamide composition of the present invention includes a mixture of at least one liquid low-viscosity siloxane-based polymer (e.g., PDMS) having a viscosity of 100000000000 / s. The reinforced polyamide composition of the present invention exhibits several advantageous advantages. For example, when a polyamide is mixed with POE-g-MAH and PDMS, the resulting reinforced polyamide composition advantageously exhibits enhanced room temperature impact strength. In addition, in some cases, the flowability of the reinforced polyamide composition (nylon composition) of the present invention can also be improved. Thus, the combination of at least one nylon, at least one POE-g-MAH and at least one PDMS forms a reinforced polyamide composition of the present invention having at least increased impact strength. In addition, the impact properties of the reinforced polyamide composition of the present invention can be improved when the polyamide is blended with POE-g-MAH and PDMS to form a reinforced nylon composition, while other mechanical performances of the reinforced nylon composition, such as flexural modulus, tensile strength, elongation, heat distortion temperature (HDT), etc., are maintained at an optimized level.

[0074] For example, in one typical embodiment, a reinforced polyamide composition containing a toughener component (e.g., POE-g-MAH) and a siloxane-based polymer (e.g., PDMS) advantageously exhibits at least a 10% improvement (e.g., increase) in impact strength at room temperature (RT) or at temperatures below -30°C, as compared to a nylon composition containing a toughener component (e.g., POE-g-MAH) of the present invention but not a siloxane-based polymer (e.g., PDMS). In another embodiment, a reinforced polyamide composition of the present invention comprising the toughener component and a siloxane-based polymer exhibits at least a 15% improvement in impact strength as compared to a polyamide composition containing the toughener component but not a siloxane-based polymer of the present invention; in yet another embodiment, a reinforced polyamide composition of the present invention comprising the toughener component and a siloxane-based polymer of the present invention exhibits at least a 20% improvement in impact strength as compared to a polyamide composition containing the toughener component but not a siloxane-based polymer of the present invention. In yet another embodiment, the reinforced polyamide composition of the present invention comprising the toughening agent component and the siloxane-based polymer of the present invention exhibits a 10% to 100% improvement in impact strength compared to a polyamide composition containing the toughening agent component but not the siloxane-based polymer of the present invention.

[0075] Surprisingly, it has been found that the above improvements to the RT / low temperature impact strength of the reinforced polyamide composition of the present invention can be achieved by adding only small amounts (e.g., less than 5 wt%) of PDMS to the reinforced nylon composition. For example, low loadings (e.g., 0.4 wt% to 2 wt% based on the total weight of the reinforced polyamide formulation) of PDMS together with POE-g-MAH form an impact modifier effective in improving the RT / low temperature impact strength of the reinforced polyamide composition of the present invention, compared to high loadings, e.g., 20 wt% to 80 wt% of PDMS required by compositions known in the art. Also, the molecular weight of the PDMS used in the prior art is greater than the molecular weight (determined by measuring the viscosity) of the PDMS used in the present invention. In the present invention, the reinforced polyamide composition does not require a specific molecular weight of PDMS. However, in one preferred embodiment, a 1 mm PDMS is added to improve the impact strength of the composition of the present invention. 2 / s~100,000mm 2 A PDMS with a measured viscosity in the range of 1 / s is desirable.

[0076] Another advantage of the nylon composition of the present invention is that the nylon composition can be used to make lighter weight articles / products or parts that have thinner walls and use less composition because of the above-mentioned improved properties of impact strength (e.g., at RT and low temperatures) while maintaining the flexural modulus of the composition.

[0077] Articles / products or parts made from the reinforced nylon compositions of the present invention can include, for example, electronic devices, automotive parts, gear, toys, and the like.

[0078] Once the components of the reinforced nylon composition of the present invention: (a) at least one polyamide (e.g., nylon compound), (b) at least one toughening agent component, and (c) at least one siloxane-based polymer are thoroughly and uniformly mixed, e.g., at melt mixing temperatures, the resulting molten mixture can be used to form an article / product or molded part using conventional methods and equipment. For example, an article / product or molded part can be formed from the reinforced nylon composition using methods such as injection molding, extrusion, or blow molding methods.

[0079] In one preferred embodiment, the article / product or molded part is produced and processed using, for example, an injection molding process and an extrusion device such as a twin screw extruder. In general, a method for producing an article from the reinforced polyamide composition of the present invention includes, for example, (1) providing a reinforced polyamide composition by combining (a) at least one polyamide, (b) at least one toughening agent component, and (c) at least one siloxane-based polymer using any one of the methods for producing a reinforced polyamide composition described above, and (2) processing the composition of step (1) into an article using, for example, an extrusion or injection process to form the article.

[0080] In order to create thinner and therefore lighter parts, it is necessary for the nylon composition to have high impact strength. The nylon composition of the present invention can exhibit improved impact strength (or toughness) by using appropriate components (a)-(c) to form the reinforced nylon composition of the present invention while maintaining other properties of the composition such as flexural modulus. Such high performance properties of the reinforced nylon composition allow for downgauging of interior and exterior parts and articles requiring superior impact properties made from the reinforced nylon composition of the present invention.

[0081] The impact modifier additive, the reinforced nylon composition, and the articles, products or parts made from the reinforced nylon composition described above can be used in a wide range of polymer compositions and structures. In general, the reinforced nylon composition of the present invention is used in applications that require parts with higher impact strength (i.e., increased toughness and durability) than parts made from conventional copolymers. For example, but not limited to, the reinforced nylon composition can be used in a variety of applications and can be formed into molded articles useful in areas requiring impact resistance and strength. In one embodiment, for example, the reinforced nylon composition can be used in automotive applications to make rigid parts and components for automobiles. The automotive products can be manufactured by conventional polymer processing. EXAMPLES

[0082] The following inventive examples (Inv. Ex.) and comparative examples (Comp. Ex.) (collectively "Examples") are presented herein to more fully illustrate the features of the present invention, but are not intended to be construed, either explicitly or implicitly, as limiting the scope of the claims. Inventive examples are identified by Arabic numerals, and comparative examples are represented by alphabetical letters. The following experiments analyzed the performance of embodiments of the compositions described herein. Unless otherwise indicated, all parts and percentages are by weight based on total weight.

[0083] raw materials The raw materials (ingredients) used in the examples to prepare the reinforced nylon composite formulations included PA6 B3s, polyamide nylon (available from BASF); and POE-g-MAH1 (0.50 wt% MAH graft level) and POE-g-MAH2 (0.90 wt% MAH graft level), maleic anhydride grafted polyolefin elastomers. POE-g-MAH1 had a melt index (MI) of 1.6 g / 10 min and POE-g-MAH2 had an MI of 1.3 g / 10 min as measured by ASTM D1238 at 190° C. with a load of 2.16 kg. The PDMS materials used in the examples are listed in Table I.

[0084] [Table 1]

[0085] compound The reinforced nylon composite formulations used in the examples were made based on the formulations set forth in Tables II and III for the Series 1 experiments and Tables IV and V for the Series 2 experiments.

[0086] [Table 2] Notes about Table II: * The amount of PDMS is based on the total weight of the nylon composition.

[0087] [Table 3] Notes for Table III: * The amount of PDMS is based on the total weight of the nylon composition.

[0088] [Table 4] Notes to Table IV: * The amount of PDMS is based on the total weight of the nylon composition.

[0089] [Table 5] Notes for Table V: * The amount of PDMS is based on the total weight of the nylon composition.

[0090] In general, the reinforced nylon composite formulations described in Tables II-V were prepared by a first step of blending the PDMS component with the POE component, followed by a second step of mixing the blended PDMS / POE component with the nylon component.

[0091] The first step of blending the PDMS component with the POE component is performed by utilizing either a dipping procedure or a compounding procedure as described herein below.

[0092] Immersion method for blending PDMS with POE PDMS including PDMS of KF-6000 (Inventive Examples 1-3 and Inventive Example 21), KF-6001 (Inventive Examples 4 and 5); KF-8010 (Inventive Examples 6 and 7); X-22-161A (Inventive Examples 8 and 9); X-22-162C (Inventive Examples 10 and 11); PMX-200 Fluid 10 cSt (Inventive Examples 12-14 and Inventive Example 22), PMX-200 Fluid 20 cSt (Inventive Examples 15-16 and Inventive Examples 23 and 24) and PMX-200 Fluid 100 cSt (Inventive Example 17 and Inventive Example 25) were blended with POE pellets by the immersion method. PDMS was first mixed with POE at room temperature, and then PDMS was allowed to soak, i.e., permeate, into the body of the POE pellets. 400g of POE pellets were first placed in a 2L plastic container, and then PDMS was added to the container according to the weight percentages in Tables II and III. The container with the mixture of POE pellets and PDMS was shaken by hand in different directions (up and down and left and right with similar frequency) for 5 minutes. The shaking was stopped, the container was turned on its side, and the container was allowed to stand for 5 minutes. The shaking and turning of the container was repeated six times, and then kept at room temperature for another 3 hours. Alternatively, PDMS can be premixed with POE at room temperature, then placed in an automatic shaker and shaken in the automatic shaker at 60°C and 85 rpm for 4 hours to 12 hours.

[0093] Formulation method for blending PDMS with POE PDMS containing PMX-200 Fluid 1K cSt PDMS (Inventive Example 18, and Inventive Examples 26 and 27); PMX-200 Fluid 1K cSt (15%) (Inventive Examples 28-30); PMX-200 Fluid 10K cSt (Inventive Example 19); PMX-200 Fluid 60k cSt (Inventive Example 20); and DOWSIL™ SGM 15 GUM (Comparative Examples B and C) were each blended with POE pellets by twin-screw extruder compounding method. Before feeding the blend into the extruder, PDMS was first blended with POE, and then the blend was fed into the extruder. The extruder used had the following conditions / parameters:

[0094] The equipment used was a ZSK-18 twin screw extruder; the power of the extruder was 19.2 KW; the diameter D of the extruder was D=18 mm; the L / D ratio of the extruder was L / D=48; the temperatures of the various zones of the extruder barrel were set as follows: zone 1=60°C, zone 2=90°C, zone 3=120°C, zone 4=120°C, zone 5=120°C, zone 6=120°C, and zone 7=110°C, in the range of RT-150°C; the screw speed of the extruder was 300 rpm, and the feeding rate of the blended material to the extruder was 5-12 kg / h.

[0095] After the compounding process of PDMS and POE in a twin-screw extruder, the resulting PDMS / POE compound blend was cut into pellets with a diameter of 0.5 mm-1 mm and a length of 2 mm-5 mm.

[0096] Compounding PDMS / POE blends into nylon The nylon samples were first dried in a dehumidifier at 120°C for at least 4 hours. The blended PDMS / POE pellets produced using the methods described above: "Soaking Method for Blending PDMS with POE" or "Compounding Method for Blending PDMS with POE" were then blended with the dried nylon samples by compounding the PDMS / POE pellets and nylon samples in an extruder. The extruder used was the same extruder used for blending PDMS with POE by compounding as described above. The extruder conditions / parameters for compounding the PDMS / POE pellets and nylon samples were as follows: the extruder barrel temperatures were set as follows, in the range of RT to about 350°C: Zone 1 = 150°C, Zone 2 = 195°C, Zone 3 = 260°C, Zone 4 = 260°C, Zone 5 = 260°C, Zone 6 = 260°C, Zone 7 = 250°C; the extruder screw speed was 250 rpm, and the feed rate of the blended material to the extruder was 8-10 kg / hr.

[0097] After compounding the PDMS / POE pellets and nylon samples, the resulting compound containing a blend of PDMS, POE and nylon was cut into pellets with diameters of 0.5 mm to 1 mm and lengths of 2 mm to 5 mm.

[0098] Test Method The following test methods and measurement procedures were used to test the reinforced nylon compositions and test specimens prepared from the reinforced nylon compositions according to the following methods.

[0099] Capillary Viscosity Test The compounded nylon / POE samples were first dried in a dehumidifier at 120°C for at least 4 hours, and after drying the compounded samples, the compounded samples were sealed in aluminum bags under vacuum. The moisture content in the compounded nylon / POE samples was tested by the so-called Karl Fischer method using an 874 Oven Sample Processor (available from Thermo-Fisher Co.Ltd.). It is recommended that the moisture in the compounded nylon / POE samples be less than 1,000 ppm before testing the samples using the capillary viscosity test. The capillary rheometer instrument used for the capillary viscosity test was a Gottfert rheograph 26 (available from Gottfert Inc.). The test temperature used for the capillary viscosity test was 260°C. The length of the capillary used was 30 mm, and the diameter of the capillary was 1 mm. The shear rates used for the tests ranged from 90 1 / s to 7,000 1 / s. Tabulated data on viscosity are reported at a shear rate of 770 1 / s.

[0100] Injection molding method The compounded nylon / POE pellets were first dried in a dehumidifier at 120°C for at least 4 hours, and then the pellets were subjected to injection molding. An injection molding machine Fanuc Roboshot S-2000i100BH (available from Fanuc) was used for the injection molding process. The compounded samples were subjected to injection molding to produce test specimens, and impact tests were performed on the test specimens using the impact strength test described herein below. The parameters of the injection molding machine and process were as follows: the barrel temperature of the injection screw was set at 250°C-260°C, the cooling temperature was 190°C, the cooling time was 15 seconds, the injection speed was 30 mm / sec, and the injection pressure was 200 MPa.

[0101] Impact Strength Test The impact strength test method used to test the impact performance of the specimens prepared in the examples is described in CHARPY, ISO 179 ("ISO" stands for "International Organization for Standardization"). CHARPY, ISO 179 specifies a method for determining the Charpy impact strength of plastics under defined conditions. The specimens used in this test are flat specimens made from the formulations in Tables II to V and have the following dimensions: 80 mm length x 10 mm width x 4 mm thickness. CHARPY, ISO 179 defines a method used to determine the resistance of plastics to fracture when impacted in a three-point bending configuration using a pendulum system with an appropriately sized hammer arm. The test is uninstrumented and is used to determine the energy required to break the specimen. The different test parameters are specified according to the type of material the specimens are made of as well as the type of notch cut in the specimens being tested.

[0102] In the examples described herein, the following general procedure was followed: All specimens were notched with a radius of 2 mm. Before testing the specimens, all specimens were first dried in a dehumidifier at 120° C. for 4 hours. The specimens were then equilibrated in the humidifier at room temperature for 2 days.

[0103] Each specimen to be tested was mounted horizontally in a pendulum impact tester and supported free at both ends. The hammer of the tester was released and allowed to penetrate the specimen. If no breakage occurred with the first hammer arm used, successively heavier hammers were used until breakage occurred. At breakage, the energy obtained and the type of breakage were then recorded.

[0104] The impact test conditions used were as follows: 4 Joule pendulum capacity and specimen conditioning at room temperature for ≧6 hours or in a freezer at −30° C. and / or −40° C. for ≧6 hours. The specimens in the freezer were removed from the freezer and impact tested within 5 seconds. The test conditions were room temperature (i.e., a temperature of 23° C.±2° C.) and 50% RH±10% RH.

[0105] Test results Viscosity results for the reinforced nylon compounds were obtained by performing the Capillary Viscosity Test described above; the viscosity results for Series 1 experiments are set forth in Table VI; and the viscosity results for Series 2 experiments are set forth in Table VII. Normalized capillary viscosity results were calculated by dividing the capillary viscosity value of the sample by the capillary viscosity value of the particular comparative example shown in the column heading of the table below, and then multiplied by 100 to convert to a percentage. Normalized Izod impact results were also calculated by dividing the Izod impact value of the sample by the Izod impact value of the particular comparative example shown in the column heading of the table below, and then multiplied by 100 to convert to a percentage.

[0106] [Table 6] Notes to Table VI: (1) A lower viscosity is better and desirable.

[0107] [Table 7] Notes for Table VII: (1) A lower viscosity is better and desirable.

[0108] The impact strength results for the injection molded specimens made from the reinforced nylon compounds were obtained by conducting the above-described impact strength tests on the injection molded specimens prepared according to the above-described injection molding method. The impact strength results for the Series 1 experiments are listed in Table VIII, and the impact strength results for the Series 2 experiments are listed in Table IX.

[0109] [Table 8] Notes for Table VIII: (1) Higher flexural modulus values ​​are better or not significantly reduced compared to the control; these values ​​are desirable.

[0110] [Table 9]

[0111] Discussion of results In series 1 experiments, different types of PDMS (carbinol, amino, carboxyl and non-functionalized) were soaked in POE-g-MAH1 with different PDMS loadings. The PDMS soaked POE was then blended with PA6 B3s (a medium viscosity polyamide nylon (nylon 6) available from BASF). The capillary viscosity properties of the blends in series 1 experiments are listed in Table VI, and the impact strength properties of the specimens made from the blends are listed in Table VIII.

[0112] When comparing the inventive reinforced polyamide compositions with control formulations, such as reinforced polyamide nylon PA6 B3s reinforced with toughening agent POE-g-MAH1, all of the inventive examples showed significant improvement over room temperature impact strength properties of the reinforced polyamide compositions containing PDMS. Samples of the inventive reinforced polyamide compositions reinforced with POE and containing PDMS additive also showed significant improvement in impact strength properties at low temperatures of -30°C. In addition, the inventive examples showed maintained or improved flexural modulus performance over the comparative examples.

[0113] The results support the conclusion that PDMS additives can significantly improve the reinforcement efficiency of POE. Furthermore, there is no significant difference in impact strength whether the PDMS is functionalized or not. Also, the viscosity of PDMS (correlated to molecular weight) did not show a significant difference in impact strength at room temperature for the reinforced polyamide compositions, however, higher viscosity PDMS (correlated to higher molecular weight PDMS) showed less improvement in impact strength at -30°C for the reinforced polyamide compositions. For example, comparing the −30° C. impact strength of reinforced polyamide compositions containing PDMS, PMX-200 fluid 10 cSt to PMX-200 fluid 100 cSt (inventive examples 12-17) with the −30° C. impact strength of reinforced polyamide compositions containing PDMS, PMX-200 fluid 1k cSt and PMX-200 fluid 10 k cSt (inventive examples 18 and 19), the higher viscosity PMX-200 fluid PDMS (meaning higher Mw PMX-200 fluid PDMS) has much less improvement on the −30° C. impact strength of the reinforced polyamide compositions. It should be noted that in the series 1 experiment, PMX-200 fluid 1k cSt and PMX-200 fluid 10 k cSt PDMS have high Mw properties, so these two PDMS samples cannot be immersed in POE. These two PDMS samples were first blended with POE under 100° C. using a blending method instead of the immersion method.

[0114] In addition to impact strength, the amino and carboxyl PDMS showed a significant reduction in capillary viscosity. Tables VI and VII list the capillary viscosity of PDMS at 770-s (a typical shear for capillary viscosity testing). The results show that about a 30% reduction in the viscosity of PDMS occurs. The amines or organic acids can improve the flow properties of the reinforced nylon composition.

[0115] In series 2 experiments, various PDMS were mixed with POE-g-MAH2 with different PDMS loadings. The capillary viscosity properties of the formulations in series 2 experiments are listed in Table VII, and the impact strength properties of the specimens made from the formulations are listed in Table IX. The results in Table IX show the same improvement in impact strength at room temperature and at temperatures of -30°C. Formulations with 15% POE loading were also examined, and the improvement trend is the same. For formulations with too high PDMS loading (e.g., 10% PDMS in POE), the results show a decrease in impact strength at room temperature compared to formulations with 2% to 5% PDMS loading. Unexpectedly, it was found that the results of the PDMS loading in the reinforced polyamide composition can affect the improvement in impact strength, and therefore, a proper selection of the PDMS loading is necessary to provide the desired impact strength of the reinforced polyamide composition.

Claims

1. 1. A reinforced polyamide composition comprising: (a) at least one polyamide; (b) at least one toughening agent component; and (c) a 1 mm thick polyamide composition having increased impact strength; 2 / s~100,000mm 2 and at least one siloxane-based component having a viscosity of about 1 / s.

2. 2. The reinforced polyamide composition of claim 1, wherein the functionalized polar end groups in the at least one siloxane-based component comprise hydroxyl groups; amino groups; epoxy groups; carbonyl groups; mercapto groups, and mixtures thereof.

3. 10. The reinforced polyamide composition of claim 1, wherein the non-functionalized non-polar end groups in the at least one siloxane-based component comprise allyl groups; alkyl groups; and mixtures thereof.

4. 2. The reinforced polyamide composition of claim 1, wherein the concentration of the at least one polyamide, component (a), is from 50% to 98.99% by weight, the concentration of the at least one toughener component, component (b), is from 1% to 50% by weight, and the concentration of the at least one siloxane-based component is from 0.01% to 10% by weight, based on the total weight of the reinforced polyamide composition.

5. 2. The reinforced polyamide composition of claim 1, wherein the polyamide component (a) is selected from the group consisting of: (ai) nylon-4,6; (ai) nylon-6,6; (aiii) nylon-6,10; (aiv) nylon-6,9; (av) nylon-6,12; (avi) nylon-11; (avii) nylon-12; (aviiii) 6T-12T; (aix) 6I-12I; (ax) polyamides formed from 2-methylpentamethylenediamine and / or hexamethylenediamine and one or more acids selected from the group consisting of adipic acid, isophthalic acid, and terephthalic acid; and (axi) blends and / or copolymers of the nylons and the polyamides.

6. 10. The reinforced polyamide composition of claim 1, wherein the reinforced polyamide composition exhibits at least a 10 percent increase in impact strength compared to a polyamide composition that does not contain the at least one siloxane-based component.

7. 2. The reinforced polyamide composition of claim 1, wherein the composition comprises up to 50 weight percent, based on the composition, of a component selected from the group consisting of fillers, lubricants, plasticizers, pigments, dyes, antioxidants, stabilizers, nucleating agents, flame retardants, blowing agents, and combinations thereof.

8. 1. A method for preparing a reinforced polyamide composition exhibiting high flow and toughness, comprising the steps of: (a) at least one polyamide; (b) at least one toughening agent component; and (c) a 1 mm thick polyamide composition having increased impact strength; 2 / s~100,000mm 2 and at least one siloxane-based component having a viscosity of 100 / s in a single step at a predetermined temperature and for a predetermined time, said melt mixing of components (a)-(c) being carried out at a temperature above 200° C.

9. 1. A method for preparing a reinforced polyamide composition exhibiting high flow and toughness, comprising the steps of: (I) A method for mixing the following two components at a temperature of less than 60° C.: (α) at ​​least one toughening agent component; (β) mixing at least one siloxane-based component to form a blend composite component; (II) At a temperature above 200° C., the following two components: (γ) at least one polyamide; and (ε) melt mixing said blend composite components from step (I) to form a reinforced polyamide composition having increased impact strength.

10. 1. A method for preparing a reinforced polyamide composition exhibiting high flow and toughness, comprising the steps of: (A) a mixture of two components at a temperature above 100° C.: (α) at ​​least one toughening agent component; (β) melt mixing at least one siloxane-based component to form a blend composite component; (B) pelletizing the blended composite components from step (A) to form a plurality of composite pellets; (C) At a temperature above 200° C., the following two components: (γ) at least one polyamide; (ε) melt mixing the plurality of composite pellets from step (B) to form a reinforced polyamide composition having increased impact strength.

11. 10. An article made from the reinforced polyamide composition of claim 1.

Citation Information

Patent Citations

  • Super-flexible PA6 (Polyamide 6) composite material for automobile bottom plate blank cap and preparation method thereof

    CN108178922A

  • Ultralow-temperature-resistant nylon toughening agent, preparation method and applications thereof

    CN110591100A

  • Resin composition

    JP1992175370A

  • Antistatic resin composition excellent in mold releasability

    JP1998310713A

  • Polyamide composition for sliding member and sliding member composed of the same

    JP2002363403A